Ultra-large current lithium iron phosphate battery and preparation method thereof

Through the combination of non-covalent modified carbon nanotubes and lithium iron phosphate, a network is formed, which solves the problem of insufficient performance of lithium iron phosphate batteries under low temperature and high magnification conditions, and significantly improves its electrochemical performance. It is suitable for High energy, high power applications.

CN118919680AActive Publication Date: 2024-11-08SHANGHAI XINZHI RUIQIAO POWER TECHNOLOGY CO LTD
View PDF 17 Cites 0 Cited by

Patent Information

Application Number
CN202410966894.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-08
Estimated Expiration
2044-07-18

AI Technical Summary

Technical Problem

Lithium iron phosphate batteries have poor performance under low temperature conditions and are not ideal in high-rate charging and discharging and high current, limiting their use in applications such as electric vehicles and smart grids.

Method used

Using a combination of non-covalent modified carbon nanotubes and lithium iron phosphate, the modified carbon nanotubes are mixed with carbon nanotubes by oligomerizing polyethylene glycol with carbon nanotubes to form a modified carbon nanotube dispersion and sintered with materials such as lithium iron phosphate. A mesh-like conductive network is formed to increase the diffusion rate of Li+.

Benefits of technology

The electrochemical performance of lithium iron phosphate batteries is significantly improved, including charging and discharging capacity, discharge current and rate performance, meeting the needs of high-energy and high-power lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of battery packs, in particular to an ultra-large current lithium iron phosphate battery and a preparation method thereof. The lithium iron phosphate battery is prepared by the following steps: preparing positive electrode slurry, coating the surface of an aluminum foil with the obtained positive electrode slurry to obtain a positive electrode plate, assembling the positive electrode plate, a negative electrode and a diaphragm, injecting an electrolyte, and sealing. Compared with the prior art, the lithium iron phosphate is coated with the modified carbon nanotubes, so that the charge-discharge capacity of the material under high current is improved, the rate capability and the cycle performance of the battery are improved, and the requirements of the market on high-energy and high-power lithium ion batteries can be met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of battery packs, and in particular to an ultra-large current lithium iron phosphate battery and a preparation method thereof. Background Art

[0002] Lithium iron phosphate is a highly regarded cathode material for lithium-ion batteries, known for its stable olivine structure. Batteries made of this material surpass lithium-ion batteries made of other cathode materials in terms of safety and cycle life, and are considered a strong candidate to replace traditional fossil energy, especially in the large-scale application of electric vehicles and energy storage systems.

[0003] CN106876705B provides a method for preparing an in-situ synthesized carbon / carbon nanotube-coated lithium iron phosphate composite material, which relates to the technical field of battery materials. The preparation method of the invention is: weighing raw materials lithium source, iron powder, phosphate, and carbon source; first ball-milling the iron powder and phosphate, adding hydrogen peroxide; then adding lithium source and carbon source to obtain slurry, drying, and sintering under the protection of reducing / inert gas; the invention adopts an in-situ synthesis method to prepare a carbon / carbon nanotube-coated lithium iron phosphate composite material with a short heat treatment time; the composite material has a high carbon coverage rate, stable electrochemical performance and good consistency, and the cycle performance and rate performance are greatly improved. The entire preparation process is simple and has the advantages of safety, high efficiency, low cost and green environmental protection.

[0004] CN102227024B discloses a positive electrode material lithium iron phosphate suitable for power lithium-ion batteries and a preparation method thereof, and the technical problem to be solved is to obtain a higher capacity. The positive electrode material lithium iron phosphate suitable for power lithium-ion batteries of the invention is based on doped lithium iron phosphate, and the matrix is ​​coated with carbon. The mass ratio is: lithium iron phosphate 50-99%, dopant 0.01-49%, carbon precursor 0.01-20%. The preparation method of the invention includes the following steps: mixing, doping, carbon coating, and sintering. Compared with the prior art, the invention adopts a multi-composite method to coat the lithium iron phosphate material with a carbon source, and the electronic conductivity reaches 6.2×10 -3 Scm -1 , reversible specific capacity greater than 155mAh / g, excellent rate performance, 20C / 1C retention rate greater than 90%, stable safety performance, suitable for lithium-ion battery power batteries, energy storage batteries, power tools, and various portable device batteries.

