Micro-LED light-emitting structure, manufacturing method thereof and electronic equipment

By using dry etching mask passivation layer and wet process in the Micro-LED device to remove the pixel isolation portion to form a step pixel structure without sidewall damage, the sidewall damage problem caused by conventional dry etching is solved. The electro-optical conversion efficiency and external quantum efficiency are improved, and the production process is simplified.

CN118919614APending Publication Date: 2024-11-08SHENZHEN SITAN TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411177575.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The sidewall damage caused by conventional dry etching during the production process of Micro-LED devices affects the electro-optical conversion efficiency, and the small-sized pixel sidewall effect leads to low external quantum efficiency, and the prior art fails to completely prevent or remove sidewall damage.

Method used

The buffer layer and epitaxial layer are grown on the substrate, a mask passivation layer is formed and the pixel space and isolation portion are formed by dry etching, and then the quantum well luminescent layer, an electron restriction layer and a current diffusion layer are deposited layer by layer, combined with wet The pixel isolation part is removed by a process to form a step pixel structure without side wall damage.

Benefits of technology

The Micro-LED luminescent structure without sidewall damage is realized, which improves the electro-optical conversion efficiency and external quantum efficiency, simplifies the production process, and avoids defects and damage caused by traditional dry etching.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919614A_ABST
    Figure CN118919614A_ABST
Patent Text Reader

Abstract

The invention provides a manufacturing method of a Micro-LED light-emitting structure, the Micro-LED light-emitting structure and electronic equipment. The manufacturing method comprises the steps of growing a buffer layer and an epitaxial layer on a substrate, forming a mask passivation layer on the epitaxial layer, performing dry etching on the mask passivation layer to form a plurality of pixel spaces and a plurality of pixel isolation parts, and forming a quantum well light-emitting layer, an electron limiting layer and a current diffusion layer on the etched mask passivation layer layer by layer, and etching the pixel isolation part by applying a wet process until the epitaxial layer is exposed to obtain a step pixel structure with an intact side wall formed in the pixel space. The side wall of the Micro-LED light-emitting structure manufactured by the method is intact, the photoelectric efficiency is improved, and the processing flow of the light-emitting structure is simplified by the method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a Micro-LED device, and in particular, to the fabrication of a Micro-LED light-emitting structure. Background Art

[0002] Micro-LED display technology is a display technology that miniaturizes and arrays the traditional LED structure and uses CMOS or TFT to make the driving circuit to achieve addressing control and individual driving of each pixel. With the development of technology, the pixel size of Micro-LED is getting smaller and smaller. At present, the pixel size of Micro-LED related products, especially AR / VR related products, can be made to 5um or even smaller. Electronic devices that require the use of Micro-LED devices, especially AR / VR wearable devices, have high brightness and low power consumption as their most significant characteristics. To achieve high brightness and low power consumption, high electro-optical conversion efficiency is required. However, on the one hand, the sidewall damage caused by conventional dry etching will adversely affect the electro-optical conversion efficiency of the Micro-LED device. On the other hand, according to the characteristics of the LED itself, the smaller the size, the more obvious the sidewall effect (the adverse effect of non-radiative recombination centers caused by pixel sidewall defects on luminous efficiency) and the lower the EQE (External Quantum Efficiency) efficiency. The industry and scientific research community are both developing how to reduce sidewall etching damage and how to repair the sidewall, but no solution has been proposed to completely prevent or remove sidewall damage. Summary of the invention

[0003] The purpose of this application is to provide a technical solution for manufacturing a Micro-LED light-emitting structure without sidewall damage and without the need to repair the sidewalls.

[0004] In order to achieve the above-mentioned purpose, in the first aspect of the present application, a method for manufacturing a Micro-LED light-emitting structure is proposed, comprising the following steps:

[0005] growing a buffer layer and an epitaxial layer on the substrate;

[0006] forming a mask passivation layer on the epitaxial layer;

[0007] dry etching the mask passivation layer to form a plurality of pixel spaces and a plurality of pixel isolation parts;

[0008] forming a quantum well light-emitting layer, an electron confinement layer and a current diffusion layer layer by layer on the etched mask passivation layer;

[0009] The pixel isolation portion is etched using a wet process until the epitaxial layer is exposed, thereby obtaining a step pixel structure with a complete side wall formed in the pixel space.

