Nanocrystalline magnetic core material and preparation method thereof

By using the cladding of boron nitride and molybdenum disulfide in nanocrystalline magnetic core materials, the problems of particle agglomeration and oxidation corrosion are solved, the heat resistance and magnetic properties of the material are improved, the service life is extended, and at high frequency Maintain stability under high temperature conditions.

CN118919198AActive Publication Date: 2024-11-08TIANJIN AONA TECH
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411030474.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-08
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

During the preparation process, nanocrystalline magnetic core materials are prone to particle agglomeration, resulting in uneven size distribution, and due to the high surface area, it is easy to oxidize or corrode, resulting in unsatisfactory magnetic properties.

Method used

The nanocrystalline alloy FeaNibSicMndLae is used with boron nitride and molybdenum disulfide as the main components. Through vacuum smelting, single-roll fast quenching method and high shear disperser, the coating layer of boron nitride and molybdenum disulfide is formed to improve the The material's oxidation resistance and magnetic properties.

Benefits of technology

Through the use of the cladding layer, the heat resistance, wear resistance and insulation of the material are significantly improved, the service life is extended, and the stability and reliability of the magnetic core are enhanced, especially under high frequency and high temperature conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004969801510000081
    Figure BDA0004969801510000081
  • Figure BDA0004969801510000091
    Figure BDA0004969801510000091
  • Figure BDA0004969801510000092
    Figure BDA0004969801510000092
Patent Text Reader

Abstract

The invention relates to a nanocrystalline magnetic core material and a preparation method thereof. The nanocrystalline magnetic core material disclosed by the invention is prepared from the following components: nanocrystalline alloy, boron nitride and molybdenum disulfide, wherein the molecular formula of the nanocrystalline alloy is Fe Ni S < c > Mn < d > La < e >. According to the invention, boron nitride and molybdenum disulfide are both layered structure materials, and have good lubricity and low friction coefficient. When the magnetic particles are applied to the surface of the nanocrystalline magnetic core material as a coating layer, friction and abrasion among the magnetic particles can be reduced, interface contact among the particles can be improved, and therefore the processability and the yield of the material can be possibly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of magnetic core materials, and in particular to a nanocrystalline magnetic core material and a preparation method thereof. Background Art

[0002] Nano-magnetic core materials, due to their unique size effect, surface effect and quantum confinement effect, exhibit magnetic properties different from those of traditional macro-scale magnetic materials, including enhanced magnetization, improved magnetic loss characteristics, higher magnetic permeability, and potential new magnetic phenomena. Nano-magnetic core materials have broad application prospects in modern science and technology, and their main application areas include: information storage, magnetic sensors, high-frequency devices, magnetic random access memory, biomedical applications, energy conversion and storage, etc.

[0003] Although these materials have made significant technological progress, there are still some technical challenges and problems. Under the current conventional technology, during the preparation process of nanocrystalline magnetic core materials, the materials are prone to particle agglomeration, resulting in uneven distribution of magnetic core material particle sizes, and nanocrystalline materials are often more susceptible to oxidation or corrosion than traditional materials due to their high surface area, resulting in unsatisfactory magnetic properties of the materials. Therefore, those skilled in the art are committed to developing new materials, by adjusting the chemical composition, microstructure design and processing technology of the materials, in order to prepare a new type of magnetic core material with stable magnetic properties that is resistant to oxidation. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a nanocrystalline magnetic core material and a preparation method thereof.

[0005] The first object of the present invention is to provide a nanocrystalline magnetic core material, which comprises the following components by mass:

[0006] 60-80 parts of nanocrystalline alloy; wherein the molecular formula of the nanocrystalline alloy is: Fe a Ni b Si c Mn d La e ; Wherein, a, b, c, d and e represent the atomic percentage of the corresponding elements respectively: 60≤a≤70, 10≤b≤20, 5≤c≤10, 3≤d≤5, e=100-abcd;

[0007] Boron nitride 15-30 parts;

[0008] 10-15 parts of molybdenum disulfide.

[0009] In some specific embodiments of the present invention, a, b, c, d and e respectively represent the atomic percentage content of the corresponding elements: 65≤a≤70, 10≤b≤15, 5≤c≤10, 3≤d≤5, e=100-abcd.