[0005] However, there are some challenges with lithium iron phosphate materials. Its inherent conductivity is relatively low, and the diffusion coefficient of lithium ions is not high, which leads to unsatisfactory performance of lithium iron phosphate batteries under low temperature conditions, and mediocre performance in high-rate charge and discharge performance and maximum current. These limitations hinder its application in electric vehicle power batteries (including pure electric vehicles and hybrid vehicles), starting power supplies, and smart grids for regulating peak and valley loads. Summary of the invention

[0006] In view of the above-mentioned defects of the prior art, the technical problem to be solved by the present invention is to provide an ultra-large current lithium iron phosphate battery and a preparation method thereof.

[0007] Lithium iron phosphate has the advantages of low price, excellent cycle performance, safety and stability, and has become the main cathode material for lithium-ion batteries. However, the arrangement of Fe, O, and P atoms in the bulk structure limits the Li + The capacity of the battery decays quickly under high current and the rate performance is poor. + The key is to improve the diffusion rate in LiFePO4 and thus increase its battery charge and discharge capacity and discharge current. At present, the main methods used are surface modification and element doping to improve the conductivity, or to shorten the LiFePO4 by nano-particle size. + Diffusion distance improves migration ability. The main way to modify the surface of lithium iron phosphate is to coat carbon, but although carbon materials such as carbon nanotubes, graphene and other carbon sources have excellent electrochemical properties, they have problems such as uneven structural coverage and easy agglomeration. At present, most carbon nanotubes are acidified to improve their defects of easy agglomeration, but this method will destroy the structure of the surface of carbon nanotubes. Therefore, the present invention provides a method of non-covalently modifying carbon nanotubes, mixing polyethylene glycol terminated with oligofuran with carbon nanotubes, because the polyethylene glycol terminated with oligofuran has amphiphilicity, and furan, as an aromatic ring with a π electron cloud, can form π-π interactions with the surface of carbon nanotubes, including van der Waals interaction forces and electrostatic interactions, so that the oligofuran end can be well adsorbed on the surface of carbon nanotubes, and the hydrophilic end of polyethylene glycol can enhance the dispersibility of carbon nanotubes in water. This non-covalent modification method not only improves the defect of easy agglomeration of carbon nanotubes when dispersed, but also improves the dispersibility of carbon nanotubes in solvents. The modified carbon nanotube dispersion is sintered with iron phosphate, lithium carbonate, etc. to obtain the positive electrode material. The oligofuran-terminated polyethylene glycol on the surface of the carbon nanotubes is cracked into a carbon network under high temperature, which plays the role of a conductive layer and a binder. The carbon network covers the surface of the lithium iron phosphate to form a mesh-like fast conductive network, which can well improve the Li + The diffusion rate in LiFePO4 increases its battery charge and discharge capacity and discharge current.

[0008] To achieve the above object, the present invention provides a method for preparing an ultra-high current lithium iron phosphate battery, comprising the following steps:

[0009] S1. Add lithium iron phosphate positive electrode material, conductive material and binder into N-methylpyrrolidone and stir evenly to obtain slurry, evenly coat it on aluminum foil, bake and compact it to obtain positive electrode sheet;

[0010] S2. Use the above-mentioned positive electrode sheet as the positive electrode, graphite as the negative electrode, and polypropylene film as the separator. After assembling, inject the electrolyte and seal it to obtain a battery.

[0011] Furthermore, the conductive material is acetylene black.

[0012] Furthermore, the binder is polyvinylidene fluoride.

[0013] Furthermore, the mass ratio of the lithium iron phosphate positive electrode material to the conductive material and the binder is 100:3-5:2-6.

[0014] Furthermore, the solid content of the positive electrode slurry is 40wt%.

[0015] Furthermore, the electrolyte includes lithium hexafluorophosphate, ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate, the concentration of lithium hexafluorophosphate is 1 mol / L, and the volume ratio of ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate is 1:1:1.

[0016] Preferably, the method for preparing the ultra-high current lithium iron phosphate battery comprises the following steps:

[0017] S1. Add lithium iron phosphate positive electrode material, acetylene black and polyvinylidene fluoride in a mass ratio of 100:3-5:2-6 to N-methylpyrrolidone and stir evenly to obtain a slurry, wherein the solid content of the positive electrode slurry is 40wt%, and the slurry is evenly coated on an aluminum foil, baked and compacted to obtain a positive electrode sheet;

[0018] S2. Use the above-mentioned positive electrode sheet as the positive electrode, graphite as the negative electrode, and a polypropylene film as a separator. After assembly, inject the electrolyte and seal it. The electrolyte includes lithium hexafluorophosphate, ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate. The concentration of lithium hexafluorophosphate is 1 moL / L, and the volume ratio of ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate is 1:1:1. Then, a battery is obtained.

