High-capacity lithium ion battery negative electrode material and preparation method thereof

By preparing Cu2O porous carbon material and doping with Sn metal, the problem of Cu2O volume change and insufficient conductivity in lithium-ion batteries is solved, the conductivity and cyclic stability of lithium-ion batteries are improved, and the capacity retention rate of the battery is significantly improved. and cycle life.

CN118919670AActive Publication Date: 2024-11-08DONGGUAN SANMO MATERIALS CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410937325.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-08
Estimated Expiration
2044-07-12

AI Technical Summary

Technical Problem

The volume change of Cu2O as the negative electrode material of lithium-ion batteries when reacting with lithium ions leads to structural rupture and electrode peeling, and the conductivity is insufficient, limiting its performance under fast charging and discharge conditions.

Method used

The copper benzene tricarboxylic acid metal organic frame material is prepared, and Cu2O porous carbon material is formed through carbonization and oxidation treatment, and ball milling with Sn metal under a protective atmosphere to form CuO/Cu2O/Sn three-component particles, which improve the conductivity and alleviate the volume change. .

Benefits of technology

It improves the conductivity and cyclic stability of the negative electrode material of lithium-ion battery, enhances the capacity retention rate, and significantly improves the cycle life and energy density of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919670A_ABST
    Figure CN118919670A_ABST
Patent Text Reader

Abstract

The invention discloses a high-capacity lithium ion battery negative electrode material and a preparation method thereof.The preparation method of the high-capacity lithium ion battery negative electrode material comprises the steps that S1, a copper benzene tricarboxylic acid metal organic framework material is prepared; s2, preparing a Cu2O porous carbon material; s3, preparing a Sn-doped Cu2O porous carbon material negative electrode material; the Cu particles play a catalytic role when forming the carbon material, so that a highly graphitized carbon matrix is formed, and the Cu2O porous carbon material has a three-dimensional porous morphology after the copper benzene tricarboxylic acid metal organic framework material is subjected to oxidation treatment, and is very beneficial to doping of Sn metal.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of battery materials, and in particular to a high-capacity lithium-ion battery negative electrode material and a preparation method thereof. Background Art

[0002] As one of the most mainstream rechargeable battery technologies, lithium-ion batteries are widely used in portable electronic devices, electric vehicles, energy storage systems and other fields. With the development of science and technology and the continuous pursuit of energy efficiency, the requirements for battery performance are getting higher and higher, especially for the energy density and cycle life of batteries. The negative electrode material of the battery is one of the key factors affecting these performances.

[0003] Although Cu2O has a high theoretical capacity as a negative electrode material for lithium-ion batteries, it has some shortcomings and disadvantages in practical applications. Cu2O undergoes a large volume change when reacting with lithium ions, which may lead to the rupture of the material structure and the peeling of the electrode, affecting the cycle stability of the battery; Cu2O's conductivity is not as good as some carbon-based materials, which limits its performance under fast charging and discharging conditions. Summary of the invention

[0004] In view of the above-mentioned deficiencies in the prior art, the present invention proposes a high-capacity lithium-ion battery negative electrode material and a preparation method thereof, aiming to further improve the capacity of the lithium-ion battery.

[0005] To achieve the above object, the present invention provides a method for preparing a negative electrode material for a high-capacity lithium-ion battery, comprising the following steps: A method for preparing a negative electrode material for a high-capacity lithium-ion battery, characterized in that it comprises the following steps:

[0006] S1. Preparation of copper trimesic acid metal organic framework material: dissolving copper salt and trimesic acid in a mixed solvent for reaction; after the reaction is completed, filtering the mixed solvent to obtain a reaction product, washing the reaction product with DMF, and then soaking it in a DCM solvent; the DCM solvent used for soaking needs to be replaced with a new DCM solvent every day, and the soaking time is 6 days; drying the soaked product at room temperature to obtain a copper trimesic acid metal organic framework material;

[0007] S2, preparing Cu2O porous carbon material: placing the copper benzene trimecate metal organic framework material prepared in S1 in a tube furnace, and firstly purging the tube furnace with N2 for 2 hours to perform carbonization treatment, and then cooling to room temperature after carbonization treatment; then switching the gas flow from N2 to O2 and performing oxidation treatment to obtain a Cu2O porous carbon material, wherein part of the Cu2O is further oxidized to CuO;

