Layered oxide positive electrode material and preparation method and application thereof

By controlling the ratio of C+S to α, β, and γ and low-temperature sintering technology, the problem of increasing viscosity of the positive electrode material during the slurry combination process is solved, the stability and energy density of the battery are improved, and better Cyclic performance.

CN118919672APending Publication Date: 2024-11-08LIYANG HINA BATTERY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410949623.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The contact between the layered oxide positive electrode material of ionic battery with carbon dioxide and water in the air during the slurry process leads to a rapid increase in viscosity, affecting the battery circulation performance and consistency, and has a low capacity performance.

Method used

Using a specific layered oxide positive electrode material chemical formula is NaNiaFebMncCu(1-a-b-c)O2+αMO/(βBO3/2+γAlO3/2), by controlling the ratio of C+S to α, β, and γ, The slurry viscosity increase rate is delayed and the air stability of the material is improved by low temperature sintering and the introduction of the cladding.

Benefits of technology

It effectively improves the air stability of the positive electrode material, delays deterioration time, improves the slurry performance, improves the capacity and energy density of the battery, and improves the circulation performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919672A_ABST
    Figure CN118919672A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of batteries, in particular to a layered oxide positive electrode material and a preparation method and application thereof. The layered oxide positive electrode material comprises NaNiaFebMncCu (1-a-b-c) O2 + alphaMO / (betaBO3 / 2 + gammaAlO3 / 2), a is greater than 0 and less than or equal to 0.5, b is greater than 0 and less than or equal to 0.4, c is greater than 0 and less than or equal to 0.4, a + b + c is greater than or equal to 0.8 and less than 1, alpha is greater than or equal to 0.05 and less than or equal to 0.1, beta is greater than or equal to 0.0005 and less than or equal to 0.001, and gamma is greater than or equal to 0.01 and less than or equal to 0.05; in the positive electrode material, the theoretical value of C + S, alpha, beta and gamma meet the equation that the theoretical value of C + S is equal to 100 / alpha + 1 / 4 * 1 / beta + 1 / gamma; and the difference value between the C + S theoretical value and the C + S measured value is-100 to 100 ppm. The positive electrode material has good air stability, can delay the rising rate of slurry viscosity, improves the first efficiency and capacity of the obtained battery, and improves the cycle performance of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of battery technology, and in particular to a layered oxide positive electrode material and a preparation method and application thereof. Background Art

[0002] During the slurrying process of the layered oxide positive electrode material of the ion battery, the positive electrode material comes into contact with carbon dioxide and water in the air, which will cause the slurry state to deteriorate during the slurrying process, and the viscosity will increase rapidly, affecting the battery cycle performance and product consistency. In addition, the capacity is relatively low, resulting in low energy density, which limits its application. Therefore, the problem of blocking the positive electrode material from contacting carbon dioxide and water in the air during the slurrying process needs to be solved urgently.

[0003] In view of this, the present invention is proposed. Summary of the invention

[0004] One object of the present invention is to provide a layered oxide positive electrode material to solve the technical problems of the prior art that the positive electrode material has poor air stability, a fast increase in the viscosity of the positive electrode slurry, and poor stability. The positive electrode material of the present invention has good air stability, can inhibit the rapid increase in the viscosity of the positive electrode slurry, and improve the stability of the slurry.

[0005] Another object of the present invention is to provide a method for preparing the layered oxide positive electrode material, which is simple and easy to implement. The obtained positive electrode material has excellent air stability, can slow down the viscosity increase rate of the positive electrode slurry, and improve the stability of the slurry.

[0006] Another object of the present invention is to provide a positive electrode sheet.

[0007] Another object of the present invention is to provide a battery.

[0008] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0009] A layered oxide positive electrode material, the chemical formula of the layered oxide positive electrode material includes NaNi a Fe b Mn c Cu (1-a-b-c) O2+αMO / (βBO 3 / 2 +γAlO 3 / 2), wherein 0<a≤0.5, 0<b≤0.4, 0<c≤0.4, 0.8≤a+b+c<1, 0.05≤α≤0.1, 0.0005≤β≤0.001, 0.01≤γ≤0.05, M comprises at least one of Mg, Ca, Sr and Ba; the layered oxide positive electrode material comprises C element and S element, and the theoretical value of C+S satisfies the relationship between the α, the β and the γ: C+S theoretical value=100 / α+1 / 4×1 / β+1 / γ; the difference between the C+S theoretical value and the C+S measured value is -100 to 100 ppm.

[0010] In some implementations, the ratio of β to γ ​​satisfies: 0.01≤β / γ≤0.1.

[0011] In some implementations, the ratio of α to γ ​​satisfies: 1≤α / γ≤2.

[0012] In some embodiments, the measured value of C+S satisfies: 1400ppm≤measured value of C+S≤2400ppm;

[0013] In some implementations, the ratio of the measured value of C to the measured value of S satisfies: 2≤C / S measured value≤3.

[0014] In some embodiments, in the layered oxide positive electrode material, NaNi a Fe b Mn c Cu (1-a-b-c) O2+αMO is the matrix material, βBO 3 / 2 +γAlO 3 / 2 It is a coating layer coated on the surface of the base material.

[0015] In some embodiments, the particle size D50 of the layered oxide positive electrode material satisfies: 5 μm≤D50≤20 μm.

[0016] The method for preparing the layered oxide positive electrode material as described above comprises the following steps:

[0017] A mixture of a copper-nickel-iron-manganese source, a sodium source and an element M source is subjected to a first sintering to obtain a first material; a mixture of the first material, a boron source and an aluminum source is subjected to a second sintering to obtain a positive electrode material.

