Preparation method of integrally-formed inductance coil

By using materials such as silicates and nitrides to form a high-temperature resistant insulation layer in the inductor coil, the problem of easy damage to the insulation layer of enameled wire at high temperatures is solved, and the high-temperature stability and low-loss performance of the inductor coil are achieved.

CN118919292APending Publication Date: 2024-11-08NBTM NEW MATERIALS GRP
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411120351.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the existing technology, the insulation layer of the enameled wire is easily damaged during the high-temperature heat treatment of the powder core integral molding inductor coil, which leads to increased loss and limits the temperature resistance and low-loss high-current application of the inductor coil.

Method used

A primary insulating liquid is formed by mixing silicates, nitrides, Y2O3, Bi2O3, TiO2, and water. The mixture is then immersed in a secondary insulating liquid and heat-treated under a non-oxidizing atmosphere to form a high-temperature resistant insulating layer.

Benefits of technology

It improves the heat resistance and operating temperature of inductor coils, reduces device temperature rise, enhances the efficiency and lifespan of magnetic materials, simplifies the preparation process, and reduces the volatile emissions of organic solvents.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919292A_ABST
    Figure CN118919292A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of an integrally formed inductance coil. The preparation method comprises the following steps: (1) preparing a primary insulating liquid: mixing silicate, nitride, Y2O3, Bi2O3, TiO2 and water to form the primary insulating liquid; (2) primary insulation: placing the metal coil in primary insulation liquid, soaking for 0.1-500 minutes, and then taking out the coil to obtain a primary insulation coil; (3) preparing a secondary insulating liquid: mixing silicon resin and nitride to obtain the secondary insulating liquid; (4) secondary insulation: putting the coil subjected to primary insulation in the step (2) into secondary insulation liquid, soaking for 0.1-500 minutes, and then taking out the coil to obtain a coil subjected to secondary insulation; and (5) heat treatment: calcining the coil subjected to secondary insulation under a non-oxidizing atmosphere condition, wherein the calcining temperature is 80-400 DEG C. Compared with the prior art, the heat resistance is good, and the heat conductivity is high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of integrally formed inductors, and in particular to a method for preparing an integrally formed inductor coil. Background Art

[0002] One-piece molded inductors refer to inductor components made of composite profiles as the main material through one-time molding, injection molding and other processes. Powder core one-piece molded inductors are one of them. The core is mainly made of a mixture of iron core powder, magnetic particles, barium silicate and other structural conditioners. This type of inductor component has the advantages of high efficiency and convenience, and is widely used in modern economic development. As the information industry develops towards integration and high frequency, one-piece molded inductors, especially one-piece molded inductors made of iron powder cores, are becoming more and more widely used.

[0003] The one-piece molded inductor is mainly composed of three parts: the core, the winding and the package. The core of the powder core one-piece molded inductor is made of a specific powder material, which is evenly dispersed and mixed to form a magnetic core with high magnetic permeability and low heat loss. The winding part adopts vertical winding or radial winding to make the coil in the polarized core material. Finally, the core and the winding are integrated together through the packaging process to form a complete one-piece molded inductor. The one-piece molded inductor has the following characteristics: ① High efficiency: Due to its unique structure and material selection, the powder core one-piece molded inductor has high magnetic permeability and low heat loss, thereby improving the overall performance of the circuit. ② High compactness: The one-piece molded inductor can realize the coexistence of multiple inductors or the embedding of inductors and other electronic components in space, which improves the compactness of the circuit. ③ Good stability: Because it is made by one-time molding, injection molding and other processes, the powder core one-piece molded inductor has high stability and reliability. Powder core one-piece molded inductors are widely used in various electronic products, such as circuit boards of mobile phones, computers, tablets and other devices, as well as various types of motors, transformers and other power equipment. With the rapid development of the electronics industry and the continuous upgrading of electronic products, the application areas of powder core one-piece molded inductors are also constantly expanding.

[0004] In the prior art, the one-piece molded inductor coil is mainly made of enameled wire. The enameled wire consists of two parts: a conductor and an insulating layer. The preparation method is: the bare wire is annealed and softened, and then painted and baked multiple times; the enameled wire has four major properties, namely, high mechanical properties, chemical properties, electrical properties, and thermal properties. It has good insulation performance, high temperature resistance, and chemical corrosion resistance, which helps to improve the working stability of electrical equipment.

