ZnAl-LDH functional layer modified aqueous zinc ion battery zinc negative electrode, preparation method thereof and button battery

By preparing the ZnAl-LDH functional layer on the surface of the zinc negative electrode, the corrosion problem caused by the contact between the zinc negative electrode and the electrolyte is solved, the electrochemical performance and cyclic stability are improved, and the commercial application of aqueous zinc ion batteries is supported.

CN118919634APending Publication Date: 2024-11-08SHANGHAI UNIVERSITY OF ELECTRIC POWER
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410970386.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The reactivity of zinc negative electrode and aqueous solution leads to dendrite growth, surface corrosion, and hydrogen evolution problems, which reduces the performance of aqueous zinc ion batteries. In addition, existing LDH materials are prone to fall off during the modification of zinc negative electrodes, increasing interface resistance.

Method used

The ZnAl-LDH functional layer was used to prepare a coating on the surface of the metal zinc sheet by constant potential deposition method to form a ZnAl-LDH coating with good adhesion, overcome the corrosion problems caused by the contact between the zinc negative electrode and the electrolyte, and improve the electrochemical performance.

Benefits of technology

It improves the electrochemical performance of zinc negative electrode, extends the cycle stability and Coulomb efficiency of the battery, reduces dendrites' growth and side reactions, and supports the commercial application of aqueous zinc ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919634A_ABST
    Figure CN118919634A_ABST
Patent Text Reader

Abstract

The invention provides a ZnAl-LDH functional layer modified aqueous zinc ion battery zinc negative electrode, a preparation method thereof and a button battery, and belongs to the field of aqueous zinc ion battery zinc negative electrodes. The preparation method is characterized by comprising the following steps: S1, mixing a zinc salt solution or concentrated nitric acid with an aluminum salt solution to obtain a mixed solution; s2, by taking a metal zinc sheet as a working electrode, an Ag / AgCl electrode as a reference electrode, a Pt sheet as a counter electrode and the mixed solution as an electro-deposition solution, carrying out i-t constant potential deposition by adopting a CHI660 electrochemical workstation to obtain a metal zinc sheet with a ZnAl-LDH coating; and S3, washing and drying the metal zinc sheet with the ZnAl-LDH coating to obtain the ZnAl-LDH functional layer modified aqueous zinc ion battery zinc negative electrode.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of zinc negative electrodes for aqueous zinc ion batteries, and in particular to a zinc negative electrode for aqueous zinc ion batteries modified with a ZnAl-LDH functional layer, a preparation method thereof, and a button battery. Background Art

[0002] Among various energy storage devices, electrochemical energy storage devices have become an important means to accelerate the low-carbon transformation of energy, promote sustainable development, and achieve dual carbon goals due to their advantages of short construction period and abundant resources. At present, lithium-ion batteries (LIBs) are in a leading position in rechargeable batteries with their high specific capacity and high power, and are widely used in portable digital devices and electric vehicles. However, the shortage of lithium resources on the earth, the use of flammable and toxic organic electrolytes in LIBs and other safety issues have seriously restricted their further large-scale application. In recent years, the research on aqueous zinc-ion batteries (AZIBs) has attracted widespread attention, mainly due to their advantages such as high theoretical capacity, suitable plating / stripping potential, good safety, high ionic conductivity, no need for special atmosphere for assembly, low cost, and non-toxicity. However, the reactivity of zinc anode with aqueous solution leads to problems such as dendrite growth, surface corrosion, and hydrogen evolution, which can reduce battery performance. Among the many optimization strategies to improve battery performance, interface coating modification is one of the effective methods.

[0003] Layered double hydroxides (LDH) are an important class of nanostructured materials. With their unique negative ion capacity, anion exchange capacity and barrier properties, they have been widely developed in the field of metal corrosion protection. However, they are rarely used in AZIBs zinc anodes. The existing LDH materials have defects such as non-in-situ coatings that are easy to fall off during the cycle and increase the interface resistance. Therefore, it is worth exploring how to synthesize functional LDH coatings in situ on the surface of zinc anodes to improve the performance of AZIBs. Summary of the invention

[0004] The present invention is made to solve the above problems, and aims to provide a ZnAl-LDH functional layer modified aqueous zinc ion battery zinc negative electrode, a preparation method thereof and a button battery.