[0019] The method for preparing the lithium iron phosphate positive electrode material comprises the following steps:

[0020] X1. Add 3-furanacetic acid to N,N-dimethylformamide, then add N-bromosuccinimide, stir at room temperature for 16-24 hours under nitrogen atmosphere, dilute with ethyl acetate, extract with water three times, dry and concentrate the organic phase after synthesis to obtain a residue, and recrystallize from ethanol for the next step;

[0021] X2. The product of the previous step was mixed with methoxy polyethylene glycol-hydroxy, and the temperature was raised to remove moisture. After adding dichloromethane and 4-dimethylaminopyridine, a dichloromethane solution of 1 mol / L dicyclohexylcarbodiimide was added dropwise. The mixture was stirred at room temperature for 40 to 60 hours and filtered. After adding ether to the filtrate, a precipitate appeared. The mixture was filtered and the residue was dried and added to N,N-dimethylformamide together with 2-(tributyltinyl)furan. Bistriphenylphosphine palladium dichloride was added under a nitrogen atmosphere. The mixture was heated and stirred for 40 to 60 hours and then ether was added to dilute the mixture. A precipitate appeared. The mixture was filtered and the residue was dried to obtain oligofuran-terminated polyethylene glycol. The oligofuran-terminated polyethylene glycol was mixed with multi-walled carbon nanotubes at a mass ratio of 10:1 and added to water to obtain a 10 wt% modified carbon nanotube dispersion.

[0022] X3. Li2CO3 and FePO4 are weighed and mixed in a molar ratio of 1:1, and 12wt% glucose is added. After ball milling and mixing evenly, a modified carbon nanotube dispersion is added to make the added amount of the modified carbon nanotubes 1-5wt%. After ball milling and spray drying, the mixture is heated to 700-800°C at a rate of 5°C / min and calcined for 4-6h to obtain a lithium iron phosphate positive electrode material.

[0023] Furthermore, the molar ratio of 3-furanacetic acid to N-bromosuccinimide is 3 to 5:8.

[0024] Furthermore, in step X2, the molar ratio of the product of the previous step to methoxypolyethylene glycol-hydroxy, 4-dimethylaminopyridine and dicyclohexylcarbodiimide is 5-15:5-10:1:1.

[0025] Furthermore, the temperature range of the heating and stirring in step X2 is 50-60°C.

[0026] Furthermore, in step X2, the molar ratio of the residue to 2-(tributylstannyl)furan and bistriphenylphosphine palladium dichloride is 1:4-5:0.1-0.25.

[0027] Preferably, the method for preparing the lithium iron phosphate positive electrode material comprises the following steps:

[0028] X1. Add 3-furanacetic acid to N,N-dimethylformamide, and then add N-bromosuccinimide, the molar ratio of 3-furanacetic acid to N-bromosuccinimide is 3-5:8, stir at room temperature for 16-24 hours under nitrogen atmosphere, add ethyl acetate to dilute, and extract with water three times. After the organic phase is synthesized, dry and concentrate to obtain a residue, which is recrystallized from ethanol for the next step;

[0029] X2. After mixing the product of the previous step with methoxy polyethylene glycol-hydroxy, the temperature was raised to remove moisture, dichloromethane and 4-dimethylaminopyridine were added, and then a 1 mol / L dicyclohexylcarbodiimide dichloromethane solution was added dropwise, and the mixture was stirred at room temperature for 40 to 60 hours and filtered. The molar ratio of the product of the previous step to methoxy polyethylene glycol-hydroxy, 4-dimethylaminopyridine, and dicyclohexylcarbodiimide was 5 to 15:5 to 10:1:1. After adding ether to the filtrate, a precipitate appeared, which was filtered. The residue was dried and then mixed with 2-(tributyltinyl)furan. Add to N,N-dimethylformamide, add bistriphenylphosphine palladium dichloride under nitrogen atmosphere, the molar ratio of the residue to 2-(tributyltinyl)furan and bistriphenylphosphine palladium dichloride is 1:4-5:0.1-0.25, heat and stir for 40-60 hours, then add ether to dilute, precipitate appears, filter, and dry the residue to obtain oligofuran-terminated polyethylene glycol, mix the oligofuran-terminated polyethylene glycol and multi-walled carbon nanotubes in a mass ratio of 10:1, and then add to water to obtain a 10wt% modified carbon nanotube dispersion;

[0030] X3. Li2CO3 and FePO4 are weighed and mixed in a molar ratio of 1:1, and 12wt% glucose is added. After ball milling and mixing evenly, a modified carbon nanotube dispersion is added to make the added amount of the modified carbon nanotubes 1-5wt%. After ball milling and spray drying, the mixture is heated to 700-800°C at a rate of 5°C / min and calcined for 4-6h to obtain a lithium iron phosphate positive electrode material.