[0010] Optionally, a transition improvement layer is formed between the epitaxial layer and the quantum well light-emitting layer, and the epitaxial layer and the transition improvement layer are formed of the same material.

[0011] Optionally, the mask passivation layer is formed to have a thickness greater than that of the pixel structure or higher than the horizontal position of the current diffusion layer, and the pixel space is formed to have a vertical or inclined sidewall.

[0012] Optionally, the pixel structure is formed such that the size of the current diffusion layer is the same as the size of the upper end surface of the step.

[0013] Optionally, the method further comprises the following steps:

[0014] Depositing an electrode metal layer includes forming a P electrode on the pixel structure and an N electrode on the exposed portion of the epitaxial layer, wherein the P electrode and the N electrode have a wide bottom extending laterally and a vertical portion extending vertically and are flush with the top to allow bonding metals to be at the same horizontal position.

[0015] Optionally, the method further comprises the following steps:

[0016] Depositing a protective passivation layer to cover the epitaxial layer, the pixel structure, and the P electrode and the N electrode;

[0017] Etching the protective passivation layer to expose the P electrode and the N electrode;

[0018] Bonding metal is deposited on the exposed P-electrode and N-electrode.

[0019] According to the second aspect of the present application, a Micro-LED light-emitting structure is provided, comprising: a substrate, an epitaxial layer on the substrate, and a plurality of step pixel structures on the epitaxial layer, the pixel structure comprising a quantum well light-emitting layer, an electron confinement layer and a current diffusion layer formed layer by layer, wherein the pixel structure has side walls with intact microstructure.

[0020] Optionally, the size of the current diffusion layer of the pixel structure is the same as the size of the upper end surface of the step.

[0021] Optionally, the Micro-LED light-emitting structure also includes a P electrode formed on the pixel structure and an N electrode on the epitaxial layer, a protective passivation layer covering the P electrode, the N electrode, the pixel structure and the epitaxial layer, and a bonding metal formed on the P electrode and the N electrode, wherein the P electrode and the N electrode are exposed from an opening at the top of the protective passivation layer and are in contact with the bonding metal, and the P electrode and the N electrode include a wide bottom extending laterally and a vertical portion extending vertically and are flush with the top so that the bonding metal is located at the same horizontal position.

[0022] According to the third aspect of the present application, an electronic device is provided, which includes a Micro-LED light-emitting structure manufactured using the method of the first aspect of the present application or the Micro-LED light-emitting structure of the second aspect of the present application, and the electronic device is an AR / VR wearable device.

[0023] The technical solution provided by the embodiments of the present application may include the following beneficial effects: a pixel structure is manufactured using a dry-etched mask passivation layer combined with a wet process to selectively remove the pixel isolation portion and the pixel structure thereon, so that a pixel structure with straight and complete side walls and no surface defects or grain damage can be obtained; the mask passivation layer provides a clear boundary for the pixel structure to be manufactured, which is conducive to the wet process to accurately remove redundant pixel structures and obtain a pixel structure in which the current diffusion layer is the same size as the upper end surface of the step; the pixel structure can be manufactured on the entire area of ​​the mask passivation layer, and there is no need to use a pixel mask that requires precise alignment to form the pixel structure, thereby simplifying the manufacturing process of the pixel structure. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The drawings constituting a part of this application are used to provide a further understanding of this application, so that other features, purposes and advantages of this application become more obvious. The schematic embodiment drawings and their descriptions of this application are used to explain this application and do not constitute an improper limitation on this application. In the drawings:

[0025] Figure 1 is a schematic cross-sectional view of an epitaxial growth structure of a Micro-LED light-emitting structure according to an embodiment of the present application;