[0005] The invention provides a method for preparing a zinc negative electrode of an aqueous zinc ion battery modified by a ZnAl-LDH functional layer. The method has the following characteristics and comprises the following steps: step S1, mixing a zinc salt solution or concentrated nitric acid and an aluminum salt solution to obtain a mixed solution; step S2, using a metal zinc sheet as a working electrode, an Ag / AgCl electrode as a reference electrode, a Pt sheet as a counter electrode, and the mixed solution as an electrodeposition liquid, and performing it constant potential deposition using a CHI660 electrochemical workstation to obtain a metal zinc sheet with a ZnAl-LDH coating; and step S3, washing and drying the metal zinc sheet with the ZnAl-LDH coating to obtain a zinc negative electrode of an aqueous zinc ion battery modified by a ZnAl-LDH functional layer.

[0006] In the preparation method of the ZnAl-LDH functional layer modified aqueous zinc ion battery zinc negative electrode provided by the present invention, it can also have the following characteristics: wherein the aluminum salt solution is obtained by dissolving aluminum salt in water, and the aluminum salt is any one of aluminum nitrate, aluminum carbonate, aluminum sulfate, and aluminum chloride.

[0007] In the preparation method of the ZnAl-LDH functional layer modified aqueous zinc ion battery zinc negative electrode provided by the present invention, it can also have the following characteristics: wherein, in step S1, the zinc salt solution is obtained by dissolving a zinc salt in water, or by reacting an acid with metallic zinc, the zinc salt is any one of zinc nitrate, zinc carbonate, zinc sulfate, and zinc chloride, and the aluminum salt is any one of aluminum nitrate, aluminum carbonate, aluminum sulfate, and aluminum chloride.

[0008] The method for preparing the zinc negative electrode of the aqueous zinc ion battery modified with the ZnAl-LDH functional layer provided by the present invention may also have the following characteristics: wherein, in step S1, the molar ratio of the zinc salt to the aluminum salt is 1:1-5:1, and the concentration of the aluminum salt solution is 0.1 mol / L to 0.5 mol / L.

[0009] The method for preparing the zinc negative electrode of the aqueous zinc ion battery modified with the ZnAl-LDH functional layer provided by the present invention may also have the following characteristics: wherein, in step S1, the molar ratio of concentrated nitric acid to aluminum salt is 1:1-5:1, and the concentration of the aluminum salt is 0.1 mol / L to 0.5 mol / L.

[0010] In the preparation method of the ZnAl-LDH functional layer modified aqueous zinc ion battery zinc negative electrode provided by the present invention, it can also have the following characteristics: wherein, in step S2, the voltage of the constant potential deposition reaction is -1.1V to -1.9V, and the duration is 100s to 1000s.

[0011] The method for preparing the zinc negative electrode of the aqueous zinc ion battery modified with the ZnAl-LDH functional layer provided by the present invention may also have the following characteristics: wherein, in step S3, during rinsing and drying, the metal zinc sheet with the ZnAl-LDH coating is rinsed with water and then dried in an oven at 60°C.

[0012] The present invention also provides a ZnAl-LDH functional layer modified aqueous zinc ion battery zinc negative electrode, which is characterized in that it is prepared by adopting the preparation method of the ZnAl-LDH functional layer modified aqueous zinc ion battery zinc negative electrode.

[0013] The present invention provides a button battery, characterized in that the zinc negative electrode of the aqueous zinc ion battery modified by the ZnAl-LDH functional layer is used as the negative electrode.

[0014] The button battery provided by the present invention may also have the following characteristics: the button battery is obtained by assembling the zinc negative electrode of the aqueous zinc ion battery modified with the ZnAl-LDH functional layer in combination with the positive electrode material and the electrolyte.

[0015] Functions and Effects of the Invention

[0016] According to the ZnAl-LDH functional layer modified aqueous zinc ion battery zinc negative electrode, its preparation method and button battery involved in the present invention, because the ZnAl-LDH coating is prepared on the surface of the metal zinc sheet by a simple constant potential deposition method, it has good adhesion to the substrate and improves the electrochemical performance of the metal zinc sheet as the negative electrode of AZIBs, and can overcome the corrosion problem caused by the contact between the zinc negative electrode and the electrolyte in AZIBs and the influence of the coating material and inactive material added to the zinc negative electrode by the squeeze casting technology on the battery performance. The preparation method of the present invention is simple, environmentally friendly, meets the needs of the sustainable development concept, and provides strong support for the commercial application of AZIBs. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 This is a SEM image of the zinc negative electrode of the aqueous zinc ion battery modified by the ZnAl-LDH functional layer in Example 1 of the present invention.

