Pole piece, battery cell, battery and preparation method of pole piece

By marking the active material layer on the electrode sheet to form a depression, the contact area of ​​the electrolyte is increased, the problem of lithium extraction risk in lithium-ion batteries is solved, and the charging and discharging performance and stability of the battery are improved.

CN118919646APending Publication Date: 2024-11-08ZHUHAI COSMX BATTERY CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411220166.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Lithium excision in lithium-ion batteries has a high risk, affecting battery performance.

Method used

By marking the active material layer of the electrode sheet to form an open area and a normal area, the arithmetic average height of the opening area is greater than that of the normal area, forming a recess, increasing the contact area between the electrode sheet and the electrolyte, and improving the wettability of the electrolyte and The deintercalation ability of lithium ions reduces the risk of lithium separation.

Benefits of technology

It improves the charge and discharge rate, cycle performance and stability of the battery, reduces heat loss and electricity waste during energy conversion, and enhances the overall performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919646A_ABST
    Figure CN118919646A_ABST
Patent Text Reader

Abstract

The invention provides a pole piece, a battery cell, a battery and a preparation method of the pole piece. The pole piece comprises a current collector and an active substance layer arranged on at least one side of the current collector, in the first direction, the active material layer comprises at least one opening region and at least one normal region adjacent to the opening region; a sunken part which is sunken towards the direction of the current collector is formed on one side, deviating from the current collector, of the opening region; the arithmetic mean height Sa of the opening area is greater than the arithmetic mean height Sa of the normal area, so that the wettability of the electrolyte on a pole piece is improved, the de-intercalation capability of lithium ions is improved, the risk of lithium precipitation is reduced, and the charge-discharge performance, the cycle performance and the stability of the battery are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of batteries, and in particular to a pole piece, a battery cell, a battery and a method for preparing the pole piece. Background Art

[0002] Currently, lithium-ion batteries are widely used not only in portable electronic devices such as mobile phones and laptops, but also in electric equipment such as electric vehicles and electric bicycles.

[0003] The battery cell is the core component of the lithium-ion battery. The battery cell includes a positive electrode sheet, a negative electrode sheet, and a separator disposed between the positive electrode sheet and the negative electrode sheet. The battery cell is immersed in an electrolyte, and lithium ions move between the positive and negative electrodes through the electrolyte, thereby realizing the charging and discharging of the battery. However, the battery of the related technology has a high risk of lithium plating, which affects the performance of the battery. Summary of the invention

[0004] In view of this, the embodiments of the present invention are directed to providing a pole piece, a battery cell, a battery, and a method for preparing a pole piece, so as to reduce the risk of lithium plating to a certain extent.

[0005] In a first aspect, the present invention provides a pole piece, comprising a current collector and an active material layer disposed on at least one side of the current collector;

[0006] In the first direction, the active material layer includes at least one opening area and at least one normal area adjacent to the opening area; a side of the opening area away from the current collector is formed into a concave portion concave toward the current collector;

[0007] The arithmetic mean height Sa of the opening area is greater than the arithmetic mean height Sa of the normal area.

[0008] Optionally, the arithmetic mean height Sa of the opening area ranges from 0.3 μm to 2.5 μm;

[0009] Optionally, the arithmetic mean height Sa of the opening area ranges from 0.3 μm to 1.6 μm.

[0010] Optionally, along the first direction, the width of the opening area ranges from 40 μm to 100 μm;

[0011] And / or, along the first direction, there are at least two opening areas, and the distance between two adjacent opening areas ranges from 0.6 mm to 2 mm;

[0012] and / or, along the second direction, the depression depth of the depression is in the range of 2 μm to 12 μm;

[0013] Optionally, along the second direction, the depression depth of the depression portion ranges from 2 μm to 8 μm.

[0014] Optionally, the arithmetic mean height Sa of the normal area ranges from 0.1 μm to 1.2 μm;

[0015] And / or, the difference between the arithmetic mean height Sa of the opening area and the arithmetic mean height Sa of the normal area is in the range of 0.01 μm to 2.4 μm;

[0016] Optionally, the difference between the arithmetic mean height Sa of the opening area and the arithmetic mean height Sa of the normal area ranges from 0.01 μm to 1.4 μm.

[0017] Optionally, the maximum height Sz of the opening area is greater than the maximum height Sz of the normal area.

[0018] Optionally, the maximum height Sz of the opening area is in the range of 2 μm to 15 μm;

[0019] Optionally, the maximum height Sz of the opening area is in the range of 2 μm to 11 μm.

[0020] Optionally, the maximum height Sz of the normal zone ranges from 1 μm to 6 μm;

[0021] And / or, the difference between the maximum height Sz of the opening area and the maximum height Sz of the normal area is in the range of 0.01 μm to 13 μm;

[0022] Optionally, the difference between the maximum height Sz of the opening area and the maximum height Sz of the normal area is in the range of 0.01 μm to 9 μm.

[0023] Optionally, the ratio of the thickness of the active material layer in the opening area to the thickness of the active material layer in the normal area is in the range of 0.85 to 0.99.

[0024] Optionally, the compaction density of the normal area is greater than the compaction density of the opening area.

[0025] Optionally, the compaction density of the opening area is in the range of 1.0 g / cm 3 ~1.75g / cm 3 ;

[0026] And / or, the compaction density of the normal zone is in the range of 1.45 g / cm 3 ~1.85g / cm 3 .

[0027] In a second aspect, the present invention provides a battery cell, comprising a first pole piece, a second pole piece, and a diaphragm disposed between the first pole piece and the second pole piece, wherein the first pole piece and the second pole piece have opposite polarities;

[0028] At least one of the first pole piece and the second pole piece is the pole piece as described above.

[0029] In a third aspect, the present invention provides a battery, comprising the battery cell as described above.

[0030] In a fourth aspect, the present invention provides a method for preparing the pole piece as described above, the method comprising:

[0031] An active material layer is coated on at least one side of the current collector; wherein, along the first direction, the active material layer includes at least one preset opening area and at least one normal area adjacent to the preset opening area;

[0032] Drawing a line on a side of the preset opening area away from the current collector to form the recessed portion;

[0033] The active material layer is roll-pressed.

