Laminated glass and vehicle

By adopting a laminated glass structure in automotive glass and using nanoreflective layer or micro-absorbing layer to shield UV rays, the problem of performance degradation of polymer network liquid crystals and dye liquid crystals under ultraviolet light is solved, achieving higher UV resistance and longer Service life.

CN118915349AActive Publication Date: 2024-11-08FUYAO GLASS IND GROUP CO LTD

Patent Information

Application Number
CN202411119935.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-08
Estimated Expiration
2044-08-15

AI Technical Summary

Technical Problem

Polymer network liquid crystals (PNLC) and dye liquid crystals (DDLC) have poor resistance to UV rays in applications, resulting in their performance deterioration or color changes under long-term ultraviolet irradiation, especially in automotive glass applications. Effect.

Method used

A laminated glass structure is adopted, including an outer glass plate, a first ultraviolet shielding layer, a first thermoplastic polymer layer, a dimming layer, a second thermoplastic polymer layer and an inner glass plate, and the dimming layer includes a polymer network liquid crystal and/or The dye liquid crystal, the first ultraviolet shielding layer is a nanoreflective layer or a micro-absorbing layer, which effectively absorbs or reflects ultraviolet rays of 280 nm to 400 nm to protect liquid crystals and dye molecules.

Benefits of technology

It significantly improves the resistance of laminated glass to UV rays, prevents performance degradation and color changes, maintains optical and mechanical properties for a long time, extends product life, and provides higher contrast and clear visual effects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118915349A_ABST
    Figure CN118915349A_ABST
Patent Text Reader

Abstract

The invention provides laminated glass and a vehicle. The laminated glass comprises an outer glass plate, a first ultraviolet shielding layer, a first thermoplastic polymer layer, a dimming layer, a second thermoplastic polymer layer and an inner glass plate which are sequentially stacked, the dimming layer comprises a first resin substrate, a first planar electrode layer, a liquid crystal layer, a second planar electrode layer and a second resin substrate which are sequentially stacked; the material of the liquid crystal layer comprises polymer network liquid crystal and / or dye liquid crystal; the first ultraviolet shielding layer is a nano reflecting layer and / or a micron absorbing layer; the laminated structure of the outer glass plate, the first ultraviolet shielding layer and the first thermoplastic polymer layer has a first ultraviolet transmittance Tuv1 for ultraviolet rays with the wavelength of 280-400 nm, and the Tuv1 is smaller than or equal to 0.05%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of glass products, and in particular to a laminated glass and a vehicle. Background Art

[0002] Polymer network liquid crystal (PNLC) and dye liquid crystal (DDLC) surpass traditional polymer dispersed liquid crystal (PDLC) in some optical properties, such as faster response, higher contrast, better photosensitivity, and more diverse color adjustability.

[0003] However, these two technologies have the problem of poor resistance to ultraviolet rays when applied, because their structure and material composition make them more sensitive to ultraviolet rays.

[0004] For PNLC, PNLC is composed of liquid crystal molecules and tiny polymer network structures. Although this structure provides higher stability and fast response, the polymer itself is easily damaged by ultraviolet rays, causing degradation or color change, thus affecting the overall optical performance. Specifically:

[0005] (1) Polymer molecular size: Polymer structures are usually on a nanometer to micrometer scale. The specific size can be adjusted according to the type of monomer used, its concentration, and the photopolymerization conditions. In general, the size of polymer domains ranges from tens of nanometers to several micrometers.

[0006] (2) Polymer molecular morphology: These polymer structures can be continuous networks, or discrete particles or short chains. Their morphology depends on the polymerization conditions and the materials used.

[0007] (3) Polymer molecule function: The main function of the polymer network is to provide a stable framework for the liquid crystal molecules and fix their default arrangement direction. When an external electric field is applied to the PNLC, the liquid crystal molecules will rearrange in response to the electric field. When the electric field is removed, the polymer network will help the liquid crystal molecules quickly return to their default orientation.

[0008] However, prolonged exposure to UV light will cause the polymer network (mainly the photopolymerizer therein) to decompose or denature, thereby making it impossible for the liquid crystal molecules to effectively rotate under the action of the electric field, causing partial or total failure of the dimming function.

[0009] For DDLC, the dye molecules in DDLC will interact with the liquid crystal molecules, thus changing its optical properties. However, the dye itself is often very sensitive to ultraviolet rays. Long-term ultraviolet radiation may cause structural damage to the dye molecules or fading of the color, thus affecting the display effect and stability of DDLC. Specifically:

[0010] (1) High-energy photons: UV light has a short wavelength, so the photons it carries have higher energy. When these high-energy photons interact with dye molecules, they may break chemical bonds, especially π-π bonds and n-π bonds, leading to changes in the molecular structure of the dye.

[0011] (2) Photochemical reaction: Some parts of the dye molecule, especially the conjugated π electron system, are very easy to interact with UV light. This interaction may cause electrons to jump from one energy level to a higher energy level, thus putting the dye molecule into a more active excited state. In this excited state, the molecule is more likely to undergo chemical reactions or decompose.

[0012] (3) Free radical generation: UV radiation may cause the dye molecule or its surrounding environment to generate free radicals. Free radicals are very active chemicals with unpaired electrons that can attack and destroy the structure of the dye molecule.

[0013] (4) Color change or fading: Because the color of the dye molecule is determined by its structure, any factor that destroys the structure of the dye molecule may cause its color to change or fade.

[0014] (5) Influence of molecular environment: The environment in which the dye molecules are located, such as the medium used, other chemicals present, and temperature, may affect their stability to UV light. Certain environmental conditions may increase the sensitivity of the dye to UV radiation.

[0015] In summary, existing polymer network liquid crystal (PNLC) and dye liquid crystal (DDLC) have the defect of poor resistance to ultraviolet rays when used, especially when subsequently used on automotive glass. If exposed to sunlight for a long time, performance degradation or color change will soon occur, and the performance and visual effects of the automotive glass cannot be maintained. Summary of the invention

[0016] In order to solve the above technical problems, the purpose of the present application is to provide a laminated glass and a vehicle, wherein the laminated glass has excellent ultraviolet resistance.

[0017] To achieve the above-mentioned purpose, the present application provides a laminated glass, which includes an outer glass plate, a first ultraviolet shielding layer, a first thermoplastic polymer layer, a dimming layer, a second thermoplastic polymer layer and an inner glass plate which are stacked in sequence; the dimming layer includes a first resin substrate, a first planar electrode layer, a liquid crystal layer, a second planar electrode layer and a second resin substrate which are stacked in sequence; the material of the liquid crystal layer includes polymer network liquid crystal and / or dye liquid crystal; the first ultraviolet shielding layer is a nano-reflective layer and / or a micron absorption layer; the stacked structure of the outer glass plate, the first ultraviolet shielding layer and the first thermoplastic polymer layer has a first ultraviolet transmittance Tuv1 for ultraviolet rays with a wavelength of 280nm to 400nm, and Tuv1≤0.05%.

[0018] Based on the above structure, the laminated glass of the present application can effectively absorb or reflect incident ultraviolet rays, thereby preventing them from directly irradiating the PNLC and / or DDLC materials, and protecting the liquid crystal molecules and dye molecules from damage. Furthermore, the laminated glass of the present application can withstand long-term ultraviolet radiation without performance degradation or color change. Moreover, compared with the traditional technology of only using PVB to block ultraviolet rays, the present application adopts the use of a nano-reflective layer and / or a micron absorption layer to shield ultraviolet rays, which can not only make the product more resistant to ultraviolet rays, but also enable the product to maintain excellent mechanical properties during subsequent long-term application.

[0019] It should be noted that the nano-reflective layer mentioned in the present application refers to a layer structure with a thickness of nanometers and can reflect ultraviolet rays. Further, the thickness of the nano-reflective layer is 100nm to 1000nm, for example, 100nm, 200nm, 300nm, 400nm, 500nm, 600nm, 700nm, 800nm, 900nm or 1000nm. More preferably, the thickness of the nano-reflective layer is 100nm to 500nm. Among them, the nano-reflective layer has a second ultraviolet transmittance Tuv2 for ultraviolet rays with a wavelength of 280nm to 400nm, Tuv2≤10%, preferably Tuv2≤8%, further preferably Tuv2≤5%, and even more preferably Tuv2≤3%.

[0020] Further, the nano-reflective layer includes at least two first metal layers and at least three first dielectric layers, and a first metal layer is arranged between two adjacent first dielectric layers; the material of the first metal layer is selected from at least one of a first silver metal and a first silver alloy; the first silver alloy is an alloy of silver metal and at least one of gold, aluminum, copper, indium and platinum; the material of the first dielectric layer is selected from oxides, nitrides or oxynitrides of at least one element of Zn, Ti, Si, Al, Sn, Se, Zr, Ni, In, Cr, W, Ca, Y, Nb, Cu and Sm. In some optional embodiments, the above-mentioned nano-reflective layer can be obtained by deposition by a magnetron sputtering process.

[0021] It should be noted that the micron absorption layer mentioned in the present application refers to a layer structure with a thickness of micron level and capable of absorbing ultraviolet rays. Furthermore, the thickness of the micron absorption layer is 2μm to 20μm, for example, 2μm, 5μm, 8μm, 10μm, 12μm, 15μm, 17μm or 20μm. More preferably, the thickness of the micron absorption layer is 5 to 15μm. Among them, the micron absorption layer has a third ultraviolet transmittance Tuv3 for ultraviolet rays with a wavelength of 280nm to 400nm, Tuv3≤1%, preferably Tuv3≤0.5%, further preferably Tuv3≤0.1%, and further preferably Tuv3≤0.05%.