[0010] The second object of the present invention is to provide a method for preparing the nanocrystalline magnetic core material, comprising the following steps:

[0011] S1. According to the molecular formula of the nanocrystalline alloy FeaNibSicMndLae, metals are selected for mixing, and vacuum smelting is performed to obtain a metal alloy ingot; then, the metal alloy ingot is prepared by a single-roller rapid quenching method to obtain an alloy strip;

[0012] S2. In an inert atmosphere, placing the obtained alloy strip in a heating device for heat treatment to obtain a nanocrystalline alloy;

[0013] S3, ball-milling the boron nitride and molybdenum disulfide, and then dispersing them in a solvent using a high shear disperser to obtain a suspension;

[0014] S4, adding the nanocrystalline alloy obtained in step S2 to the suspension obtained in step S3, adjusting the pH value of the mixed solution to 7-9, mixing and stirring, and standing to allow the surface of the nanocrystalline alloy to be coated with a coating layer containing boron nitride and molybdenum disulfide;

[0015] S5, performing solid-liquid separation on the reaction solution obtained in step S4 and taking the solid phase, washing and drying to obtain the nanocrystalline magnetic core material.

[0016] In some specific embodiments of the present invention, in step S2, the gas in the inert atmosphere is nitrogen or argon;

[0017] The heat treatment conditions are: heating to 290°C ~ 360°C and keeping warm for 1.5h ~ 3h; then heating to 500°C ~ 600°C and keeping warm for 2.5h ~ 4h.

[0018] In some specific embodiments of the present invention, in step S3, the solvent is selected from ethanol;

[0019] The rotation speed of the high shear disperser is 2000 rpm / min to 5000 rpm / min.

[0020] In some specific embodiments of the present invention, in step S4, the standing time is 1 hour to 3 hours.

[0021] In some specific embodiments of the present invention, in step S5, the drying temperature is 50-80° C., and the drying time is 1-2 hours.

[0022] The third object of the present invention is to provide a magnetic core, which includes the nanocrystalline magnetic core material.

[0023] A fourth object of the present invention is to provide a transformer, an inductor core, a relay, a high-frequency sensor or a wireless charger, comprising the magnetic core.

[0024] The above technical solution of the present invention has the following advantages compared with the prior art:

[0025] The present invention uses boron nitride as an additive. Modified boron nitride can improve the heat resistance, wear resistance and insulation of the material. At the same time, due to its high thermal conductivity, it helps thermal management and prevents local overheating, which is particularly important for high-frequency applications. Molybdenum disulfide can improve the lubricity of the material and reduce friction and wear, which is beneficial for applications that require frequent flux reversal and can increase the service life and reliability of the material. Boron nitride has good stability to a variety of chemicals and is not easy to react chemically with other materials, which helps protect the magnetic core from corrosion or oxidation, especially in applications working in harsh environments.

[0026] Boron nitride also has good mechanical strength and wear resistance. It can be used as a coating or additive to enhance the hardness and wear resistance of nanocrystalline magnetic core materials and extend the service life of the device. Boron nitride, as an excellent electrical insulating material, can provide the necessary electrical insulation performance while maintaining the original magnetic properties of the magnetic material. This is especially important for magnetic components that require insulating coatings or isolation layers, such as in high-frequency transformers or inductors, to avoid leakage and short circuit risks. Boron nitride has high thermal conductivity and can be used as a heat dissipation material. When it is applied to the surface treatment of nanocrystalline magnetic core materials or as part of a composite material, it can significantly improve the thermal conductivity efficiency of the core, help dissipate heat quickly, and reduce temperature rise during operation, thereby improving the stability and reliability of the core in high temperature or high power applications.

[0027] The present invention utilizes boron nitride and molybdenum disulfide, both of which are layered structural materials with good lubricity and low friction coefficient. Applying them as coating layers to the surface of nanocrystalline magnetic core materials can reduce friction and wear between magnetic particles and improve interfacial contact between particles, thereby possibly improving the processing performance and yield of the material. Boron nitride is one of the materials with higher known thermal conductivity, and although the thermal conductivity of molybdenum disulfide is not as good as that of boron nitride, it also has good heat transfer capabilities. Using these two materials as coating layers or dispersing them in nanocrystalline magnetic powder, the synergistic effect can effectively improve the thermal management performance of the magnetic core and accelerate the dissipation of heat, especially under high-frequency working conditions, which is crucial to maintaining the stability of magnetic properties.

