Method for preparing coated porous silica negative electrode based on polymethylsilsesquioxane
The coating porous silicon oxygen negative electrode material is prepared by combining polymethylsilsesquioxane with magnesium, silicon and carbon sources, which solves the problems of insufficient capacity and volume expansion of graphite negative electrode materials in lithium-ion batteries, and achieves high efficiency The energy density and cycle stability are suitable for the negative electrode materials of lithium-ion batteries.
Patent Information
- Application Number
- CN202411027706.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-30
AI Technical Summary
The theoretical capacity of graphite negative electrode materials in lithium-ion batteries is insufficient. The first Coulomb efficiency is low due to volume expansion and poor conductivity of silicon oxygen materials, which is difficult to meet the needs of high energy density energy storage.
The coated porous silicon oxygen negative electrode material is prepared by using polymethylsilsesquioxane and magnesium, silicon and carbon sources through ball mill mixing, high-temperature calcining and acid etching processes to form dual protection of silicon magnesate and amorphous carbon. layer to improve conductivity and electrochemical stability.
The theoretical capacity of silicon oxygen negative electrode material has been improved to 1500~1800 mAh/g, the first Coulomb efficiency has reached about 75%, the volume expansion is controlled within 30%, and the circulation stability is good, which is suitable for large-scale popularization.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to a method for preparing a coated porous silicon-oxygen composite negative electrode based on polymethylsilsesquioxane. Polymethylsilsesquioxane is prepared by a series of processes such as ball milling, high-temperature calcination, and acid etching with a magnesium source, a silicon source, and a carbon source. The preparation technology is beneficial to improving the energy density and first coulomb efficiency of the material and reducing volume expansion. It belongs to the negative electrode direction of lithium-ion batteries in the field of lithium-ion new energy material technology. Background Art
[0002] Lithium-ion batteries are widely used in the field of new energy. Graphite, as the most widely used negative electrode material in lithium-ion batteries, has a stable voltage platform and long cycle stability. However, the theoretical capacity of the material is only 372 mAh / g, which cannot meet human needs for high energy density energy storage devices. Silicon-based negative electrode materials have become one of the most promising negative electrode materials in the future due to their ultra-high specific capacity, but the volume expansion of pure silicon materials is large, and silicon oxide materials can alleviate the volume expansion problem of materials to a certain extent due to their special structural characteristics. The main structure of silicon oxide materials is silicon nanocrystals dispersed in silicon dioxide. During the first charge and discharge process, silicon dioxide will consume lithium salts, resulting in a decrease in the first efficiency of the material. Therefore, how to improve the first efficiency of silicon oxide materials is crucial. In addition, the conductivity of the silicon oxide negative electrode itself is poor, so how to improve the conductivity of the material itself is also something we need to consider.
[0003] In order to solve the above problems, multiple means are used to solve them. Patent CN117855434A discloses a lithium-ion battery pre-magnesium silicon oxide negative electrode material and preparation method. The invention simply mixes the magnesium source and silicon oxide in liquid phase, and then obtains the product by high-temperature pre-magnesium sintering and carbon coating. The preparation scheme is simple, the cost is low, and the experiment is safe and easy to scale up. Patent CN110550635B discloses a novel method for preparing carbon-coated silicon oxide negative electrode material. The invention adopts a combination of segmented mechanical fusion and carbon coating technology to achieve a good coating effect on SiO material particles. The coated material has the advantages of high first coulomb efficiency, good cycle performance, low cost, and environmental friendliness. Patent CN117038926A discloses a porous silicon oxide negative electrode material obtained by etching, and its preparation method and application. Among them, the porous silicon oxide particles have a porous structure, and the pore depth of the holes contained in the porous silicon oxide particles is above 200 nm. In the present invention, holes are etched on the surface of the silicon material through a porosification process to increase lithium ion transmission channels and shorten lithium ion diffusion paths. Metal-assisted acid etching, alkaline etching and other etching methods are used in combination, which has the characteristics of deep pore-making effect and good morphology control. The presence of the ion conductor layer makes the outer carbon shell more compact, and the ion migration rate and cycle are effectively improved. Summary of the invention
[0004] The purpose of the present invention is to pre-magnesiumize a silicon-oxygen material formed by polymethylsilsesquioxane using a magnesium source and a silicon source, coat the material with a carbon source, and finally obtain a silicon-oxygen negative electrode material with a porous structure by acid etching.