[0022] Furthermore, the material of the micron absorption layer includes silicon dioxide and ultraviolet blocking material, the ultraviolet blocking material is selected from at least one of organic ultraviolet absorbers and inorganic ultraviolet nanoparticles, and the average particle size of the inorganic ultraviolet nanoparticles is 10nm to 100nm; the organic ultraviolet absorber is selected from at least one of benzophenone ultraviolet absorbers, benzimidazole ultraviolet absorbers and triazine ultraviolet absorbers; the maximum absorption peak of the organic ultraviolet absorber is within the wavelength range of 330nm to 390nm; the inorganic ultraviolet nanoparticles are selected from at least one of titanium oxide nanoparticles, zinc oxide nanoparticles and cerium oxide nanoparticles.

[0023] Furthermore, the material of the micron absorption layer also includes at least one of infrared blocking nanoparticles and blue light absorbers; the average particle size of the infrared blocking nanoparticles is 10nm to 200nm, preferably 10nm to 150nm. The infrared blocking nanoparticles are selected from indium tin oxide (ITO) nanoparticles, cesium tungsten bronze (Cs x WO 3 ) nanoparticles and antimony tin oxide (ATO) nanoparticles; the blue light absorber is selected from at least one of azo blue light absorbers, isoindolinone blue light absorbers, quinophthalone blue light absorbers, benzimidazolone blue light absorbers and organic-inorganic composite blue light absorbers; the maximum absorption peak of the blue light absorber is in the wavelength range of 400nm to 420nm.

[0024] In a preferred embodiment, the laminated glass also includes a second ultraviolet shielding layer, which is arranged between the first thermoplastic polymer layer and the dimming layer; the second ultraviolet shielding layer is a micron reflection layer, the thickness of the micron reflection layer is 50μm~200μm, and the micron reflection layer has a fourth ultraviolet transmittance Tuv4 for ultraviolet rays with a wavelength of 280nm~400nm, Tuv4≤10%.

[0025] It should be noted that the micron reflective layer mentioned in the present application refers to a layer structure with a thickness of micron level and capable of reflecting ultraviolet rays. Preferably, the thickness of the micron reflective layer can be 50 μm, 80 μm, 100 μm, 120 μm, 150 μm, 180 μm or 200 μm. Tuv4≤8%, or Tuv4≤5%, or Tuv4≤3%, or Tuv4≤1%.

[0026] Furthermore, the micron reflective layer includes a resin film and a functional reflective layer arranged on the resin film, wherein the functional reflective layer is an inorganic metal reflective layer, an inorganic dielectric reflective layer or an organic reflective layer (the functional reflective layer can be arranged on a side of the resin film close to the first thermoplastic polymer layer, or on a side of the resin film close to the dimming layer); the inorganic metal reflective layer includes at least one second metal layer and at least two second dielectric layers, and a second metal layer is arranged between two adjacent second dielectric layers; the material of the second metal layer is selected from at least one of a second silver metal and a second silver alloy; the second silver alloy is an alloy of silver metal and at least one of gold, aluminum, copper, indium and platinum, and the material of the second dielectric layer is selected from nitrides, oxides and other elements of at least one of Zn, Sn, Ti, Si, Al, Mg and Zr. The inorganic medium reflective layer comprises a plurality of alternately stacked high refractive index layers and a low refractive index layer, the material of the high refractive index layer is a first inorganic oxide or an inorganic nitride, the refractive index of the high refractive index layer is greater than or equal to 2.0, the material of the low refractive index layer is a second inorganic oxide, and the refractive index of the low refractive index layer is less than or equal to 1.8; the organic reflective layer comprises a plurality of alternately stacked organic polymer layers, the material of the organic polymer layers is selected from at least one of polyethylene, polypropylene, polylactic acid, poly(4-methyl-1-pentene), polyvinylidene fluoride, cyclic polyolefin, polymethyl methacrylate, polyvinyl chloride, polyvinyl alcohol, polyamide, polystyrene, polycarbonate, polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polyphenylene sulfide or polyetherimide.

[0027] In a preferred embodiment, the laminated glass further comprises a low-emissivity layer, which is arranged on the outer surface of the inner glass plate away from the second thermoplastic polymer layer; the low-emissivity layer comprises at least one transparent conductive oxide layer, the material of the transparent conductive oxide layer is selected from at least one of doped zinc oxide, indium tin oxide (ITO), chromium-doped nickel oxide, fluorine-doped tin oxide (FTO), and zinc tin oxide (ZTO), and the doped zinc oxide is zinc oxide doped with at least one element of aluminum, tungsten, hafnium, gallium, yttrium, niobium, and neodymium. Based on this, the emissivity of the laminated glass measured from the side of the low-emissivity layer is less than or equal to 0.3, or less than or equal to 0.25, or less than or equal to 0.2, which helps to improve the effect of heat insulation in summer and heat preservation in winter.

[0028] In a preferred embodiment, the laminated glass has a light-transmitting state and a light-shielding state, the laminated glass in the light-transmitting state has a first visible light transmittance TL1, the laminated glass in the light-shielding state has a second visible light transmittance TL2, and the ratio of TL1 to TL2 is TL1 / TL2≥2. Among them, TL1=2% to 70%, TL2=0.1% to 20%, and the time for the laminated glass to change from TL1 to TL2 is t, t≤100ms.

[0029] In a preferred embodiment, after the laminated glass is subjected to a 2000-hour xenon lamp aging test from the outer glass plate side, the laminated glass in a light-transmitting state has a third visible light transmittance TL3, |TL3-TL1|≤2%.

[0030] In a preferred embodiment, the laminated glass in a light-transmitting state has a scattering index S, where S≤0.25.

[0031] In a preferred embodiment, the laminated glass with a first ultraviolet shielding layer has a fourth transmittance TL4 in the wavelength range of 450nm to 650nm in the light-transmitting state, and the laminated glass without a first ultraviolet shielding layer has a fifth transmittance TL5 in the wavelength range of 450nm to 650nm in the light-transmitting state, TL4 / TL5=101% to 110%.

[0032] The present application also provides a vehicle, which includes a power supply, a control device and the laminated glass as above, wherein the positive pole of the power supply is connected to the first planar electrode layer, the negative pole of the power supply is connected to the second planar electrode layer, and the control device puts the laminated glass in a light-transmitting state or a light-shielding state.

[0033] Based on the above reasons, the laminated glass of the present application has better UV resistance when used in automotive glass, and can withstand long-term UV exposure without performance degradation or color change. At the same time, it can also improve optical performance, enhance mechanical properties, and extend the service life of the product, thereby providing higher contrast and clearer visual effects, and can achieve true light and dark adjustment, and can reduce the cost of repair or replacement caused by the external environment. More importantly, the color performance of the laminated glass of the present application is richer and more advanced, meeting the high quality requirements of modern consumers for dimming products. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 A schematic structural diagram of a first embodiment of the laminated glass provided in the present application;

[0035] Figure 2 A schematic structural diagram of a second embodiment of the laminated glass provided in the present application;

[0036] Figure 3 This is a schematic structural diagram of a third embodiment of the laminated glass provided in the present application;

[0037] Figure 4 A schematic diagram of the structure of the dimming layer provided in this application;

[0038] Figure 5 This is a schematic diagram of the structure of the second ultraviolet shielding layer provided in this application.

[0039] Explanation of the reference numerals: 1-outer glass plate; 2-first ultraviolet shielding layer; 3-first thermoplastic polymer layer; 4-dimming layer; 5-second thermoplastic polymer layer; 6-inner glass plate; 7-second ultraviolet shielding layer; 8-low-emissivity layer; 41-first resin substrate; 42-first planar electrode layer; 43-liquid crystal layer; 44-second planar electrode layer; 45-second resin substrate; 71-resin film; 72-functional reflective layer. DETAILED DESCRIPTION

[0040] In order to have a clearer understanding of the technical features, objectives and beneficial effects of the present application, the technical solution of the present application is now described in detail below, but it should not be construed as a limitation on the applicable scope of the present application.

[0041] It is explained that the terms "first", "second", etc. in the specification and claims of the present application are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequential order. It should be understood that the data used in this way can be interchanged in appropriate circumstances, so that the embodiments of the present application described here. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions, for example, the process, method, system, product or equipment that includes a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or equipment.

[0042] like Figure 1 , Figure 2 and Figure 3 As shown, the present application provides a laminated glass used as a vehicle window glass, specifically, a skylight glass, a side window glass or a rear windshield. The laminated glass comprises an outer glass plate 1, a first ultraviolet shielding layer 2, a first thermoplastic polymer layer 3, a dimming layer 4, a second thermoplastic polymer layer 5 and an inner glass plate 6 which are stacked in sequence.

[0043] When the laminated glass is applied to a vehicle, the outer glass plate 1 is located on the outside of the vehicle, the outer glass plate 1 has a first surface facing away from the first thermoplastic polymer layer 3 and a second surface facing the first thermoplastic polymer layer 3, and the first surface is the outer surface of the laminated glass; the inner glass plate 6 is located on the inner side of the vehicle, the inner glass plate 6 has a third surface facing the second thermoplastic polymer layer 5 and a fourth surface facing away from the second thermoplastic polymer layer 5, and the fourth surface is the inner surface of the laminated glass.

[0044] The thickness of the outer glass plate 1 is 0.7 mm to 4 mm, and the visible light transmittance of the outer glass plate 1 is greater than or equal to 80%. The inner glass plate 6 is transparent glass or tinted glass, the thickness of the inner glass plate 6 is 0.7 mm to 4 mm, and the visible light transmittance of the inner glass plate 6 is greater than or equal to 80%. The total iron content (in terms of Fe 2 O 3 The total iron content of the tinted glass (in terms of Fe 2 O 3 The content of tinted glass is 0.1wt% to 0.8wt%, preferably 0.1wt% to 0.5wt%, and the visible light transmittance of the tinted glass is 80% to 90%.