[0026] Figure 2 A schematic diagram of forming a pre-mask passivation layer in a method for manufacturing a Micro-LED light emitting structure according to an embodiment of the present application;

[0027] Figure 3 A schematic diagram of forming a partition mask in a method for manufacturing a Micro-LED light emitting structure according to an embodiment of the present application;

[0028] Figure 4 A schematic diagram of depositing a pixel structure array on a partition mask in a method for manufacturing a Micro-LED light-emitting structure according to an embodiment of the present application;

[0029] Figure 5 A schematic diagram of selectively retaining a portion of a pixel structure in a method for manufacturing a Micro-LED light-emitting structure according to an embodiment of the present application;

[0030] Figure 6 It is a schematic cross-sectional view of a Micro-LED light-emitting structure according to an embodiment of the present application. DETAILED DESCRIPTION

[0031] In order to enable those skilled in the art to better understand the solution of the present application, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present application.

[0032] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequential order. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present application described here. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device comprising a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0033] In the present application, the terms "upper", "lower", "left", "right", "front", "back", "top", "bottom", "inner", "outer", "middle", "vertical", "horizontal", "lateral", "longitudinal" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the drawings. These terms are mainly used to better describe the present application and its embodiments, and are not used to limit the indicated devices, elements or components to have a specific orientation, or to be constructed and operated in a specific orientation.

[0034] In addition, some of the above terms may be used to express other meanings in addition to indicating orientation or positional relationship. For example, the term "on" may also be used to express a certain dependency or connection relationship in some cases. For those of ordinary skill in the art, the specific meanings of these terms in this application can be understood according to specific circumstances.

[0035] In addition, the terms "installed", "set", "provided with", "connected", "connected", and "socketed" should be understood in a broad sense. For example, "connection" can be a fixed connection, a detachable connection, or an integral structure; it can be a mechanical connection or an electrical connection; it can be a direct connection, or an indirect connection through an intermediate medium, or it can be an internal connection between two devices, elements, or components. For those of ordinary skill in the art, the specific meanings of the above terms in this application can be understood according to specific circumstances.

[0036] The present application aims to provide a Micro-LED light-emitting structure with no sidewall damage and a method for manufacturing the same. The intact sidewalls of the pixel structure can provide high electro-optical conversion efficiency and external quantum efficiency, reduce the sidewall effect, and produce high-brightness and low-power Micro-LED products.

[0037] At present, one of the commonly used methods for making Micro-LED pixel structures is "growing a flat layer structure + etching the redundant structure", and the other is "forming a pixel retaining wall + filling the pixel structure". In the first method, only dry etching is suitable for removing redundant pixel structures. The dry etching process will cause damage to the sidewalls of the pixel structure, affecting the photoelectric conversion efficiency; in the second method, the pixel retaining wall will affect the light emission from the edge of the pixel structure and occupy more space.

[0038] To this end, the present application provides a "growing pixel array + selective retention" solution, which is to make a partition mask by prefabricating a mask passivation layer on the epitaxial layer, depositing a pixel structure layer on part or the entire surface of the partition mask to form a pixel structure array, and then using a wet process to selectively remove the structure around the pixel structure to be retained to obtain a complete pixel structure without sidewall defects and damage. Compared with the traditional method of dry etching the pixel structure layer to form a pixel structure, and using a mask to fill the pixel structure in the pixel area, the sidewalls of the pixel structure produced by the solution of the present application are completely free of damage and defects, and the production process is simplified. Since a partition mask is used, it is not required to use a mask for forming a pixel structure and a precise alignment process, or at least allows for a more generous tolerance for the pixel mask and alignment process.

[0039] The specific implementation of the present application is described below by way of examples with reference to the accompanying drawings.

