Alloy negative electrode for lithium ion battery and lithium battery
By adopting an alloy negative electrode structure in lithium-ion batteries, including metal foil layer, alloy layer and supplementary layer, the problems of volume changes in the negative electrode material and poor structural stability of the lithium battery are solved, and the Coulomb efficiency and cycle capacity retention rate of the battery are improved. Extend battery life.
Patent Information
- Application Number
- CN202411235586.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-11-08
AI Technical Summary
The negative electrode material of lithium batteries has large volume changes and poor structural stability, which leads to electrolyte contamination and rapid failure, affecting the cyclic charging and discharge performance of lithium-ion batteries.
An alloy negative electrode structure is adopted, including a metal foil layer, a binary and above alloy layer arranged by evaporation, and a supplementary layer. One of the alloy layer materials is the same as the metal foil layer. The supplementary layer is used to configure the lithium ion concentration and control the evaporation. Plating rate and layer thickness to optimize structure and performance.
The Coulomb efficiency, cycle life and cycle capacity retention rate of lithium-ion batteries are improved, the expansion/shrinkage effect of aluminum metal during the embedding/detachment process is alleviated, the structural integrity of the alloy negative electrode is protected, and the lithium ion concentration is supplemented.
Smart Images

Figure BDA0005027641300000091 
Figure HDA0005027641320000011 
Figure HDA0005027641320000012
Abstract
Description
Technical Field
[0001] The present disclosure relates to the field of batteries, and in particular to an alloy negative electrode for a lithium-ion battery and a lithium battery. Background Art
[0002] With the rapid development of the new energy industry, lithium-ion batteries, as one of the main ways of electrochemical energy storage, have developed rapidly. Reducing the weight of lithium-ion batteries and increasing their energy density are the main demand directions.
[0003] At present, the negative electrode material of lithium batteries is mainly graphite negative electrode material, which has low specific capacity and poor battery performance. The negative electrode materials of lithium batteries also include composite negative electrode materials such as silicon, aluminum, and tin, but the composite negative electrode material has a large volume change during the lithium removal / intercalation process, poor structural stability, and electrolyte contamination, resulting in rapid failure of the negative electrode during the cyclic charge and discharge process.
[0004] Therefore, proposing an alloy negative electrode for a lithium ion battery can solve or at least alleviate at least one of the above technical problems. Summary of the invention
[0005] In view of the above technical problems, the present disclosure provides an alloy negative electrode for a lithium ion battery and a lithium battery to solve or at least alleviate at least one technical problem existing in the above lithium battery.
[0006] According to a specific embodiment of the present disclosure, the present disclosure provides an alloy negative electrode for a lithium ion battery, comprising:
[0007] Metal foil layer;
[0008] An alloy layer is disposed on at least one side of the metal foil layer by evaporation, the alloy layer is a binary or higher alloy material, and one of the materials of the alloy layer is the same as the material of the metal foil layer;
[0009] The supplementary layer is disposed on a side of the alloy layer away from the metal foil layer by evaporation, and is configured to supplement the lithium ion concentration.
[0010] In some embodiments, the metal foil layer includes at least one of the following: aluminum foil, copper foil, nickel and nickel alloy, stainless steel;
[0011] Optionally, the metal foil layer includes aluminum foil or copper foil.
[0012] In some embodiments, the alloy layer includes at least two of the following: Cu, Al, Si, Zn, Ga, Ag, Sb, Ba, Pt, Au;
[0013] Optionally, the alloy layer includes Cu and Al.
[0014] In some embodiments, the supplemental layer includes at least one of lithium, sodium, and potassium;
[0015] Optionally, the supplemental layer comprises lithium.
[0016] In some embodiments, the same alloy as the metal foil layer material accounts for 80%-95% by weight of the alloy layer material.
[0017] In some embodiments, the alloy layer has a thickness of 0.5-2 um, and / or the supplementary layer has a thickness of 200-500 nm.