[0005] The theoretical capacity of silicon-oxygen negative electrode materials can be maintained at 1500~1800 mAh / g. During the charge and discharge process, lithium ions first react with oxygen atoms to replace oxygen atoms in silicon oxide to form Li2O compounds and silicon. Therefore, the first-cycle coulomb efficiency of silicon-oxygen negative electrode materials can reach up to about 75%. Due to the introduction of oxygen atoms to alleviate the volume effect, its volume expansion can be limited to within ~30%, and more preferably within 20%, and more preferably within 10%. It has good cycle stability and is a silicon-based negative electrode material that is expected to be widely popularized. Ball milling modification process: ball milling is used to crush multi-component materials and evenly mix them, providing a basis for stable reaction in the subsequent high-temperature calcination process.
[0006] High-temperature calcination process: Polymethylsilsesquioxane is converted into silicon-oxygen negative electrode material by high-temperature calcination in an inert atmosphere. In addition, the added carbon source material will also be pyrolyzed in the outer layer to form an amorphous carbon coating layer.
[0007] Pre-magnesiation process: Through the synergistic effect of magnesium salt and silicon source, while adjusting the silicon-oxygen ratio of the silicon-oxygen material, a magnesium silicate with a hard structure is formed as a protective layer for the silicon-oxygen negative electrode to inhibit the expansion of the material.
[0008] In some embodiments, the present invention also includes an acid etching process: using dilute acid to etch the material to remove components such as magnesium salts that have not reacted completely, making pores in the material to provide expansion space, and improving the wettability of the electrolyte to the material.
[0009] The dilute acid includes any one of 0.001-1 mol / L dilute hydrochloric acid, 0.001-1 mol / L dilute sulfuric acid, and 0.001-1 mol / L dilute nitric acid.
[0010] Based on the above-mentioned related means, the material is prepared by modifying polymethylsilsesquioxane as the basic raw material by adding magnesium salt, silicon source and carbon source: first, the polymethylsilsesquioxane, magnesium salt and other raw materials are further fully mixed when they are crushed by ball milling to ensure the uniformity of the subsequent reaction and to ensure the formation of more uniform magnesium silicate layer and carbon layer to protect the material; second, the silicon-oxygen composite material after high-temperature calcination is etched by dilute acid to form a void structure inside the material, which has a certain effect on improving ion mobility and reducing material volume expansion; third, the material is carbon-coated by adding a carbon source. After high-temperature calcination, the carbon source material will be converted into an amorphous carbon layer coating the outer layer of the material, which will improve the conductivity of the material while supporting the material structure.
[0011] In view of the above-mentioned related technical means, the present invention provides a coated porous silicon-oxygen negative electrode material prepared based on polymethylsilsesquioxane.
[0012] The technical solution provided by the present invention is as follows, comprising the following steps: Step (1): Weigh polymethylsilsesquioxane and magnesium salt in a certain mass ratio, add anhydrous ethanol, and mix thoroughly, which is recorded as mixed solution A.
[0013] Step (2): Transfer the mixed solution A to a ball mill, add zirconium beads, and ball mill at 300-800 rpm for 1-5 hours. Then add silicon powder and organic carbon source and continue ball milling for 1-2 hours. Take out the ball milling solution and filter to remove the dispersion. The solid component after removing the dispersion is recorded as solid A.
[0014] Step (3): Use a corundum ark to assemble a certain amount of solid A, and transfer the corundum to a tube furnace. The material is calcined at high temperature under an argon atmosphere, and two temperature gradients are set for calcination. In the first stage, the temperature is increased to 300-500 °C at a heating rate of 1-3 °C / min, and the temperature is kept at this temperature for 1-5 h; in the second stage, the temperature is increased to 800-1200 °C at a heating rate of 3-5 °C / min, and the temperature is kept at this temperature for 5-10 h. After sintering, it is naturally annealed. After the material is cooled to room temperature, it is taken out for use and recorded as solid B.