[0040] Figure 1 It is an example of the epitaxial growth structure of the Micro-LED light-emitting structure (optical chip) according to the present application. The epitaxial growth structure includes from bottom to top: a substrate 100, a buffer layer 101 and an epitaxial layer 102 grown above the substrate 100, and a plurality of step (mesa) pixel structures D grown on the epitaxial layer 102. Depending on the material of the substrate 100, the buffer layer 101 is optional. In the case of using a sapphire substrate, due to the difference in lattice constants between the substrate 100 and the epitaxial layer 102, a buffer layer 101 is usually grown on the substrate 100 as a transition layer to reduce heterogeneous structure growth defects. Figure 1The step pixel structure D includes, for example, a transition improvement layer 104, a quantum well light emitting layer 105, an electron confinement layer 106, and a current diffusion layer 107, which are formed layer by layer from bottom to top by deposition. The transition improvement layer 104 is used to remove the influence of the previous process on the surface of the epitaxial layer 102. The transition improvement layer 104 is optional and the material can be the same as that of the epitaxial layer 102. The current diffusion layer 107 can be deposited by evaporation and combined with an annealing process to repair possible lattice damage and increase diffusion.

[0041] The pixel structure D of the Micro-LED light-emitting structure of the present application has a sidewall with a complete microstructure and no damage, and no sidewall repair is required. Whether the microstructure of the sidewall is intact is determined by microscopic inspection. According to an example of the present application, FIB (Focused Ion Beam) and SEM / EDS can be used to detect the microstructure of the pixel structure D. The results of analyzing the sidewall and cross-section of the pixel structure D show that the sidewall is straight and complete without surface defects and grain damage, indicating that the sidewall microstructure is intact. According to the detection requirements, the cross-section of the entire light-emitting structure can be analyzed to comprehensively detect the microstructure of all pixel structures D.

[0042] The Micro-LED light-emitting structure having the above structure is obtained by a new manufacturing method. According to the present application, a method for manufacturing a Micro-LED light-emitting structure without sidewall damage is also provided. Figures 2 to 6 Describe the specific steps of the method.

[0043] refer to Figure 2 , first grow a buffer layer 101 and an epitaxial layer 102 on a substrate 100. Before growth, the surface of the substrate 100 is cleaned with H2. The growth of the buffer layer 101 includes three-dimensional growth and two-dimensional growth. The epitaxial layer 102 is grown at a high temperature, which will be described in more detail later.

[0044] Continue to refer Figure 2 , a mask passivation layer 103 is deposited on the epitaxial layer 102 to form.

[0045] refer to Figure 3 , a plurality of pixel spaces 103a penetrating the mask passivation layer 103 and a plurality of pixel isolation portions 103b formed by the mask passivation layer 103 itself are produced on the mask passivation layer 103 by dry etching. The mask passivation layer 103 after etching is used to produce a pixel structure array. In this article, the mask passivation layer 103 after etching is referred to as a partition mask 103m.

[0046] like Figure 3As shown. The pixel space 103a penetrates the mask passivation layer 103 and exposes a portion of the epitaxial layer 102, and the pixel isolation portion 103b is defined by the non-penetrating portion of the mask passivation layer 103 and covers another portion of the epitaxial layer 102. The pixel space 103a can be formed to have a vertical or inclined sidewall, thereby forming a pixel structure D with a corresponding configuration, and the wet process is conducive to using this flexible design.

[0047] exist Figure 4 In the example, a transition improvement layer 104, a quantum well light-emitting layer 105, an electron confinement layer 106 and a current diffusion layer 107 are fabricated on the entire area of ​​the partition mask 103m formed by the pixel space 103a and the pixel isolation portion 103b to form a pixel structure array. All pixel structures D formed by deposition form an array with different heights. The pattern of the partition mask 103m itself divides the deposited pixel structures D into different areas, and there are clear boundaries between the pixel structures D in different areas. Since the pixel isolation portion 103b defines the height and boundary of the pixel space 103a, the wet process can easily remove the pixel isolation portion 103b and the pixel structure D thereon, and obtain a pixel structure D in which the current diffusion layer 107 is the same size as the upper end surface of the step.