[0045] For example, the outer glass plate 1 may be a transparent glass with a thickness of 2.1 mm and a visible light transmittance of 89%, and the inner glass plate 6 may be a green glass with a thickness of 1.6 mm and a visible light transmittance of 83%, or a green glass with a thickness of 2.1 mm and a visible light transmittance of 80%.

[0046] Further, the outer glass plate 1 is transparent glass or tinted glass, and the thickness of the outer glass plate 1 is 1.6 mm to 4 mm, and the visible light transmittance of the outer glass plate 1 is 10% to 95%. The thickness of the outer glass plate 1 can be, but not limited to, 1.6 mm, or 2.0 mm, or 2.4 mm, or 2.8 mm, or 3.2 mm, or 3.6 mm, or 4 mm, or other values ​​between 1.6 mm and 4 mm. The visible light transmittance of the outer glass plate 1 can be, but not limited to, 10%, or 20%, or 30%, or 40%, or 50%, or 60%, or 70%, or 80%, or 85%, or 90%, or 95%, or other values ​​between 10% and 95%. The inner glass plate 6 is transparent glass or tinted glass, and the thickness of the inner glass plate 6 is 0.7 mm to 3.5 mm, and the visible light transmittance of the inner glass plate 6 is 25% to 90%. The thickness of the inner glass plate 6 may be, but is not limited to, 0.7 mm, 1.1 mm, 1.5 mm, 2.1 mm, 2.5 mm, 2.8 mm, 3.5 mm, or other values ​​between 0.7 mm and 3.5 mm. The visible light transmittance of the inner glass plate 6 may be, but is not limited to, 25%, 30%, 40%, 50%, 60%, 70%, 80%, 85%, 90%, 95%, or other values ​​between 25% and 90%. The total iron content (in Fe) of the transparent glass may be, but is not limited to, 25%, 30%, 40%, 50%, 60%, 70%, 80%, 85%, 90%, 95%, or other values ​​between 25% and 90%. 2 O 3 The total iron content of tinted glass (in terms of Fe) is less than or equal to 0.1 wt%, further less than or equal to 0.05 wt%, and even less than or equal to 0.01 wt%. The visible light transmittance of transparent glass is 80% to 95%. 2 O 3 The tinted glass has a visible light transmittance of 10% to 85%; the tinted glass may be, but is not limited to, green glass, gray glass, etc.

[0047] For example, the outer glass plate 1 is a transparent glass with a thickness of 2.1 mm and a visible light transmittance of 91%, or a green glass with a thickness of 2.1 mm and a visible light transmittance of 80%, or a gray glass with a thickness of 2.1 mm and a visible light transmittance of 28%. The inner glass plate 6 is a transparent glass with a thickness of 2.1 mm and a visible light transmittance of 88%, or a green glass with a thickness of 1.6 mm and a visible light transmittance of 83%, or a gray glass with a thickness of 1.6 mm and a visible light transmittance of 45%, or a gray glass with a thickness of 2.1 mm and a visible light transmittance of 28%.

[0048] The first thermoplastic polymer layer 3 and the second thermoplastic polymer layer 5 are used to connect the outer glass plate 1, the dimming layer 4 and the inner glass plate 6 to form a laminated glass structure. The first thermoplastic polymer layer 3 is a transparent thermoplastic polymer film or a colored thermoplastic polymer film, and the thickness of the first thermoplastic polymer layer 3 is 0.38 mm to 1.52 mm, and specifically can be 0.38 mm, or 0.76 mm, or 0.85 mm, or 0.96 mm, or 1.28 mm, or 1.52 mm, or other values ​​between 0.38 mm and 1.52 mm. The second thermoplastic polymer layer 5 is a transparent thermoplastic polymer film or a colored thermoplastic polymer film, and the thickness of the second thermoplastic polymer layer 5 is 0.38 mm to 1.52 mm, specifically 0.38 mm, 0.76 mm, 0.85 mm, 0.96 mm, 1.28 mm, 1.52 mm, or other values ​​between 0.38 mm and 1.52 mm.

[0049] The material of the thermoplastic polymer film can be selected from at least one of polyvinyl butyral (PVB), polyurethane (PU), ethylene-vinyl acetate copolymer (EVA) and ionomer (SGP). The visible light transmittance of the transparent thermoplastic polymer film is greater than or equal to 80%, and can be specifically exemplified as 80%, or 85%, or 90%, or 95%. The visible light transmittance of the colored thermoplastic polymer film is 1% to 45%, and can be specifically exemplified as 1%, or 7%, or 12%, or 18%, or 24%, or 29%, or 35%, or 40%, or 42%, or 44%, or 45%, or other values ​​between 1% and 45%. The colored thermoplastic polymer film can be selected from gray thermoplastic polymer film, green thermoplastic polymer film or blue thermoplastic polymer film.

[0050] Specifically, the first thermoplastic polymer layer 3 and the second thermoplastic polymer layer 5 are made of transparent PVB with a thickness of 0.76 mm and a visible light transmittance of 88%, or a gray PVB with a thickness of 0.76 mm and a visible light transmittance of 2%, or a gray PVB with a thickness of 0.76 mm and a visible light transmittance of 6%, or a gray PVB with a thickness of 0.76 mm and a visible light transmittance of 8%, or a gray PVB with a thickness of 0.76 mm and a visible light transmittance of 18%, or a gray PVB with a thickness of 0.76 mm and a visible light transmittance of 44%.

[0051] like Figure 4The dimming layer 4 includes a first resin substrate 41, a first planar electrode layer 42, a liquid crystal layer 43, a second planar electrode layer 44 and a second resin substrate 45 which are stacked in sequence. The material of the liquid crystal layer 43 includes polymer network liquid crystal and / or dye liquid crystal. Among them, polymer network liquid crystal (PNLC) has a faster response speed and better light isolation ability, and dye liquid crystal (DDLC) can provide more color adjustment, higher contrast and better photosensitivity, thereby providing higher contrast and clearer visual effects, and realizing true brightness and darkness adjustment, and the color performance is richer and more advanced, meeting the high quality requirements of modern consumers for dimming products.

[0052] The material of the first resin substrate 41 and the second resin substrate 45 is polyethylene terephthalate (PET) or a mixture containing PET. The mixture containing PET may also contain polypropylene, polycarbonate, polymethyl methacrylate, polyacrylate, polyvinyl chloride or glass fiber. The thickness of the first resin substrate 41 and the second resin substrate 45 is 50μm to 500μm, and specifically can be 50μm, 100μm, 150μm, 200μm, 250μm, 300μm, 350μm, 400μm, 450μm, 500μm, etc., preferably 100μm to 300μm. The first resin substrate 41 is located between the first thermoplastic polymer layer 3 and the liquid crystal layer 43, and the second resin substrate 45 is located between the liquid crystal layer 43 and the second thermoplastic polymer layer 5.

[0053] The first planar electrode layer 42 and the second planar electrode layer 44 are transparent conductive layers, and the material of the transparent conductive layer is metal, metal alloy or transparent conductive oxide (TCO). The thickness of the transparent conductive layer is preferably 50nm to 500nm, such as 50nm, 100nm, 200nm, 300nm, 400nm or 500nm. The transparent conductive oxide (TCO) can be exemplified by at least one of doped zinc oxide, indium tin oxide (ITO), and fluorine-doped tin dioxide (FTO). The doped zinc oxide is one or more doped zinc oxides of elements such as aluminum, tungsten, hafnium, gallium, yttrium, niobium, and neodymium, and can be specifically at least one of aluminum-doped zinc oxide (AZO), yttrium-doped zinc oxide (YZO), hafnium and aluminum-doped zinc oxide (HAZO), tungsten and aluminum-doped zinc oxide (W-AZO), and gallium-doped zinc oxide (GZO). Preferably, the transparent conductive oxide (TCO) is ITO. Examples of metals include silver (Ag), gold (Au), copper (Cu), etc. Examples of metal alloys include silver alloys, such as silver-copper alloys, silver-indium alloys, silver-nickel alloys, and the like.

[0054] After the laminated glass is installed on the vehicle, the vehicle is often in an outdoor environment and is exposed to sunlight for a long time, in which the ultraviolet radiation is particularly strong. The present application adds a first ultraviolet shielding layer 2 between the outer glass plate 1 and the dimming layer 4. The first ultraviolet shielding layer 2 is a nano-reflection layer and / or a micron absorption layer. The laminated structure of the outer glass plate 1, the first ultraviolet shielding layer 2 and the first thermoplastic polymer layer 3 has a first ultraviolet transmittance Tuv1 for ultraviolet rays with a wavelength of 280nm to 400nm from the outer surface of the outer glass plate away from the first ultraviolet shielding layer. Tuv1≤0.05%, thereby better protecting the polymer network liquid crystal (PNLC) and the dye liquid crystal (DDLC), preventing them from being damaged by ultraviolet rays, and solving the problem of performance degradation or color change of the dimming layer 4. Preferably, Tuv1≤0.03%, or Tuv1≤0.01%, or even Tuv1≤0.005%, so that the laminated glass can maintain the best dimming performance and visual effect for a long time. The measuring method of Tuv1 is as follows: stack the outer glass plate 1, the first ultraviolet shielding layer 2 and the first thermoplastic polymer layer 3 together to form a stacked structure, and then vertically incident ultraviolet rays with a wavelength of 280nm to 400nm are directed onto the first surface of the outer glass plate 1, and the transmission spectrum is measured by a spectrophotometer, and the first ultraviolet transmittance Tuv1 is measured according to ISO13837.