[0018] In some embodiments, the copper-nickel-iron-manganese source includes: a mixture of a nickel-iron-manganese ternary precursor and a Cu source, or a copper-nickel-iron-manganese quaternary precursor.

[0019] In some embodiments, the chemical formula of the copper-nickel-iron-manganese quaternary precursor is Ni u Fe v Mn w Cu(1-u-v-w) (OH)2, wherein 0<u≤0.5, 0<v≤0.4, 0<w≤0.4, 0.8≤u+v+w≤1.

[0020] In some embodiments, the particle size D50 of the copper-nickel-iron-manganese quaternary precursor is 2.5 to 8.5 μm.

[0021] In some embodiments, the specific surface area of ​​the copper-nickel-iron-manganese quaternary precursor is 10 to 30 m 2 / g.

[0022] In some embodiments, the copper-nickel-iron-manganese quaternary precursor contains impurity elements Na, S, Ca, Mg, Al, Zn, Co and Li, and the total content is less than 5000 ppm.

[0023] In some embodiments, the sodium source includes at least one of sodium carbonate and sodium bicarbonate.

[0024] In some implementations, the temperature of the first sintering is 920-1050° C., and the holding time of the first sintering is 8-24 hours.

[0025] In some implementations, the heating rate of the first sintering is 1-10° C. / min.

[0026] In some embodiments, the sintering atmosphere of the first sintering is a compressed air atmosphere or an oxygen atmosphere.

[0027] In some implementations, the sintered material obtained by the first sintering is crushed and sieved to obtain a first material with a particle size D50 of 5 to 15 μm.

[0028] In some implementations, the temperature of the second sintering is 200-400° C., and the holding time of the second sintering is 8-24 hours.

[0029] In some embodiments, the heating rate of the second sintering is 1-10° C. / min.

[0030] In some embodiments, the sintering atmosphere of the second sintering is a compressed air atmosphere or an oxygen atmosphere.

[0031] In some implementations, the material obtained by the second sintering is crushed and sieved to obtain a layered oxide positive electrode material with a particle size D50 of 5 to 20 μm.

[0032] A positive electrode sheet comprises the layered oxide positive electrode material or the layered oxide positive electrode material obtained by the method for preparing the layered oxide positive electrode material.

[0033] A sodium ion battery comprises the positive electrode sheet.

[0034] Compared with the prior art, the present invention has the following beneficial effects:

[0035] (1) In the positive electrode material of the present invention, C, S and α, β and γ satisfy the above relationship, which can effectively improve the air stability of the positive electrode material, delay the air deterioration time of the positive electrode material, slow down the rate of increase of the slurry viscosity, and thus improve the performance of the positive electrode slurry, increase the capacity and energy density of the obtained battery, and improve the cycle performance.

[0036] (2) The preparation method of the positive electrode material of the present invention can slow down the rate of increase of the slurry viscosity by controlling the C+S theoretical value and the M source addition molar ratio α, the boron source addition molar ratio β and the aluminum source addition molar ratio γ in the positive electrode material to satisfy the above relationship; wherein, after the M source is added, its properties are close to those of Cu, which can make Cu better promote the degree of sintering reaction, thereby reducing the number of sintering times; the second calcination introduces a specific ratio of boron source and aluminum source at a low temperature, which can consume excess hydroxide while increasing the coating layer, thereby improving the air stability of the material.

[0037] (3) The battery obtained by the present invention has the characteristics of high initial efficiency, high capacity and good cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0039] Figure 1 It is a curve diagram showing the change of viscosity of the slurry prepared from the layered oxide positive electrode material in Example 6 and Comparative Examples 1 to 4 of the present invention over time;

[0040] Figure 2 This is an electron probe X-ray microanalysis diagram of the B element on the surface of the layered oxide positive electrode material in Example 6 of the present invention;

[0041] Figure 3 This is an electron probe X-ray microanalysis diagram of the Al element on the surface of the layered oxide positive electrode material in Example 6 of the present invention. DETAILED DESCRIPTION

[0042] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. If no specific conditions are specified in the examples, the conditions are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be obtained commercially.

[0043] According to one aspect of the present invention, the present invention relates to a layered oxide positive electrode material, the chemical formula of which includes NaNi a Fe b Mn c Cu (1-a-b-c) O2+αMO / (βBO 3 / 2 +γAlO 3 / 2 ), wherein 0<a≤0.5, 0<b≤0.4, 0<c≤0.4, 0.8≤a+b+c<1, 0.05≤α≤0.1, 0.0005≤β≤0.001, 0.01≤γ≤0.05, M comprises at least one of Mg, Ca, Sr and Ba; the layered oxide positive electrode material comprises C element and S element, and the theoretical value of C+S satisfies the relationship between the α, the β and the γ: C+S theoretical value=100 / α+1 / 4×1 / β+1 / γ; the difference between the C+S theoretical value and the C+S measured value is -100~100ppm.

[0044] In the positive electrode material of the present invention, C, S and α, β and γ satisfy the above relationship, which can improve the stability of the positive electrode material, effectively delay the air deterioration time of the positive electrode material, slow down the rate of increase of the slurry viscosity, and thus improve the performance of the positive electrode slurry, increase the capacity and energy density of the obtained battery, and improve the cycle performance.