[0048] Depositing the pixel structure D on the entire area of ​​the partition mask 103m is very beneficial for simplifying the process flow, especially for making tiny pixel structures. It can save the process of making a photoresist mask for precise etching and precise alignment during etching, which not only saves time but also simplifies the process. At the same time, the partition structure provided by the partition mask 103 allows the formation of a pixel structure array with clear boundaries between units, providing a favorable structural basis for the subsequent wet removal step. In other embodiments, the pixel structure array is formed only in the area of ​​the pixel space 103a of the partition mask 103m, and the structure around the pixel structure D (the structure of the partition mask 103m) is subsequently removed. In this case, a pixel mask will be used, but the wet process allows a sufficiently wide processing tolerance, thereby simplifying the processing process.

[0049] In one embodiment, the process of making the partition mask 103m specifically includes the following steps:

[0050] a. Spin-coating a photoresist on the mask passivation layer 103;

[0051] b. After exposure and development, a pixel area (not shown) is exposed on the photoresist to obtain a photoresist mask, wherein the position of the pixel area corresponds to the area where the pixel space 103a is to be formed on the mask passivation layer 103;

[0052] c. Using a photoresist mask, the SiO2 / SiN passivation layer of the pixel area is removed by dry etching to obtain a SiO2 / SiN partition mask 103m having a pixel space 103a and a pixel isolation portion 103b;

[0053] d. Remove the photoresist using an organic solution such as acetone.

[0054] refer to Figure 5 , the pixel isolation part 103b and the pixel structure D thereon are selectively removed by a wet process until the epitaxial layer 102 is exposed, while the pixel structure D formed in the pixel space 103a in the pixel structure array is retained to obtain a step pixel structure D with a straight sidewall and no surface defects and grain damage, and the retained pixel structure D is used as the light-emitting area. Figure 5 In the example of , the pixel structure D has a vertical sidewall, and the transition improvement layer 104, the quantum well light emitting layer 105 and the electron confinement layer 106 have the same area as the current diffusion layer 107. In other embodiments, the pixel structure D may be formed to have an inclined sidewall, and the sidewall may be a curved surface.

[0055] The Micro-LED light-emitting structure and its manufacturing method of the present application have the following advantages: the side wall of the pixel structure D is intact without surface defects and grain damage, and the integrity of the microstructure can significantly improve the external quantum efficiency and electro-optical conversion efficiency; the partition mask 103m provides a clear boundary for the pixel structure D to be manufactured, allowing the pixel structure D to be deposited on the entire area of ​​the partition mask 103m, and the deposition process does not require the use of a pixel mask and a precise alignment process, thereby simplifying the processing flow; the process of wet removal of the pixel structure D can provide surface finishing for the side wall of the pixel structure D to be retained, making the side wall of the pixel structure D flatter; the partition mask 103m combined with the wet removal can simply obtain a pixel structure D with the current diffusion layer 107 having the same size as the upper end face of the step, and the removal process does not require a dedicated mask and an alignment process; the partition mask 103m can be used to manufacture Micro-LED light-emitting structures with micro-size and macro-pitch pixel structures D, and the size and arrangement of the pixels can be more flexible and diverse. The process of manufacturing the pixel structure D of the present application does not involve any process that would damage the sidewalls, and thus a pixel structure D with intact sidewalls can be obtained. The existing manufacturing process cannot manufacture a pixel structure D with no sidewall damage at all as in the present application.

[0056] Other aspects and advantages of the present application will be described below with reference to the accompanying drawings.

[0057] The above steps produce the epitaxial growth structure of the Micro-LED light-emitting structure. Figure 6 , which shows how to make the electrode structure of the Micro-LED light-emitting structure, specifically including the following steps:

[0058] The electrode metal layer is deposited, including forming a P electrode 110a on the pixel structure D and an N electrode 110b on the exposed portion of the epitaxial layer 102, wherein the P electrode 110a and the N electrode 110b have a wide bottom 110c extending laterally and a vertical portion 110d extending vertically upward. Figure 6 In the example, the tops of the P electrode 110a and the N electrode 110b are flush, so that the multiple bonding metals 112 formed subsequently are at the same horizontal position, and the manufactured light-emitting structure has a regular geometric shape as a whole.