[0018] In some embodiments, the alloy layer is disposed on at least one side of the metal foil layer by evaporation, including:
[0019] Aluminum is used as the first metal and is evaporated by electron gun heating; copper is used as the second metal and is evaporated by resistance heating.
[0020] In some embodiments, the evaporation rate of aluminum is 15-20 angstroms / second, and the evaporation rate of copper is 1-2 angstroms / second.
[0021] In some embodiments, the supplementary layer is evaporated by electron gun heating or resistance heating, and the evaporation rate is 40-60 angstroms / second.
[0022] The disclosed embodiments further provide a lithium battery, comprising the alloy negative electrode for a lithium ion battery as described in any one of the above.
[0023] Compared with the prior art, the above solution of the embodiment of the present disclosure has at least the following beneficial effects:
[0024] An embodiment of the present disclosure provides an alloy negative electrode for a lithium-ion battery, wherein the alloy negative electrode includes a metal foil layer, an alloy layer disposed on at least one side of the metal foil layer, and a supplementary layer disposed on a side of the alloy layer away from the metal foil layer. The lithium-ion battery formed by the alloy negative electrode provided by the present disclosure has high coulombic efficiency, long cycle life, and high cycle capacity retention rate. In addition, the lithium-ion battery formed by the alloy negative electrode provided by the present disclosure can alleviate the pulverization of the metal layer caused by the volume effect of expansion / contraction caused by aluminum metal during the embedding / ejection process of the lithium-ion negative electrode. The supplementary layer in the lithium-ion battery formed by the alloy negative electrode provided by the present disclosure can supplement the lithium ion concentration while protecting the structural integrity of the alloy negative electrode. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] The drawings herein are incorporated into the specification and constitute a part of the specification, showing embodiments consistent with the present disclosure, and together with the specification, are used to explain the principles of the present disclosure. Obviously, the drawings described below are only some embodiments of the present disclosure, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work. In the drawings:
[0026] Figure 1 Schematic diagram of the cross-sectional structure of the alloy negative electrode in some embodiments of the present disclosure;
[0027] Figure 2 A schematic diagram of the evaporation process of the alloy layer in some embodiments of the present disclosure;
[0028] Figure 3 Schematic diagram of the evaporation process of the supplementary layer in some embodiments of the present disclosure.
[0029] The reference numerals in the specific implementation manner are as follows:
[0030] The metal foil layer 10 , the alloy layer 11 , the first metal aluminum 111 , the second metal copper 112 , the supplementary layer 12 , the sample stage 20 , the copper evaporation boat 30 , the aluminum evaporation boat 40 , and the lithium evaporation boat 50 . DETAILED DESCRIPTION
[0031] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention will be further described in detail below with reference to the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the present disclosure belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the present disclosure.
[0033] It should also be noted that the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a product or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such product or device. In the absence of more restrictions, the elements defined by the sentence "comprises a" do not exclude the presence of other identical elements in the product or device including the elements.
[0034] In the description of the embodiments of the present invention, the orientations or positional relationships indicated by technical terms such as "upper", "lower", and "thickness" are based on the orientations or positional relationships shown in the accompanying drawings and are only for the convenience of describing the embodiments of the present invention and simplifying the description. They do not indicate or imply that the devices or elements referred to must have a specific orientation, be constructed and operated in a specific orientation. Therefore, they cannot be understood as limitations on the embodiments of the present invention.
[0035] In the description of the embodiments of the present invention, the term "and / or" is only a description of the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B may represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.
[0036] In the description of the embodiments of the present invention, the symbol “~” represents the two endpoint data before and after the “~” and all data between the two endpoints. For example, A~B represents all data greater than or equal to A and less than or equal to B.
[0037] Reference to "embodiments" in this disclosure means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the disclosure. The appearance of the phrase in various places in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described in this disclosure may be combined with other embodiments.