[0015] Step (4): Add dilute hydrochloric acid to solid B in multiple batches, with the concentration of dilute hydrochloric acid being 0.001 to 1 mol / L. Centrifuge at 400 to 2000 rpm for 2 to 7 min. After centrifugation, remove the dilute hydrochloric acid, wash with deionized water and anhydrous ethanol three times, take out the sample, dry it for later use, and record it as solid C.
[0016] Step (5): The silicon oxide negative electrode material prepared above is mixed with a binder (CMC) and acetylene black (AB) in a mass ratio of 8:1:1, mixed in a deionized water solvent to form a slurry, coated on a copper foil, and vacuum dried at 80 °C. The sheet is punched out as a working electrode, a metal lithium sheet is used as a counter electrode, and 1 M LiTFSI in DOL:DME (V:V = 1:1) + 1 wt.% LiNO3 is used as the experimental electrolyte system to assemble a button cell (half cell) and perform a charge and discharge cycle test.
[0017] Preferably, the mass ratio in step (1) is polymethylsilsesquioxane: magnesium salt: silicon powder: organic carbon source = 90: (1-5): (1-5): (1-5); preferably, the magnesium salt in step (1) is one of magnesium oxide, magnesium chloride and magnesium carbonate; preferably, the silicon powder in step (1) is micron-sized and has a size of 5-20 μm; preferably, the organic carbon source is one of glucose, citric acid and oxalic acid; preferably, the amount of anhydrous ethanol in step (1) is 10-50 ml, and more preferably, the amount of anhydrous ethanol is 150-250 ml.
[0018] Preferably, the rotation speed in step (2) is set between 350 and 550 rpm, and the ball milling time is controlled at 2 to 3 h.
[0019] Preferably, in step (3), the temperature of the first stage is controlled between 350 and 400° C., and the insulation time is 2 to 4 h; the temperature of the second stage is controlled between 1000 and 1150° C., and the insulation time is 6 to 8 h.
[0020] The numerical range of the present invention includes not only the point values listed above, but also any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0021] The technical solution of the present invention has the following beneficial effects: Improve the first effect: Use magnesium salt and silicon source as additives to regulate the interface layer of silicon-oxygen materials, improve the silicon-oxygen ratio of the material, and form a hard structure of magnesium silicate to protect the material structure. In this way, the purpose of improving the first effect of the material is achieved.
[0022] Improve electrical conductivity: By adding a carbon source, a carbon layer structure with good electrical conductivity is formed on the outside of the material to improve the electrical conductivity of the material.
[0023] Reduce volume expansion: A double protective layer structure of magnesium silicate and amorphous carbon layer is formed outside the silicon-oxygen material converted from polymethylsilsesquioxane, which can limit the volume expansion of the silicon-oxygen material. In addition, pores are formed in the material through acid etching to provide more space for volume expansion.
[0024] Improve electrochemical stability: Under the double protective layer structure, the material has better electrochemical stability and higher reversible specific capacity after cycling. DETAILED DESCRIPTION
[0025] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0026] Example 1 (1) Weigh 30 g of polymethylsilsesquioxane and place it in a beaker. Add 300 ml of anhydrous ethanol to disperse it and mix thoroughly.
[0027] (2) Transfer the mixed solution to a 500 ml ball mill, add an appropriate amount of 3 mm zirconium beads, adjust the ball mill speed to 400 rpm, and ball mill for 3 h. Remove the ball mill liquid by filtration to remove the dispersed liquid, collect the solid components, and keep them for later use.
[0028] (3) The material was calcined at high temperature using an atmosphere tube furnace. In the first stage, the temperature was increased to 350°C at a rate of 3°C / min and kept at this temperature for 3 h. In the second stage, the temperature was increased to 1000°C at a rate of 5°C / min and kept at this temperature for 6 h. After sintering, the material was naturally annealed. After cooling, the sample was taken out for later use.