[0031] The present invention also provides an ultra-large current lithium iron phosphate battery prepared by the above method.

[0032] Beneficial effects of the present invention:

[0033] The present invention improves the shortcomings of poor electronic conductivity and poor ionic conductivity of lithium iron phosphate materials by coating lithium iron phosphate with modified carbon nanotubes, improves the charge and discharge capacity of the material under large currents, improves the battery rate and cycle performance, and can meet the market demand for high-energy, high-power lithium-ion batteries. DETAILED DESCRIPTION

[0034] Methoxypolyethylene glycol-hydroxy, product number: YS-M4201, Mw=2000, Chongqing Yusi Pharmaceutical Technology.

[0035] Multi-walled carbon nanotubes, length: 10-20μm, diameter: 30-60nm.

[0036] Example 1

[0037] A method for preparing an ultra-high current lithium iron phosphate battery comprises the following steps:

[0038] S1. Add 100 g of lithium iron phosphate positive electrode material, 4 g of acetylene black and 5 g of polyvinylidene fluoride into N-methylpyrrolidone and stir evenly to obtain a slurry. The solid content of the positive electrode slurry is 40 wt %. The slurry is evenly coated on an aluminum foil, baked and compacted to obtain a positive electrode sheet.

[0039] S2. Use the above-mentioned positive electrode sheet as the positive electrode, graphite as the negative electrode, and a polypropylene film as a separator. After assembly, inject the electrolyte and seal it. The electrolyte includes lithium hexafluorophosphate, ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate. The concentration of lithium hexafluorophosphate is 1 moL / L, and the volume ratio of ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate is 1:1:1. Then, a battery is obtained.

[0040] The method for preparing the lithium iron phosphate positive electrode material comprises the following steps:

[0041] X1. Add 5 g of 3-furanacetic acid to 50 mL of N,N-dimethylformamide, then add 14.24 g of N-bromosuccinimide, stir at room temperature for 20 h under a nitrogen atmosphere, dilute with ethyl acetate, and extract with water three times. After the organic phase is synthesized, dry and concentrate to obtain a residue, which is recrystallized from ethanol for the next step;

[0042] X2. Mix 3.2 g of the product from the previous step with 15 g of methoxy polyethylene glycol-hydroxy, heat to 80° C. to remove moisture, add 100 mL of dichloromethane and 0.13 g of 4-dimethylaminopyridine, then dropwise add 10.6 mL of a 1 mol / L dicyclohexylcarbodiimide dichloromethane solution, stir at room temperature for 50 h, filter, add ether to the filtrate to produce a precipitate, filter, dry the residue, and add it together with 6 g of 2-(tributyltinyl)furan to 50 mL of N,N-dimethylformamide, add 0.5 g of bistriphenylphosphine palladium dichloride under a nitrogen atmosphere, heat to 60° C. to stir for 50 h, then add ether to dilute, produce a precipitate, filter, and dry the residue to obtain oligofuran-terminated polyethylene glycol, mix the oligofuran-terminated polyethylene glycol with multi-walled carbon nanotubes at a mass ratio of 10:1, and add them to water to obtain a 10 wt% modified carbon nanotube dispersion;

[0043] X3. Mix 73.89g of Li2CO3 and 150.79g of FePO4, add 26.96g of glucose, and add modified carbon nanotube dispersion after ball milling to make the added amount of modified carbon nanotubes 4wt%. After ball milling, spray dry and heat to 750℃ at a rate of 5℃ / min and calcine for 5h to obtain lithium iron phosphate positive electrode material.

[0044] Example 2

[0045] It is basically the same as Example 1, the only difference being that the added amount of the modified carbon nanotubes is 1 wt %.

[0046] Example 3

[0047] It is basically the same as Example 1, the only difference being that the added amount of the modified carbon nanotubes is 2 wt %.

[0048] Example 4

[0049] It is basically the same as Example 1, the only difference being that the added amount of the modified carbon nanotubes is 3 wt %.