[0038] In the related art, the negative electrode of lithium batteries usually uses copper foil, and the thickness of copper foil is generally 4.5 to 9 microns. Copper has a high density and a high price, so aluminum with a lower density can be used to make the negative electrode. The density of aluminum is about 30% of that of copper. Aluminum replaces part of copper as part of the negative electrode composite current collector, which can not only ensure the conductivity of the current collector, but also improve the energy density of lithium-ion batteries, and save a lot of material costs.
[0039] Based on this, according to the specific embodiments of the present disclosure, the present disclosure provides an alloy negative electrode for a lithium-ion battery, comprising: a metal foil layer; an alloy layer, which is arranged on at least one side of the metal foil layer by evaporation, and the alloy layer is a binary or higher alloy material, and one of the materials of the alloy layer is the same as the material of the metal foil layer; a supplementary layer, which is arranged on a side of the alloy layer away from the metal foil layer by evaporation, and is configured to supplement the lithium ion concentration.
[0040] The lithium-ion battery formed by the alloy negative electrode provided by the present disclosure has high coulombic efficiency, long cycle life and high cycle capacity retention rate. In addition, the lithium-ion battery formed by the alloy negative electrode provided by the present disclosure can alleviate the pulverization of the metal layer caused by the volume effect of expansion / contraction caused by aluminum metal during the insertion / extraction process of the lithium-ion negative electrode. The supplementary layer in the lithium-ion battery formed by the alloy negative electrode provided by the present disclosure can supplement the lithium ion concentration while protecting the structural integrity of the alloy negative electrode.
[0041] The specific implementation of the present disclosure will be described in detail below with reference to the accompanying drawings.
[0042] like Figure 1 As shown, the present disclosure provides an alloy negative electrode for a lithium-ion battery, comprising: a metal foil layer 10, an alloy layer 11 and a supplementary layer 12, wherein the alloy layer 11 is disposed on at least one side of the metal foil layer 10 by evaporation, for example, disposed on one side or both sides of the metal foil layer 10, the alloy layer 11 is a binary or higher alloy material, and one of the materials of the alloy layer 11 is the same as the material of the metal foil layer 10; the supplementary layer 12 is disposed on a side of the alloy layer 11 away from the metal foil layer 10 by evaporation, and the supplementary layer 12 is configured to protect the structural integrity of the alloy negative electrode while supplementing the lithium ion concentration.
[0043] In some embodiments, the metal foil layer 10 includes at least one of the following: aluminum foil, copper foil, nickel and nickel alloy, stainless steel; optionally, the metal foil layer 10 includes aluminum foil or copper foil. Lithium-ion batteries generally use aluminum as the positive electrode current collector metal material and copper as the negative electrode current collector metal material. This is because the oxidation potential of metal aluminum is high, and the size of the lattice octahedral voids of metal aluminum is similar to that of lithium, making it very easy for metal aluminum to react with lithium to form alloys such as LiAl, Li3Al2, and Li4Al3, which not only consumes a large amount of Li + , and it will also destroy the structure and morphology of the metal aluminum itself. Therefore, aluminum can be directly used as the current collector of the positive electrode of a lithium-ion battery, but it cannot be directly used as the current collector of the negative electrode of a lithium-ion battery. Cu has only a small lithium insertion capacity during the battery charge and discharge process, and maintains the stability of the structure and electrochemical properties. Therefore, it can be directly used as the current collector of the negative electrode of the ion battery. However, the density of aluminum is lower than that of copper, and it is cheap. Using aluminum as the negative electrode of a lithium-ion battery can reduce the weight of the battery and reduce costs. The disclosed embodiment can select aluminum foil or copper foil as the substrate, and improve its structure to form an alloy negative electrode that meets the battery performance.