[0059] A protective passivation layer 111 is deposited to cover the epitaxial layer 102, the pixel structure D, and the P electrode 103a and the N electrode 103b. The protective passivation layer 111 is deposited along the boundaries and sidewalls of the above structure, so it has a high and low structure. Such a configuration saves space and is conducive to the light output of the pixel structure D and the arrangement of additional structures.

[0060] The protective passivation layer 111 is etched to provide a top opening to expose the P-electrode 110 a and the N-electrode 110 b .

[0061] A bonding metal 112 is deposited on the exposed top of the P-electrode 110 a and the N-electrode 110 b for connecting to a driving board or a packaging substrate.

[0062] An independent and complete Micro-LED light-emitting structure is manufactured through the above steps.

[0063] Figure 6 The Micro-LED light emitting structure in the example is a normal structure. It should be understood that Figure 1 The epitaxial growth structure of the display is also suitable for flip-chip structures, and the corresponding electrodes and other structures can be processed according to product requirements. The processing includes the deposition and etching of protective passivation layers, the deposition of P / N electrodes of pixel structure D, the deposition of bonding metals, and the selection of deposition and etching processes.

[0064] Continue to refer Figure 6 Specifically, the P electrode 110a and the N electrode 110b have a wide bottom 110c extending laterally and a vertical portion 110d extending vertically upward, and the top of the vertical portion 110d is exposed from the opening of the protective passivation layer 111. The protective passivation layer 111 is formed by, for example, atomic layer deposition, and adheres to and covers the surface, sidewalls, and edges of the epitaxial layer 102, the pixel structure D, the P electrode 110a, and the N electrode 110b, providing protection against air erosion.

[0065] The following will describe by way of example how to select the material and processing technology of the epitaxial growth structure and the electrode structure to achieve the required chip performance.

[0066] Epitaxial growth structure:

[0067] The substrate 100 is a sapphire, Si, or SiC substrate. In the case of using sapphire, a buffer layer 101 should usually be grown on the substrate 100 first, and the buffer layer 101 grows into U-GaN. In the present application, three-dimensional GaN growth is first performed on the substrate 100, and the growth temperature should be increased during the growth process. During the temperature increase process, GaN seeds are formed, and three-dimensional GaN growth is performed on this basis. After the three-dimensional growth of GaN is completed, two-dimensional growth of GaN is performed to fill the uneven area of ​​the three-dimensionally grown buffer layer 101. The epitaxial layer 102 is formed of GaN and grows into N-GaN at high temperature, in which donor impurities such as Si are doped to provide N-type carriers for the N-GaN layer.

[0068] The mask passivation layer 103 is formed by growing SiO2 or SiN at a growth temperature above 600°C to ensure that the formed mask passivation layer 103 can withstand the subsequent growth temperature of the quantum well light emitting layer 105 and the electron confinement layer 106. The thickness T of the mask passivation layer 103 (please refer to Figure 4 ) should be greater than the thickness of the pixel structure D or higher than the height of the electron confinement layer 106 of the pixel structure D. On the one hand, this ensures that a pixel structure array with clear boundaries can be formed on the partition mask 103m, and ensures that the wet process can completely remove the pixel isolation portion 103b and the pixel structure D thereon. On the other hand, after the wet removal, the pixel structure D having the same size as the upper end surface of the step structure can be obtained, without the need for photolithography alignment. In one embodiment of the present application, the mask passivation layer 103 can be grown using a conventional LPCVD (Low Pressure Chemical Vapor Deposition) method. In the case of using SiO2 to grow the mask passivation layer 103, a SiO2 layer is formed by reacting a reactive gas precursor such as silane with oxygen or ozone on the substrate 100, and the reaction temperature is generally 700-800° C.; in the case of using SiC to grow the mask passivation layer 103, silane and ammonia are used to react at low pressure and high temperature (e.g., 700-900° C.) on the substrate 100 to form a SiN layer. In other embodiments, the mask passivation layer 103 may be formed by growing SiO2 or SiN using APCVD or molecular beam MBE.