[0055] Ultraviolet rays in sunlight can usually be divided into long-wave ultraviolet rays (UVA: 315nm-400nm), medium-wave ultraviolet rays (UVB: 280nm-315nm) and short-wave ultraviolet rays (UVC: 100nm-280nm) according to their wavelengths.

[0056] Among them, UVA is generally considered to be a relatively weak ultraviolet light, but due to its strong penetrating ability, long-term exposure may cause chronic damage to the material; experiments show that after about 2000 hours of UVA irradiation, the optical properties of polymer network liquid crystal (PNLC) and dye liquid crystal (DDLC) (such as visible light transmittance and contrast) will be significantly reduced. UVB has higher energy and can cause more direct chemical damage to PNLC and DDLC. Experiments show that after about 500 hours of UVB irradiation, the optical properties of polymer network liquid crystal (PNLC) and dye liquid crystal (DDLC) (such as visible light transmittance and contrast) will be significantly reduced. UVC is the most destructive ultraviolet light, but because UVC is usually absorbed by the ozone layer in the atmosphere, in normal surface environments, almost no UVC reaches the earth's surface. Therefore, in the automotive-grade ultraviolet suppression experiment, a mixture of UVA and UVB is used to simulate full-day ultraviolet radiation, that is, the transmittance of ultraviolet rays with a wavelength of 280nm to 400nm is tested.

[0057] This application uses Tuv1≤0.01% as an example: the average ultraviolet intensity of direct sunlight at noon near the earth's equator is 10W / m 2 (Irradiance) For example, Tuv1≤0.01% means that at least 99.99% of ultraviolet rays can be blocked, which means that the irradiance reaching the dimming layer 4 is only 0.001W / m 2 For molecular absorption threshold: up to 0.001W / m 2 The UV intensity of 0.1W / m means that the absorbed energy is low and is unlikely to reach the threshold of destroying the molecular structure of polymer network liquid crystal and dye liquid crystal, that is, it is not enough to cause the breaking of chemical bonds or the rearrangement of molecular structure. For cumulative effect: the destruction of molecular structure may also be the result of cumulative effect. 2 The ultraviolet intensity will cause the cumulative effect to accelerate, so the maximum is 0.001W / m 2 Ultraviolet light intensity of 0.001W / m2 slows down the process significantly, which means that PLCs and DLCs have more time to repair minor damage or the laminated glass may no longer be exposed to UV light before the damage accumulates to a significant degree. Regarding the heating effect: UV absorption also causes local heating of the molecules of PLCs and DLCs, which may also accelerate chemical reactions and cause faster damage to the molecular structure, up to 0.001W / m2 2 The intensity of UV rays can reduce this heating effect.

[0058] This application continues to use dye liquid crystal (DDLC) as an example: Assuming that the size of a dye molecule is about 1 nanometer (10 -9 Each dye molecule occupies a cubic nanometer of space, so there is about 1 / (10 -9 )2=10 18 dye molecules. The energy of each UVA photon is E = hc / λ≈5×10 -19 J, where h is Planck's constant (6.63×10 -34 J·s), c is the speed of light (3×10 8 m / s), λ is the wavelength (about 400nm). Number of photons per square meter: UV intensity is 0.001W / m 2 , that is, there is 0.001 J of energy per square meter per second, then the number of photons = total energy / energy of a single photon = 0.001 / 5×10 -19 ≈2×10 15 , that is, 2×10 per square meter per second. 15 photons. Then, the probability of each dye molecule being hit by a UVA photon is 2×10 15 / 10 18=0.002, that is, the probability of each dye molecule being hit by a photon per second is about 0.002, that is, on average, each dye molecule will be hit by a UVA photon once every 500 seconds, which is a very small probability. Moreover, a single discrete hit usually does not cause the denaturation of the dye molecule. The dye molecule can absorb the energy of the photon and enter the excited state, and then return to the ground state through a non-radiative transition (such as thermal release) without causing a change in the chemical structure. Therefore, Tuv1≤0.01% can reduce the damage of ultraviolet rays to the dye liquid crystal (DDLC) to a negligible level, thereby protecting the dye liquid crystal (DDLC) to the greatest extent.

[0059] exist Figure 1 , Figure 2 and Figure 3 In the laminated glass, the first ultraviolet shielding layer 2 is arranged between the outer glass plate 1 and the first thermoplastic polymer layer 3, and the first ultraviolet shielding layer 2 can be a nano-reflection layer or a micron absorption layer. It can be understood that the first ultraviolet shielding layer 2 can be a nano-reflection layer and a micron absorption layer, that is, the nano-reflection layer and the micron absorption layer are arranged at the same time, for example, the nano-reflection layer is directly arranged on the second surface of the outer glass plate 1, and then the micron absorption layer is arranged on the nano-reflection layer, for example, the micron absorption layer is directly arranged on the second surface of the outer glass plate 1, and then the nano-reflection layer is arranged on the nano-reflection layer, or the nano-reflection layer is arranged between the outer glass plate 1 and the first thermoplastic polymer layer 3 and the micron absorption layer is arranged between the first thermoplastic polymer layer 3 and the first resin substrate 41. When the nano-reflection layer and the micron absorption layer are arranged at the same time, it is preferred that the nano-reflection layer is closer to the outer glass plate 1 than the micron absorption layer, so that more ultraviolet rays can be reflected and more reflected ultraviolet rays do not enter the laminated glass.

[0060] Among them, the nano-reflective layer can block the transmission of ultraviolet rays to avoid ultraviolet rays damaging the dimming layer 4, the thickness of the nano-reflective layer is 100nm to 500nm, and the nano-reflective layer has a second ultraviolet transmittance Tuv2 for ultraviolet rays with a wavelength of 280nm to 400nm, Tuv2≤10%. Preferably, Tuv2≤8%, further preferably Tuv2≤5%, or even Tuv2≤3%, so that the laminated glass can maintain the best dimming performance and visual effect for a long time. The measurement method of Tuv2 is: deposit the nano-reflective layer on one surface of a transparent glass plate with a thickness of 2.1mm and a visible light transmittance of 88%, and then vertically incident ultraviolet rays with a wavelength of 280nm to 400nm on the other surface of the transparent glass plate, use a spectrophotometer to measure the transmission spectrum, and measure the second ultraviolet transmittance Tuv2 according to ISO13837.

[0061] Specifically, the nano-reflective layer includes at least two first metal layers and at least three first dielectric layers, each first metal layer is located between two adjacent first dielectric layers; the material of the first metal layer is selected from at least one of silver metal and silver alloy, and the silver alloy is an alloy of silver and at least one of gold, aluminum, copper, indium and platinum; wherein the first metal layer can reflect infrared and ultraviolet rays, which can not only make the laminated glass have excellent heat insulation performance, thereby improving the thermal comfort of the vehicle interior environment, but also can shield ultraviolet rays to protect the dimming layer 4.

[0062] The nano-reflective layer can be a double silver nano-coating, a triple silver nano-coating or a quadruple silver nano-coating. The double silver nano-coating is a transparent nano-coating having two silver layers and at least three first dielectric layers, the triple silver nano-coating is a transparent nano-coating having three silver layers and at least four first dielectric layers, and the quadruple silver nano-coating is a transparent nano-coating having four silver layers and at least five first dielectric layers. Preferably, the total solar transmittance of the laminated glass having the nano-reflective layer is less than or equal to 20%, more preferably less than or equal to 15%, or even less than or equal to 13%. The lower the total solar transmittance, the better the thermal insulation performance of the laminated glass.

[0063] Wherein, the material of the first dielectric layer is selected from at least one oxide, nitride, or oxynitride of Zn, Ti, Si, Al, Sn, Se, Zr, Ni, In, Cr, W, Ca, Y, Nb, Cu, and Sm, such as ZnSnOx, TiOx, SiNx, SiOx, and NbOx. Preferably, the material of at least one first dielectric layer is titanium oxide TiOx, which can improve the ultraviolet light blocking effect of the nano-reflective layer, thereby further reducing the second ultraviolet transmittance Tuv2. The physical thickness of the first dielectric layer containing TiOx is 5nm to 80nm, such as 5nm, 10nm, 20nm, 30nm, 40nm, 50nm, 60nm, 70nm, 80nm, etc., preferably 10nm to 50nm.

[0064] The nano-reflective layer further includes a nano-absorption layer in direct contact with the first metal layer, the nano-absorption layer is disposed on the first metal layer, and / or the absorption layer is disposed under the first metal layer, and the material of the nano-absorption layer is selected from at least one of NiCr, NiAl, NiSi, Cr, TiN, NbN, and MoTi. The nano-absorption layer can also improve the ultraviolet light blocking effect of the nano-reflective layer, thereby further reducing the second ultraviolet light transmittance Tuv2, and the physical thickness of the absorption layer is 5nm to 40nm, such as 5nm, 10nm, 20nm, 30nm, 40nm, etc., preferably 10nm to 20nm.

[0065] The micron absorption layer can absorb ultraviolet rays to prevent ultraviolet rays from damaging the dimming layer 4, and the thickness of the micron absorption layer is 2μm to 20μm, for example, 2μm, 5μm, 8μm, 10μm, 12μm, 15μm, 17μm or 20μm. More preferably, the thickness of the micron absorption layer is 5 to 15μm. The micron absorption layer has a third ultraviolet transmittance Tuv3 for ultraviolet rays with a wavelength of 280nm to 400nm, Tuv3≤1%, preferably Tuv3≤0.5%, further preferably Tuv3≤0.1%, or even Tuv3≤0.05%, so that the laminated glass can maintain the best dimming performance and visual effect for a long time. The measurement method of Tuv3 is as follows: a micron absorption layer is coated on one surface of a transparent glass plate with a thickness of 2.1 mm and a visible light transmittance of 88%, and then ultraviolet rays with a wavelength of 280 nm to 400 nm are vertically incident on the other surface of the transparent glass plate, and the transmission spectrum is measured by a spectrophotometer. The third ultraviolet transmittance Tuv3 is measured according to ISO13837.