[0034] The pole piece, battery cell, battery and pole piece preparation method provided by the present invention form an opening area and a normal area on the pole piece by scribing the pole piece, and the side of the opening area away from the current collector is formed into a recessed portion, so that the arithmetic mean height Sa of the opening area is greater than the arithmetic mean height Sa of the normal area, that is, the roughness of the opening area is greater than that of the normal area. In other words, by scribing on the pole piece to form a recessed portion, the roughness of the opening area is greater than that of the normal area, that is, the active material in the opening area is looser than that in the normal area, so that the contact area between the pole piece and the electrolyte is increased, the wettability of the electrolyte is improved, thereby improving the ion transfer rate, reducing the internal impedance between the pole piece and the electrolyte, thereby improving the deintercalation ability of lithium ions in the active material layer, reducing the risk of lithium plating, and improving the charge and discharge rate of the battery. Moreover, the improved wettability reduces the internal resistance of the battery to a certain extent, thereby reducing the heat loss and electric energy waste during energy conversion, thereby improving the charge and discharge performance, cycle performance and stability of the battery. Moreover, since the side of the opening area away from the current collector is formed as a recessed portion, the liquid retention of the battery cell can be increased, thereby improving the cycle performance of the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 A schematic diagram of a top view of a pole piece according to an embodiment of the present invention;

[0036] Figure 2 It is a schematic cross-sectional structure diagram of a pole piece according to an embodiment of the present invention;

[0037] Figure 3 This is a SEM electron microscope of the pole piece according to an embodiment of the present invention Figure 1 ;

[0038] Figure 4The SEM electron microscope of the pole piece according to one embodiment of the present invention Figure 2 ;

[0039] Figure 5 This is a plane electron microscope image of a pole piece according to an embodiment of the present invention;

[0040] Figure 6 An interface diagram for calculating the arithmetic mean height and maximum height of the opening area of ​​the pole piece according to an embodiment of the present invention;

[0041] Figure 7 This is an interface diagram for calculating the arithmetic mean height and maximum height of the normal area of ​​the pole piece described in one embodiment of the present invention.

[0042] Among them, 1, current collector; 2, active material layer; 21, opening area; 210, recessed part; 22, normal area. DETAILED DESCRIPTION

[0043] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field based on the embodiments of the present invention belong to the scope of protection of the present invention.

[0044] The battery cell is an important component of the battery. The battery cell includes a positive electrode sheet, a negative electrode sheet and a separator. The positive electrode sheet includes a positive electrode collector and a positive electrode active layer arranged on the surface of the positive electrode collector. The negative electrode sheet includes a negative electrode collector and a negative electrode active layer arranged on the surface of the negative electrode collector. The capacity of the battery is provided by the electrochemical reaction between the active material of the positive electrode active layer and the active material of the negative electrode active layer. The separator is located between the positive electrode sheet and the negative electrode sheet to isolate the contact between the positive electrode sheet and the negative electrode sheet. The battery cell is immersed in the electrolyte, and the battery is obtained after a series of operations such as packaging. Among them, the electrolyte acts as a carrier for ion transmission, and lithium ions move between the positive and negative electrodes through the electrolyte, thereby realizing the charging and discharging of the battery.

[0045] In the related art, the risk of lithium plating in batteries is relatively high, which directly affects the battery's charging, discharging, and cycling performance. Based on this, the present invention provides a pole piece, a battery cell, a battery, and a method for preparing a pole piece, by making the active material layer of the pole piece include an opening area and a normal area, forming a recessed portion on the side of the opening area away from the current collector, and making the surface roughness of the opening area greater than the surface roughness of the normal area, thereby increasing the contact area between the pole piece and the electrolyte, improving the wettability of the electrolyte, and improving the deintercalation ability of lithium ions, thereby reducing the risk of lithium plating and improving the battery's charging and discharging performance, cycling performance, and stability.

[0046] The following is a detailed description of the pole piece, battery cell, battery and pole piece preparation method provided by the present invention through specific embodiments in conjunction with the accompanying drawings:

[0047] Reference Figures 1 to 7 As shown, this embodiment provides a pole piece, which is applied to a battery cell, which may be a wound battery cell or a stacked battery cell, and the battery cell is applied to a battery, which may be a lithium-ion battery.

[0048] The pole piece provided in this embodiment includes: a current collector 1 and an active material layer 2 arranged on at least one side of the current collector 1 .

[0049] Specifically, the current collector 1 has two opposite sides, and the two opposite sides are used to coat the active material layer 2. In specific implementation, only one side of the current collector 1 (for example Figure 2 The active material layer 2 may be disposed on the upper side of the current collector 1. Of course, in other implementations, the active material layer 2 may be disposed only on the lower side of the current collector 1. Alternatively, the active material layer 2 may be disposed on both sides of the current collector 1 (e.g. Figure 3 and Figure 4 ) are provided with an active material layer 2.

[0050] Along the first direction, the active material layer 2 includes at least one opening region 21 and at least one normal region 22 adjacent to the opening region 21 .

[0051] Specifically, there may be one or more opening areas 21 , and there may be one or more normal areas 22 . The opening area 21 and the normal area 22 are arranged adjacent to each other.

[0052] The first direction here can be, for example, the length direction of the pole piece, such as Figure 1 and Figure 2 The first direction may also be the width direction of the pole piece, or the first direction may be an inclined direction having an angle with the length direction or the width direction of the pole piece.

[0053] The side of the opening area 21 away from the current collector 1 is formed as a recessed portion 210 recessed toward the current collector 1 , that is, the side of the opening area 21 away from the current collector 1 is formed as a pit.

[0054] In specific implementation, the surface of the active material layer 2 of the electrode can be scribed by laser equipment or a needle plate, that is, a certain number of pits are formed on the surface of the active material layer 2, that is, the area corresponding to the pits is the above-mentioned opening area 21, and the area outside the opening area 21 corresponds to the normal area 22.

[0055] When the active material layer 2 includes a plurality of opening areas 21 and a plurality of normal areas 22, lines can be drawn along the width direction of the pole piece so that the plurality of recessed portions 210 formed by the lines are arranged at intervals along the length direction of the pole piece, and a normal area 22 is provided between two opening areas 21. Alternatively, lines can be drawn along the length direction of the pole piece so that the plurality of recessed portions 210 formed by the lines are arranged at intervals along the width direction of the pole piece, and a normal area 22 is provided between two opening areas 21. Alternatively, lines can be drawn along both the width direction and the length direction of the pole piece so that the plurality of opening areas 21 and the plurality of normal areas 22 are arranged in a staggered manner, such as an overall arrangement forming a tic-tac-toe structure. In addition, lines can also be drawn along an inclined direction having an angle with the length direction or the width direction of the pole piece.

[0056] The arithmetic mean height Sa of the opening area 21 is greater than the arithmetic mean height Sa of the normal area 22 .

[0057] It should be noted that the arithmetic mean height is one of the characterization parameters of roughness, denoted by Sa. In the present application, the arithmetic mean height Sa specifically refers to the average value of the absolute value of the height difference of each point relative to the average surface.

[0058] The average plane of the opening area 21 and the average plane of the normal area 22 are different planes. The average plane of the opening area 21 specifically refers to the plane where the average value of the heights of the points on the upper surface of the opening area 21 (such as the bottom surface of the pit) is located, and the average plane of the normal area 22 specifically refers to the plane where the average value of the heights of the points on the upper surface of the normal area 22 (such as the side of the normal area 22 away from the current collector 1) is located.