[0028] The present invention utilizes molybdenum disulfide and boron nitride, both of which have good chemical stability, to form a barrier as a coating layer to protect the internal nanocrystalline magnetic material from erosion by environmental factors (such as humidity, oxygen, etc.), thereby extending the service life of the material. Although boron nitride and molybdenum disulfide do not directly enhance magnetism, they indirectly help stabilize the electromagnetic properties of magnetic materials under different conditions, especially in high temperature or high frequency working environments, by improving the microstructure and thermodynamic properties of the materials. DETAILED DESCRIPTION

[0029] In order to solve the technical problems pointed out in the background technology: the magnetic core material is prone to particle agglomeration during the preparation process, resulting in uneven distribution of the particle size of the magnetic core material; and the nanocrystalline material is easily oxidized or corroded due to its high surface area, resulting in unsatisfactory magnetic properties of the material. Therefore, the present invention achieves the purpose of the present invention through the following scheme.

[0030] The present invention is further described below in conjunction with specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.

[0031] The present invention provides a nanocrystalline magnetic core material, which comprises the following components by mass:

[0032] 60-80 parts of nanocrystalline alloy; wherein the molecular formula of the nanocrystalline alloy is: Fe a Ni b Si c Mn d La e ; Wherein, a, b, c, d and e represent the atomic percentage of the corresponding elements respectively: 60≤a≤70, 10≤b≤20, 5≤c≤10, 3≤d≤5, e=100-abcd;

[0033] Boron nitride 15-30 parts;

[0034] 10-15 parts of molybdenum disulfide.

[0035] In a specific embodiment of the present invention, a, b, c, d and e respectively represent the atomic percentage content of the corresponding elements: 65≤a≤70, 10≤b≤15, 5≤c≤10, 3≤d≤5, e=100-abcd.

[0036] In the present invention, the nanocrystalline alloy is applicable to conventional nanocrystalline in the art, and can also be obtained by conventional preparation methods in the art, such as in the process of preparing the strip, the metal melting method, the single-roller rapid quenching method, and the heat treatment of the strip, which are all conventional methods in the art and are not particularly limited. The present invention aims to package the nanocrystalline alloy, so the selection of the nanocrystalline alloy can also be obtained in the form of purchase, or can be prepared by means of literature.

[0037] For example, the steps of preparing the alloy strip by the single-roller rapid quenching method may be:

[0038] According to the predetermined alloy composition ratio (such as Fe a Ni b Si c Mn d La e , wherein a, b, c, d and e represent the atomic percentage of each corresponding component respectively), prepare corresponding metal or alloy raw materials;

[0039] The prepared raw materials are vacuum smelted at 1200-1500°C for 10-20 minutes to ensure that the raw materials are fully melted and mixed evenly to obtain alloy ingots;

[0040] The alloy ingot is crushed and placed in a test tube with a nozzle, and remelted under high-frequency induction heating; the molten alloy is ejected from the nozzle under pressure and directly sprayed onto a high-speed rotating water-cooled copper roller, and finally an alloy strip is obtained. Due to the high-speed rotation and strong cooling capacity of the copper roller, the alloy solution is quickly cooled and solidified into a continuous thin strip, and the cooling rate can be about 10K / s. At this temperature, the grain size can reach the nanometer level, and the roller speed is 30m / s.