[0066] Specifically, the micron absorption layer comprises silicon dioxide and ultraviolet blocking material, and the ultraviolet blocking material is selected from at least one of organic ultraviolet absorbers and inorganic ultraviolet nanoparticles. The micron absorption layer can be formed by surface coating technology, and the surface coating technology can be exemplified by spraying, wiping, flow coating, brushing or dipping, and a composite coating method formed by combining ultrasound, centrifugation or rotation technology.

[0067] The organic ultraviolet absorber is selected from at least one of benzophenone ultraviolet absorbers, benzimidazole ultraviolet absorbers and triazine ultraviolet absorbers; wherein the maximum absorption peak of the organic ultraviolet absorber is within the wavelength range of 330nm to 390nm. In view of coating uniformity and use effect, the hydroxyl content in the organic ultraviolet absorber is preferably greater than or equal to 5% by mass.

[0068] Specific examples of the benzophenone-based ultraviolet absorber include 2,4-dihydroxybenzophenone, 2,2',3 (or any one of 4, 5, and 6)-trihydroxybenzophenone, 2,2',4,4'-tetrahydroxybenzophenone, 2,4-dihydroxy-2',4'-dimethoxybenzophenone, and 2-hydroxy-4-n-octyloxybenzophenone.

[0069] Specific examples of the benzimidazole ultraviolet absorber include 2-(2H-benzotriazole-2)-4,6-di(1-methyl-1-phenylethyl)phenol (ultraviolet absorber, trade name UV-234), 2-(5-chloro(2H)-benzotriazole-2-yl)-4-methyl-6-(tert-butyl)phenol, octyl-3-[3-tert-4-hydroxy-5-[5-chloro-2H-benzotriazole-2-yl]propionate, 2-(2H-benzotriazole-2-yl)-4,6-di-tert-amylphenol, 2-(2-hydroxy-5-methylphenyl)benzotriazole, 2-[2-hydroxy-3-(3, 4,5,6-tetrahydrophthalimide-methyl)-5-methylphenyl]benzotriazole, 2-(2-hydroxy-5-tert-octylphenyl)benzotriazole, 2-(2-hydroxy-5-tert-butylphenyl)-2H-benzotriazole, methyl 3-(3-(2H-benzotriazol-2-yl)-5-tert-butyl-4-hydroxyphenyl)propionate, 2-(2H-benzotriazol-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol, 2-(2H-benzotriazol-2-yl)-6-(1-methyl-1-phenylethyl)-4-(1,1,3,3-tetramethylbutyl)phenol, etc.

[0070] Specific examples of the triazine ultraviolet absorber include 2-[4-[(2-hydroxy-3-dodecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2-[4-[(2-hydroxy-3-(2'-ethyl)hexyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2,4-bis(2-hydroxy-4-butoxyphenyl)-6-(2,4-bis-butoxyphenyl)-1,3,5-triazine, 2-(2-hydroxy-4-[1-octylcarbonylethoxy]phenyl)-4,6-bis(4-phenylphenyl)-1,3,5-triazine, and TINUVIN 477 (trade name, manufactured by Ciba Japan Co., Ltd.).

[0071] The above-mentioned organic ultraviolet absorbers can absorb ultraviolet rays in a wide wavelength range. In the present invention, these organic ultraviolet absorbers can be used alone or in combination of two or more. The specific use depends on actual needs.

[0072] The average particle size of the inorganic ultraviolet nanoparticles is 10 nm to 100 nm, specifically 10 nm, 30 nm, 50 nm, 80 nm, 100 nm, etc. The inorganic ultraviolet nanoparticles are selected from at least one of titanium oxide (TiOx) nanoparticles, zinc oxide (ZnO) nanoparticles and cerium oxide (CeOx) nanoparticles.

[0073] Optionally, the micron absorption layer further includes at least one of infrared blocking nanoparticles and blue light absorbers.

[0074] The infrared blocking nanoparticles can reduce the infrared transmittance of the micron absorption layer, thereby making the laminated glass with the micron absorption layer heat-insulating. The average particle size of the infrared blocking nanoparticles is 10nm to 200nm, and specific examples include 10nm, 30nm, 50nm, 80nm, 100nm, 150nm, 200nm, etc. The infrared blocking nanoparticles are selected from indium tin oxide (ITO) nanoparticles, cesium tungsten bronze (Cs x WO 3 ) nanoparticles and at least one of antimony tin oxide (ATO) nanoparticles.

[0075] The blue light absorber can reduce the blue light transmittance of the micron absorption layer. Generally, light with a wavelength range of 400nm to 500nm is defined as blue light, among which the short-wave blue light of 400nm to 420nm has higher energy and will cause certain damage to the dimming layer 4. The maximum absorption peak of the blue light absorber selected in the present application is within the wavelength range of 400nm to 420nm, and is preferably selected from at least one of azo blue light absorbers, isoindolinone blue light absorbers, quinophthalone blue light absorbers, benzimidazolone blue light absorbers and organic-inorganic composite blue light absorbers. Considering the uniformity of the coating and the use effect, it is preferred that the hydroxyl content in the blue light absorber is greater than or equal to 5% by mass.

[0076] Specific examples of the above-mentioned azo blue light absorbers include azophenyl methacrylate, 2-[(4-methyl-2-nitrophenyl)azo]-3-oxo-N-phenylbutyramide, 2-[(4-chloro-2-nitrophenyl)azo]-N-(2-chlorophenyl)-3-oxo-butyramide, JEDYING 1226 (trade name, manufactured by Qingdao JEDYA New Materials Technology Co., Ltd.), 2'-(3,3'-dichloro-1,1'-biphenyl-4,4'-disazo)bis[N-(4-chloro-2,5-dimethoxyphenyl)-3-oxo-butyramide], and the like.

[0077] Specific examples of the isoindolinone-based blue light absorber include 1,3,3-trimethyl-2-methyleneindoline, 3,3'-[(2-methyl-1,3-phenylene)diimino]bis[4,5,6,7-tetrachloro-1H-isoindol-1-one], hexachloroisoindolone, 2-[[3,3'-dichloro-4'-[[1-[[(2,4-dimethylphenyl)amino]carbonyl]-2-oxopropyl]azo][1,1'-biphenyl]-4-yl]-azo]-N-(2-methylphenyl)-3-oxo-butyramide, and the like.

[0078] Specific examples of the quinophthalone blue light absorber include 3-(2-cyclopropyl-4-(4-fluorophenyl)-3-quinolyl)acrolein and 3,4,5,6-tetrachloro-N-[2-(4,5,6,7-tetrachloro-2,3-dihydro-1,3-dioxo-2-indenyl)-8-quinoline]phthalimide.

[0079] Specific examples of the above-mentioned benzimidazolone-based blue light absorbers include 2-(2-hydroxy-5-isoethylacrylatephenyl)-2H-benzotriazole, 5-[[1-[[(2,3-dihydro-2-oxo-1H-benzimidazol-5-yl)amino]carbonyl, 2-[[1-[[(2,3-dihydro-2-oxo-1H-benzimidazol-5-yl)amino]carbonyl]-2-oxopropyl]azo]-1,4-phthalic acid dimethyl ester, and JEDYING 1227 (trade name, manufactured by Qingdao JEDYA New Material Technology Co., Ltd.).

[0080] Specific examples of the above-mentioned organic-inorganic composite blue light absorbers include U400 (trade name, manufactured by Shanghai Huzheng Nano Technology Co., Ltd.), U410 (trade name, manufactured by Shanghai Huzheng Nano Technology Co., Ltd.), U420 (trade name, manufactured by Shanghai Huzheng Nano Technology Co., Ltd.), and U460 (trade name, manufactured by Shanghai Huzheng Nano Technology Co., Ltd.).

[0081] exist Figure 2 In the laminated glass, the second ultraviolet shielding layer 7 can further improve the shielding effect of the laminated glass against ultraviolet rays. The second ultraviolet shielding layer 7 is arranged between the first thermoplastic polymer layer 3 and the dimming layer 4 to reduce the ultraviolet rays incident on the dimming layer 4 as much as possible. The second ultraviolet shielding layer 7 provided in the present application is a micron reflective layer.

[0082] The micron reflective layer can reflect ultraviolet rays to prevent ultraviolet rays from damaging the dimming layer 4, and the thickness of the micron reflective layer is 50 μm to 200 μm, 50 μm, 80 μm, 100 μm, 120 μm, 150 μm, 180 μm or 200 μm. More preferably, the thickness of the micron reflective layer is 80 μm to 150 μm. The micron reflective layer has a fourth ultraviolet transmittance Tuv4 for ultraviolet rays with a wavelength of 280 nm to 400 nm, and Tuv4 ≤ 10%. Preferably, Tuv4 ≤ 8%, or Tuv4 ≤ 5%, or Tuv4 ≤ 3%, or Tuv4 ≤ 1%, so that the laminated glass can maintain the best dimming performance and visual effect for a long time. The measurement method of Tuv4 is as follows: a micron reflective layer is attached to one surface of a transparent glass plate with a thickness of 2.1 mm and a visible light transmittance of 88%, and then ultraviolet rays with a wavelength of 280 nm to 400 nm are vertically incident on the other surface of the transparent glass plate, and the transmission spectrum is measured by a spectrophotometer. The fourth ultraviolet transmittance Tuv4 is measured according to ISO13837.