[0005] However, for one-piece molded inductors made with powder cores, the coil is molded into the powder core and then subjected to high-temperature heat treatment. The heat treatment temperature often exceeds 500°C. The use temperature of enameled wire does not exceed 300°C, which means that the maximum heat treatment temperature of the powder core does not exceed 300°C. However, under the temperature condition of 300°C, the stress generated by the powder core during pressing cannot be effectively removed, and the hysteresis loss of the powder core is relatively high; and excessively high heat treatment temperature will cause the insulation layer of the enameled wire to be destroyed, resulting in increased losses. It can be said that the insulation ability of the coil at high temperatures limits the development of one-piece molded inductors, especially for one-piece molded inductors for low-loss and high-current applications.

[0006] Therefore, it is necessary to improve the existing inductor coil. Summary of the invention

[0007] The technical problem to be solved by the present invention is to provide a method for preparing an integrally formed inductor coil with good temperature resistance in view of the above technical status.

[0008] The technical solution adopted by the present invention to solve the above technical problem is: a method for preparing an integrally formed inductor coil, characterized in that it comprises the following steps:

[0009] ①Preparing a primary insulating liquid: Mixing silicate, nitride, Y2O3, Bi2O3, TiO2 and water to form a primary insulating liquid;

[0010] ② Primary insulation: Place the metal coil in the primary insulation liquid, soak for 0.1 to 500 minutes, then take out the coil to obtain the primary insulation coil;

[0011] ③Preparing secondary insulating liquid: mixing silicone resin and nitride to obtain secondary insulating liquid;

[0012] ④ Secondary insulation: Place the primary insulated coil in step ② in a secondary insulating liquid, soak for 0.1 to 500 minutes, then take out the coil to obtain a secondary insulated coil;

[0013] ⑤ Heat treatment: Calcine the secondary insulated coil in a non-oxidizing atmosphere at a temperature of 80 to 400°C.

[0014] The electrical conductivity of TiO2 is about 10 -15 ~10 -9 S / cm, the conductivity of silicate is about 10 -3 S / cm, the conductivity of Y2O3 is about 10 -2 S / cm, so the primary insulating layer formed by the primary insulating liquid has better insulating performance.

[0015] Preferably, the silicate is one or more of lithium silicate, ammonium silicate, sodium silicate and potassium silicate.

[0016] Preferably, the nitride in the step is one or more of aluminum nitride, hexagonal boron nitride, cubic boron nitride, titanium nitride, tantalum nitride, vanadium nitride, phosphorus nitride, silicon nitride, lithium nitride and magnesium nitride.

[0017] Preferably, the particle size of the nitride is 10 <10μm,d 50 <30μm,d 99 <60μm.

[0018] Preferably, the ratio of the surface area of ​​the metal coil to the volume of the primary insulating liquid in step ② is (0.01-200 cm 2 ):1cm 3 The immersion temperature is -5 to 100° C. In the primary insulation treatment process, the metal coil and the insulating liquid can be mixed evenly by stirring or pumping circulation.

[0019] Preferably, the ratio of the surface area of ​​the metal coil to the volume of the secondary insulating liquid in step ④ is (0.01-200cm 2 ):1cm 3 The immersion temperature is -5 to 100° C. During the secondary insulation treatment, the metal coil and the insulating liquid can be mixed evenly by stirring or pumping circulation.

[0020] Preferably, the nitride in step ③ is one or more of aluminum nitride, hexagonal boron nitride, cubic boron nitride, titanium nitride, tantalum nitride, vanadium nitride, phosphorus nitride, silicon nitride, lithium nitride and magnesium nitride.

[0021] Preferably, the chemical formula of the silicone resin is [(CH3) x (R) y SiO 24-x-y ] n , x is the number of methyl groups on the silicon atom, y is the number of R groups, and x+y≤4. Silicone resin is a polysiloxane resin. The structural feature of this siloxane polymer is that the silicon atoms and oxygen atoms in its molecules are covalently bonded to form a silicon-oxygen chain. In addition to the main siloxane polymer, silicone resin can also include other ingredients such as silicone monomers, diluents, cross-linking agents, catalysts, etc. These ingredients play different roles in the preparation process of silicone resin, such as promoting polymerization reactions, adjusting the physical and chemical properties of silicone resins, etc.