[0044] In some embodiments, the alloy layer 11 includes at least two of the following: Cu, Al, Si, Zn, Ga, Ag, Sb, Ba, Pt, Au; optionally, the alloy layer 11 includes Cu and Al. In some embodiments, the thickness of the alloy layer 11 is 0.5-2um. In some embodiments, one of the materials of the alloy layer 11 is the same as the material of the metal foil layer 10, and the alloy that is the same as the material of the metal foil layer 10 accounts for 80%-95% of the weight of the alloy layer material. Optionally, the material of the metal foil layer 10 is aluminum foil, and the alloy layer material can be selected from Cu and Al, wherein the mass proportion of Al is 80%-95% of the total mass of the alloy layer 11, for example, 80%, 85%, 90%, 95%, etc., which is not limited to this. Since aluminum foil is selected as the metal foil layer 10, the mass of the negative electrode and the mass of the lithium battery are greatly reduced, and the convenience of using the lithium battery is improved. In addition, in the alloy layer 11, aluminum replaces part of copper as part of the negative electrode composite current collector, which can not only ensure the conductivity of the current collector, but also improve the energy density of the lithium-ion battery, and save a lot of material costs. The alloy layer 11 can prevent the metal aluminum foil from consuming a large amount of Li + , reduce the volume effect, avoid pulverization under the action of stress, and avoid the destruction of the surface structure. At the same time, due to the presence of copper in the alloy layer 11, copper has only a small lithium insertion capacity during the battery charging and discharging process, and has high chemical and electrochemical stability, which can ensure the overall performance of the aluminum current collector. Therefore, the performance and structure of the metal foil layer 10 are improved by the provision of the alloy layer 11, especially aluminum foil can be used to make the negative electrode of the lithium battery, which greatly reduces the cost and weight of the battery.
[0045] In some embodiments, the alloy layer 11 is disposed on at least one side of the metal foil layer 10 by evaporation, including: using aluminum as the first metal and evaporating by electron gun heating; and using copper as the second metal and evaporating by resistance heating. In some embodiments, the evaporation rate of aluminum is 15-20 angstroms / second, and the evaporation rate of copper is 1-2 angstroms / second.
[0046] Figure 2 The process of evaporating the alloy layer 11 on the metal foil layer 10 is given, such as Figure 2 As shown, a metal foil (copper foil or aluminum foil) is pasted onto a sample stage 20, and then the sample stage 20 is mounted on a base in a deposition chamber. The base drives the sample stage 20 to rotate under the action of a driving force, and the rotation speed of the sample stage 20 is 5-15r / min, for example, 10r / min. The metal vapor to be evaporated is placed in a crucible or an evaporation boat, such as a copper evaporation boat 30 and an aluminum evaporation boat 40. Before evaporation, the deposition chamber is evacuated to a vacuum degree of 1.0*10 -4 Pa~1.0*10 -5Pa. Before evaporation, different deposition rates of the two metals are set according to the control program, and the corresponding relationship between the deposition rate and the required control power is recorded. The deposition rates of the two metals are controlled by power during evaporation. In this embodiment, aluminum is used as the first metal and is evaporated by electron gun heating; copper is used as the second metal and is evaporated by resistance heating. The evaporation rates of the two metals can be regulated by power regulation, wherein the evaporation rate of copper is 1-2 angstroms / second and the evaporation rate of aluminum is 15-20 angstroms / second. By evaporating metal copper and metal aluminum at the deposition rate described above, the ratio of copper to aluminum in the alloy layer 11 can be accurately controlled to achieve the best ratio relationship to meet the optimal battery performance under the test conditions. As described above, by controlling the evaporation rate, the mass proportion of Al in the alloy layer 11 is 80%-95% of the total mass of the alloy layer 11, such as 80%, 85%, 90%, 95%, etc., to improve the energy density and coulomb efficiency of the battery.
[0047] The rotation speed of the sample stage 20 is controlled to be 5-15r / min, preferably 10r / min. The control of the rotation speed of the sample stage 20 can ensure the uniformity of metal deposition. The rotation speed matches the evaporation rate of the above alloy to ensure uniform control of the ratio of two or more alloys. By controlling the film formation time, a metal mixed layer with a thickness of 0.5 to 2um can be evaporated. Considering the process and film formation uniformity, 1um is preferred in the experiment.