[0059] By making the arithmetic mean height Sa of the opening area 21 greater than the arithmetic mean height Sa of the normal area 22, that is, making the pole piece form a pole piece structure with variable roughness, the roughness of the opening area 21 is made greater than the roughness of the normal area 22. Figure 3 As shown, the active material in the opening area 21 is looser than that in the normal area 22, thereby improving the wettability of the electrolyte to the electrode, increasing the ion transfer rate, improving the lithium ion deintercalation ability, and reducing the risk of lithium plating.

[0060] When implementing it specifically, Figure 6 and Figure 7 As shown, for example, the arithmetic mean height Sa can be measured by adjusting the magnification to 500 using an optical microscope VHX-7000N, using a deep synthetic three-dimensional image, and correcting the placement flatness of the pole piece being measured.

[0061] Exemplarily, the active material layer 2 is coated on the current collector 1 and then dried, and then a scribing technique is used to scribble on the surface of the active material layer 2 of the electrode, such as scribing along the length direction and / or width direction of the electrode, to form a certain number of pits on the surface of the active material layer 2. After scribing, the roughness of the opening area 21 is greater than the roughness of the normal area 22, and then the electrode is rolled.

[0062] Specifically, laser scribing may be used, or a needle plate or the like may be used for scribing.

[0063] The electrode sheet provided in this embodiment can be a negative electrode sheet, the current collector 1 can be copper foil, and the material of the active material layer 2 can be graphite, silicon-based negative electrode active materials, etc. This embodiment does not specifically limit the specific materials of the current collector 1 and the active material layer 2, which can be selected according to actual needs.

[0064] Of course, in other embodiments, the electrode sheet may also be a positive electrode sheet. In this case, the current collector 1 may be, for example, aluminum foil, and the material of the active material layer 2 may be, for example, a ternary material or a positive electrode active material such as lithium iron phosphate.

[0065] The pole piece provided in this embodiment is formed with an opening area 21 and a normal area 22 by scribing the pole piece, and a side of the opening area 21 away from the current collector 1 is formed as a recessed portion 210, so that the arithmetic mean height Sa of the opening area 21 is greater than the arithmetic mean height Sa of the normal area 22, that is, the roughness of the opening area 21 is greater than the roughness of the normal area 22, that is, by scribing the pole piece to form a recessed portion 210, the roughness of the opening area 21 is greater than the roughness of the normal area 22, that is, the active material in the opening area 21 is greater than that in the normal area 22. The active material is relatively loose, which increases the contact area between the pole piece and the electrolyte, improves the wettability of the electrolyte, thereby increasing the ion transfer rate, reducing the internal impedance between the pole piece and the electrolyte, thereby improving the deintercalation ability of lithium ions in the active material layer 2, reducing the risk of lithium precipitation, and improving the charge and discharge rate of the battery. In addition, the improved wettability reduces the resistance inside the battery to a certain extent, thereby reducing heat loss and power waste during energy conversion, thereby improving the charge and discharge performance, cycle performance and stability of the battery. Moreover, since the side of the opening area 21 that is away from the current collector 1 is formed as a recessed portion 210, this can also increase the liquid retention of the battery cell, thereby improving the cycle performance of the battery.

[0066] In specific implementation, if the arithmetic mean height Sa of the opening area 21 is too small, it will affect the good infiltration of the electrolyte; if the arithmetic mean height Sa of the opening area 21 is too large, it will cause the surface unevenness of the opening area 21 to be higher, thereby affecting the consistency of the thickness of the battery cell, resulting in uneven pressure on the battery cell during the battery formation process, thereby affecting the electrical performance of the battery.

[0067] Based on this, in some embodiments, the arithmetic mean height Sa of the opening area 21 can be set between 0.3 μm and 2.5 μm, for example, 0.3 μm, 0.32 μm, 0.5 μm, 0.53 μm, 0.6 μm, 0.8 μm, 0.85 μm, 0.95 μm, 1 μm, 1.03 μm, 1.2 μm, 1.3 μm, 1.4 μm, 1.5 μm, 1.6 μm, 1.61 μm, 1.8 μm, 2 μm, 2.2 μm, 2.39 μm, 2.5 μm.

[0068] By setting the arithmetic mean height Sa of the opening area 21 within the above range, the good wetting of the electrolyte and the surface flatness of the opening area 21 are taken into account at the same time. That is to say, such a setting not only ensures the contact area between the electrolyte and the active material layer 2, ensures the good wettability of the electrolyte, and thus ensures the smooth transmission of lithium ions and reduces the risk of lithium plating, but also improves the flatness of the surface of the opening area 21, thereby improving the consistency of the thickness of the battery cell, and further improves the uniformity of the pressure on the battery cell during the formation process, thereby further ensuring that the battery has good electrical properties such as charging rate performance and cycle performance, and also ensures the appearance quality of the battery cell.

[0069] Furthermore, the arithmetic mean height Sa of the opening area 21 can be set between 0.3 μm and 1.6 μm. This can further ensure good wettability of the electrode and further improve the flatness of the surface of the opening area 21, thereby further improving the consistency of the thickness of the battery cell while further ensuring that the risk of lithium deposition is improved.

[0070] Exemplarily, in some embodiments, reference Figure 6 As shown, the opening area 21 is selected, and after testing, the arithmetic mean height Sa of the opening area 21 is specifically 1 μm.

[0071] Combination Figure 1 , Figure 2 and Figure 5 As shown, in some embodiments, along the first direction, the width c of the opening area 21 can be set between 40 μm and 100 μm, such as 40 μm, 50 μm, 60 μm, 65 μm, 70 μm, 75 μm, 80 μm, 90 μm, or 100 μm.

[0072] Reference Figure 2 As shown, the first direction can be specifically Figure 2 In the left and right directions, for example, the length direction of the electrode, the width c of the opening area 21 is the width of the opening area 21 along the Figure 2 The size in the left-right direction.

[0073] By setting the width c of the opening area 21 within the above range, the contact area between the electrolyte and the active material layer 2 is ensured while avoiding the situation where the width of the opening area 21 is too large and affects the unit volume energy density of the battery cell. In other words, by setting the width of the opening area 21 within the above range, the good wettability of the electrolyte is improved while taking into account and ensuring the unit volume energy density of the battery cell.

[0074] In addition, by setting the width c of the opening area 21 within the above range, the opening area 21 is prevented from being too wide and affecting the adhesion between the electrode and the diaphragm, thereby improving the bonding strength between the electrode and the diaphragm, thereby improving the stability of the battery cell during use and storage, and improving the battery life.

[0075] Reference Figure 5 As shown, by way of example, the width c of the opening region 21 can be 56.4 μm.

[0076] Continue to refer to Figure 1 and Figure 2 As shown, in some embodiments, there are at least two opening areas 21 along the first direction.