[0022] Preferably, in step ①, the mass ratio of nitride to water is 0.05-80:100; the mass ratio of silicate to water is 0.03-2:1; the mass ratio of Y2O3 to water is 0-0.5:1; the mass ratio of Bi2O3 to water is 0-0.5:1; and the mass ratio of TiO2 to water is 0-0.5:1.

[0023] Preferably, in step ③, the mass ratio of silicone resin to nitride is 100:0.1-60. The silicone resin includes one or more of methyl silicone resin (MQ resin), phenyl silicone resin, fluorosilicone resin, polyester silicone resin, phenolic silicone resin and modified silicone resin. The mass ratio of silicone resin to nitride is 100:0.1-60; below this ratio, the insulating performance of the insulating layer formed by the obtained secondary insulating liquid will be reduced, and above this ratio, the viscosity of the secondary insulating liquid is too high to be coated on the surface of the copper coil to form an insulating layer.

[0024] Compared with the prior art, the advantages of the present invention are:

[0025] ① Simplify the preparation process, the method is simple, the preparation cost is reduced, and the surface damage of the coil with insulation layer during the winding process is reduced;

[0026] ② The insulating layer obtained after the primary insulation and the secondary insulation of the present invention is an inorganic material, which has good heat resistance and can maintain the original performance in the heat treatment temperature range of the integrally formed inductor, thereby increasing the use temperature of the inductor coil and being able to withstand a higher use current;

[0027] ③ Increase thermal conductivity: The insulating layer contains materials with insulating and thermal conductive properties, which can remove the heat generated by the coil and the powder core and reduce the temperature rise of the device, which will improve the efficiency and life of the magnetic material;

[0028] ④ Do not use low-flash point organic solvents such as alcohol and methyl acetate to reduce the emission of volatile organic compounds during the insulation process and ensure production safety. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is the morphology of the metal coil of Example 1 of the present invention;

[0030] Figure 2 The microscopic morphology of the metal coil of Example 1 of the present invention;

[0031] Figure 3 The microscopic morphology of the integrally formed inductor coil of Example 1 of the present invention;

[0032] Figure 4 This is the microscopic morphology of the one-piece formed inductor coil after heat treatment again in Example 1 of the present invention;

[0033] Figure 5 This is the microscopic morphology of the primary insulation coil of Example 2 of the present invention;

[0034] Figure 6 This is the microscopic morphology of the secondary insulated coil of Example 2 of the present invention.

[0035] Figure 7 This is the microscopic morphology of the enameled wire of Comparative Example 1 of the present invention;

[0036] Figure 8 This is the microscopic morphology of the enameled wire after heat treatment in Comparative Example 1 of the present invention; DETAILED DESCRIPTION

[0037] The present invention is further described in detail below with reference to the accompanying drawings.

[0038] Example 1

[0039] The method for preparing the integrally formed inductor coil comprises the following steps:

[0040] ① Preparation of metal coil: Copper wire is used to make the coil. The microscopic photo of the coil of this embodiment is as follows: Figure 1 shown.

[0041] ② Primary insulation layer liquid: Silicate, nitride, Y2O3, Bi2O3, TiO2 are mixed with water according to the proportions in Table 1 to form a primary insulation liquid. The particle size of the nitride in Table 1 is d 10 <10μm,d 50 <30μm,d 99 <60μm.

[0042] ③ Primary insulation treatment: Place the metal coil obtained in step ① in a primary insulation liquid and soak it. The ratio of the metal coil surface area to the insulation liquid volume is (1cm 2 ):1cm 3 The soaking time is 1 minute and the soaking temperature is 25°C. After the soaking is completed, the metal coil is taken out to obtain a primary insulated coil. The surface state of the primary insulated coil is observed, such as Figure 3 As shown, a small amount of material has been applied to the coil that has received the primary insulation.

[0043] ④ Preparation of secondary insulating liquid: prepare secondary insulating liquid according to the proportions in Table 2. The resin in this embodiment is (R1R2SiO 1 / 2 ) m (SiO 4 / 2 ) n , wherein R1 and R2 are methyl or phenyl.