[0048] Aluminum, as the first metal, forms an alloy compound with lithium to increase the capacity of lithium batteries. The theoretical capacity of the currently more mature graphite negative electrode is 372mAh / g, while the theoretical capacity of the aluminum negative electrode can reach 993mAh / g, which is about 2.67 times that of the graphite negative electrode.
[0049] Copper as the second metal can improve and refine the overall grain size of the alloy, reduce stress concentration problems, weaken the volume effect of the first metal during the alloying / de-alloying process, enhance stability during the charge and discharge process, maintain the overall structural stability of the current collector and electrode, and thus improve the battery cell cycle performance.
[0050] The disclosed embodiment adopts aluminum foil as the negative electrode current collector substrate, copper-aluminum alloy as the alloy layer 11, and adopts different proportions for electron gun and barrier evaporation co-deposition, and makes the mass proportion of Al account for 80%-95% of the total mass of the alloy layer 11, so that the volume effect of the lithium battery can be alleviated and the cycle performance of the battery cell is greatly improved.
[0051] In some embodiments, Figure 1 and Figure 3As shown, the alloy layer 11 is formed by evaporation on the metal foil layer 10 (taking aluminum foil as an example), and the alloy layer 11 has a first metal aluminum 111 and a second metal copper 112. The first metal aluminum 111 is evaporated by electron gun heating; and the second metal copper 112 is evaporated by resistance heating. A supplementary layer 12 is evaporated on the alloy layer 11 by lithium evaporation boat 50 or lithium crucible, and the supplementary layer 12 includes at least one of lithium, sodium, and potassium; in this embodiment, the supplementary layer 12 is lithium. In some embodiments, the thickness of the supplementary layer 12 is 200-500nm, for example, the thickness is 200nm, 300nm, 400nm, 500nm. In some embodiments, the supplementary layer 12 is evaporated by electron gun heating or resistance heating, and the evaporation speed is 40-60 angstroms / second, and the evaporation speed is 50 angstroms / second, for example. The role of the Li supplementary layer 12 coating is to supplement the irreversible capacity loss of the negative electrode during the first charging process, so as to achieve the purpose of improving the first coulomb efficiency and battery capacity.
[0052] The embodiment of the present disclosure also provides a lithium battery, comprising the alloy negative electrode for lithium ion battery as described in any one of the above. The positive electrode material is 90wt% lithium iron phosphate, 2-5wt% PVDF, 8-5wt% CNTS & conductive carbon black. The electrolyte is commercial electrolyte HR9212.
[0053] An embodiment of the present disclosure provides an alloy negative electrode for a lithium-ion battery, wherein the alloy negative electrode includes a metal foil layer, an alloy layer disposed on at least one side of the metal foil layer, and a supplementary layer disposed on a side of the alloy layer away from the metal foil layer. The lithium-ion battery formed by the alloy negative electrode provided by the present disclosure has high coulombic efficiency, long cycle life, and high cycle capacity retention rate. In addition, the lithium-ion battery formed by the alloy negative electrode provided by the present disclosure can alleviate the pulverization of the metal layer caused by the volume effect of expansion / contraction caused by aluminum metal during the embedding / ejection process of the lithium-ion negative electrode. The supplementary layer in the lithium-ion battery formed by the alloy negative electrode provided by the present disclosure can supplement the lithium ion concentration while protecting the structural integrity of the alloy negative electrode.
[0054] The following is an introduction to the test data of alloy negative electrode lithium battery through specific examples:
[0055] Embodiment 1:
[0056] In this embodiment, the negative electrode current collector is aluminum foil, the first metal of the alloy layer 11 is aluminum, accounting for 95% by mass, the second metal of the alloy layer 11 is copper, accounting for 5% by mass, and the supplementary layer 12 is lithium, with a thickness of 200nm.