[0077] In some embodiments, the spacing between two adjacent opening areas 21 can be set between 0.6 mm and 2 mm, such as 0.6 mm, 0.7 mm, 0.8 mm, 0.9 mm, 1 mm, 1.1 mm, 1.2 mm, 1.3 mm, 1.4 mm, 1.5 mm, 1.6 mm, 1.7 mm, 1.8 mm, 1.9 mm, and 2 mm.

[0078] Reference Figure 2 As shown, the spacing between two adjacent opening areas 21 here specifically refers to the spacing between the adjacent opening areas 21 along the Figure 2 In the left-right direction, the center-to-center distance e between two adjacent opening areas 21.

[0079] By setting the spacing e between two adjacent opening areas 21 within the above range, not only is good infiltration of the electrolyte ensured, but also the situation where the spacing is too small and the volume energy density of the battery cell is too low can be avoided, that is, the unit volume energy density of the battery cell and the wettability of the electrode are taken into account at the same time.

[0080] In addition, by setting the distance between two adjacent opening areas 21 within the above-mentioned range, it is avoided that the recessed portions 210 are arranged too densely and affect the adhesion between the electrode and the diaphragm, thereby improving the bonding strength between the electrode and the diaphragm, thereby improving the stability of the battery cell during use and storage, and improving the battery life.

[0081] Continue to refer to Figure 2As shown, along the second direction, the recessed portion 210 may have a depth between 2 μm and 12 μm, such as 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, or 12 μm.

[0082] The second direction here can be specifically Figure 2 In the vertical direction, the depth of the depression is specifically the depth of the depression 210 along the Figure 2 The dimension d in the up and down direction.

[0083] By setting the depression depth d of the depression area within the above range, the contact area between the active material layer 2 and the electrolyte is further guaranteed, the wettability and liquid retention of the electrode are further improved, and the situation where the energy density per unit volume of the battery cell is reduced due to the excessive depression depth d is avoided to a certain extent, that is, the energy density per unit volume of the battery cell is guaranteed to a certain extent.

[0084] Furthermore, the depression depth d of the depression 210 can be set between 2 μm and 8 μm. For example, it can be 2 μm, 3 μm, 4 μm, 4.5 μm, 5 μm, 5.5 μm, 6 μm, 7 μm, and 8 μm. This setting further takes into account the wettability of the electrode and the unit volume energy density of the battery cell.

[0085] If the arithmetic mean height Sa of the normal area 22 is too small, it will affect the good infiltration of the electrolyte in the normal area 22; if the arithmetic mean height Sa of the normal area 22 is too large, it will cause the surface unevenness of the normal area 22 to be high, thereby affecting the consistency of the thickness of the battery cell. Based on this, in some embodiments, the arithmetic mean height Sa of the normal area 22 can be set between 0.1 μm and 1.2 μm.

[0086] For example, it can be 0.1μm, 0.2μm, 0.23μm, 0.3μm, 0.4μm, 0.5μm, 0.6μm, 0.65μm, 0.7μm, 0.8μm, 0.9μm, 1μm, 1.1μm, and 1.2μm.

[0087] By setting the arithmetic mean height Sa of the normal area 22 within the above range, not only the contact area between the electrolyte and the active material layer of the normal area 22 is guaranteed, the good wettability of the electrolyte is guaranteed, thereby ensuring the smooth transmission of lithium ions and reducing the risk of lithium plating, but also the flatness of the surface of the normal area 22 is improved, thereby improving the consistency of the thickness of the battery cell, further improving the uniformity of the pressure on the battery cell during the formation process, thereby further ensuring that the battery has good electrical properties such as charge and discharge performance and cycle performance, and also ensuring the appearance quality of the battery cell.

[0088] Exemplarily, in some embodiments, reference Figure 7As shown, the normal area 22 is selected, and after testing, the arithmetic mean height Sa of the normal area 22 is specifically 0.54 μm.

[0089] If the difference between the arithmetic mean height Sa of the opening area 21 and the arithmetic mean height Sa of the normal area 22 is too large, the roughness difference between the opening area 21 and the roughness difference between the normal area 22 will be too large, thereby affecting the consistency of the thickness of the battery cell. Based on this, in some embodiments, the difference between the arithmetic mean height Sa of the opening area 21 and the arithmetic mean height Sa of the normal area 22 can be set between 0.01 μm and 2.4 μm.

[0090] That is, the arithmetic mean height Sa of the opening area 21 is 0.01μm to 2.4μm larger than the arithmetic mean height of the normal area 22. For example, the specific difference can be 0.01μm, 0.05μm, 0.1μm, 0.3μm, 0.5μm, 0.6μm, 0.62μm, 0.7μm, 0.8μm, 1μm, 1.18μm, 1.2μm, 1.38μm, 1.4μm, 1.6μm, 1.79μm, 2μm, 2.16μm, and 2.4μm.

[0091] For example, the arithmetic mean height Sa of the opening area 21 is 2.5 μm, the arithmetic mean height Sa of the normal area 22 is specifically 1.2 μm, and the difference between the arithmetic mean height Sa of the opening area 21 and the arithmetic mean height Sa of the normal area 22 is specifically 1.3 μm. For example, the arithmetic mean height Sa of the opening area 21 is 0.3 μm, the arithmetic mean height Sa of the normal area 22 is specifically 0.1 μm, and the difference between the arithmetic mean height Sa of the opening area 21 and the arithmetic mean height Sa of the normal area 22 is specifically 0.2 μm.

[0092] By setting the difference between the arithmetic mean height Sa of the opening area 21 and the arithmetic mean height Sa of the normal area 22 within the above range, the difference in roughness between the opening area 21 and the normal area 22 is reduced on the basis of ensuring the improvement of the wettability of the electrode, thereby improving the overall thickness consistency of the electrode, further improving the uniformity of the pressure on the battery cell during the formation process, and further ensuring that the battery has good electrical properties such as charging rate performance and cycle performance, and also ensuring the appearance quality of the battery cell. In addition, since the difference in roughness between the opening area 21 and the normal area 22 is reduced, it is conducive to the bonding of the electrode and the diaphragm, improves the bonding strength between the electrode and the diaphragm, ensures the structural strength and stability of the battery cell, and thereby improves the stability of the battery during use and storage.

[0093] Furthermore, the difference between the arithmetic mean height Sa of the opening area 21 and the arithmetic mean height Sa of the normal area 22 can be set between 0.01 μm and 1.4 μm. This setting improves the wettability of the electrode piece, further improves the consistency of the thickness of the battery cell, and is more conducive to the bonding between the electrode piece and the diaphragm.

[0094] In some embodiments, the maximum height Sz of the opening area 21 is greater than the maximum height Sz of the normal area 22 .