[0029] (4) The calcined samples were acid washed in batches, with a dilute hydrochloric acid concentration of 0.015 mol / L, a single hydrochloric acid dosage of 7 ml, a centrifuge speed of 700 rpm, and a centrifugal time of 4 min. After centrifugation, the material was washed and dried for later use to obtain a silicon-oxygen negative electrode material.
[0030] (5) Assemble the battery using the materials from step (4).
[0031] Example 2 (1) Weigh 30 g of the material with a mass ratio of polymethylsilsesquioxane:magnesium oxide = 95:5, place it in a beaker, add 300 ml of anhydrous ethanol to disperse it, and mix it thoroughly.
[0032] (2) Transfer the mixed solution to a 500 ml ball mill, add an appropriate amount of 3 mm zirconium beads, adjust the ball mill speed to 400 rpm, and ball mill for 3 h. Remove the ball mill liquid by filtration to remove the dispersed liquid, collect the solid components, and keep them for later use.
[0033] (3) Use an atmosphere tube furnace to calcine the material at high temperature. In the first stage, the temperature is increased to 350°C at a rate of 3°C / min and kept at this temperature for 3 h. In the second stage, the temperature is increased to 1000°C at a rate of 5°C / min and kept at this temperature for 6 h. After sintering, natural annealing is performed. After cooling, the sample is taken out for use.
[0034] (4) The calcined samples were acid washed in batches, with a dilute hydrochloric acid concentration of 0.015 mol / L, a single hydrochloric acid dosage of 7 ml, a centrifuge speed of 700 rpm, and a centrifugal time of 4 min. After centrifugation, the material was washed and dried for later use to obtain a silicon-oxygen negative electrode material.
[0035] (5) Assemble the battery using the materials from step (4).
[0036] Example 3 (1) Weigh 30 g of the material with a mass ratio of polymethylsilsesquioxane:silicon powder = 95:5, place it in a beaker, add 300 ml of anhydrous ethanol to disperse it, and mix it thoroughly.
[0037] (2) Transfer the mixed solution to a 500 ml ball mill, add an appropriate amount of 3 mm zirconium beads, adjust the ball mill speed to 400 rpm, and ball mill for 3 h. Remove the ball mill liquid by filtration to remove the dispersed liquid, collect the solid components, and keep them for later use.
[0038] (3) The material was calcined at high temperature using an atmosphere tube furnace. In the first stage, the temperature was increased to 350°C at a rate of 3°C / min and kept at this temperature for 3 h. In the second stage, the temperature was increased to 1000°C at a rate of 5°C / min and kept at this temperature for 6 h. After sintering, the material was naturally annealed. After cooling, the sample was taken out for later use.
[0039] (4) The calcined samples were acid washed in batches, with a dilute hydrochloric acid concentration of 0.015 mol / L, a single hydrochloric acid dosage of 7 ml, a centrifuge speed of 700 rpm, and a centrifugal time of 4 min. After centrifugation, the material was washed and dried for later use to obtain a silicon-oxygen negative electrode material.
[0040] (5) Assemble the battery using the materials from step (4).
[0041] Example 4 (1) Weigh 30 g of the material with a mass ratio of polymethylsilsesquioxane: magnesium oxide = 95:2.5, place it in a beaker, add 300 ml of anhydrous ethanol to disperse it, and mix it thoroughly.
[0042] (2) Transfer the mixed solution to a 500 ml ball mill, add an appropriate amount of 3 mm zirconium beads, adjust the ball mill speed to 400 rpm, ball mill for 3 h, add 7.5 g of silicon powder, and ball mill for another 1 h. Remove the ball milling liquid, filter to remove the dispersed liquid, collect the solid components, and keep them for later use.
[0043] (3) Use an atmosphere tube furnace to calcine the material at high temperature. In the first stage, the temperature is increased to 350°C at a rate of 3°C / min and kept at this temperature for 3 h. In the second stage, the temperature is increased to 1000°C at a rate of 5°C / min and kept at this temperature for 6 h. After sintering, natural annealing is performed. After cooling, the sample is taken out for use.