[0057] Embodiment 2:
[0058] In this embodiment, the negative electrode current collector is aluminum foil, the first metal of the alloy layer 11 is aluminum, accounting for 90% by mass, the second metal of the alloy layer 11 is copper, accounting for 10% by mass, and the supplementary layer 12 is lithium, with a thickness of 200nm.
[0059] Embodiment 3:
[0060] In this embodiment, the negative electrode current collector is aluminum foil, the first metal of the alloy layer 11 is aluminum, accounting for 85% by mass, and the second metal of the alloy layer 11 is copper, accounting for 15% by mass. The supplementary layer 12 is lithium, with a thickness of 200nm.
[0061] Embodiment 4:
[0062] In this embodiment, the negative electrode current collector is aluminum foil, the first metal of the alloy layer 11 is aluminum, accounting for 80% by mass, the second metal of the alloy layer 11 is copper, accounting for 20% by mass, and the supplementary layer 12 is lithium, with a thickness of 200nm.
[0063] Comparative Example 1:
[0064] In this comparative example, the negative electrode current collector is aluminum foil, the alloy layer 11 contains only aluminum but no copper, and the supplementary layer 12 contains lithium with a thickness of 200 nm.
[0065] Embodiment 5:
[0066] In this embodiment, the negative electrode current collector is aluminum foil, the first metal of the alloy layer 11 is aluminum, accounting for 95% by mass, the second metal of the alloy layer 11 is copper, accounting for 5% by mass, and the supplementary layer 12 is lithium, with a thickness of 300nm.
[0067] Embodiment 6:
[0068] In this embodiment, the negative electrode current collector is aluminum foil, the first metal of the alloy layer 11 is aluminum, accounting for 90% by mass, the second metal of the alloy layer 11 is copper, accounting for 10% by mass, and the supplementary layer 12 is lithium, with a thickness of 300nm.
[0069] Embodiment 7:
[0070] In this embodiment, the negative electrode current collector is aluminum foil, the first metal of the alloy layer 11 is aluminum, accounting for 85% by mass, the second metal of the alloy layer 11 is copper, accounting for 15% by mass, and the supplementary layer 12 is lithium, with a thickness of 300nm.
[0071] Embodiment 8:
[0072] In this embodiment, the negative electrode current collector is aluminum foil, the first metal of the alloy layer 11 is aluminum, accounting for 80% by mass, the second metal of the alloy layer 11 is copper, accounting for 20% by mass, and the supplementary layer 12 is lithium, with a thickness of 300nm.
[0073] Comparative Example 2:
[0074] In this comparative example, the negative electrode current collector is aluminum foil, the alloy layer 11 contains only aluminum but no copper, and the supplementary layer 12 contains lithium with a thickness of 300 nm.
[0075] Embodiment 9:
[0076] In this embodiment, the negative electrode current collector is aluminum foil, the first metal of the alloy layer 11 is aluminum, accounting for 95% by mass, the second metal of the alloy layer 11 is copper, accounting for 5% by mass, and the supplementary layer 12 is lithium, with a thickness of 500nm.
[0077] Embodiment 10:
[0078] In this embodiment, the negative electrode current collector is aluminum foil, the first metal of the alloy layer 11 is aluminum, accounting for 90% by mass, the second metal of the alloy layer 11 is copper, accounting for 10% by mass, and the supplementary layer 12 is lithium, with a thickness of 500nm.
[0079] Embodiment 11:
[0080] In this embodiment, the negative electrode current collector is aluminum foil, the first metal of the alloy layer 11 is aluminum, accounting for 85% by mass, the second metal of the alloy layer 11 is copper, accounting for 15% by mass, and the supplementary layer 12 is lithium, with a thickness of 500nm.