[0095] It should be noted that, in the present application, the maximum height Sz specifically refers to the sum of the maximum peak height and the maximum valley depth in the region. It is understandable that the sum of the maximum peak height and the maximum valley depth of the opening area 21 is the maximum height Sz of the opening area 21, and the sum of the maximum peak height and the maximum valley depth of the normal area 22 is the maximum height Sz of the normal area 22.

[0096] By making the maximum height Sz of the opening area 21 greater than the maximum height Sz of the normal area 22, the active material in the opening area 21 is made looser, thereby further improving the wettability of the electrolyte, increasing the ion transfer rate, and improving the lithium ion deintercalation ability in the active material layer 2, thereby increasing the battery's charge and discharge rate, further reducing the risk of lithium plating, and improving the battery's charge and discharge performance, cycle performance, and stability.

[0097] When implementing it, refer to Figure 6 and Figure 7 As shown, for example, the maximum height Sz can be measured by using an optical microscope VHX-7000N, adjusting the magnification to 500, using a deep synthetic three-dimensional image, and correcting the placement flatness of the pole piece being measured.

[0098] If the maximum height Sz of the opening area 21 is larger, the wettability of the active material layer 2 with the electrolyte will be better. However, if the maximum height Sz is too large, the transmission distance of lithium ions from the positive electrode active material layer to the negative electrode active material layer or from the negative electrode active material layer to the positive electrode active material layer will be too large, which will affect the transmission rate of lithium ions. Based on this, in some embodiments, the maximum height Sz of the opening area 21 can be set between 2μm and 15μm.

[0099] For example, it can be 2μm, 2.3μm, 3μm, 4μm, 4.73μm, 5μm, 6μm, 6.55μm, 6.69μm, 7μm, 8μm, 8.5μm, 8.75μm, 9μm, 9.31μm, 10μm, 10.95μm, 11μm, 12μm, 13.43μm, 14.55μm, and 15μm.

[0100] By setting the maximum height Sz of the opening area 21 within the above range, while ensuring the improvement of the wettability of the electrode sheet, the transmission distance of the lithium ions in the opening area 21 from the positive electrode active material layer to the negative electrode active material layer or from the negative electrode active material layer to the positive electrode active material layer is shortened, thereby accelerating the transmission rate of lithium ions, further improving the deintercalation ability of lithium ions in the active material layer, further reducing the risk of lithium precipitation, and further improving the charge and discharge rate of the battery. Moreover, since the lithium ion transmission path is shortened, the degree of electrolyte loss and fatigue of the electrode material during the charge and discharge process of the battery are reduced, thereby improving the cycle life and long-term stability of the battery. Moreover, since the lithium ion transmission path is shortened, the heat loss and power waste during the battery energy conversion are also reduced to a certain extent. In addition, such a setting can also prevent the active material of the electrode sheet from expanding during the charge and discharge process, causing the active material to squeeze each other and cause powder loss, thereby causing the problem of poor K value.

[0101] Furthermore, the maximum height Sz of the opening area 21 can be set between 2 μm and 11 μm. This further improves the wettability of the electrode, further shortens the transmission path of lithium ions, further reduces the risk of lithium plating, and further improves the charge and discharge performance, cycle life and long-term stability of the battery, and further reduces heat loss and power waste during energy conversion.

[0102] Exemplarily, in some embodiments, reference Figure 6 As shown, the opening area 21 is selected, and after testing, the maximum height Sz of the opening area 21 is specifically 6.55 μm.

[0103] In some embodiments, the maximum height Sz of the normal area 22 may be set between 1 μm and 6 μm, such as 1 μm, 2 μm, 2.25 μm, 3 μm, 3.5 μm, 4 μm, 4.48 μm, 5 μm, 5.2 μm, and 6 μm.

[0104] By setting the maximum height Sz of the normal zone 22 within the above range, while ensuring the improvement of the wettability of the electrode sheet, the transmission distance of lithium ions from the positive electrode active material layer to the negative electrode active material layer or from the negative electrode active material layer to the positive electrode active material layer is shortened, thereby accelerating the transmission rate of lithium ions, reducing the risk of lithium precipitation, and further improving the charge and discharge rate of the battery. Moreover, since the lithium ion transmission path is shortened, the electrolyte loss degree and the fatigue degree of the electrode material of the battery during the charge and discharge process are reduced, thereby improving the cycle life and long-term stability of the battery. Moreover, by shortening the lithium ion transmission path, the heat loss and power waste during the battery energy conversion are also reduced to a certain extent.

[0105] Exemplarily, in some embodiments, reference Figure 7 As shown, the normal area 22 is selected, and after testing, the maximum height Sz of the normal area 22 is specifically 4.48 μm.

[0106] If the difference between the maximum height Sz of the opening area 21 and the maximum height Sz of the normal area 22 is too large, the surface flatness of the electrode sheet will be poor, thereby affecting the flatness of the battery cell. Based on this, in some embodiments, the difference between the maximum height Sz of the opening area 21 and the maximum height Sz of the normal area 22 can be set between 0.01 μm and 13 μm.

[0107] That is, the maximum height Sz of the opening area 21 is 0.01μm to 13μm greater than the maximum height Sz of the normal area 22. For example, the difference can be 0.01μm, 0.05μm, 1μm, 2μm, 2.48μm, 4μm, 4.5μm, 5μm, 6.5μm, 7μm, 8μm, 8.7μm, 9μm, 11μm, 11.18μm, 12μm, 12.3μm, and 13μm.

[0108] For example, the maximum height Sz of the opening area 21 is 2 μm, the maximum height Sz of the normal area 22 is 1 μm, and the difference between the two is 1 μm. For another example, the maximum height Sz of the opening area 21 is 15 μm, the maximum height Sz of the normal area 22 is 6 μm, and the difference between the two is 9 μm.

[0109] By setting the difference between the maximum height Sz of the opening area 21 and the maximum height Sz of the normal area 22 within the above range, while ensuring good infiltration of the electrolyte, the surface flatness of the electrode is improved, thereby improving the flatness of the battery cell, ensuring the appearance quality of the battery cell, and improving the uniformity of the pressure on the battery cell during the formation process, thereby further ensuring that the battery has good charge and discharge performance and cycle performance.

[0110] Furthermore, the maximum height Sz of the opening area 21 and the maximum height Sz of the normal area 22 can be set between 0.01 μm and 9 μm, which further ensures the wettability of the electrolyte and further improves the surface flatness of the electrode piece.

[0111] Reference Figure 2 As shown, in some embodiments, the ratio of the thickness of the active material layer 2 in the opening area 21 to the thickness of the active material layer 2 in the normal area 22 can be set between 0.85 and 0.99.

[0112] The thickness of the active material layer 2 in the normal region 22 here refers to Figure 2 The thickness H of the active material layer 2 on one side of the middle current collector 1 in the vertical direction and the thickness of the active material layer 2 in the opening area 21 are Figure 2The thickness of the active material layer 2 in the vertical direction after the middle opening area 21 is scribed is h.