[0045] It should be noted that the theoretical value of C+S mentioned above refers to the theoretical value of the sum of the C element content and the S element content in the layered oxide positive electrode material obtained by calculation, in ppm. The measured value of C+S refers to the sum of the C element content and the S element content in the layered oxide positive electrode material obtained by measuring and characterizing means, in ppm.

[0046] In some embodiments, the difference between the theoretical value of C+S and the measured value of C+S is -100 to 100 ppm, including but not limited to -100 ppm, -80 ppm, -50 ppm, -30 ppm, -10 ppm, 0 ppm, 10 ppm, 20 ppm, 30 ppm, 40 ppm, 50 ppm, 60 ppm, 70 ppm, 80 ppm, 90 ppm or 100 ppm, etc.

[0047] It should be noted that the sources of the C element of the present invention include but are not limited to sodium carbonate, sodium bicarbonate, other raw material impurities, introduction of sintering atmosphere and air introduction during the preparation process, etc. The sources of sulfur element include but are not limited to raw materials such as precursors, Cu sources, sodium sources, additives, etc.

[0048] In some embodiments, the value of a includes but is not limited to 0.01, 0.02, 0.05, 0.08, 0.1, 0.15, 0.2, 0.3, 0.4 or 0.5, etc., or a range value between any two. In some embodiments, the value of b includes but is not limited to 0.01, 0.05, 0.08, 0.1, 0.15, 0.2, 0.3 or 0.4, etc., or a range value between any two. In some embodiments, the value of c includes but is not limited to 0.01, 0.05, 0.08, 0.1, 0.2, 0.3 or 0.4, etc., or a range value between any two. In some embodiments, the value of a+b+c includes but is not limited to 0.8, 0.85, 0.88, 0.9, 0.95 or 0.98, etc., or a range value between any two.

[0049] In some embodiments, the value of γ includes but is not limited to 0.01, 0.02, 0.03, 0.04 or 0.05, etc. In some embodiments, 0.05≤α≤0.1, the value of α includes but is not limited to 0.05, 0.06, 0.07, 0.08, 0.09 or 0.1, etc., and α represents the molar sum of all elements M in MO. The value of β includes but is not limited to 0.0005, 0.0006, 0.0008, 0.0009 or 0.001, etc.

[0050] In some embodiments, the ratio of β to γ ​​satisfies: 0.01≤β / γ≤0.1. In some embodiments, the value of β / γ includes but is not limited to 0.01, 0.02, 0.03, 0.05, 0.06, 0.08 or 0.1, or any range between the two.

[0051] In some embodiments, the ratio of α to γ ​​satisfies: 1≤α / γ≤2. The value of α / γ includes but is not limited to 1, 1.1, 1.2, 1.3, 1.5, 1.6, 1.8 or 2, or any range between the two.

[0052] In some embodiments, the measured value of C+S satisfies: 1400ppm≤C+S measured value≤2400ppm; in some embodiments, the measured value of C+S includes but is not limited to 1400ppm, 1500ppm, 1600ppm, 1700ppm, 1800ppm, 1900ppm, 2000ppm, 2100ppm, 2200ppm, 2200ppm or 2400ppm, etc., or a range value between any two.

[0053] In some implementations, the ratio of the measured value of C to the measured value of S satisfies: 2≤C / S measured value≤3; for example, 2, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3, etc.

[0054] In some embodiments, in the layered oxide positive electrode material, NaNi a Fe b Mn c Cu (1-a-b-c) O2+αMO is the matrix material, βBO 3 / 2 +γAlO 3 / 2 It is a coating layer coated on the surface of the base material.

[0055] In some embodiments, the particle size D50 of the layered oxide positive electrode material satisfies: 5 μm ≤ D50 ≤ 20 μm. In some embodiments, the particle size D50 of the layered oxide positive electrode material is 5 μm, 8 μm, 10 μm, 12 μm, 15 μm, 18 μm, 20 μm, etc., or any range between the two.

[0056] In some embodiments, the layered oxide cathode material includes a single crystal cathode material having an O3 structure.

[0057] According to another aspect of the present invention, the present invention also relates to a method for preparing the layered oxide positive electrode material as described above, comprising the following steps:

[0058] A mixture of a copper-nickel-iron-manganese source, a sodium source and an element M source is subjected to a first sintering to obtain a first material; a mixture of the first material, a boron source and an aluminum source is subjected to a second sintering to obtain a positive electrode material.

[0059] The preparation method of the positive electrode material of the present invention is simple, easy and environmentally friendly. By controlling the total amount of carbon content C and sulfur content S in the positive electrode material and the M source addition molar ratio α, boron source addition molar ratio β and aluminum source addition molar ratio γ to satisfy the above relationship, the rate of increase of the slurry viscosity can be slowed down; wherein, after the M source is added, the properties of the M source are close to those of Cu, which can make Cu better promote the degree of sintering reaction, thereby reducing the number of sintering times; the second calcination introduces a specific ratio of boron source and aluminum source at a low temperature, which can consume excess hydroxide while increasing the coating layer, thereby improving the air stability of the material.

[0060] In the present invention, with the introduction of the boron source and the aluminum source, the sintering difficulty is reduced, the total CS value is at a low value, and a linear inverse relationship can be presented. The boron source includes H3BO3. The aluminum source includes aluminum hydroxide.

[0061] In some embodiments, the added molar ratio of the element M source is α, the added molar ratio of the boron source is β, and the added molar ratio of the aluminum source is γ; the added molar ratio of the element M source is α, the added molar ratio of the boron source is β, and the added molar ratio of the aluminum source is γ. The theoretical value of C+S in the layered oxide positive electrode material is controlled to satisfy the relationship between α, β and γ: C+S theoretical value = 100 / α+1 / 4×1 / β+1 / γ.