[0041] The present invention also provides a method for preparing the nanocrystalline magnetic core material, comprising the following steps:

[0042] S1, according to the molecular formula of nanocrystalline alloy Fe a Ni b Si c Mn d La e Selecting metal raw materials for batching, vacuum smelting, and obtaining a metal alloy melt; then preparing the metal alloy melt by a single-roller rapid quenching method to obtain an alloy strip;

[0043] S2. In an inert atmosphere, placing the obtained alloy strip in a heating device for heat treatment to obtain a nanocrystalline alloy;

[0044] S3, ball-milling the boron nitride and molybdenum disulfide, and then dispersing them in a solvent using a high shear disperser to obtain a suspension;

[0045] S4, adding the nanocrystalline alloy obtained in step S2 to the suspension obtained in step S3, adjusting the pH value of the mixed solution to 7-9, mixing and stirring, and standing to allow the surface of the nanocrystalline alloy to be coated with a coating layer containing boron nitride and molybdenum disulfide;

[0046] S5, performing solid-liquid separation on the reaction solution obtained in step S4 and taking the solid phase, washing and drying to obtain the nanocrystalline magnetic core material.

[0047] In a specific embodiment of the present invention, in step S2, the gas in the inert atmosphere is nitrogen or argon;

[0048] The heat treatment conditions are: heating to 290°C ~ 360°C and keeping warm for 1.5h ~ 3h; then heating to 500°C ~ 600°C and keeping warm for 2.5h ~ 4h.

[0049] In a specific embodiment of the present invention, in step S3, the solvent is selected from ethanol;

[0050] The speed of the high shear disperser is 2000 rpm / min to 5000 rpm / min. By setting the speed, the boron nitride and molybdenum disulfide can be fully mixed, the shear between the solid matter and the solvent can be increased, and the dispersion performance can be enhanced.

[0051] In a specific embodiment of the present invention, in step S4, the standing time is 1h to 3h. During the standing time of the present invention, the mixed suspension of boron nitride and molybdenum disulfide can be evenly coated on the surface of the nanocrystalline alloy; when it is less than 1h, the coating thickness is not enough and the effect is minimal; when it is greater than 2h, the coating thickness is too thick, and the coating may hinder the magnetic performance of the magnetic core and reduce its magnetic permeability and saturation magnetization. This is because the coating itself is not magnetic or has weak magnetism, thereby diluting the magnetism of the overall material. In an AC magnetic field, an overly thick coating may lead to an increase in eddy current losses. This is because the interface between the coating and the magnetic core may become an obstacle to the current loop, causing the current to generate eddy currents in the coating, thereby causing energy loss.

[0052] In a specific embodiment of the present invention, in step S5, the drying temperature is 50-80° C., and the drying time is 1-2 hours.

[0053] The present invention also provides a magnetic core, which comprises the nanocrystalline magnetic core material.

[0054] The present invention also provides a transformer, an inductor core, a relay, a high-frequency sensor or a wireless charger, comprising the magnetic core.

[0055] Example 1

[0056] This embodiment provides a nanocrystalline magnetic core material, wherein the molecular formula of the nanocrystalline alloy is Fe70 Ni 15 Si 10 Mn 3 La 2 , the specific steps are as follows:

[0057] S1, according to the molecular formula of nanocrystalline alloy Fe 70 Ni 15 Si 10 Mn 3 La 2 Select metals for batching, and smelt in vacuum at 1350° C. for 20 minutes to obtain a metal alloy melt; then, the metal alloy melt is prepared by a single-roller rapid quenching method to obtain an alloy strip;

[0058] S2. In an inert atmosphere, the obtained alloy strip is placed in a heating device for heat treatment. The heat treatment conditions are: heating to 320° C. and keeping the temperature for 2 hours; then heating to 500° C. and keeping the temperature for 2.5 hours to obtain a nanocrystalline alloy;

[0059] S3, 15 parts by mass of boron nitride and 15 parts by mass of molybdenum disulfide were ball-milled and mixed, and then dispersed in 150 ml of ethanol solvent at a speed of 5000 rpm / min using a high shear disperser to obtain a suspension;

[0060] S4, adding 60 parts by mass of the nanocrystalline alloy obtained in step S2 to the suspension obtained in step S3, adjusting the pH value of the mixed solution to 7, mixing and stirring, and standing for 2 hours, so that the surface of the nanocrystalline alloy is coated with a coating layer containing boron nitride and molybdenum disulfide;

[0061] S5, filtering the reaction solution obtained in step S4, washing and drying the solid matter obtained by filtration, wherein the drying temperature is 60° C., to obtain the nanocrystalline magnetic core material.