[0113] For example, the ratio of the thickness h of the active material layer in the opening area 21 to the thickness H of the active material layer in the normal area 22 can be set to 0.85, 0.9, 0.91, 0.92, 0.93, 0.94, 0.95, 0.96, 0.97, 0.98, or 0.99.

[0114] For example, the thickness H of the active material layer in the normal area 22 is 20 μm, the thickness h of the active material layer in the opening area 21 is 17 μm, and the ratio between the two is 0.85. For another example, the thickness H of the active material layer in the normal area 22 is 20 μm, the thickness h of the active material layer in the opening area 21 is 19.8 μm, and the ratio between the two is 0.99. For another example, the thickness H of the active material layer in the normal area 22 is 20 μm, the thickness h of the active material layer in the opening area 21 is 18.4 μm, and the ratio between the two is 0.92.

[0115] By setting the ratio of the thickness of the active material layer in the opening area 21 to the thickness of the active material layer in the normal area 22 within the above range, that is, making the depth of the recessed portion 210 shallower, while improving the wettability of the electrolyte, the transmission path of lithium ions is shortened to a certain extent, thereby improving the transmission rate of lithium ions, further improving the deintercalation ability of lithium ions, improving the lithium precipitation phenomenon, and improving the charge and discharge rate of the battery. Moreover, by such a setting, since the transmission path of lithium ions is shortened to a certain extent, the electrolyte loss and fatigue of the electrode material during the use of the battery can be reduced to a certain extent, thereby improving the cycle life and long-term stability of the battery. Moreover, on this basis, such a setting is also conducive to improving the flatness of the entire electrode surface, thereby improving the consistency of the thickness of the battery cell.

[0116] The above-mentioned thickness h of the active material layer in the opening area 21 and the thickness H of the active material layer in the normal area 22 may specifically be the thickness measured after the electrode sheet is scribed and rolled.

[0117] If the compaction density of the active material layer is too high, it will affect the infiltration of the pole piece, increase the transmission impedance of lithium ions, make the transmission of lithium ions inside the pole piece more difficult, and cause a large temperature rise of the battery. However, if the compaction density of the active material layer is too low, the energy density per unit volume of the battery cell will be reduced. Based on this, in some embodiments, the compaction density of the normal area 22 is greater than the compaction density of the opening area 21.

[0118] In the present application, the compaction density of the active material layer 2 refers to the compaction density of the active material coated on the current collector 1. The compaction density of the active material layer 2 is equal to the ratio of the surface density per unit area to the thickness of the active material. Among them, the thickness of the active material refers to the thickness of the active material after being pressed, and the surface density refers to the mass per unit area of ​​the active material of a specified thickness.

[0119] For example, after the active material layer 2 is scribed as above, the electrode is rolled, and after rolling, the compaction density of the normal area 22 is greater than the compaction density of the opening area 21. During rolling, the roller surface contacted by the normal area 22 is larger, and the force is relatively large, so the compaction density is larger. The roller surface contacted by the opening area 21 is relatively small, and after scribing, the surface density and thickness of the original preset opening area are reduced, so the compaction density is relatively small.

[0120] By making the compaction density of the normal area 22 greater than the compaction density of the opening area 21, that is, realizing a variable compaction density pole piece structure, the compaction density of the opening area 21 is relatively small, and the compaction density of the normal area 22 is relatively large. The relatively small compaction density of the opening area 21 can not only further improve the wettability of the electrolyte, reduce the resistance of lithium ion deintercalation, further improve the lithium precipitation phenomenon, and improve the charging and discharging performance and cycle performance of the battery, but also the smaller compaction density of the opening area 21 can reduce the internal resistance of the battery, thereby reducing the heat loss and electric energy waste caused by the large resistance during energy conversion. The relatively large compaction density of the normal area 22 can reduce the thickness of the pole piece, further reduce the thickness of the battery cell, and thus improve the energy density per unit volume of the battery cell. That is, by setting the variable compaction density, the wettability of the pole piece, the improvement of the deintercalation ability of lithium ions and the improvement of the energy density per unit volume of the battery cell are taken into account at the same time.

[0121] At the same time, since the compaction density of adjacent opening areas 21 and normal areas 22 is different, this can block the heat conduction inside the battery to a certain extent. For example, the opening area 21 with a smaller compaction density located between the two normal areas 22 can play a blocking role during heat conduction, reducing the heat conduction rate between active substances, helping to reduce the temperature rise rate of the battery at high temperatures, improving the thermal management effect of the battery, reducing the safety risks caused by overheating, and improving the safety performance of the battery.

[0122] In some embodiments, by making the arithmetic mean height Sa of the opening area 21 greater than the arithmetic mean height Sa of the normal area 22, making the maximum height Sz of the opening area 21 greater than the maximum height Sz of the normal area 22, and the compaction density of the normal area 22 greater than the compaction density of the opening area 21, the wettability of the electrode is improved, the transmission impedance of lithium ions is reduced, the deintercalation ability of lithium ions in the active material layer 2 is increased, the lithium precipitation phenomenon is improved, the battery charging and discharging performance, cycle performance, etc. are improved, while the internal resistance of the battery is reduced, the heat loss and electric energy loss during battery energy conversion are reduced, and the heat conduction inside the battery is cut off to a certain extent, the heat conduction speed between the active material layers 2 is reduced, the safety performance of the battery is improved, and the energy density per unit volume of the battery cell is guaranteed to a certain extent.

[0123] In some embodiments, the compaction density of the opening area 21 can be set at 1.0 g / cm 3 ~1.75g / cm 3 For example, it can be 1.0g / cm 3 , 1.1g / cm 3 , 1.2g / cm 3 , 1.3g / cm 3 , 1.35g / cm 3 , 1.375g / cm 3 , 1.4g / cm 3 , 1.5g / cm 3 , 1.6g / cm 3 , 1.7g / cm 3 , 1.75g / cm 3 .

[0124] By setting the compaction density of the opening area 21 within the above range, the wettability of the electrolyte is further improved, the resistance to lithium ion insertion and extraction is reduced, the lithium precipitation phenomenon is improved, and the heat conduction speed between active materials is further reduced, thereby improving the safety performance of the battery.

[0125] In some embodiments, the compaction density of the normal area 22 can be set at 1.45 g / cm 3 ~1.85g / cm 3 For example, it can be 1.45g / cm 3 , 1.5g / cm 3 , 1.55g / cm 3 , 1.6g / cm 3 , 1.65g / cm 3 , 1.7g / cm 3 , 1.75g / cm 3 , 1.8g / cm 3 , 1.85g / cm3 .

[0126] By setting the compaction density of the normal area 22 within the above range, the thickness range of the pole piece is further ensured, thereby further reducing the thickness of the battery cell, thereby ensuring the energy density per unit volume of the battery cell.