[0062] In some embodiments, the ratio of β to γ ​​is controlled to satisfy: 0.01≤β / γ≤0.1, and β / γ is, for example, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09 or 0.1, etc. In some embodiments, the ratio of α to γ ​​is controlled to satisfy: 1≤α / γ≤2, and α / γ is, for example, 1, 1.1, 1.3, 1.5, 1.6, 1.8 or 2, etc. In some embodiments, the measured values ​​of C and S are controlled to satisfy: 1400ppm≤C+S≤2400ppm, and the measured values ​​of C+S are, for example, 1400ppm, 1500ppm, 1600ppm, 1700ppm, 1800ppm, 1900ppm, 2000ppm, 2100ppm, 2200ppm, 2300ppm, 2400ppm, etc. The ratio of the measured value of C to the measured value of S is controlled to satisfy: 2≤C / S measured value≤3; C / S can be, for example, 2, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9 or 3, etc.

[0063] In some embodiments, the copper-nickel-iron-manganese source of the present invention includes a mixture of a nickel-iron-manganese ternary precursor and a Cu source, or a copper-nickel-iron-manganese quaternary precursor.

[0064] In some embodiments, in the copper-nickel-iron-manganese source, the chemical formula of the copper-nickel-iron-manganese quaternary precursor is Ni uFe v Mn w Cu (1-u-v-w) (OH)2, 0<u≤0.5, 0<v≤0.4, 0<w≤0.4, 0.8≤u+v+w≤1; the value of u is 0.01, 0.02, 0.05, 0.08, 0.1, 0.2, 0.3, 0.4 or 0.5, etc. The value of v is 0.01, 0.02, 0.05, 0.06, 0.08, 0.1, 0.2, 0.3 or 0.4, etc. The value of W is 0.01, 0.02, 0.05, 0.06, 0.08, 0.1, 0.2, 0.3 or 0.4, etc. The value of u+v+w is 0.8, 0.82, 0.85, 0.88, 0.9, 0.91, 0.92, 0.95, 0.98 or 1, etc.

[0065] In some embodiments, the particle size D50 of the copper-nickel-iron-manganese quaternary precursor is 2.5 to 8.5 μm, including but not limited to 2.5 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm or 8.5 μm, or any range between the two.

[0066] In some embodiments, the copper-nickel-iron-manganese quaternary precursor of the present invention has a suitable specific surface area. The specific surface area of ​​the copper-nickel-iron-manganese quaternary precursor is 10 to 30 m 2 / g, for example 10m 2 / g, 15m 2 / g, 20m 2 / g, 25m 2 / g, 30m 2 / g, etc., or any range between the two.

[0067] In some embodiments, the copper-nickel-iron-manganese quaternary precursor contains impurity elements Na, S, Ca, Mg, Al, Zn, Co and Li, and the content is less than 5000 ppm, for example, 1000 ppm, 2000 ppm, 3000 ppm, 4000 ppm, etc.

[0068] In some embodiments, the sodium source includes at least one of sodium carbonate (Na2CO3) and sodium bicarbonate (NaHCO3).

[0069] In some embodiments, the temperature of the first sintering is 920-1050°C, including but not limited to 920°C, 930°C, 950°C, 960°C, 975°C, 980°C, 990°C, 1000°C or 1050°C, or any range between the two. The holding time of the first sintering is 8-24h, including but not limited to 8h, 9h, 10h, 12h, 15h, 18h, 20h, 24h, or any range between the two. The heating rate of the first sintering is 1-10°C / min, such as 1°C / min, 2°C / min, 4°C / min, 5°C / min, 10°C / min, etc. The sintering atmosphere of the first sintering is a compressed air atmosphere or an oxygen atmosphere. The present invention ensures the effect of the first sintering by suitable first sintering conditions to ensure the physical and chemical properties of the obtained first material.

[0070] Furthermore, the sintered material obtained by the first sintering is crushed and sieved to obtain a first material with a particle size D50 of 5 to 15 μm, such as 5 μm, 6 μm, 8 μm, 10 μm, 12 μm or 15 μm, etc. The sintered material obtained by the first sintering is further crushed and sieved to obtain the first material with the above-mentioned suitable particle size.

[0071] In some embodiments, the temperature of the second sintering is 200-400°C, including but not limited to 200°C, 220°C, 250°C, 280°C, 300°C, 350°C, 400°C, etc., or any range between the two. The holding time of the second sintering is 8-24h, such as 8h, 10h, 12h, 15h, 18h, 20h, 22h or 24h, etc., or any range between the two. The heating rate of the second sintering is 1-10°C / min, such as 1°C / min, 2°C / min, 4°C / min, 5°C / min, 10°C / min, etc. The sintering atmosphere of the second sintering is a compressed air atmosphere or an oxygen atmosphere. The present invention adopts a suitable second sintering condition to ensure the effect of the second sintering, so as to ensure the physical and chemical properties and electrical properties of the positive electrode material.

[0072] Furthermore, the material obtained by the second sintering is crushed and sieved to obtain a layered oxide positive electrode material with a particle size D50 of 5 to 20 μm.

[0073] According to another aspect of the present invention, the present invention also relates to a positive electrode sheet, comprising the above-mentioned layered oxide positive electrode material, or the layered oxide positive electrode material obtained by the preparation method of the above-mentioned layered oxide positive electrode material.