[0008] S3, doping with Sn metal: adding the Cu2O porous carbon material and Sn metal powder obtained in S2 into a ball mill, and mixing by ball milling under a protective atmosphere to obtain a Sn-doped Cu2O porous carbon material negative electrode material;

[0009] Optionally, the copper salt is one of copper nitrate, copper sulfate and copper chloride;

[0010] Optionally, the concentration of the copper salt in the mixed solvent is 0.15-0.2 mol / L, and the concentration of trimesic acid in the mixed solvent is 0.1-0.15 mol / L;

[0011] Optionally, the mixed solvent is a mixture of DMF, ethanol and deionized water in a volume ratio of 1:1:1;

[0012] Optionally, the reaction time in S1 is 23-24 hours, the reaction temperature is 70-75° C., and the soaking time is 6 days;

[0013] Optionally, the specific steps of the carbonization treatment are: heating the tube furnace to 800°C at a heating rate of 5°C per minute, and maintaining it in a N2 atmosphere for 5 hours; the specific steps of the oxidation treatment are: heating the tube furnace to 200°C at a heating rate of 3°C per minute, and maintaining it in an O2 gas flow for 9 hours;

[0014] Optionally, the mass ratio of the Cu2O porous carbon material to the Sn metal powder is 1:1-1:2; the ball milling mixing time is 3-4h; and the protective atmosphere is an argon atmosphere;

[0015] In order to achieve the above object, the present invention also provides a high-capacity lithium-ion battery negative electrode material prepared by the above method.

[0016] In order to achieve the above object, the present invention also provides a high-capacity lithium-ion battery negative electrode, comprising the above-mentioned high-capacity lithium-ion battery negative electrode material.

[0017] The beneficial effects of the present invention are as follows: since the Cu particles play a catalytic role when forming the carbon material, a highly graphitized carbon matrix is ​​formed; after oxidation treatment, the obtained Cu2O porous carbon material has a three-dimensional porous morphology, which is very conducive to the doping of Sn metal; the CuO / Cu2O / Sn three-component particles formed after doping with Sn metal have a synergistic effect on the conduction of lithium ions, thereby improving the conductivity of the negative electrode material; at the same time, the Sn-doped Cu2O porous carbon material can effectively alleviate the volume change of the negative electrode material due to its porous structure. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 This is a flow chart for preparing the Sn-doped Cu2O porous carbon material negative electrode material of Example 1. DETAILED DESCRIPTION

[0019] The embodiments of the present invention are described in detail below. The following embodiments are implemented on the premise of the technical solution of the present invention, and detailed implementation methods and specific operation processes are given, but the protection scope of the present invention is not limited to the following embodiments.

[0020] Example 1

[0021] 0.2 mol of copper nitrate and 0.1 mol of benzene trimecyl acid are dissolved in 1000 ml of a mixed solvent of DMF, ethanol and deionized water, wherein the volume ratio of DMF, ethanol and deionized water is 1:1:1, and the prepared solution is reacted in an oven at 75°C for 24 hours; after the reaction is completed, the mixed solvent is filtered to obtain a reaction product, the reaction product is washed with DMF, and then immersed in a DCM solvent; the DCM solvent used for immersion needs to be replaced with a new DCM solvent every day, and the immersion time is 6 days, and the product after immersion is dried at room temperature to obtain a copper benzene trimecyl acid metal organic framework material; the prepared copper benzene trimecyl acid metal organic framework material is placed in a tubular furnace, and the tubular furnace is first purged with N2 for 2 hours, and then the tubular furnace is heated to 800°C at a heating rate of 5°C per minute, and maintained for 5 hours under N2 atmosphere, and then cooled to room temperature; then the gas flow is switched from N2 to O 2, The tube furnace was heated to 200° C. at a heating rate of 3° C. per minute and maintained in an O 2 gas flow for 9 h to obtain a Cu 2 O porous carbon material, wherein a portion of the Cu 2 O was further oxidized to CuO;

[0022] The prepared Cu2O porous carbon material and Sn metal powder were added into a ball mill in a mass ratio of 1:1, and the Sn-doped Cu2O porous carbon material negative electrode material was obtained after ball milling and mixing for 4 hours under an argon atmosphere;

[0023] Preparation of negative electrode sheet: Add PVDF binder and N-methylpyrrolidone solvent into a stirrer, stir until the binder is completely dissolved, then add a conductive agent and the Sn-doped Cu2O porous carbon material negative electrode material prepared in the above Example 1, stir to obtain a negative electrode slurry, evenly coat the negative electrode slurry on an aluminum foil as a negative electrode current collector, and obtain a negative electrode sheet after rolling and slicing; the negative electrode active material in the negative electrode material accounts for 96% of the total weight, the weight ratio of the binder is 1%, the weight ratio of the conductive agent is 3%, the binder is PVDF, and the conductive agent is carbon black.