[0127] This embodiment further provides a battery cell, including a first pole piece, a second pole piece, and a diaphragm arranged between the first pole piece and the second pole piece.

[0128] The polarities of the first electrode and the second electrode are opposite. For example, the first electrode is a positive electrode and the second electrode is a negative electrode. Alternatively, the first electrode is a negative electrode and the second electrode is a positive electrode.

[0129] Among them, at least one of the positive electrode sheet and the negative electrode sheet has the same structure and implementation principle as the electrode sheet provided in the above embodiment, and can bring the same or similar technical effects, which will not be described one by one here, and the details can be referred to the description of the above embodiment.

[0130] This embodiment also provides a battery, comprising a battery cell, a shell and an electrolyte, wherein the battery cell is located in the shell, and the electrolyte is injected into the shell in which the battery cell is installed.

[0131] The battery may be, for example, a lithium-ion battery. The battery may be used as a power source or energy storage unit for electronic devices, which may be, but are not limited to, mobile devices (mobile phones, laptops, tablet computers, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, electric bicycles, etc.).

[0132] Among them, the structure and implementation principle of the battery cell in this embodiment are the same as the battery cell provided in the above embodiment, and can bring the same or similar technical effects, which will not be described one by one here, and the details can be referred to the description of the above embodiment.

[0133] This embodiment also provides a method for preparing a pole piece. The structure of the prepared pole piece is the same as the structure of the pole piece provided in the above embodiment, and the implementation principle is the same, and it can bring the same or similar technical effects. For details, please refer to the description of the above embodiment.

[0134] The preparation method of the pole piece is described below:

[0135] Step 1): coating an active material layer 2 on at least one side of a current collector 1 .

[0136] The active material layer 2 includes at least one preset opening area and at least one normal area 22 adjacent to the preset opening area.

[0137] Step 2): A line is drawn on the side of the preset opening area of ​​the active material layer 2 away from the current collector 1 to form a recessed portion 210 .

[0138] It can be understood that the preset opening area forms the above-mentioned opening area 21 after being marked.

[0139] Specifically, the active material is coated on the current collector 1 to form the active material layer 2, and then dried. For example, the above-mentioned preset opening area is pre-set, and the position of the preset opening area on the active material layer 2, the width of the preset opening area, the depth of the line, etc. are determined. Then, a line is drawn on the side of the preset opening area away from the current collector 1, so that a pit that is concave toward the current collector 1 is formed on the side of the preset opening area away from the current collector 1.

[0140] Step 3): Roll-pressing the active material layer 2 .

[0141] Specifically, the active material layer 2 can be rolled by a roller, and specifically, the side of the active material layer 2 facing away from the current collector 1 contacts the roller. After rolling, the compaction density of the normal area 22 is greater than the compaction density of the opening area 21.

[0142] After rolling, the sheet is cut and sliced, and then rolled or stacked to form a core or a stacked core.

[0143] That is to say, the preparation method of the electrode provided in this embodiment prepares the electrode by first scoring and then rolling, so that the arithmetic mean height Sa of the opening area 21 is greater than the arithmetic mean height Sa of the normal area 22, and the maximum height Sz of the opening area 21 is greater than the maximum height Sz of the normal area 22, and the compaction density of the normal area 22 is greater than the compaction density of the opening area 21, thereby improving the wettability of the electrode and the transmission rate of lithium ions, improving the lithium ion deintercalation ability in the active material layer 2, improving the lithium precipitation phenomenon, improving the battery charging and discharging performance and cycle performance, and also blocking the heat conduction inside the battery to a certain extent, thereby improving the battery safety performance.

[0144] Performance Testing:

[0145] The lithium ion batteries prepared in the following Examples 1 to 8 and Comparative Examples 1 to 4 were tested for lithium plating results.

[0146] Test conditions: At a temperature of 25±2℃, charge the battery to 4.1V at 3C, then charge the battery to 4.25V at 2C, then charge the battery to 4.3V at 1.5C, then discharge the battery to 3V at 1C, cycle for 200T, and record the non-lithium deposition rate of the battery. The test results are shown in Table 1.

[0147] Table 1

[0148] Note: ρ1 is the compaction density of the opening area, and ρ2 is the compaction density of the normal area.

[0149]

[0150] The battery non-lithium deposition rate in the above Table 1 is determined by counting the proportion of batteries without lithium deposition after the batteries are disassembled under the same number of cycles (for example, 200T).

[0151] From Table 1 above, we can conclude that:

[0152] 1. In Examples 1 to 8, the arithmetic mean height Sa of the opening area 21 is greater than the arithmetic mean height Sa of the normal area 22, the maximum height Sz of the opening area 21 is greater than the maximum height Sz of the normal area 22, and the compaction density ρ2 of the normal area 22 is greater than the compaction density ρ1 of the opening area 21.

[0153] It can be seen from Examples 1 to 8 that when the battery is cycled for 200T, the lithium-ion battery obviously has a higher non-lithium deposition rate, that is, the above configuration of the present invention significantly improves the lithium deposition phenomenon of the battery.

[0154] At the same time, it can be seen from Examples 1 to 8 that as Sa and Sz of the opening area 21 gradually decrease, the non-lithium precipitation rate gradually increases. This is because as Sa and Sz of the opening area 21 decrease, the transmission distance of lithium ions between the positive and negative active materials is shortened, thereby accelerating the lithium ion transmission rate, and thus the lithium precipitation phenomenon is improved more significantly.

[0155] Moreover, from the comparison between Examples 1 to 6 and Examples 7 to 8, when the arithmetic mean height Sa of the opening area 21 is between 0.3 μm and 1.6 μm and the maximum height Sz of the opening area 21 is between 2 μm and 11 μm, the improvement of the battery lithium deposition phenomenon is better than that of Examples 7 to 8.

[0156] 2. In Comparative Examples 1 to 2, the arithmetic mean height Sa of the opening area 21 is greater than the arithmetic mean height Sa of the normal area 22, the maximum height Sz of the opening area 21 is greater than the maximum height Sz of the normal area 22, and the compaction density ρ2 of the normal area 22 is equal to the compaction density ρ1 of the opening area 21.

[0157] From the comparison between comparative example 1 and embodiment 5, when the arithmetic mean height Sa of the opening area 21 of comparative example 1 is basically the same as the arithmetic mean height Sa of the opening area 21 of embodiment 5, and the maximum height Sz of the opening area 21 of comparative example 1 is basically the same as the maximum height Sz of the opening area 21 of embodiment 5, the compaction density ρ1 of the opening area 21 in comparative example 1 is equal to the compaction density ρ2 of the normal area 22, then the non-lithium precipitation rate of comparative example 1 is significantly reduced. This is because the compaction density ρ2 of the normal area 22 in embodiment 5 is greater than the compaction density ρ1 of the opening area 21, and the relatively small compaction density of the opening area 21 is conducive to the wetting of the electrolyte, improves the wettability of the electrode, makes the transmission of lithium ions smoother, and further improves the lithium ion deintercalation ability, thereby improving the lithium precipitation phenomenon to a large extent, and then improving the non-lithium precipitation rate.