[0074] The positive electrode sheet of the present invention comprises a positive electrode current collector and a positive electrode material layer located on the surface of the positive electrode current collector, and the positive electrode material layer comprises the above-mentioned layered oxide positive electrode material.

[0075] According to another aspect of the present invention, the present invention also relates to a sodium ion battery, comprising the above-mentioned positive electrode sheet.

[0076] In some embodiments, a sodium ion battery includes the above-mentioned positive electrode sheet, negative electrode sheet, separator and electrolyte.

[0077] The battery of the present invention has high initial efficiency, high capacity and high cycle stability.

[0078] The following is further explained in conjunction with specific embodiments and comparative examples.

[0079] Example 1

[0080] A method for preparing a layered oxide positive electrode material comprises the following steps:

[0081] Weigh 1.652kg Na2CO3 (purity 99.72%), 0.291kg NaHCO3 (purity 99.68%), 40.608g Mg(OH)2 (purity 99.21%), 104.630g CaCO3 (purity 99.12%), 4kg spherical precursor Cu 0.1 Mn 0.25 Ni 0.15 Fe 0.5 (OH)2, after high-speed mixing, sintered at high temperature at 920℃ oxygen atmosphere for 15h, with a heating rate of 2℃ / min, to obtain a primary sintered material, which was further crushed to obtain a first material (D50=14.7μm), and then 2.157g H3BO3 (purity of 99.02%) and 135.743g Al(OH)3 (purity of 99.24%) were added and mixed at high speed, and sintered at high temperature at 300℃ air atmosphere for 18h, with a heating rate of 3℃ / min, to obtain an O3 type positive electrode material with a particle size of D50=14.6μm; the chemical formula of the positive electrode material is: NaCu 0.1 Mn 0.25 Ni 0.15 Fe 0.5 O2+0.01Mg2Ca3O5 / (0.001BO 3 / 2 +0.05AlO 3 / 2 ).

[0082] Example 2

[0083] A method for preparing a layered oxide positive electrode material comprises the following steps:

[0084] Weigh 1.836kg Na2CO3 (purity 99.72%), 104.677g CaCO3 (purity 99.12%), 205.844g SrCO3 (purity 99.13%), 4kg precursor Cu0.01 Mn 0.45 Ni 0.44 Fe 0.1 (OH)2, after high-speed mixing, sintered at 1050℃ in air atmosphere for 18h, with a heating rate of 3℃ / min, to obtain a primary sintered material, which was further crushed to obtain a first material (D50=8.1μm), and then 10.789g H3BO3 (purity of 99.02%) and 135.803g Al(OH)3 (purity of 99.24%) were added for high-speed mixing, and sintered at 400℃ in air atmosphere for 16h, with a heating rate of 2℃ / min, to obtain an O3 type positive electrode material with a particle size D50 of 8.2μm; Chemical formula: NaCu 0.01 Mn 0.45 Ni 0.44 Fe 0.1 O2+0.01Ca3Sr4O7 / (0.005BO 3 / 2 +0.05AlO 3 / 2 ).

[0085] Example 3

[0086] A method for preparing a layered oxide positive electrode material comprises the following steps:

[0087] Weigh 1.838kg Na2CO3 (purity 99.72%), 103.025g SrCO3 (purity 99.13%), 275.45g BaCO3 (purity 99.12%), 4kg precursor Cu 0.03 Mn 0.34 Ni 0.31 Fe 0.32 (OH)2, after high-speed mixing, sintered at 980℃ air atmosphere for 10h, with a heating rate of 3℃ / min, to obtain a primary sintered material, which was further crushed to obtain a first material (D50=9.5μm), and then 2.160g H3BO3 (purity of 99.02%) and 135.938g Al(OH)3 (purity of 99.24%) were added for high-speed mixing, and sintered at 300℃ air atmosphere for 6h, with a heating rate of 3℃ / min, to obtain an O3 type positive electrode material with a particle size of D50=9.7μm, and a chemical formula of: NaCu 0.03 Mn 0.34 Ni 0.31 Fe 0.32 O2+0.02SrBa2O3 / (0.001BO 3 / 2 +0.05AlO 3 / 2 ).

[0088] Example 4

[0089] A method for preparing a layered oxide positive electrode material comprises the following steps:

[0090] Weigh 1.832kg Na2CO3 (purity 99.72%), 60.796g Mg(OH)2 (purity 99.21%), 256.703g SrCO3 (purity 99.13%), 4kg precursor Cu 0.05 Mn 0.49 Ni 0.44 Fe 0.02 (OH)2, after high-speed mixing, sintered at 1050℃ in air atmosphere for 18h, with a heating rate of 3℃ / min, to obtain a primary sintered material, which was further crushed to obtain the first material (D50=6.8μm), and then 2.153g H3BO3 (purity of 99.02%) and 135.485g Al(OH)3 (purity of 99.24%) were added for high-speed mixing, and sintered at 400℃ in air atmosphere for 18h, with a heating rate of 10℃ / min, to obtain an O3 type positive electrode material with a particle size of D50=6.7μm, and a chemical formula of: NaCu 0.05 Mn 0.49 Ni 0.44 Fe 0.02 O2+0.01Mg3Sr5O8 / (0.001BO 3 / 2 +0.05AlO 3 / 2 ).