[0044] ⑤ Secondary insulation treatment: Place the primary insulated coil in the secondary insulation liquid and soak it. The ratio of the coil surface area to the volume of the secondary insulation liquid is (1cm 2 ):1cm 3 The soaking time is 1 minute and the soaking temperature is 25°C, after which the coil is taken out to obtain a secondary insulated coil.

[0045] ⑥ Heat treatment: The coil with secondary insulation is heat treated in nitrogen at 150℃ for 5 minutes to obtain an integrated inductor coil; the microstructure of the integrated inductor coil is as follows Figure 3As shown, it can be seen that the coil surface has been coated with a thicker inorganic layer.

[0046] The coil that has been heat treated is heat treated again in a nitrogen atmosphere at 730℃ for one hour. The microstructure is as follows Figure 4 As shown, it can be seen that the insulation layer is still intact after 730°C.

[0047] Example 2

[0048] ①Preparation of metal coil: Use copper wire coil.

[0049] ② Primary insulating layer liquid: Mix silicate, nitride, Y2O3, Bi2O3, TiO2 with water according to the proportions in Table 1 to form a primary insulating liquid.

[0050] ③ Primary insulation treatment: Place the metal coil obtained in step ① in a primary insulation liquid and soak it. The ratio of the metal coil surface area to the insulation liquid volume is (0.1cm 2 ):1cm 3 The soaking time is 2 minutes and the soaking temperature is 25°C. After the soaking is completed, the metal coil is taken out to obtain a primary insulated coil. Figure 5 As shown, more material has been coated on the coil.

[0051] ④Preparation of secondary insulating liquid: prepare secondary insulating liquid according to the proportions in Table 2. The silicone resin is polyester silicone resin, which is a composite of siloxane and polyester chains, and its structure contains both siloxane units (-Si-O-) and polyester units (-COO-).

[0052] ⑤ Secondary insulation treatment: Place the primary insulated coil in the secondary insulation liquid and soak it. The ratio of the coil surface area to the volume of the secondary insulation liquid is 1cm 2 :1cm 3 The soaking time is 1 minute and the soaking temperature is 25°C, after which the coil is taken out to obtain a secondary insulated coil.

[0053] ⑥ Heat treatment: Heat the coil with secondary insulation in nitrogen at 25℃ for 2min to obtain an integrated inductor coil. The microstructure of the inductor coil is as follows: Figure 6 As shown, it can be seen that more material has been coated on the surface of the inductor coil.

[0054] Example 3

[0055] ①Preparation of metal coil: The coil is made of copper wire.

[0056] ② Primary insulating layer liquid: Mix silicate, nitride, Y2O3, Bi2O3, TiO2 with water according to the proportions in Table 1 to form a primary insulating liquid.

[0057] ③ Primary insulation treatment: Place the metal coil obtained in step ① in a primary insulation liquid and soak it. The ratio of the metal coil surface area to the insulation liquid volume is 5cm 2 :1cm 3 The soaking time is 2 minutes and the soaking temperature is 25° C. After the soaking is completed, the metal coil is taken out to obtain a primary insulated coil.

[0058] ④Prepare secondary insulating liquid: Prepare secondary insulating liquid according to the proportion in Table 2. Silicone resin is (R3SiO 1 / 2 ) m (SiO 4 / 2 ) n , where R is typically a methyl group (-CH3), and m and n are the number of M units and Q units, respectively.

[0059] ⑤ Secondary insulation treatment: Place the primary insulated coil in the secondary insulation liquid and soak it. The ratio of the coil surface area to the volume of the secondary insulation liquid is 1cm 2 :1cm 3 The soaking time is 3 minutes and the soaking temperature is 25°C. Then the coil is taken out to obtain a secondary insulated coil.

[0060] ⑥ Heat treatment: heat treat the coil with secondary insulation in nitrogen at 25°C for 2 minutes to obtain an integrally formed inductor coil.

[0061] Comparative Example 1

[0062] The commercially available enameled wire was heat treated. The microstructure of the enameled wire before heat treatment is as follows: Figure 7 As shown, after heat treatment Figure 8 As shown. Figure 8 It can be seen that the insulation layer of the enameled wire has been completely destroyed and turned into a conductor. Compared with Example 1, it can be seen that the insulation layer prepared in Example 1 has good temperature resistance.