[0158] From the comparison between Comparative Example 2 and Example 6, when Sa of the opening area 21 of Comparative Example 2 is basically the same as Sa of the opening area 21 of Example 6, and Sz of the opening area 21 of Comparative Example 2 is basically the same as Sz of the opening area 21 of Example 6, the compaction density ρ1 of the opening area 21 in Comparative Example 2 is equal to the compaction density ρ2 of the normal area 22, then the non-lithium precipitation rate of Comparative Example 2 is significantly reduced. This is because the compaction density ρ2 of the normal area 22 in Example 6 is greater than the compaction density ρ1 of the opening area 21, and the relatively small compaction density of the opening area 21 is conducive to the infiltration of the electrolyte, improves the wettability of the electrode, makes the transmission of lithium ions smoother, and further improves the deintercalation ability of lithium ions, thereby improving the lithium precipitation phenomenon to a large extent, and then improving the non-lithium precipitation rate.

[0159] 3. In Comparative Examples 3 and 4, the arithmetic mean height Sa of the opening area 21 is greater than the arithmetic mean height Sa of the normal area 22, the maximum height Sz of the opening area 21 is greater than the maximum height Sz of the normal area 22, and the compaction density ρ2 of the normal area 22 is greater than the compaction density ρ1 of the opening area 21.

[0160] It can be seen from Comparative Examples 3 and 4 that the arithmetic mean height Sa of the opening area 21 is significantly higher than the arithmetic mean height Sa of the opening area 21 in Examples 1 to 8, the maximum height Sz of the opening area 21 is significantly higher than the maximum height Sz of the opening area 21 in Examples 1 to 8, and the non-lithium deposition rate of Comparative Examples 3 and 4 is significantly reduced. This is because Sa and Sz in Comparative Examples 3 and 4 are too large, which increases the transmission path of lithium ions between the positive and negative electrode materials, affects the transmission rate of lithium ions, and thus increases the lithium deposition rate.

[0161] In this article, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense. For example, it can be a fixed connection, or it can be indirectly connected through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to the specific circumstances. In addition, the orientation or position relationship indicated by the terms "upper", "lower", "left", "right", "front", "back", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc. are based on the orientation or position relationship shown in the accompanying drawings, which is only for the convenience of describing the present application and simplifying the description, and does not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present application.

[0162] In this article, relational terms such as "first" and "second" are used only to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "comprises", "comprising" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, an element defined by the statement "comprising a ..." does not exclude the presence of other identical elements in the process, method, article or device including the element.

[0163] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A pole piece, characterized in that: It comprises a current collector (1) and an active material layer (2) arranged on at least one side of the current collector (1); Along a first direction, the active material layer (2) comprises at least one opening area (21) and at least one normal area (22) adjacent to the opening area (21); a side of the opening area (21) facing away from the current collector (1) is formed as a recessed portion (210) recessed in a direction toward the current collector (1); The arithmetic mean height Sa of the opening area (21) is greater than the arithmetic mean height Sa of the normal area (22).

2. The pole piece according to claim 1, characterized in that: The arithmetic mean height Sa of the opening area (21) ranges from 0.3 μm to 2.5 μm; Preferably, the arithmetic mean height Sa of the opening area (21) is in the range of 0.3 μm to 1.6 μm.

3. The pole piece according to claim 1, characterized in that: Along the first direction, the width of the opening area (21) ranges from 40 μm to 100 μm; And / or, along the first direction, there are at least two opening areas (21), and the spacing between two adjacent opening areas (21) ranges from 0.6 mm to 2 mm; And / or, along the second direction, the depression depth of the depression (210) ranges from 2 μm to 12 μm; Preferably, along the second direction, the depression depth of the depression (210) ranges from 2 μm to 8 μm.

4. The pole piece according to claim 1, characterized in that: The arithmetic mean height Sa of the normal area (22) ranges from 0.1 μm to 1.2 μm; and / or, the difference between the arithmetic mean height Sa of the opening area (21) and the arithmetic mean height Sa of the normal area (22) is in the range of 0.01 μm to 2.4 μm; Preferably, the difference between the arithmetic mean height Sa of the opening area (21) and the arithmetic mean height Sa of the normal area (22) is in the range of 0.01 μm to 1.4 μm.

5. The pole piece according to any one of claims 1 to 4, characterized in that: The maximum height Sz of the opening area (21) is greater than the maximum height Sz of the normal area (22).

6. The pole piece according to claim 5, characterized in that: The maximum height Sz of the opening area (21) is in the range of 2 μm to 15 μm; Preferably, the maximum height Sz of the opening area (21) is in the range of 2 μm to 11 μm.

7. The pole piece according to claim 1, characterized in that: The maximum height Sz of the normal area (22) is in the range of 1 μm to 6 μm; And / or, the difference between the maximum height Sz of the opening area (21) and the maximum height Sz of the normal area (22) is in the range of 0.01 μm to 13 μm; Preferably, the difference between the maximum height Sz of the opening area (21) and the maximum height Sz of the normal area (22) is in the range of 0.01 μm to 9 μm.

8. The pole piece according to any one of claims 1 to 4, characterized in that: The ratio of the thickness of the active material layer in the opening area (21) to the thickness of the active material layer in the normal area (22) is in the range of 0.85 to 0.

99.

9. The pole piece according to any one of claims 1 to 4, characterized in that: The compaction density of the normal area (22) is greater than the compaction density of the opening area (21).

10. The pole piece according to claim 9, characterized in that: The compaction density of the opening area (21) is in the range of 1.0 g / cm 3 ~1.75g / cm 3 ; And / or, the compaction density of the normal zone (22) is in the range of 1.45 g / cm 3 ~1.85g / cm 3 .

11. A battery cell, characterized in that: It comprises a first pole piece, a second pole piece and a diaphragm arranged between the first pole piece and the second pole piece, wherein the first pole piece and the second pole piece have opposite polarities; At least one of the first pole piece and the second pole piece is the pole piece according to any one of claims 1 to 10.

12. A battery, characterized in that: Comprising the battery cell as claimed in claim 11.

13. A method for preparing a pole piece according to any one of claims 1 to 10, characterized in that: The method comprises: An active material layer is coated on at least one side of the current collector; wherein, along the first direction, the active material layer includes at least one preset opening area and at least one normal area adjacent to the preset opening area; Drawing a line on a side of the preset opening area away from the current collector to form the recessed portion; The active material layer is roll-pressed.

Citation Information

Cited By

  • Preparation method of battery pole piece, battery pole piece and battery

    CN121641814A