[0018] Figure 2 It is a cycle comparison of the aqueous zinc ion battery zinc negative electrode modified with the ZnAl-LDH functional layer in Example 1 of the present invention and a blank metal zinc negative electrode after being assembled into symmetrical batteries.

[0019] Figure 3 It is a comparison of the cycle conditions and coulombic efficiency of the zinc negative electrode of the aqueous zinc ion battery modified with the ZnAl-LDH functional layer in Example 1 of the present invention and a blank metal zinc negative electrode after being assembled into full batteries. DETAILED DESCRIPTION

[0020] The present invention provides a ZnAl-LDH functional layer modified aqueous zinc ion battery zinc negative electrode and a preparation method thereof, the preparation method comprising the following steps:

[0021] Step S1, mixing a zinc salt solution or concentrated nitric acid and an aluminum salt solution to obtain a mixed solution. The zinc salt solution is obtained by dissolving a zinc salt in water, or by reacting an acid with metallic zinc. The aluminum salt solution is obtained by dissolving an aluminum salt in water. The zinc salt is any one of zinc nitrate, zinc carbonate, zinc sulfate, and zinc chloride, and the aluminum salt is any one of aluminum nitrate, aluminum carbonate, aluminum sulfate, and aluminum chloride. The molar ratio of the zinc salt to the aluminum salt is 1:1-5:1, or the molar ratio of concentrated nitric acid to the aluminum salt is 1:1-5:1. The concentration of the aluminum salt solution is 0.1 mol / L to 0.5 mol / L.

[0022] Step S2, using the metal zinc sheet as the working electrode, the Ag / AgCl electrode as the reference electrode, the Pt sheet as the counter electrode, and the mixed solution as the electrodeposition solution, using a CHI660 electrochemical workstation to perform it constant potential deposition, the voltage of the constant potential deposition reaction is -1.1V to -1.9V, and the duration is 100s to 1000s, to obtain a metal zinc sheet with a ZnAl-LDH coating.

[0023] Step S3, washing the metal zinc sheet with the ZnAl-LDH coating with water, and then drying it in an oven at 60° C. to obtain a ZnAl-LDH functional layer modified aqueous zinc ion battery zinc negative electrode.

[0024] The water used in the above steps can be any one of deionized water, ultrapure water and triple-distilled water.

[0025] The present invention also provides a button battery, which is prepared by using the above-mentioned ZnAl-LDH functional layer modified aqueous zinc ion battery zinc negative electrode as the negative electrode, and assembling it in combination with a positive electrode material and an electrolyte.

[0026] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the following examples and drawings specifically describe the zinc negative electrode of the aqueous zinc ion battery modified with the ZnAl-LDH functional layer, its preparation method and button battery of the present invention.

[0027] Example 1

[0028] A ZnAl-LDH functional layer modified aqueous zinc ion battery zinc negative electrode and a preparation method thereof of the present embodiment, the preparation method comprising the following steps:

[0029] Step S1, prepare 30 ml of 0.3 mol / L Al(NO3)3 solution (referred to as solution A), add 2 ml of concentrated HNO3 (referred to as solution B) into 10 ml of deionized water, mix solution A and solution B to obtain a mixed solution.

[0030] Step S2, using the metal zinc sheet as the working electrode, the Ag / AgCl electrode as the reference electrode, the Pt sheet as the counter electrode, and the mixed solution prepared in step S1 as the electrodeposition solution, using a CHI660 electrochemical workstation to perform it constant potential deposition, setting the voltage to -1.7V, and the deposition time to 300s, to obtain a metal zinc sheet with a ZnAl-LDH coating.

[0031] Step S3, rinsing the metal zinc sheet with the ZnAl-LDH coating obtained in step S2 with deionized water, and then drying it in an oven at 60° C. to obtain a ZnAl-LDH functional layer modified aqueous zinc ion battery zinc negative electrode.

[0032] Figure 1 This is a SEM image of the zinc negative electrode of the aqueous zinc ion battery modified by the ZnAl-LDH functional layer in Example 1 of the present invention.