[0081] Embodiment 12:
[0082] In this embodiment, the negative electrode current collector is aluminum foil, the first metal of the alloy layer 11 is aluminum, accounting for 80% by mass, the second metal of the alloy layer 11 is copper, accounting for 20% by mass, and the supplementary layer 12 is lithium, with a thickness of 500nm.
[0083] Comparative Example 3:
[0084] In this comparative example, the negative electrode current collector is aluminum foil, the alloy layer 11 contains only aluminum but no copper, and the supplementary layer 12 contains lithium with a thickness of 500 nm.
[0085] Table 1 Comparison of alloy negative electrode performance
[0086]
[0087] It can be seen from the comparison results of the alloy negative electrode performance in Table 1 that the thickness of the supplementary layer of Examples 1-4 and Comparative Example 1 is the same, and under the same number of cycles, as the aluminum content in the alloy layer exceeds 95% or is less than 80%, the lithium battery capacity retention rate is significantly reduced. When the aluminum content is 85%-90%, the lithium battery capacity retention rate is relatively high, exceeding 80%, indicating that the battery cell formed at this time has good discharge performance. Compared with the lithium battery capacity retention rate in Comparative Example 1, the lithium battery capacity retention rates in Examples 1-4 are all relatively high, so a single aluminum cannot be used as the negative electrode.
[0088] The coulombic efficiency of Examples 1-4 is higher than that of Comparative Example 1. In particular, when the aluminum content is 85%-90%, the coulombic efficiency of the lithium battery is higher, exceeding 95%, indicating that the battery cell formed at this time has good discharge performance. Compared with the coulombic efficiency of the lithium battery in Comparative Example 1, the coulombic efficiency of the lithium battery in Examples 1-4 is higher, so a single aluminum cannot be used as the negative electrode.
[0089] From the comparison results of the alloy negative electrode performance in Table 1, it can be seen that the supplementary layer thickness of Examples 5-8 and Comparative Example 2 is the same, and under the same number of cycles, as the aluminum content in the alloy layer 11 exceeds 95% or is less than 80%, the lithium battery capacity retention rate is significantly reduced. When the aluminum content is 85%-90%, the lithium battery capacity retention rate is relatively high, close to 90%, indicating that the battery cell formed at this time has good discharge performance. Compared with the lithium battery capacity retention rate in Comparative Example 2, the lithium battery capacity retention rates in Examples 5-8 are all relatively high, so a single aluminum cannot be used as the negative electrode.
[0090] The coulombic efficiency of Examples 5-8 is higher than that of Comparative Example 2. In particular, when the aluminum content is 85%-90%, the coulombic efficiency of the lithium battery is higher, exceeding 97%, indicating that the battery cell formed at this time has good discharge performance. Compared with the coulombic efficiency of the lithium battery in Comparative Example 2, the coulombic efficiency of the lithium battery in Examples 5-8 is higher, so a single aluminum cannot be used as the negative electrode.
[0091] It can be seen from the comparison results of the alloy negative electrode performance in Table 1 that the supplementary layer thickness of Examples 9-12 and Comparative Example 3 is the same, and under the same number of cycles, as the aluminum content in the alloy layer 11 exceeds 95% or is less than 80%, the lithium battery capacity retention rate is significantly reduced. When the aluminum content is 85%-90%, the lithium battery capacity retention rate is relatively high, exceeding 90%, indicating that the battery cell formed at this time has good discharge performance. Compared with the lithium battery capacity retention rate in Comparative Example 3, the lithium battery capacity retention rates in Examples 9-12 are all relatively high, so a single aluminum cannot be used as the negative electrode.
[0092] The coulombic efficiency of Examples 9-12 is higher than that of Comparative Example 3. In particular, when the aluminum content is 85%-90%, the coulombic efficiency of the lithium battery is higher, exceeding 98%, indicating that the battery cell formed at this time has good discharge performance. Compared with the coulombic efficiency of the lithium battery in Comparative Example 3, the coulombic efficiency of the lithium battery in Examples 9-12 is higher, so a single aluminum cannot be used as the negative electrode.