[0091] Example 5

[0092] A method for preparing a layered oxide positive electrode material comprises the following steps:

[0093] Weigh 2.907kg NaHCO3 (purity 99.68%), 174.167g CaCO3 (purity 99.12%), 343.396g BaCO3 (purity 99.12%), 4kg precursor Cu 0.07 Mn 0.4 Ni 0.33 Fe 0.2 (OH)2, after high-speed mixing, sintered at 990℃ air atmosphere for 15h, with a heating rate of 3℃ / min, to obtain a primary sintered material, which was further crushed to obtain the first material (D50=5.4μm), and then 10.771g H3BO3 (purity of 99.02%) and 135.575g Al(OH)3 (purity of 99.24%) were added for high-speed mixing, and sintered at 200℃ oxygen atmosphere for 12h, with a heating rate of 8℃ / min, to obtain an O3 type positive electrode material with a particle size of D50=5.6μm, and a chemical formula of: NaCu 0.07 Mn 0.4 Ni0.33 Fe 0.2 O2+0.05CaBaO2 / (0.005BO 3 / 2 +0.05AlO 3 / 2 ).

[0094] Example 6

[0095] A method for preparing a layered oxide positive electrode material comprises the following steps:

[0096] Weigh 1.832kg Na2CO3 (purity 99.72%), 101.342g Mg(OH)2 (purity 99.21%), 4kg precursor Cu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 (OH)2, after high-speed mixing, sintered at 960℃ air atmosphere for 15h, with a heating rate of 3℃ / min, to obtain a primary sintered material, which was further crushed to obtain the first material (D50=10.1μm), and then 2.153g H3BO3 (purity of 99.02%) and 135.505g Al(OH)3 (purity of 99.24%) were added for high-speed mixing, and sintered at 200℃ air atmosphere for 16h, with a heating rate of 5℃ / min, to obtain a positive electrode material, D50=10.2μm, the chemical formula of the positive electrode material is: NaCu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 O2+0.05MgO / (0.001BO 3 / 2 +0.05AlO 3 / 2 ).

[0097] Example 7

[0098] A method for preparing a layered oxide positive electrode material comprises the following steps:

[0099] Weigh 1.999 kg Na2CO3 (purity 99.72%), 310.986 g CuO (purity 95.34%, D50 = 12.4 μm), 189.897 g CaCO3 (purity 99.12%), 4 kg precursor Mn 0.37 Ni 0.25 Fe 0.38After high-speed mixing, the mixture was sintered at 980°C in an air atmosphere for 24 hours at a heating rate of 5°C / min to obtain a primary sintered material, which was further crushed to obtain a first material (D50 = 9.8 μm). 2.349 g H3BO3 (purity 99.02%) and 147.819 g Al(OH)3 (purity 99.24%) were added for high-speed mixing, and sintered at 200°C in an air atmosphere for 14 hours at a heating rate of 5°C / min to obtain an O3 type positive electrode material with D50 = 9.8 μm and a chemical formula of: NaCu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 O2+0.05CaO / (0.001BO 3 / 2 +0.05AlO 3 / 2 ).

[0100] Example 8

[0101] A method for preparing a layered oxide positive electrode material comprises the following steps:

[0102] Weigh 1.832kg Na2CO3 (purity 99.72%), 256.741g SrCO3 (purity 99.13%), 4kg specific characteristic spherical precursor Cu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 After high-speed mixing, the mixture was sintered at 960°C in an air atmosphere for 15 hours at a heating rate of 3°C / min to obtain a primary sintered material, which was further crushed to obtain a first material (D50 = 9.8 μm). 2.153 g H3BO3 (purity 99.02%) and 135.505 g Al(OH)3 (purity 99.24%) were added for high-speed mixing, and sintered at 200°C in an air atmosphere for 16 hours at a heating rate of 5°C / min to obtain an O3 type positive electrode material with a particle size of D50 = 10.1 μm. The chemical formula of the positive electrode material is: NaCu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 O2+0.05SrO / (0.001BO 3 / 2 +0.05AlO 3 / 2 ).

[0103] Example 9

[0104] A method for preparing a layered oxide positive electrode material comprises the following steps:

[0105] Weigh 1.832kg Na2CO3 (purity 99.72%), 343.221g BaCO3 (purity 99.12%), 4kg precursor Cu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 (OH)2, after high-speed mixing, high-temperature sintering at 960℃ air atmosphere for 15h, heating rate of 3℃ / min, to obtain a primary sintered material, further crushed to obtain the first material (D50=9.7μm), then added 2.153gH3BO3 (purity of 99.02%), 135.505gAl(OH)3 (purity of 99.24%) for high-speed mixing, and high-temperature sintering at 200℃ air atmosphere for 16h, heating rate of 5℃ / min, to obtain O3 type positive electrode material, D50=9.6μm, the chemical formula of the positive electrode material is: NaCu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 O2+0.05BaO / (0.001BO 3 / 2 +0.05AlO 3 / 2 ).

[0106] Comparative Example 1

[0107] A method for preparing a layered oxide positive electrode material comprises the following steps:

[0108] Weigh 1.832kg Na2CO3 (purity 99.72%), 196.155g Y2O3 (purity 99.23%), 4kg precursor Cu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 (OH)2, after high-speed mixing, sintered at 960℃ air atmosphere for 15h, with a heating rate of 3℃ / min, to obtain a primary sintered material, which was then crushed to obtain the first material (D50=9.8μm), and then 2.153gH3BO3 (purity of 99.02%) and 135.505gAl(OH)3 (purity of 99.24%) were added and mixed at high speed, and sintered at 300℃ air atmosphere for 12h, with a heating rate of 3℃ / min, to obtain an O3 type positive electrode material with a particle size of D50=9.7μm. The chemical formula of the positive electrode material is: NaCu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 O2+0.05YO 3 / 2 / (0.001BO 3 / 2 +0.05AlO 3 / 2 ).