[0033] like Figure 1 As shown, the surface of the zinc negative electrode of the aqueous zinc ion battery modified with the ZnAl-LDH functional layer prepared in this embodiment presents slight layered protrusions as a whole, and there are densely distributed thin layered structures on the surface. The layered structure is conducive to the uniform electroplating / stripping process of zinc ions.

[0034] This embodiment also provides a button battery, and the preparation method thereof is as follows:

[0035] A CR2025 button cell was assembled using V2O5 positive electrode, the above-mentioned ZnAl-LDH functional layer modified aqueous zinc ion battery zinc negative electrode / pure zinc negative electrode, a glass microfiber filter membrane (Whatman, GF / D), and 3M Zn(CF3SO3)2 electrolyte as materials.

[0036] Figure 2 It is a cycle comparison of the aqueous zinc ion battery zinc negative electrode modified with the ZnAl-LDH functional layer in Example 1 of the present invention and a blank metal zinc negative electrode after being assembled into symmetrical batteries.

[0037] like Figure 2 As shown, at 0.1 mA cm -2 The current density is 0.1 mAh cm -2Under the condition of surface capacity, the symmetric battery made of the zinc negative electrode of the aqueous zinc ion battery modified with the ZnAl-LDH functional layer showed a smaller overpotential, and the symmetric battery could be stably cycled for more than 470 hours; while the symmetric battery made of the pure zinc negative electrode showed an obvious fluctuating voltage platform after about 70 hours, that is, short-circuit behavior occurred, which may be due to the strong side reactions and dendrite growth in the symmetric battery made of the pure zinc negative electrode.

[0038] Figure 3 It is a comparison of the cycle conditions and coulombic efficiency of the zinc negative electrode of the aqueous zinc ion battery modified with the ZnAl-LDH functional layer in Example 1 of the present invention and a blank metal zinc negative electrode after being assembled into full batteries.

[0039] like Figure 3 As shown in a, at 2A g -1 At a current density of 2.5 Å, the full battery made of pure zinc anode showed a significant decrease in specific capacity after 500 cycles, and Figure 3 As can be seen in b, the Coulomb efficiency becomes unstable after 500 cycles, and only about 15 mAh g remains after 1000 cycles. -1 Specific capacity. In contrast, the specific capacity of the full battery made of the zinc negative electrode of the aqueous zinc ion battery modified with the ZnAl-LDH functional layer is always higher than that of the full battery made of the pure zinc negative electrode during the cycle process, and its coulombic efficiency remains stable at around 100% without significant fluctuations. Therefore, the full battery made of the zinc negative electrode of the aqueous zinc ion battery modified with the ZnAl-LDH functional layer exhibits better electrochemical performance and good practical application potential as a whole.

[0040] Example 2

[0041] Example 2 provides a ZnAl-LDH functional layer modified aqueous zinc ion battery zinc negative electrode and a preparation method thereof, the preparation method is different from Example 1 only in that the volume of concentrated HNO3 added in step S1 is different, and the rest is exactly the same as the preparation method of Example 1. 1 mL of concentrated HNO3 is added in step S1 of this Example 2.

[0042] Comparative Example

[0043] The comparative example provides a LDH functional layer modified battery zinc negative electrode and a preparation method thereof. The preparation method is different from Example 1 only in that the volume of concentrated HNO3 added in step S1 of the comparative example is 0 mL, and the rest is exactly the same as the preparation method of Example 1.

[0044] Test Case

[0045] The potentiodynamic polarization parameters of the pure zinc negative electrode, the LDH functional layer modified battery zinc negative electrode of the comparative example, the ZnAl-LDH functional layer modified aqueous zinc ion battery zinc negative electrode of Example 2, and the ZnAl-LDH functional layer modified aqueous zinc ion battery zinc negative electrode of Example 1 were detected in 2M ZnSO4, and the results obtained are shown in Table 1:

[0046] Table 1

[0047]

[0048] As shown in Table 1, the sample obtained in Example 1 (i.e., adding 2 mL of concentrated nitric acid) corresponds to corr The smallest, most efficient protection for zinc substrate.