[0044] (4) The calcined samples were acid washed in batches, with a dilute hydrochloric acid concentration of 0.015 mol / L, a single hydrochloric acid dosage of 7 ml, a centrifuge speed of 700 rpm, and a centrifugal time of 4 min. After centrifugation, the material was washed and dried for later use to obtain a silicon-oxygen negative electrode material.
[0045] (5) Assemble the battery using the materials from step (4).
[0046] Example 5 (1) Weigh 30 g of the material with a mass ratio of polymethylsilsesquioxane: glucose = 95:5, place it in a beaker, add 300 ml of anhydrous ethanol to disperse it, and mix it thoroughly.
[0047] (2) Transfer the mixed solution to a 500 ml ball mill, add an appropriate amount of 3 mm zirconium beads, adjust the ball mill speed to 400 rpm, and ball mill for 3 h. Remove the ball mill liquid by filtration to remove the dispersed liquid, collect the solid components, and keep them for later use.
[0048] (3) The material was calcined at high temperature using an atmosphere tube furnace. In the first stage, the temperature was increased to 350°C at a rate of 3°C / min and kept at this temperature for 3 h. In the second stage, the temperature was increased to 1000°C at a rate of 5°C / min and kept at this temperature for 6 h. After sintering, the material was naturally annealed. After cooling, the sample was taken out for later use.
[0049] (4) The calcined samples were acid washed in batches, with a dilute hydrochloric acid concentration of 0.015 mol / L, a single hydrochloric acid dosage of 7 ml, a centrifuge speed of 700 rpm, and a centrifugal time of 4 min. After centrifugation, the material was washed and dried for later use to obtain a silicon-oxygen negative electrode material.
[0050] (5) Assemble the battery using the materials from step (4).
[0051] Example 6 (1) Weigh 30 g of the material with a mass ratio of polymethylsilsesquioxane: magnesium oxide = 95:1, place it in a beaker, add 300 ml of anhydrous ethanol to disperse it, and mix it thoroughly.
[0052] (2) Transfer the mixed solution to a 500 ml ball mill, add an appropriate amount of 3 mm zirconium beads, adjust the ball mill speed to 400 rpm, and ball mill for 3 h. Add 3 g of silicon powder and 9 g of glucose, and ball mill for another hour. Remove the ball milling liquid, filter to remove the dispersed liquid, collect the solid components, and keep them for later use.
[0053] (3) The material was calcined at high temperature using an atmosphere tube furnace. In the first stage, the temperature was increased to 350°C at a rate of 3°C / min and kept at this temperature for 3 h. In the second stage, the temperature was increased to 1000°C at a rate of 5°C / min and kept at this temperature for 6 h. After sintering, the material was naturally annealed. After cooling, the sample was taken out for later use.
[0054] (4) The calcined samples were acid washed in batches, with a dilute hydrochloric acid concentration of 0.015 mol / L, a single hydrochloric acid dosage of 7 ml, a centrifuge speed of 700 rpm, and a centrifugal time of 4 min. After centrifugation, the material was washed and dried for later use to obtain a silicon-oxygen negative electrode material.
[0055] (5) Assemble the battery using the materials from step (4).
[0056] Example 7 (1) Weigh 30 g of the material with a mass ratio of polymethylsilsesquioxane: magnesium oxide = 95:2.5, place it in a beaker, add 300 ml of anhydrous ethanol to disperse it, and mix it thoroughly.
[0057] (2) Transfer the mixed solution to a 500 ml ball mill, add an appropriate amount of 3 mm zirconium beads, adjust the ball mill speed to 400 rpm, and ball mill for 3 h. Then add 3 g of silicon powder and 9 g of citric acid, and ball mill for another hour. Remove the ball milling liquid, filter and remove the dispersed liquid, collect the solid components, and keep them for later use.
[0058] (3) The material was calcined at high temperature using an atmosphere tube furnace. In the first stage, the temperature was increased to 350°C at a rate of 3°C / min and kept at this temperature for 3 h. In the second stage, the temperature was increased to 1000°C at a rate of 5°C / min and kept at this temperature for 6 h. After sintering, the material was naturally annealed. After cooling, the sample was taken out for later use.