[0062] Example 2

[0063] This embodiment provides a nanocrystalline magnetic core material, wherein the molecular formula of the nanocrystalline alloy is Fe 65 Ni 20 Si 10 Mn 3 La 2 , the specific steps are as follows:

[0064] S1, according to the molecular formula of nanocrystalline alloy Fe 65 Ni 20 Si 10 Mn 3 La 2 Select metals for batching, and smelt in vacuum at 1350° C. for 20 minutes to obtain a metal alloy melt; then, the metal alloy melt is prepared by a single-roller rapid quenching method to obtain an alloy strip;

[0065] S2. In an inert atmosphere, the obtained alloy strip is placed in a heating device for heat treatment, wherein the heat treatment temperature process is: heated to 310° C. and kept warm for 1.5 hours; then heated to 500° C. and kept warm for 2.5 hours to obtain a nanocrystalline alloy;

[0066] S3, 15 parts by mass of boron nitride and 15 parts by mass of 2-naphthene were ball-milled and then dispersed in 150 ml of ethanol solvent at a rotation speed of 5000 rpm using a high shear disperser to obtain a suspension;

[0067] S4, adding 60 parts by mass of the nanocrystalline alloy obtained in step S2 to the suspension obtained in step S3, adjusting the pH value of the mixed solution to 7, mixing and stirring, and standing for 2 hours, so that the surface of the nanocrystalline alloy is coated with a coating layer containing boron nitride and molybdenum disulfide;

[0068] S5. Filter the reaction solution obtained in step S4, and wash and dry the solid matter obtained by filtration, wherein the drying temperature is 50° C. to obtain the nanocrystalline magnetic core material.

[0069] Example 3

[0070] Similar to Example 1, the difference is that the molecular formula of the nanocrystalline alloy is Fe 67 Ni 18 Si 10 Mn 3 La 2 .

[0071] Comparative Example 1

[0072] Similar to Example 1, the difference is that the encapsulation layer does not include boron nitride.

[0073] Comparative Example 2

[0074] Similar to Example 1, the difference is that molybdenum disulfide is not included in the encapsulation layer.

[0075] Comparative Example 3

[0076] Similar to Example 1, except that no wrapping layer was prepared.

[0077] Comparative Example 4

[0078] Similar to Example 1, the difference is that in the process of preparing the coating layer, in step S4, the standing time is 5 hours.

[0079] Performance Testing

[0080] The nanocrystalline magnetic core materials obtained in the examples and comparative examples were subjected to performance tests, such as magnetic flux density and magnetic permeability tests, and stability tests under high temperature and high humidity conditions. The experimental results are shown in Tables 1 and 2.

[0081] Table 1 Magnetic flux density and magnetic permeability test results

[0082]

[0083]

[0084] The nanocrystalline magnetic core materials obtained in Example 1 and Comparative Example 3 were placed at a temperature of 85° C. and a humidity of 85% RH for 1000 h (performed in multiple batches), and the changes in the magnetic properties of the nanocrystalline magnetic core materials were detected. The results are shown in Table 2.

[0085] Table 2 Stability test under high temperature and high humidity conditions

[0086]

[0087] From the data in Table 1, it can be seen that compared with Comparative Examples 1-3, in Example 1, the presence of the mixed coating layer of boron nitride and molybdenum disulfide will not directly affect the change of magnetic permeability, but from the magnetic flux density, it can be seen that by adding the coating layer of boron nitride and molybdenum disulfide, the magnetic flux density of the nanocrystalline magnetic core material has been improved to a certain extent. It can be seen that the presence of the mixed coating layer of boron nitride and molybdenum disulfide can not only improve the magnetic properties of the magnetic core material, but also well protect the material stability of the nanocrystal. It can be seen from Example 1 and Comparative Example 4 that the standing time in step S4 in Comparative Example 4 is 5h. The longer the time, the greater the thickness of the coating layer formed. The greater the thickness, the magnetic properties of the nanocrystalline magnetic core material will be affected, such as the decrease in magnetic permeability, such as the decrease in magnetic permeability in Comparative Example 4 compared to Example 1. Therefore, it is necessary to reasonably set the standing time to achieve the reasonable packaging of the nanocrystalline magnetic core material, which can enhance the magnetic properties of the magnetic core material to a certain extent, otherwise the opposite effect may occur.