[0109] Comparative Example 2

[0110] A method for preparing a layered oxide positive electrode material comprises the following steps:

[0111] Weigh 1.832kg Na2CO3 (purity 99.72%), 343.221g BaCO3 (purity 99.12%), 4kg precursor Cu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 (OH)2, after high-speed mixing, sintered at 960℃ air atmosphere for 15h, with a heating rate of 3℃ / min, to obtain a primary sintered material, which was further crushed to obtain the first material (D50=9.6μm), and then 2.153gH3BO3 (purity of 99.02%) was added for high-speed mixing, and sintered at 300℃ air atmosphere for 12h, with a heating rate of 3℃ / min, to obtain an O3 type positive electrode material, D50=9.5μm, with the chemical formula: NaCu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 O2+0.05BaO / (0.001BO 3 / 2 ).

[0112] Comparative Example 3

[0113] A method for preparing a layered oxide positive electrode material comprises the following steps:

[0114] Weigh 1.832kg Na2CO3 (purity 99.72%), 256.741g SrCO3 (purity 99.13%), 4kg precursor Cu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 (OH)2, after high-speed mixing, sintered at 960℃ air atmosphere for 15h, with a heating rate of 3℃ / min, to obtain a primary sintered material, which was then crushed to obtain the first material (D50=10.2μm), and then 135.5.5g Al(OH)3 (purity of 99.24%) was added for high-speed mixing, and sintered at 300℃ air atmosphere for 12h, with a heating rate of 3℃ / min, to obtain an O3 type positive electrode material, D50=10.3μm, with the chemical formula: NaCu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 O2+0.05SrO / (0.05AlO 3 / 2 ).

[0115] Comparative Example 4

[0116] A method for preparing a layered oxide positive electrode material comprises the following steps:

[0117] Weigh 1.832kg Na2CO3 (purity 99.72%), 174.078g CaCO3 (purity 99.12%), 4kg precursor Cu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 (OH)2, after high-speed mixing, was sintered at 960℃ in air atmosphere for 15h, with a heating rate of 3℃ / min, to obtain a primary sintered material, which was further crushed to obtain the first material (D50=9.9μm), and was sintered at 300℃ in air atmosphere for 12h, with a heating rate of 3℃ / min, to obtain an O3 type positive electrode material, D50=9.8μm, the chemical formula of the positive electrode material is: NaCu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 O2 / (0.05CaO).

[0118] Experimental example

[0119] 1. Test of element content

[0120] The layered oxide positive electrode materials in each embodiment and comparative example were tested for S and C elements using a high-frequency infrared carbon-sulfur analyzer CS-2800G, specifically including: weighing 0.2g±0.001g of the standard sample, 0.5g±0.001g of the test sample, and heating at a temperature of 3000°C.

[0121] Through the test results of the above S and C content, the C+S measured value and the C / S measured value were obtained. The test results are shown in Table 1.

[0122] Table 1

[0123]

[0124] 2. Slurry viscosity test and coating element distribution test

[0125] The layered oxygen compound positive electrode materials provided in Example 6 of the present invention and Comparative Examples 1 to 4 were respectively used as active materials, mixed in a mass ratio of active material: SP: PVDF of 90:5:5, and NMP was added to prepare a viscous glue. The initial glue viscosity was tested by a viscosity tester (rotor No. 4, speed: 60 r / min), and then the glue viscosity was tested during the 12h placement. Figure 1 shown.

[0126] Depend on Figure 1It can be seen that the positive electrode material of the invention has good air stability, and the viscosity of the slurry remains basically unchanged after being placed for 12 hours. The slurries obtained from the positive electrode materials of Comparative Examples 1 to 4 all increase to 8000 mPa·s after being placed for 12 hours.

[0127] The electron probe X-ray microanalysis diagram of the B element coated on the surface of the positive electrode material in Example 6 is as follows: Figure 2 The electron probe X-ray microanalysis diagram of Al element is shown in Figure 3 shown.

[0128] 3. Battery electrochemical performance test

[0129] The positive electrode materials of each embodiment and comparative example are respectively prepared into batteries, specifically comprising:

[0130] Take 10g of the positive electrode material and place it flat on a plate cut into 100cm 2 The corresponding samples of the positive electrode material placed on A4 paper for 12 hours were used as active materials, mixed according to the mass ratio of active material: SP: PVDF of 90:5:5, and NMP was added to make a viscous glue (the glue is the slurry placed later), coated on aluminum foil, and baked in a vacuum drying oven at 120°C for 12 hours to obtain a positive electrode. A metal sodium sheet was used as the counter electrode, glass fiber (Waterman) as the diaphragm, electrolyte: 1mol / L NaPF6, solvents are EC and DMC, volume ratio = 1:1. 2032 button cells were assembled in an Ar protective glove box. The battery was tested in the voltage range of 2.5-4.0V, cycled at 0.1C for 3 weeks, and the discharge specific capacity, discharge specific capacity extreme difference and first efficiency of 5 batteries at 0.1C in the first 3 weeks were recorded.

[0131] The test results of the battery performance are shown in Table 2.