[0059] (4) The calcined samples were acid washed in batches, with a dilute hydrochloric acid concentration of 0.015 mol / L, a single hydrochloric acid dosage of 7 ml, a centrifuge speed of 700 rpm, and a centrifugal time of 4 min. After centrifugation, the material was washed and dried for later use to obtain a silicon-oxygen negative electrode material.
[0060] (5) Assemble the battery using the materials from step (4).
[0061] The preparation process of the battery assembly of the above-mentioned Examples 1 to 7 is as follows: the silicon oxide negative electrode material is mixed with a binder (CMC) and acetylene black (AB) in a mass ratio of 8:1:1, mixed in a deionized water solvent to form a slurry, coated on a copper foil, and vacuum dried at 80°C. The sheet is punched as a working electrode, a metal lithium sheet is used as a counter electrode, and 1 M LiTFSI in DOL:DME (V:V=1:1)+1wt.%LiNO3 is used as the experimental electrolyte system to assemble button cells (half cells) and perform charge and discharge cycle tests. The performance indicators include: first cycle discharge capacity, reversible capacity after 100 cycles, first coulomb efficiency, and expansion ratio (electrode sheet thickness after 50 cycles / original electrode sheet thickness). The data are summarized in the following table.
[0062] Table 1 Cyclic stability and first effect of materials prepared in each example
[0063] It should be understood that the above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a coated porous silicon-oxygen negative electrode based on polymethylsilsesquioxane, characterized in that: The preparation steps include the following: Step (1): weigh polymethylsilsesquioxane and magnesium salt in a certain mass ratio, add anhydrous ethanol, and mix thoroughly, which is recorded as mixed solution A; Step (2): ball milling the mixed solution A, adding silicon powder and an organic carbon source and continuing the ball milling, taking out the ball milled solution and filtering to remove the dispersion liquid; the solid component after removing the dispersion liquid is recorded as solid A; Step (3): Use a corundum ark to assemble a certain amount of solid A, and transfer the corundum to a tube furnace, calcine the material at high temperature under an argon atmosphere, and anneal it naturally after sintering. After the material is cooled to room temperature, take it out for use, which is recorded as solid B, that is, the porous silicon oxide negative electrode.
2. The method for preparing a coated porous silicon-oxygen negative electrode based on polymethylsilsesquioxane according to claim 1, characterized in that: The mass ratio of the materials is polymethylsilsesquioxane: magnesium salt: silicon powder: organic carbon source = 90: (1-5): (1-5): (1-5).
3. The method for preparing a coated porous silicon-oxygen negative electrode based on polymethylsilsesquioxane according to claim 2, characterized in that: The magnesium salt in step (1) is one of magnesium oxide, magnesium chloride and magnesium carbonate; the silicon powder in step (1) is in micron size with a size of 5 to 20 μm; and the selected organic carbon source is one of glucose, citric acid and oxalic acid.
4. The method for preparing a coated porous silicon-oxygen negative electrode based on polymethylsilsesquioxane according to claim 1, characterized in that: The rotation speed in step (2) is set between 350 and 550 rpm, and the ball milling time is controlled at 2 to 3 h.
5. The method for preparing a coated porous silicon-oxygen negative electrode based on polymethylsilsesquioxane according to claim 1, characterized in that: The high temperature calcination process in step (3) is divided into two stages, wherein, in the first stage, the temperature is increased to 300-500°C at a heating rate of 1-3°C / min and kept at this temperature for 1-5 hours; in the second stage, the temperature is increased to 800-1200°C at a heating rate of 3-5°C / min and kept at this temperature for 5-10 hours, and natural annealing is performed after sintering is completed.
Citation Information
Patent Citations
Silicon-carbon negative electrode material, preparation method thereof and lithium ion battery
CN117810433A
Pre-magnesium silicon-oxygen negative electrode material of lithium ion battery and preparation method of pre-magnesium silicon-oxygen negative electrode material
CN117855434A