[0083] Specifically, Figure 5 As shown, the micron reflective layer includes a resin film 71 and a functional reflective layer 72 disposed on the resin film 71. The functional reflective layer 72 may be an inorganic metal reflective layer, an inorganic medium reflective layer or an organic reflective layer. The material of the resin film 71 is preferably polyethylene terephthalate (PET) or polyethylene naphthalate (PEN). The inorganic metal reflective layer, the inorganic medium reflective layer or the organic reflective layer may be located between the resin film 71 and the first thermoplastic polymer layer 3, or between the resin film 71 and the dimming layer 4.

[0084] The inorganic metal reflective layer comprises at least one second metal layer and at least two second dielectric layers, each second metal layer is located between two adjacent second dielectric layers, the material of the second metal layer is selected from at least one of silver metal and silver alloy, the silver alloy is an alloy of silver and at least one of gold, aluminum, copper, indium and platinum, and the material of the second dielectric layer is selected from nitride, oxide or oxynitride of at least one element of Zn, Sn, Ti, Si, Al, Mg and Zr; the inorganic dielectric reflective layer comprises a plurality of alternately stacked high refractive index layers and low refractive index layers, the material of the high refractive index layer is an inorganic oxide or an inorganic nitride. The refractive index of the high refractive index layer is greater than or equal to 2.0, the material of the low refractive index layer is an inorganic oxide, and the refractive index of the low refractive index layer is less than or equal to 1.8; the organic reflective layer includes a plurality of alternately stacked organic polymer layers, and the material of the organic polymer layer is selected from at least one of polyethylene, polypropylene, polylactic acid, poly(4-methyl-1-pentene), polyvinylidene fluoride, cyclic polyolefin, polymethyl methacrylate, polyvinyl chloride, polyvinyl alcohol, polyamide, polystyrene, polycarbonate, polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polyphenylene sulfide or polyetherimide.

[0085] exist Figure 3 In the laminated glass provided by the present application, the low-emissivity layer 8 is arranged on the fourth surface of the inner glass plate 6 away from the second thermoplastic polymer layer 5; the low-emissivity layer 8 enables the laminated glass to have low-emissivity performance, which helps to improve the heat insulation in summer and the heat preservation in winter. Preferably, the emissivity of the laminated glass measured from the side of the low-emissivity layer 8 is less than or equal to 0.3, or less than or equal to 0.25, or less than or equal to 0.2.

[0086] In some embodiments, the visible light reflectance of the laminated glass measured from the side of the low-emissivity layer 8 is less than or equal to 4%. By making the visible light reflectance low, the phenomenon of obvious reflections of passengers and objects in the car on the laminated glass due to mirror reflection can be reduced or even eliminated, avoiding the reflection phenomenon from causing visual interference to passengers, especially rear passengers, and improving the passenger experience. Preferably, the visible light reflectance is less than or equal to 3%. More preferably, the visible light reflectance is less than or equal to 2%.

[0087] The low-emissivity layer 8 includes at least one transparent conductive oxide layer, the material of the transparent conductive oxide layer is selected from at least one of doped zinc oxide, indium tin oxide (ITO), chromium-doped nickel oxide, fluorine-doped tin oxide (FTO), and zinc tin oxide (ZTO), and the doped zinc oxide is zinc oxide doped with at least one element of aluminum, tungsten, hafnium, gallium, yttrium, niobium, and neodymium. The total thickness of all transparent conductive oxide layers is 50nm to 300nm, and can be specifically exemplified as 50nm, 80nm, 100nm, 120nm, 150nm, 180nm, 200nm, 250nm, or 300nm. The low-emissivity layer 8 also includes at least two third dielectric layers, each transparent conductive oxide layer is located between two adjacent third dielectric layers, and the third dielectric layer is a nitride, oxide, or oxynitride of at least one element selected from Zn, Sn, Ti, Si, Al, Mg, and Zr.

[0088] In the present application, the dimming layer 4 is used to adjust the visible light transmittance and haze of the laminated glass to meet the optical performance in different usage scenarios. The laminated glass has a light-transmitting state and a light-shielding state. The laminated glass in the light-transmitting state has a first visible light transmittance TL1, and the laminated glass in the light-shielding state has a second visible light transmittance TL2. The ratio of TL1 to TL2 is TL1 / TL2≥2, and specific examples include 2, 3, 5, 10, 15, 20, 30, 50, 80, 100, etc. Preferably, TL1 / TL2≥5, or TL1 / TL2≥10, or TL1 / TL2≥15, or TL1 / TL2≥20.

[0089] Specifically, the dimming layer 4 is in a light-transmitting state when it is powered on, and in a light-shielding state when it is powered off; or, the light layer 4 is in a light-shielding state when it is powered on, and in a light-transmitting state when it is powered off. The higher the ratio TL1 / TL2 of TL1 to TL2, the brighter the light-transmitting state and the darker the light-shielding state can be, thereby meeting the demand for higher contrast. Among them, TL1=2%~70%, TL2=0.1%~20%, for example, TL1=2%, TL2=0.1%, or TL1=5%, TL2=1%, or TL1=10%, TL2=0.5%, or TL1=20%, TL2=5%, or TL1=50%, TL2=2%, or TL1=70%, TL2=10%, etc. Preferably, the dimming layer 4 has a high response speed, and the time for the laminated glass to change from TL1 to TL2 is t, t≤100ms, more preferably t≤50ms, or even t≤10ms, to meet the demand for fast dimming.

[0090] The present application can protect the dimming layer 4 to the greatest extent by adding a first ultraviolet shielding layer 2, or adding a first ultraviolet shielding layer 2 and a second ultraviolet shielding layer 7. The laminated glass provided by the present application is subjected to a xenon lamp aging test. For example, after a 2000-hour xenon lamp aging test is performed on the laminated glass from the side of the outer glass plate 1, the laminated glass in a light-transmitting state has a third visible light transmittance TL3, |TL3-TL1|≤2%, |TL3-TL1| represents the absolute value of the difference between TL3 and TL1, indicating that the first ultraviolet shielding layer 2 successfully blocks ultraviolet rays, so that the visible light transmittance of the dimming layer 4 before and after the test has no significant change, and maintains its original light transmittance. More preferably, |TL3-TL1|≤1.5%, or |TL3-TL1|≤1%, or |TL3-TL1|≤0.5%.

[0091] The laminated glass provided by the present application has a dimming layer 4, and the material of the liquid crystal layer 43 in the dimming layer 4 includes polymer network liquid crystal and / or dye liquid crystal. The liquid crystal layer 43 is uneven. The unevenness of the liquid crystal layer 43 will cause the propagation of light to deviate from the original direction and disperse in all directions, resulting in the trajectory of the light being clearly seen from the side. This is the phenomenon of light scattering. Reducing the scattering of light can improve the permeability and visual effect of the laminated glass. By adding a first ultraviolet shielding layer 2, or adding a first ultraviolet shielding layer 2 and a second ultraviolet shielding layer 7, the scattering of the laminated glass can be reduced to the greatest extent. The laminated glass in a light-transmitting state has a scattering rate S, S≤0.25, so that the laminated glass has better permeability and clearer visual effects. Preferably, S≤0.2, or S≤0.18, or S≤0.15, or S≤0.12, or S≤0.1, or S≤0.08, etc. The scattering rate measurement method is as follows: prepare laminated glass and make the laminated glass in a light-transmitting state, and use a haze meter to measure the haze of the laminated glass from the inner surface side of the laminated glass as H. According to the formula Calculate the scattering rate S.

[0092] The present application can also improve the transmittance of visible light in the sensitive wavelength band of the human eye by adding the first ultraviolet shielding layer 2, or adding the first ultraviolet shielding layer 2 and the second ultraviolet shielding layer 7. Among them, the human eye with normal vision is most sensitive to electromagnetic waves with a wavelength of about 555nm. Therefore, the radiation energy at a wavelength of 555nm is usually taken as the reference point of the relative spectral power distribution. On this basis, the present application takes 450nm~650nm as the main wavelength range of the visible light band. The laminated glass with the first ultraviolet shielding layer 2 has a fourth transmittance TL4 in the wavelength range of 450nm~650nm in the light-transmitting state, and the laminated glass without the first ultraviolet shielding layer 2 has a fifth transmittance TL5 in the wavelength range of 450nm~650nm in the light-transmitting state. The transmittance of the laminated glass in the main wavelength range of the visible light band can be improved by adding the first ultraviolet shielding layer 2 or adding the first ultraviolet shielding layer 2 and the second ultraviolet shielding layer 7. Preferably, TL4 / TL5=101%~110%, and specific examples include 101%, 102%, 103%, 104%, 105%, 106%, 107%, 108%, 109% or 110%, etc.

[0093] The present application also provides a vehicle, which may be, but is not limited to, a sedan, a multi-purpose vehicle (MPV), a sport / suburban utility vehicle (SUV), an off-road vehicle (ORV), a pickup truck, a van, a bus, a truck, etc. The laminated glass may be, but is not limited to, a sunroof glass, a side window glass, or a rear windshield glass of the vehicle. The specific implementation of the present application is described only with the laminated glass being a sunroof glass.

[0094] The vehicle provided by the present application includes a power supply, a control device and a laminated glass. The laminated glass can be fixedly installed at the roof opening of the vehicle. The power supply and the control device are installed in the body of the vehicle. The positive electrode of the power supply is connected to the first planar electrode layer 42, and the negative electrode of the power supply is connected to the second planar electrode layer 44. The control device puts the laminated glass in a light-transmitting state or a light-shielding state. The laminated glass has a higher visible light transmittance when it is in the light-transmitting state, and has a lower visible light transmittance when it is in the light-shielding state, so as to achieve brighter light in the light-transmitting state and darker light in the light-shielding state.