[0024] The positive electrode slurry and positive electrode sheet are prepared according to a ratio of 1% by weight of the binder, 2% by weight of the conductive agent, and 97% by weight of the positive electrode active material. The positive electrode active material is lithium iron phosphate, the binder is PVDF, and the conductive agent is carbon black. The preparation method of the positive electrode slurry and the positive electrode sheet is common knowledge in the art and will not be elaborated here.

[0025] The positive electrode sheet, negative electrode sheet and separator are prepared into a battery cell 1. The preparation method of the battery cell is common knowledge in the art and will not be described in detail here.

[0026] The prepared battery cell 1 was heated to 60 mAg -1 The constant current long cycle test was carried out for 200 cycles at a specific current; the specific capacity of the first cycle was 615 mAh g -1 The initial coulombic efficiency is 47.6%. The reason for the low initial coulombic efficiency is that the lithium is consumed at the reaction interface during the first cycle of the battery cell, the SEI film is formed, and the impurities on the surface of CuO, Cu2O and Sn metal are reduced. In the subsequent cycles, as the material is gradually activated, the coulombic efficiency gradually increases to 99%, and the specific capacity after 200 cycles is 934mAhg -1 , the capacity retention rate is 98%.

[0027] Example 2

[0028] The Cu2O porous carbon material was prepared according to the preparation steps of the Cu2O porous carbon material in Example 1, and the prepared Cu2O porous carbon material and Sn metal powder were added into a ball mill at a mass ratio of 1:2, and the Sn-doped Cu2O porous carbon material negative electrode material was obtained after ball milling and mixing for 4 hours under an argon atmosphere; the battery cell 2 was prepared according to the steps of Example 1.

[0029] The prepared battery cell 2 was heated at 60 mA g -1 The constant current long cycle test was carried out for 200 cycles at a specific current; the specific capacity of the first cycle was 593 mAh g -1 The initial Coulombic efficiency was 45.3%. In the subsequent cycles, as the material was gradually activated, the specific capacity after 200 cycles was 813 mAh g -1 , the capacity retention value is 95%.

[0030] Comparative Example 1

[0031] The step of doping S3 with Sn metal is omitted, and the Cu2O porous carbon material is used as the negative electrode active material. The steps of preparing the battery cell are the same as those in Example 1, thereby preparing the battery cell 3.

[0032] The prepared battery cell 3 was heated to 60 mAg -1 The constant current long cycle test was carried out for 200 cycles at a specific current; the specific capacity of the first cycle was 512 mAh g -1 The initial Coulombic efficiency was 44.9%. In the subsequent cycles, as the material was gradually activated, the specific capacity after 200 cycles was 759 mAh g -1 , the capacity retention value is 89%.

[0033] Comparative Example 2

[0034] 3g of lignin, 3g of zinc chloride, 3g of ammonium bicarbonate, 3g of ammonium chloride and 3g of potassium ferrate were ball-milled and mixed, the diameter of the grinding ball was 5mm, the mass ratio of the grinding ball to the total mass of biomass, zinc chloride, ammonium bicarbonate, ammonium chloride and potassium ferrate was 1:5.3, the rotation speed was 400r / min, the grinding time was 3h, and the mixture was uniformly mixed to obtain a mixture; the obtained mixture was placed in a high-temperature carbonization furnace, and inert protective gas nitrogen was continuously introduced at a rate of 25mL / min, and the temperature was first raised from room temperature to 300℃ at a rate of 1.5℃ / min, and then at 2℃ / min temperature to 850℃, maintain for 2 hours, and then slowly cool to room temperature to obtain a black carbon material; wash it three times with 5wt% hydrochloric acid solution, wash it three times with deionized water, and dry it to obtain a porous carbon material; add the above-mentioned porous carbon material and Sn metal powder into a ball mill at a mass ratio of 1:1, and obtain a Sn-doped porous carbon material negative electrode material after ball milling and mixing for 4 hours under an argon atmosphere. The Sn-doped porous carbon material negative electrode material is used as the negative electrode active material, and the steps of preparing the battery cell are the same as those in Example 1, thereby preparing battery cell 4.