[0093] It can be seen from the comparison results of the alloy negative electrode performance in Table 1 that, compared with Examples 1-12, when the alloy material layer content is the same, as the thickness of the supplementary layer increases, the lithium battery capacity retention rate and coulomb efficiency both increase. Therefore, providing a supplementary layer can improve the performance of the battery cell. The Li supplementary layer can supplement the irreversible capacity loss of the negative electrode during the first charging process, thereby achieving the purpose of improving the first coulomb efficiency and battery capacity.
[0094] From the comparison results of the alloy negative electrode performance in Table 1, it can be seen that the incorporation of Cu can relieve the stress caused by the alloying of Al and Li, and the battery cell cycle performance is greatly improved compared with pure aluminum. The optimal proportion of Cu incorporation is between 10% and 15%. In the experiment, the battery cell with a Li layer thickness of 500nm has the best performance. The alloy material can be used as an electrode by depositing it on the metal current collector through a single evaporation, without the need to add a binder and a conductive material (such as conductive carbon black), which simplifies the procedure and improves efficiency.
[0095] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present disclosure, rather than to limit them; although the present disclosure has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present disclosure, and they should all be included in the scope of the claims and specification of the present disclosure. In particular, as long as there is no structural conflict, the various technical features mentioned in the various embodiments can be combined in any way. The present disclosure is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.
Claims
1. A lithium ion battery alloy negative electrode, characterized in that: include: Metal foil layer; An alloy layer is disposed on at least one side of the metal foil layer by evaporation, the alloy layer is a binary or higher alloy material, and one of the materials of the alloy layer is the same as the material of the metal foil layer; The supplementary layer is disposed on a side of the alloy layer away from the metal foil layer by evaporation, and is configured to supplement the lithium ion concentration.
2. The alloy negative electrode for lithium ion battery according to claim 1, characterized in that: The metal foil layer includes at least one of the following: aluminum foil, copper foil, nickel and nickel alloy, stainless steel; Optionally, the metal foil layer includes aluminum foil or copper foil.
3. The alloy negative electrode for lithium ion battery according to claim 1, characterized in that: The alloy layer includes at least two of the following: Cu, Al, Si, Zn, Ga, Ag, Sb, Ba, Pt, Au; Optionally, the alloy layer includes Cu and Al.
4. The alloy negative electrode for lithium ion battery according to claim 1, characterized in that: The supplemental layer includes at least one of lithium, sodium, and potassium; Optionally, the supplemental layer comprises lithium.
5. The alloy negative electrode for lithium ion battery according to claim 1, characterized in that: The alloy same as the material of the metal foil layer accounts for 80%-95% of the weight of the alloy layer material.
6. The alloy negative electrode for lithium ion battery according to claim 1, characterized in that: The thickness of the alloy layer is 0.5-2 um, and / or the thickness of the supplementary layer is 200-500 nm.
7. The alloy negative electrode for lithium ion battery according to claim 1, characterized in that: The alloy layer is disposed on at least one side of the metal foil layer by evaporation, and comprises: Aluminum is used as the first metal and is evaporated by electron gun heating; copper is used as the second metal and is evaporated by resistance heating.
8. The alloy negative electrode for lithium ion battery according to claim 7, characterized in that: The evaporation rate of aluminum is 15-20 angstroms / second, and the evaporation rate of copper is 1-2 angstroms / second.
9. The alloy negative electrode for lithium ion battery according to claim 1, characterized in that: The supplementary layer is evaporated by electron gun heating or resistance heating, and the evaporation rate is 40-60 angstroms / second.
10. A lithium battery, characterized in that: The invention comprises the alloy negative electrode for lithium ion battery according to any one of claims 1 to 9.
Citation Information
Cited By
Alloy electrode, zinc metal battery composite electrode and preparation method thereof, and zinc battery
CN120709268A