[0095] Example 1

[0096] This embodiment provides a specific laminated glass, such as Figure 1As shown, it comprises an outer glass plate 1, a first ultraviolet shielding layer 2, a first thermoplastic polymer layer 3, a dimming layer 4, a second thermoplastic polymer layer 5 and an inner glass plate 6 which are stacked in sequence.

[0097] The outer glass plate 1 is a transparent glass with a thickness of 2.1 mm and a visible light transmittance of 89%;

[0098] The first ultraviolet shielding layer 2 is a nano-reflective layer; the nano-reflective layer includes two first metal layers and three first dielectric layers, specifically: first dielectric layer (ZnSnOx 20nm / AZO 10nm) / nano-absorption layer (NiCr 5nm) / first metal layer (Ag 10nm) / first dielectric layer (TiOx 8nm / AZO 10nm / ZnSnOx 40nm / AZO 10nm / TiOx5nm) / first metal layer (Ag 10nm) / nano-absorption layer (NiCr 5nm) / first dielectric layer (AZO 10nm / ZnSnOx20nm / TiOx 20nm);

[0099] The nano-reflective layer is deposited on the second surface of the outer glass plate 1 by a magnetron sputtering process, the thickness of the nano-reflective layer is 183 nm, and the nano-reflective layer has a second ultraviolet transmittance Tuv2 for ultraviolet rays with a wavelength of 280 nm to 400 nm, and Tuv2 is 9.8%;

[0100] The material of the first thermoplastic polymer layer 3 is gray PVB with a thickness of 0.76 mm and a visible light transmittance of 44%;

[0101] The laminated structure formed by the outer glass plate 1, the first ultraviolet shielding layer 2 and the first thermoplastic polymer layer 3 has a first ultraviolet transmittance Tuv1 for ultraviolet rays with a wavelength of 280nm to 400nm, Tuv1=0.01%;

[0102] The dimming layer 4 is a commercially available polymer network liquid crystal (PNLC) dimming film;

[0103] The material of the second thermoplastic polymer layer 5 is gray PVB with a thickness of 0.38 mm and a visible light transmittance of 18%;

[0104] The inner glass plate 6 is green glass with a thickness of 2.1 mm and a visible light transmittance of 83%.

[0105] The laminated glass has a light-transmitting state and a light-shielding state. The laminated glass in the light-transmitting state has a first visible light transmittance TL1, TL1 is 10.3%, and the laminated glass in the light-shielding state has a second visible light transmittance TL2, TL2 is 4.2%, and TL1 / TL2 is 2.45. The time for the laminated glass to change from TL1 to TL2 is t, and t is 20ms.

[0106] The laminated glass was subjected to a xenon lamp aging test. After the xenon lamp aging test was performed on the laminated glass from the outer glass plate 1 side for 2000 hours, the laminated glass in a light-transmitting state had a third visible light transmittance TL3, and |TL3-TL1| was 1.2%.

[0107] Put the laminated glass in a light-transmitting state, and measure the haze of the laminated glass from the inner surface side with a haze meter to find that H = 0.9%. According to the formula Calculate the scattering rate S, which is 0.09.

[0108] With 450nm to 650nm as the main wavelength range of the visible light band, the laminated glass with the first ultraviolet shielding layer 2 has a fourth transmittance TL4 in the wavelength range of 450nm to 650nm in the light-transmitting state, and the laminated glass without the first ultraviolet shielding layer 2 has a fifth transmittance TL5 in the wavelength range of 450nm to 650nm in the light-transmitting state, TL4 / TL5=105%.

[0109] Example 2

[0110] This embodiment provides a specific laminated glass, which includes an outer glass plate 1, a first ultraviolet shielding layer 2, a first thermoplastic polymer layer 3, a dimming layer 4, a second thermoplastic polymer layer 5 and an inner glass plate 6 which are stacked in sequence.

[0111] The outer glass plate 1 is a transparent glass with a thickness of 2.1 mm and a visible light transmittance of 89%;

[0112] The first ultraviolet shielding layer 2 is a micron absorption layer; the micron absorption layer is formed by curing the micron absorption coating liquid; the thickness of the micron absorption layer is 5.2 μm; the micron absorption layer has a third ultraviolet transmittance Tuv3 for ultraviolet rays with a wavelength of 280 nm to 400 nm, and Tuv3 is 0.01%;

[0113] The micron absorption coating liquid is coated on the second surface of the outer glass plate 1 with a wire rod coater, and after being left to level and pre-dried and cured with an infrared lamp, a micron absorption layer is finally obtained. The micron absorption coating liquid is obtained by mixing and stirring 10g of silica sol and 1g of a chelating agent, the silica sol is obtained by stirring 13.56g of ethyl orthosilicate, 20g of anhydrous ethanol, 30g of isopropanol, 5.18g of γ-methacryloxypropyl trimethoxysilane, 0.1g of nitric acid with a mass fraction of 10% and 12.5g of deionized water in a 40°C water bath, and the chelating agent is obtained by mixing 10g of BP-2 ultraviolet light absorber, 10g of U410 blue light absorber, 55g of butyl acetate solvent, 0.15g of dibutyltin dilaurate catalyst and 25g of γ-methacryloxypropyl trimethoxysilane and stirring in a 100°C constant temperature oil bath and naturally cooling to room temperature;

[0114] The material of the first thermoplastic polymer layer 3 is gray PVB with a thickness of 0.76 mm and a visible light transmittance of 5%;

[0115] The laminated structure formed by the outer glass plate 1, the first ultraviolet shielding layer 2 and the first thermoplastic polymer layer 3 has a first ultraviolet transmittance Tuv1 for ultraviolet rays with a wavelength of 280nm to 400nm, Tuv1=0.005%;

[0116] The dimming layer 4 is a commercially available dye liquid crystal (DDLC) dimming film;

[0117] The material of the second thermoplastic polymer layer 5 is transparent PVB with a thickness of 0.76 mm and a visible light transmittance of 88%;

[0118] The inner glass plate 6 is green glass with a thickness of 2.1 mm and a visible light transmittance of 83%.

[0119] The laminated glass has a light-transmitting state and a light-shielding state. The laminated glass in the light-transmitting state has a first visible light transmittance TL1, TL1 is 3.8%, and the laminated glass in the light-shielding state has a second visible light transmittance TL2, TL2 is 1.2%, and TL1 / TL2 is 3.17. The time for the laminated glass to change from TL1 to TL2 is t, and t is 16ms.

[0120] The laminated glass was subjected to a xenon lamp aging test. After the xenon lamp aging test was performed on the laminated glass from the outer glass plate 1 side for 2000 hours, the laminated glass in a light-transmitting state had a third visible light transmittance TL3, and |TL3-TL1| was 0.9%.

[0121] Put the laminated glass in a light-transmitting state, and measure the haze of the laminated glass from the inner surface side with a haze meter. The haze is H = 0.5%. According to the formula Calculate the scattering rate S, which is 0.13.

[0122] With 450nm to 650nm as the main wavelength range of the visible light band, the laminated glass with the first ultraviolet shielding layer 2 has a fourth transmittance TL4 in the wavelength range of 450nm to 650nm in the light-transmitting state, and the laminated glass without the first ultraviolet shielding layer 2 has a fifth transmittance TL5 in the wavelength range of 450nm to 650nm in the light-transmitting state, TL4 / TL5=103%.

[0123] Example 3

[0124] This embodiment provides a specific laminated glass, such as Figure 2 As shown, it comprises an outer glass plate 1, a first ultraviolet shielding layer 2, a first thermoplastic polymer layer 3, a second ultraviolet shielding layer 7, a dimming layer 4, a second thermoplastic polymer layer 5 and an inner glass plate 6 which are stacked in sequence.

[0125] The outer glass plate 1 is a transparent glass with a thickness of 2.1 mm and a visible light transmittance of 89%;

[0126] The first ultraviolet shielding layer 2 is a micron absorption layer; the micron absorption layer is formed by curing the micron absorption coating liquid; the thickness of the micron absorption layer is 5.2 μm; the micron absorption layer has a third ultraviolet transmittance Tuv3 for ultraviolet rays with a wavelength of 280 nm to 400 nm, and Tuv3 is 0.03%;

[0127] The micron absorption coating liquid is coated on the second surface of the outer glass plate 1 with a wire rod coater, and after being left to level and pre-dried and cured with an infrared lamp, a micron absorption layer is finally obtained. The micron absorption coating liquid is obtained by mixing and stirring 20g of silica sol and 1.5g of a chelating agent, and the silica sol is obtained by stirring 13.56g of ethyl orthosilicate, 22g of anhydrous ethanol, 28g of isopropanol, 5.18g of γ-methacryloxypropyl trimethoxysilane, 0.1g of nitric acid with a mass fraction of 10% and 12.5g of deionized water in a 40°C water bath, and the chelating agent is obtained by mixing 10g of BP-2 ultraviolet light absorber, 10g of U420 blue light absorber, 55g of butyl acetate solvent, 0.15g of dibutyltin dilaurate catalyst and 25g of γ-methacryloxypropyl trimethoxysilane and stirring in a 100°C constant temperature oil bath and naturally cooling to room temperature;

[0128] The material of the first thermoplastic polymer layer 3 is transparent PVB with a thickness of 0.76 mm and a visible light transmittance of 88%;

[0129] The laminated structure formed by the outer glass plate 1, the first ultraviolet shielding layer 2 and the first thermoplastic polymer layer 3 has a first ultraviolet transmittance Tuv1 for ultraviolet rays with a wavelength of 280nm to 400nm, Tuv1=0.01%;

[0130] The second ultraviolet shielding layer 7 is a commercially available 50 μm thick Southwall XIR film;

[0131] The dimming layer 4 is a commercially available polymer network liquid crystal (PNLC) dimming film;

[0132] The material of the second thermoplastic polymer layer 5 is gray PVB with a thickness of 0.76 mm and a visible light transmittance of 8%;

[0133] The inner glass plate 6 is a transparent glass having a thickness of 2.1 mm and a visible light transmittance of 89%.