[0049] Functions and Effects of the Embodiments

[0050] According to the ZnAl-LDH functional layer modified aqueous zinc ion battery zinc negative electrode, its preparation method and button battery involved in this embodiment, because the ZnAl-LDH coating is prepared on the surface of the metal zinc sheet by a simple constant potential deposition method, it has good adhesion to the substrate and improves the electrochemical performance of the metal zinc sheet as the negative electrode of AZIBs, and can overcome the corrosion problem caused by the contact between the zinc negative electrode and the electrolyte in AZIBs and the effect of adding coating materials and inactive materials on the zinc negative electrode by the squeeze casting technology on the battery performance. The preparation method of the present invention is simple, environmentally friendly, meets the needs of sustainable development, and provides strong support for the commercial application of AZIBs.

[0051] Moreover, when the voltage was set to -1.7V and the deposition time was 300s, the prepared ZnAl-LDH functional layer modified aqueous zinc ion battery zinc negative electrode showed good results after being assembled into symmetrical cells and full cells.

[0052] Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A method for preparing a zinc negative electrode of an aqueous zinc ion battery modified with a ZnAl-LDH functional layer, It is characterized in that The following steps are involved: Step S1, mixing a zinc salt solution or concentrated nitric acid and an aluminum salt solution to obtain a mixed solution; Step S2, using the metal zinc sheet as the working electrode, the Ag / AgCl electrode as the reference electrode, the Pt sheet as the counter electrode, and the mixed solution as the electrodeposition solution, using a CHI660 electrochemical workstation to perform it constant potential deposition to obtain a metal zinc sheet with a ZnAl-LDH coating; Step S3, washing and drying the metal zinc sheet with the ZnAl-LDH coating to obtain a ZnAl-LDH functional layer modified aqueous zinc ion battery zinc negative electrode.

2. The method for preparing the zinc negative electrode of the aqueous zinc ion battery modified by the ZnAl-LDH functional layer according to claim 1, characterized in that: in, The aluminum salt solution is obtained by dissolving an aluminum salt in water, and the aluminum salt is any one of aluminum nitrate, aluminum carbonate, aluminum sulfate, and aluminum chloride.

3. The method for preparing the zinc negative electrode of the aqueous zinc ion battery modified by the ZnAl-LDH functional layer according to claim 1, characterized in that: in, In step S1, the zinc salt solution is obtained by dissolving a zinc salt in water, or by reacting an acid with metallic zinc, and the zinc salt is any one of zinc nitrate, zinc carbonate, zinc sulfate, and zinc chloride.

4. The method for preparing the zinc negative electrode of the aqueous zinc ion battery modified by the ZnAl-LDH functional layer according to claim 3, characterized in that: in, In step S1, the molar ratio of the zinc salt to the aluminum salt is 1:1-5:1, and the concentration of the aluminum salt solution is 0.1 mol / L to 0.5 mol / L.

5. The method for preparing the zinc negative electrode of the aqueous zinc ion battery modified by the ZnAl-LDH functional layer according to claim 2, characterized in that: in, In step S1, the molar ratio of the concentrated nitric acid to the aluminum salt is 1:1-5:1, and the concentration of the aluminum salt solution is 0.1 mol / L to 0.5 mol / L.

6. The method for preparing the zinc negative electrode of the aqueous zinc ion battery modified by the ZnAl-LDH functional layer according to claim 1, characterized in that: in, In step S2, the voltage of the constant potential deposition reaction is -1.1V to -1.9V, and the duration is 100s to 1000s.

7. The method for preparing the zinc negative electrode of the aqueous zinc ion battery modified by the ZnAl-LDH functional layer according to claim 1, characterized in that: in, In step S3, during the rinsing and drying, the metal zinc sheet with the ZnAl-LDH coating is rinsed with water and then dried in an oven at 60°C.

8. A ZnAl-LDH functional layer modified aqueous zinc ion battery zinc negative electrode, Features: The zinc negative electrode is prepared by the method for preparing a zinc negative electrode of an aqueous zinc ion battery modified with a ZnAl-LDH functional layer as described in any one of claims 1 to 7.

9. A button battery, It is characterized in that The ZnAl-LDH functional layer modified aqueous zinc ion battery zinc negative electrode as claimed in claim 8 is used as the negative electrode.

10. The button battery according to claim 9, characterized in that: in, The zinc negative electrode of the aqueous zinc ion battery modified by the ZnAl-LDH functional layer is combined with a positive electrode material and an electrolyte to be assembled to obtain a button battery.