[0035] The prepared battery cell 4 was heated to 60 mAg -1 The constant current long cycle test was carried out for 200 cycles at a specific current; the specific capacity of the first cycle was 454 mAh g -1 The initial Coulombic efficiency was 44.3%. In the subsequent cycles, as the material was gradually activated, the specific capacity after 200 cycles was 739 mAh g -1 , the capacity retention value is 88%.

[0036] Although the preferred embodiments of the present invention are described in detail above, it should be clearly understood that various modifications and variations are possible for those skilled in the art. Any modification, equivalent substitution, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a high-capacity lithium-ion battery negative electrode material, characterized in that: The following steps are involved: S1. Preparation of copper trimesic acid metal organic framework material: dissolving copper salt and trimesic acid in a mixed solvent for reaction; after the reaction is completed, filtering the mixed solvent to obtain a reaction product, washing the reaction product with DMF, and then soaking it in a DCM solvent; the DCM solvent used for soaking needs to be replaced with a new DCM solvent every day, and the soaking time is 6 days; drying the soaked product at room temperature to obtain a copper trimesic acid metal organic framework material; S2, preparing Cu2O porous carbon material: placing the copper benzene trimecate metal organic framework material prepared in S1 in a tube furnace, and firstly purging the tube furnace with N2 for 2 hours to perform carbonization treatment, and then cooling to room temperature after carbonization treatment; then switching the gas flow from N2 to O2 and performing oxidation treatment to obtain a Cu2O porous carbon material, wherein part of the Cu2O is further oxidized to CuO; S3. Preparation of Sn-doped Cu2O porous carbon material negative electrode material: Add the Cu2O porous carbon material obtained in S2 and the Sn metal powder into a ball mill, and mix them by ball milling under a protective atmosphere to obtain Sn-doped Cu2O porous carbon material negative electrode material.

2. The preparation method according to claim 1, characterized in that: The copper salt is one of copper nitrate, copper sulfate and copper chloride.

3. The preparation method according to claim 2, characterized in that: The concentration of the copper salt in the mixed solvent is 0.15-0.2 mol / L, and the concentration of trimesic acid in the mixed solvent is 0.1-0.15 mol / L.

4. The preparation method according to claim 1, characterized in that: The mixed solvent is DMF, ethanol and deionized water mixed in a volume ratio of 1:1:

1.

5. The preparation method according to claim 1, characterized in that: The specific steps of the carbonization treatment are: heating the tube furnace to 800° C. at a heating rate of 5° C. per minute and maintaining it for 5 hours under a N 2 atmosphere.

6. The preparation method according to claim 5, characterized in that: The specific steps of the oxidation treatment are: heating the tube furnace to 200° C. at a heating rate of 3° C. per minute and maintaining it in an O 2 gas flow for 9 hours.

7. The preparation method according to claim 1, characterized in that: The mass ratio of the Cu2O porous carbon material to the Sn metal powder is 1:1-1:

2.

8. The preparation method according to claim 1, characterized in that: The ball milling mixing time is 3-4 hours; the protective atmosphere is argon atmosphere.

9. A high-capacity lithium-ion battery negative electrode material prepared by the method for preparing a high-capacity lithium-ion battery negative electrode material according to claims 1-8. 10 . A high-capacity lithium-ion battery negative electrode, comprising the high-capacity lithium-ion battery negative electrode material according to claim 9 .

Citation Information

Patent Citations

  • Prismatic lithium ion battery for hybrid electric vehicle startup power supply and manufacturing method thereof

    CN105185996A

  • Preparation method of CuO / g-C3N4 composite material

    CN112978784A

  • Fiber electrodes for lithium secondary batteries, manufacturing method therefor, and lithium secondary batteries provided with fiber electrodes

    WO2010089991A1

  • Preparation method for porous graphite-doped and carbon-coated lithium titanate negative electrode material

    WO2016188130A1