[0069] After the mask passivation layer 103 is formed, in one embodiment of the present application, a photoresist mask (not shown) is made on the mask passivation layer 103 using a yellow light process, and then the passivation layer at the position where the pixel space 103a is to be formed is removed by dry etching, and then the photoresist mask is removed using an organic solution such as acetone to obtain a partition mask 103m. Figure 3As shown. F-based gas can be selected as the dry etching gas, and no or less argon gas can be added to remove or reduce the roughness of the bottom surface of the mask passivation layer 103 caused by the physical etching of argon ions. In addition, the epitaxial growth structure with the partition mask 103m can be cleaned by using deionized water and ultrasound.

[0070] Among the multiple layers constituting the pixel structure D, the quantum well light-emitting layer 105 is formed of InGan / GaN, the electron confinement layer 106 is formed of P-GaN, and the current diffusion layer 107 is formed of ITO / ZnO. Since the process of dry etching the mask passivation layer 103 will affect the surface of the epitaxial layer 102 (for example, surface roughness, grain damage), it is preferred to grow a transition improvement layer 104 for depositing the quantum well light-emitting layer 105 between the epitaxial layer 102 and the quantum well light-emitting layer 105, and its material is, for example, N-GaN, which is the same as the epitaxial layer 102. The quantum well light-emitting layer 105 is the light-emitting area of ​​the Micro-LED optical chip, in which multiple pairs of quantum wells are formed by alternating growth of InGaN / GaN. The confined space in the multiple quantum wells restricts the movement of electrons and holes, so that the light is completely compounded in this area, and the light emission wavelength and light emission intensity are determined by the material and bandgap width of the quantum well light-emitting layer 105. The growth of P-GaN of the electron confinement layer 106 includes the growth of PAlGaN and Mg-doped PGaN, wherein PAlGaN is a matrix layer, the primary purpose of which is to confine electrons in the quantum well light-emitting layer 105 so that the electrons can completely radiate and recombine to improve the internal quantum efficiency (Internal Quantum Efficiency, IQE), and the purpose of growing Mg-doped GaN is to make GaN present a P-type to become a P-GaN layer, so as to provide holes for radiating and recombinating with electrons. The current diffusion layer 107 is formed by evaporation deposition of ITO / ZnO, and annealing is performed after formation.

[0071] In the process of retaining part of the pixel structure D in the pixel structure array by applying a wet process, according to one embodiment, a BOE solution is used for immersion removal, and the BOE solution is a mixed solution of HF and NH4F. The Micro-LED optical chip with the pixel structure array is immersed in the BOE solution, and the SiO2 / SiN pixel isolation part 103b and the pixel structure D thereon are removed by the chemical reaction between F ions and Si atoms, while retaining the pixel structure D on the epitaxial layer 102. The BOE immersion time is determined by the thickness of the mask passivation layer 103 and the reaction rate with the BOE solution.

[0072] Electrode structure:

[0073] According to the embodiment of the present application, the metal materials of the P electrode 110a and the N electrode 110b include but are not limited to: Ti, Al, Au, Pt, Ni, and are formed by deposition. The material of the protective passivation layer 111 can be the same as that of the mask passivation layer 103, and the available materials include but are not limited to: SiO2, SiN or Al2O3 and other insulating materials or their combinations. The material of the bonding metal 112 includes but is not limited to: Sn, In, Au. It should be understood that Figure 6 The configuration of the positions of the P electrode 110a, the N electrode 110b, and the bonding metal 112 is only an example of a positive structured light chip. Based on the epitaxial growth structure of the present application, the positions of the P electrode 110a, the N electrode 110b, and the bonding metal 112 can be arranged and a suitable configuration can be designed according to product requirements to prepare Miro-LED light-emitting structures with different bonding methods.

[0074] According to the present application, an electronic device configured with the above-mentioned Micro-LED light-emitting structure, or configured with a Micro-LED light-emitting structure manufactured using the above-mentioned method, such as an AR / VR wearable device, is also provided, and the Micro-LED light-emitting structure provides a display function for the electronic device.