[0134] The laminated glass has a light-transmitting state and a light-shielding state. The laminated glass in the light-transmitting state has a first visible light transmittance TL1, TL1 is 6.3%, and the laminated glass in the light-shielding state has a second visible light transmittance TL2, TL2 is 2.02%, and TL1 / TL2 is 3.12. The time for the laminated glass to change from TL1 to TL2 is t, and t is 18ms.

[0135] The laminated glass is subjected to a xenon lamp aging test. After the xenon lamp aging test is performed on the laminated glass from the outer glass plate 1 side for 2000 hours, the laminated glass in a light-transmitting state has a third visible light transmittance TL3, and |TL3-TL1| is 0.5%.

[0136] Put the laminated glass in a light-transmitting state, and measure the haze of the laminated glass from the inner surface side with a haze meter. The haze is H = 0.5%. According to the formula Calculate the scattering rate S, which is 0.08.

[0137] With 450nm~650nm as the main wavelength range of the visible light band, the laminated glass with the first ultraviolet shielding layer 2 has a fourth transmittance TL4 in the wavelength range of 450nm~650nm in the light transmitting state, and the laminated glass without the first ultraviolet shielding layer 2 has a fifth transmittance TL5 in the wavelength range of 450nm~650nm in the light transmitting state, TL4 / TL5=106%.

[0138] In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, unless they contradict each other. The above are only embodiments of the embodiments of this specification and are not intended to limit the embodiments of this specification. For those skilled in the art, the embodiments of this specification may have various changes and variations. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the embodiments of this specification shall be included within the scope of the claims of the embodiments of this specification.

Claims

1. A laminated glass, characterized in that: It comprises an outer glass plate, a first ultraviolet shielding layer, a first thermoplastic polymer layer, a dimming layer, a second thermoplastic polymer layer and an inner glass plate which are stacked in sequence; The dimming layer includes a first resin substrate, a first planar electrode layer, a liquid crystal layer, a second planar electrode layer and a second resin substrate which are stacked in sequence; The material of the liquid crystal layer includes polymer network liquid crystal and / or dye liquid crystal; The first ultraviolet shielding layer is a nanometer reflection layer and / or a micrometer absorption layer; The laminated structure formed by the outer glass plate, the first ultraviolet shielding layer and the first thermoplastic polymer layer has a first ultraviolet transmittance Tuv1 for ultraviolet rays with a wavelength of 280nm to 400nm, and Tuv1 is ≤0.05%.

2. The laminated glass according to claim 1, characterized in that: The thickness of the nanometer reflective layer is 100nm-500nm, and the nanometer reflective layer has a second ultraviolet transmittance Tuv2 for ultraviolet rays with a wavelength of 280nm-400nm, and the Tuv2 is ≤10%.

3. The laminated glass according to claim 2, characterized in that: The nano-reflective layer comprises at least two first metal layers and at least three first dielectric layers, and one first metal layer is disposed between two adjacent first dielectric layers; The material of the first metal layer is selected from at least one of a first silver metal and a first silver alloy; the first silver alloy is an alloy of silver metal and at least one of gold, aluminum, copper, indium and platinum; The material of the first dielectric layer is selected from oxides, nitrides or oxynitrides of at least one element among Zn, Ti, Si, Al, Sn, Se, Zr, Ni, In, Cr, W, Ca, Y, Nb, Cu and Sm.

4. The laminated glass according to claim 1, characterized in that: The thickness of the micron absorption layer is 2 μm to 20 μm, and the micron absorption layer has a third ultraviolet transmittance Tuv3 for ultraviolet rays with a wavelength of 280 nm to 400 nm, and Tuv3 is ≤1%.

5. The laminated glass according to claim 4, characterized in that: The material of the micron absorption layer includes silicon dioxide and ultraviolet blocking material, the ultraviolet blocking material is selected from at least one of an organic ultraviolet absorber and an inorganic ultraviolet nanoparticle, and the average particle size of the inorganic ultraviolet nanoparticle is 10nm to 100nm; The organic ultraviolet absorber is selected from at least one of a benzophenone ultraviolet absorber, a benzimidazole ultraviolet absorber and a triazine ultraviolet absorber; The inorganic ultraviolet nanoparticles are selected from at least one of titanium oxide nanoparticles, zinc oxide nanoparticles and cerium oxide nanoparticles.

6. The laminated glass according to claim 5, characterized in that: The material of the micron absorption layer also includes at least one of infrared blocking nanoparticles and blue light absorbers; The average particle size of the infrared blocking nanoparticles is 10 nm to 200 nm, and the infrared blocking nanoparticles are selected from at least one of indium tin oxide nanoparticles, cesium tungsten bronze nanoparticles and antimony tin oxide nanoparticles; The blue light absorber is selected from at least one of azo blue light absorbers, isoindolinone blue light absorbers, quinophthalone blue light absorbers, benzimidazolone blue light absorbers and organic-inorganic composite blue light absorbers.

7. The laminated glass according to claim 1, characterized in that: The laminated glass further comprises a second ultraviolet shielding layer, which is disposed between the first thermoplastic polymer layer and the dimming layer; The second ultraviolet shielding layer is a micron reflective layer, the thickness of the micron reflective layer is 50 μm to 200 μm, and the micron reflective layer has a fourth ultraviolet transmittance Tuv4 for ultraviolet rays with a wavelength of 280 nm to 400 nm, and the Tuv4 is ≤10%.

8. The laminated glass according to claim 7, characterized in that: The micron reflective layer comprises a resin film and a functional reflective layer arranged on the resin film, wherein the functional reflective layer is an inorganic metal reflective layer, an inorganic medium reflective layer or an organic reflective layer; The inorganic metal reflective layer includes at least one second metal layer and at least two second dielectric layers, and one second metal layer is disposed between two adjacent second dielectric layers; The material of the second metal layer is selected from at least one of a second silver metal and a second silver alloy; the second silver alloy is an alloy of silver metal and at least one of gold, aluminum, copper, indium and platinum; the material of the second dielectric layer is selected from nitride, oxide or oxynitride of at least one of Zn, Sn, Ti, Si, Al, Mg and Zr; The inorganic medium reflective layer comprises a plurality of high refractive index layers and low refractive index layers alternately stacked, the material of the high refractive index layer is a first inorganic oxide or an inorganic nitride, the refractive index of the high refractive index layer is greater than or equal to 2.0, the material of the low refractive index layer is a second inorganic oxide, and the refractive index of the low refractive index layer is less than or equal to 1.8; The organic reflective layer includes a plurality of organic polymer layers alternately stacked, and the material of the organic polymer layer is selected from at least one of polyethylene, polypropylene, polylactic acid, poly(4-methyl-1-pentene), polyvinylidene fluoride, cyclic polyolefin, polymethyl methacrylate, polyvinyl chloride, polyvinyl alcohol, polyamide, polystyrene, polycarbonate, polyethylene terephthalate, polyethylene naphthalate, polyphenylene sulfide or polyetherimide.

9. The laminated glass according to claim 1, characterized in that: The laminated glass further comprises a low-emissivity layer disposed on the outer surface of the inner glass sheet away from the second thermoplastic polymer layer; The low-emissivity layer includes at least one transparent conductive oxide layer, the material of the transparent conductive oxide layer is selected from at least one of doped zinc oxide, indium tin oxide, chromium-doped nickel oxide, fluorine-doped tin oxide, and zinc tin oxide. The doped zinc oxide is zinc oxide doped with at least one element of aluminum, tungsten, hafnium, gallium, yttrium, niobium, and neodymium.

10. The laminated glass according to claim 1, characterized in that: The laminated glass has a light-transmitting state and a light-shielding state. The laminated glass in the light-transmitting state has a first visible light transmittance TL1, and the laminated glass in the light-shielding state has a second visible light transmittance TL2, and TL1 / TL2≥2.

11. The laminated glass according to claim 10, characterized in that: The TL1=2%-70%, the TL2=0.1%-20%, the time for the laminated glass to change from the TL1 to the TL2 is t, and t≤100ms.

12. The laminated glass according to claim 10, characterized in that: After a 2000-hour xenon lamp aging test is performed on the laminated glass from the outer glass plate side, the laminated glass in a light-transmitting state has a third visible light transmittance TL3, |TL3-TL1|≤2%.

13. The laminated glass according to claim 10, characterized in that: The laminated glass in a light-transmitting state has a scattering rate S, where S is less than or equal to 0.

25.

14. The laminated glass according to claim 10, characterized in that: The laminated glass with the first ultraviolet shielding layer has a fourth transmittance TL4 in the wavelength range of 450nm to 650nm in the light-transmitting state, and the laminated glass without the first ultraviolet shielding layer has a fifth transmittance TL5 in the wavelength range of 450nm to 650nm in the light-transmitting state, TL4 / TL5=101% to 110%.

15. A vehicle, characterized in that: The vehicle includes a power supply, a control device and the laminated glass according to any one of claims 1 to 14, the positive pole of the power supply is connected to the first planar electrode layer, the negative pole of the power supply is connected to the second planar electrode layer, and the control device puts the laminated glass in a light-transmitting state or a light-shielding state.

Citation Information

Patent Citations

  • Liquid crystal laminated glazing

    CN114556202A

  • Laminated glass

    CN114571809A

  • Dimmer object and laminated glass

    JP2007033533A

  • Dimming film

    JP2020060641A

  • Transparent sheet for light module, method for manufacturing the same and light module comprising the same

    KR1020160144234A

Cited By

  • Glass plate and vehicle

    CN119550786A