[0063] Table 1 Primary insulating liquid components of Examples 1-3

[0064] Components Example 1 Example 2 Example 3 Silicate / g 50. Sodium silicate 120. Potassium silicate 22. Lithium silicate Nitride / g 24. Cubic Boron Nitride 34. Hexagonal Boron Nitride 26. Aluminum Nitride <![CDATA[Y2O3 / g]]> 2 2 0 <![CDATA[Bi2O3 / g]]> 2 2 0 <![CDATA[TiO2 / g]]> 2 2 0 Water / g 100 100 100

[0065] Table 2 Secondary insulating liquid components of Examples 1-3

[0066]

[0067]

[0068] The resistance of the inductor coils of Examples 1-3 and the comparative example was tested, and the test results are shown in Table 3.

[0069] Table 3 Resistance of Examples 1-3 and Comparative Example 1

[0070]

[0071] It can be seen from Table 3 that the resistance of the one-piece molded inductor coils of Examples 1-3 is significantly higher than the resistance of the commercially available enameled wire, and the one-piece molded inductor coils of Examples 1-3 can still maintain good resistance after high-temperature heat treatment and have better heat resistance.

Claims

1. A method for preparing an integrally formed inductor coil, characterized in that: The following steps are involved: ①Preparing a primary insulating liquid: Mixing silicate, nitride, Y2O3, Bi2O3, TiO2 and water to form a primary insulating liquid; ② Primary insulation: Place the metal coil in the primary insulation liquid, soak for 0.1-500 minutes, then take out the coil to obtain the primary insulation coil; ③Preparing secondary insulating liquid: mixing silicone resin and nitride to obtain secondary insulating liquid; ④ Secondary insulation: Place the primary insulated coil in step ② in a secondary insulating liquid, soak for 0.1-500 minutes, then take out the coil to obtain a secondary insulated coil; ⑤ Heat treatment: Calcine the secondary insulated coil in a non-oxidizing atmosphere at a temperature of 80 to 400°C.

2. The method for preparing an integrally formed inductor coil according to claim 1, characterized in that: The silicate is one or more of lithium silicate, ammonium silicate, sodium silicate and potassium silicate.

3. The method for preparing an integrally formed inductor coil according to claim 1, characterized in that: The nitride in step ① is one or more of aluminum nitride, hexagonal boron nitride, cubic boron nitride, titanium nitride, tantalum nitride, vanadium nitride, phosphorus nitride, silicon nitride, lithium nitride and magnesium nitride.

4. The method for preparing an integrally formed inductor coil according to claim 3, characterized in that: The particle size d of the nitride 10 <10μm,d 50 <30μm,d 99 <60μm.

5. The method for preparing an integrally formed inductor coil according to claim 1, characterized in that: The ratio of the surface area of ​​the metal coil in step ② to the volume of the primary insulating liquid is (0.01-200 cm 2 ):1cm 3 The immersion temperature is -5 to 100°C; the ratio of the surface area of ​​the metal coil to the volume of the secondary insulating liquid in step ④ is (0.01 to 200 cm 2 ):1cm 3 , the soaking temperature is -5 to 100°C.

6. The method for preparing an integrally formed inductor coil according to claim 1, characterized in that: The nitride in step ③ is one or more of aluminum nitride, hexagonal boron nitride, cubic boron nitride, titanium nitride, tantalum nitride, vanadium nitride, phosphorus nitride, silicon nitride, lithium nitride and magnesium nitride.

7. The method for preparing an integrally formed inductor coil according to claim 1, characterized in that: The chemical formula of the silicone resin is [(CH3) x (R) y (SiO2) 4-x-y ] n , x is the number of methyl groups on the silicon atom, y is the number of R groups, and x+y≤4.

8. The method for preparing an integrally formed inductor coil according to claim 1, characterized in that: In step ①, the mass ratio of nitride to water is 0.05-80:100; the mass ratio of silicate to water is 0.03-2:1; the mass ratio of Y2O3 to water is 0-0.5:1; the mass ratio of Bi2O3 to water is 0-0.5:1; and the mass ratio of TiO2 to water is 0-0.5:

1.

9. The method for preparing an integrally formed inductor coil according to claim 1, characterized in that: In the step ③, the mass ratio of silicone resin to nitride is 100:0.1-60.

Citation Information

Cited By

  • Inorganic insulation integrally-formed power inductor and preparation method thereof

    CN120690589A