[0132] Table 2 Battery performance test results

[0133]

[0134] It can be seen from Table 2 that the batteries prepared from the positive electrode materials obtained by the methods of each embodiment of the present invention have high first efficiency, high capacity and small specific capacity range; among them, the first efficiency of the battery obtained from the positive electrode material in a conventional environment is above 91.7%, and the discharge specific capacity at 0.1C is above 131.06 mAh / g; the first efficiency of the battery obtained from the positive electrode material treated in a humid environment is above 91.5%, and the discharge specific capacity at 0.1C is 131.03 mAh / g and above.

[0135] The methods of Comparative Examples 1 to 4 do not meet the limitations of the present invention on raw materials and parameter conditions in the specific methods, and the air stability of the obtained positive electrode materials is poor. The batteries obtained in Comparative Examples 1 to 4 have low initial efficiency, small capacity, and large specific capacity range.

[0136] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A layered oxide positive electrode material, It is characterized in that The layered oxide positive electrode material includes NaNi a Fe b Mn c Cu (1-a-b-c) O 2 +αMO / (βBO 3 / 2 +γAlO 3 / 2 ), wherein 0<a≤0.5, 0<b≤0.4, 0<c≤0.4, 0.8≤a+b+c<1, 0.05≤α≤0.1, 0.0005≤β≤0.001, 0.01≤γ≤0.05, and M comprises at least one of Mg, Ca, Sr and Ba; The layered oxide positive electrode material contains C and S elements, and the theoretical value of C+S satisfies the relationship between α, β and γ: C+S theoretical value=100 / α+1 / 4×1 / β+1 / γ; The difference between the theoretical value of C+S and the measured value of C+S is -100 to 100 ppm.

2. The layered oxide positive electrode material according to claim 1, It is characterized in that Contains at least one of the following features (1) to (5): (1) The ratio of β to γ ​​satisfies: 0.01≤β / γ≤0.1; (2) The ratio of α to γ ​​satisfies: 1≤α / γ≤2; (3) The measured value of C+S satisfies: 1400ppm≤C+S measured value≤2400ppm; (4) The ratio of the measured value of C to the measured value of S satisfies: 2≤C / S measured value≤3; (5) In the layered oxide positive electrode material, NaNi a Fe b Mn c Cu (1-a-b-c) O 2 +αMO is the matrix material, βBO 3 / 2 +γAlO 3 / 2 It is a coating layer coated on the surface of the base material.

3. The layered oxide positive electrode material according to claim 1, It is characterized in that The particle size D50 of the layered oxide positive electrode material satisfies: 5 μm≤D50≤20 μm.

4. The method for preparing the layered oxide positive electrode material according to any one of claims 1 to 3, It is characterized in that The following steps are involved: A mixture of a copper-nickel-iron-manganese source, a sodium source and an element M source is subjected to a first sintering to obtain a first material; a mixture of the first material, a boron source and an aluminum source is subjected to a second sintering to obtain a positive electrode material.

5. The method for preparing the layered oxide positive electrode material according to claim 4, It is characterized in that Contains at least one of the following features (1) to (2): (1) The copper-nickel-iron-manganese source comprises: a mixture of a nickel-iron-manganese ternary precursor and a Cu source, or a copper-nickel-iron-manganese quaternary precursor; (2) The sodium source includes at least one of sodium carbonate and sodium bicarbonate.

6. The method for preparing the layered oxide positive electrode material according to claim 5, It is characterized in that Contains at least one of the following features (1) to (4): (1) The chemical formula of the copper-nickel-iron-manganese quaternary precursor is Ni u Fe v Mn w Cu (1-u-v-w) (OH) 2 , where 0<u≤0.5, 0<v≤0.4, 0<w≤0.4, 0.8≤u+v+w≤1; (2) The particle size D50 of the copper-nickel-iron-manganese quaternary precursor is 2.5 to 8.5 μm, (3) The specific surface area of ​​the copper-nickel-iron-manganese quaternary precursor is 10 to 30 m 2 / g; (4) The copper-nickel-iron-manganese quaternary precursor contains impurity elements Na, S, Ca, Mg, Al, Zn, Co and Li, with a total content of less than 5000 ppm.

7. The method for preparing the layered oxide positive electrode material according to claim 4, It is characterized in that Contains at least one of the following features (1) to (4): (1) The temperature of the first sintering is 920-1050° C., and the holding time of the first sintering is 8-24 hours; (2) The heating rate of the first sintering is 1 to 10°C / min; (3) The sintering atmosphere of the first sintering is a compressed air atmosphere or an oxygen atmosphere; (4) The sintered material obtained by the first sintering is crushed and sieved to obtain a first material with a particle size D50 of 5 to 15 μm.

8. The method for preparing the layered oxide positive electrode material according to claim 4, It is characterized in that Contains at least one of the following features (1) to (4): (1) The temperature of the second sintering is 200 to 400° C., and the holding time of the second sintering is 8 to 24 hours; (2) The heating rate of the second sintering is 1 to 10°C / min; (3) The sintering atmosphere of the second sintering is a compressed air atmosphere or an oxygen atmosphere; (4) The material obtained by the second sintering is crushed and sieved to obtain a layered oxide positive electrode material with a particle size D50 of 5 to 20 μm.

9. A positive electrode sheet, It is characterized in that The invention comprises the layered oxide positive electrode material according to any one of claims 1 to 3, or the layered oxide positive electrode material obtained by the preparation method of the layered oxide positive electrode material according to any one of claims 4 to 8.

10. A sodium ion battery, It is characterized in that Including the positive electrode sheet as described in claim 9.