[0088] It can be seen from Table 2 that under the conditions of high temperature and high humidity, the magnetic properties of the nanocrystalline magnetic core material obtained in Example 1 are less reduced, while the nanocrystalline magnetic core material of Comparative Example 3 has no wrapping layer on the surface, which leads to an oxidation reaction on the surface of the nanocrystalline magnetic core material under the conditions of high temperature and high humidity, resulting in a more significant reduction in the magnetic properties of the nanocrystalline magnetic core material.

[0089] Obviously, the above embodiments are merely examples for clear explanation and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the protection scope of the invention.

Claims

1. A nanocrystalline magnetic core material, It is characterized in that The nanocrystalline magnetic core material comprises the following components in parts by mass: 60-80 parts of nanocrystalline alloy; wherein the molecular formula of the nanocrystalline alloy is: Fe a Ni b Si c Mn d La e ; Wherein, a, b, c, d and e represent the atomic percentage of the corresponding elements respectively: 60≤a≤70, 10≤b≤20, 5≤c≤10, 3≤d≤5, e=100-abcd; Boron nitride 15-30 parts; 10-15 parts of molybdenum disulfide.

2. The nanocrystalline magnetic core material according to claim 1, It is characterized in that a, b, c, d and e represent the atomic percentage of the corresponding elements respectively: 65≤a≤70, 10≤b≤15, 5≤c≤10, 3≤d≤5, e=100-abcd.

3. A method for preparing the nanocrystalline magnetic core material as claimed in claim 1 or 2, It is characterized in that The following steps are involved: S1, according to the molecular formula of nanocrystalline alloy Fe a Ni b Si c Mn d La e Select metals for batching, perform vacuum smelting, and obtain metal alloy ingots; then, use a single-roller rapid quenching method to prepare alloy strips from the metal alloy ingots; S2. In an inert atmosphere, placing the obtained alloy strip in a heating device for heat treatment to obtain a nanocrystalline alloy; S3, ball-milling the boron nitride and molybdenum disulfide, and then dispersing them in a solvent using a high shear disperser to obtain a suspension; S4, adding the nanocrystalline alloy obtained in step S2 to the suspension obtained in step S3, adjusting the pH value of the mixed solution to 7-9, mixing and stirring, and standing to allow the surface of the nanocrystalline alloy to be coated with a coating layer containing boron nitride and molybdenum disulfide; S5, performing solid-liquid separation on the reaction solution obtained in step S4 and taking the solid phase, washing and drying to obtain the nanocrystalline magnetic core material.

4. The preparation method according to claim 3, It is characterized in that In step S2, the gas in the inert atmosphere is nitrogen or argon; The heat treatment conditions are: heating to 290°C ~ 360°C and keeping warm for 1.5h ~ 3h; then heating to 500°C ~ 600°C and keeping warm for 2.5h ~ 4h.

5. The preparation method according to claim 3, It is characterized in that In step S3, the solvent is selected from ethanol; and the rotation speed of the high shear disperser is 2000 rpm / min to 5000 rpm / min.

6. The preparation method according to claim 3, It is characterized in that In step S4, the standing time is 1 h to 3 h.

7. The preparation method according to claim 3, It is characterized in that In step S5, the drying temperature is 50-80° C. and the drying time is 1-2 hours.

8. A magnetic core, It is characterized in that The magnetic core comprises the nanocrystalline magnetic core material according to claim 1 or 2.

9. A transformer, an inductor core, a relay, a high-frequency sensor or a wireless charger, It is characterized in that Comprising the magnetic core as claimed in claim 8.

Citation Information

Patent Citations

  • Rare earth magnetic powder mixture and rare earth magnet

    CN104851541A

  • Dry cutting tool and preparation method thereof

    CN108624881A

  • Soft magnetic metal powder, dust core, and inductor

    CN115398570A

  • Magnetic powder core coated with nano boron nitride-aluminum oxide composite film and preparation method of magnetic powder core

    CN115631940A

  • High-frequency nanocrystalline material as well as preparation method and application thereof