[0075] In summary, in the present application, the partition mask 103m and the wet process can be used to produce a pixel structure D with intact sidewalls without damage, thereby preventing low light efficiency caused by sidewall damage; the processing flow of the Micro-LED light-emitting structure can be reduced and production efficiency can be improved; a current diffusion layer 107 with the same size as the upper end surface of the step pixel structure D can be easily produced, thereby improving light extraction efficiency.

[0076] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.

Claims

1. A method for manufacturing a Micro-LED light-emitting structure, characterized in that: The following steps are involved: Growing a buffer layer (101) and an epitaxial layer (102) on a substrate (100); forming a mask passivation layer (103) on the epitaxial layer; Dry etching the mask passivation layer to form a plurality of pixel spaces (103a) and a plurality of pixel isolation portions (103b); Forming a quantum well light-emitting layer (105), an electron confinement layer (106) and a current diffusion layer (107) layer by layer on the etched mask passivation layer; The pixel isolation portion is etched using a wet process until the epitaxial layer is exposed, thereby obtaining a step pixel structure with a complete sidewall formed in the pixel space.

2. The method according to claim 1, characterized in that A transition improvement layer (104) is formed between the epitaxial layer and the quantum well light-emitting layer, and the epitaxial layer and the transition improvement layer are formed of the same material.

3. The method according to claim 1, characterized in that The mask passivation layer is formed to have a thickness greater than that of the pixel structure or higher than the horizontal position of the current diffusion layer, and the pixel space is formed to have a vertical or inclined sidewall.

4. The method according to claim 1, characterized in that The pixel structure is formed so that the size of the current diffusion layer is the same as the size of the upper end surface of the step.

5. The method according to any one of claims 1 to 4, characterized in that The following steps are also included: Depositing an electrode metal layer includes forming a P electrode (110a) on the pixel structure and forming an N electrode (110b) on the exposed portion of the epitaxial layer, wherein the P electrode and the N electrode are formed to have a laterally extending wide bottom (110c) and a vertically extending vertical portion (110d) and are flush with the top so that the bonding metal is located at the same horizontal position.

6. The method according to claim 5, characterized in that The following steps are also included: Depositing a protective passivation layer (111) to cover the epitaxial layer, the pixel structure, the P electrode and the N electrode; Etching the protective passivation layer to expose the P electrode and the N electrode; A bonding metal (112) is deposited on the exposed P-electrode and the N-electrode.

7. A Micro-LED light-emitting structure, characterized in that: include: A substrate (100), an epitaxial layer (102) on the substrate, and a plurality of stepped pixel structures (D) on the epitaxial layer, wherein the pixel structure comprises a quantum well light-emitting layer (105), an electron confinement layer (106), and a current diffusion layer (107) formed layer by layer, wherein the pixel structure has a side wall with a complete microstructure.

8. The Micro-LED light emitting structure according to claim 7, characterized in that: The size of the current diffusion layer of the pixel structure is the same as the size of the upper end surface of the step.

9. The Micro-LED light emitting structure according to claim 7, characterized in that: It also includes a P electrode (110a) formed on the pixel structure and an N electrode (110b) on the epitaxial layer, a protective passivation layer (111) covering the P electrode, the N electrode, the pixel structure and the epitaxial layer, and a bonding metal (112) formed on the P electrode and the N electrode, wherein the P electrode and the N electrode are exposed from an opening at the top of the protective passivation layer and are in contact with the bonding metal, and the P electrode and the N electrode include a laterally extending wide bottom (110c) and a vertically extending vertical portion (110d) and are flush with the top so that the bonding metal is located at the same horizontal position.

10. An electronic device, characterized in that: It comprises a Micro-LED light-emitting structure manufactured using the method according to any one of claims 1 to 6 or a Micro-LED light-emitting structure according to any one of claims 7 to 9, and the electronic device is an AR / VR wearable device.