[0050] Example 5

[0051] It is basically the same as Example 1, the only difference being that the added amount of the modified carbon nanotubes is 5 wt %.

[0052] Comparative Example 1

[0053] A method for preparing an ultra-high current lithium iron phosphate battery comprises the following steps:

[0054] S1. Add 100 g of lithium iron phosphate positive electrode material, 4 g of acetylene black and 5 g of polyvinylidene fluoride into N-methylpyrrolidone and stir evenly to obtain a slurry. The solid content of the positive electrode slurry is 40 wt %. The slurry is evenly coated on an aluminum foil, baked and compacted to obtain a positive electrode sheet.

[0055] S2. Use the above-mentioned positive electrode sheet as the positive electrode, graphite as the negative electrode, and a polypropylene film as a separator. After assembly, inject the electrolyte and seal it. The electrolyte includes lithium hexafluorophosphate, ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate. The concentration of lithium hexafluorophosphate is 1 moL / L, and the volume ratio of ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate is 1:1:1. Then, a battery is obtained.

[0056] The method for preparing the lithium iron phosphate positive electrode material comprises the following steps:

[0057] 73.89 g of Li2CO3 and 150.79 g of FePO4 were mixed, and 26.96 g of glucose was added. After ball milling and mixing evenly, the mixture was heated to 750°C at a rate of 5°C / min and calcined for 5 h to obtain a lithium iron phosphate positive electrode material.

[0058] Comparative Example 2

[0059] A method for preparing an ultra-high current lithium iron phosphate battery comprises the following steps:

[0060] S1. Add 100 g of lithium iron phosphate positive electrode material, 4 g of acetylene black and 5 g of polyvinylidene fluoride into N-methylpyrrolidone and stir evenly to obtain a slurry. The solid content of the positive electrode slurry is 40 wt %. The slurry is evenly coated on an aluminum foil, baked and compacted to obtain a positive electrode sheet.

[0061] S2. Use the above-mentioned positive electrode sheet as the positive electrode, graphite as the negative electrode, and a polypropylene film as a separator. After assembly, inject the electrolyte and seal it. The electrolyte includes lithium hexafluorophosphate, ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate. The concentration of lithium hexafluorophosphate is 1 moL / L, and the volume ratio of ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate is 1:1:1. Then, a battery is obtained.

[0062] The method for preparing the lithium iron phosphate positive electrode material comprises the following steps:

[0063] Mix 73.89g of Li2CO3 and 150.79g of FePO4, add 26.96g of glucose, ball-mill until the mixture is uniformly mixed, then add 10wt% carbon nanotube dispersion to make the added amount of carbon nanotubes 4wt%. After ball-milling, spray-dry and heat to 750℃ at a rate of 5℃ / min and calcine for 5h to obtain lithium iron phosphate positive electrode material.

[0064] Comparative Example 3

[0065] A method for preparing an ultra-high current lithium iron phosphate battery comprises the following steps:

[0066] S1. Add 100 g of lithium iron phosphate positive electrode material, 4 g of acetylene black and 5 g of polyvinylidene fluoride into N-methylpyrrolidone and stir evenly to obtain a slurry. The solid content of the positive electrode slurry is 40 wt %. The slurry is evenly coated on an aluminum foil, baked and compacted to obtain a positive electrode sheet.

[0067] S2. Use the above-mentioned positive electrode sheet as the positive electrode, graphite as the negative electrode, and a polypropylene film as a separator. After assembly, inject the electrolyte and seal it. The electrolyte includes lithium hexafluorophosphate, ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate. The concentration of lithium hexafluorophosphate is 1 moL / L, and the volume ratio of ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate is 1:1:1. Then, a battery is obtained.

[0068] The method for preparing the lithium iron phosphate positive electrode material comprises the following steps:

[0069] X1. Add 2 g of multi-walled carbon nanotubes to 100 mL of concentrated mixed acid (concentrated sulfuric acid: concentrated nitric acid = 3:1, v:v), stir evenly, and disperse by ultrasound at 400 W, 45 kHz at 80°C for 6 h. Filter and wash until the filtrate is neutral. Dry the residue to obtain acidified carbon nanotubes.

[0070] X2. Mix 73.89g of Li2CO3 and 150.79g of FePO4, add 26.96g of glucose, ball-mill until uniformly mixed, then add 10wt% of acidified carbon nanotube dispersion to make the added amount of acidified carbon nanotubes 4wt%. After ball-milling, spray-dry and heat to 750℃ at a rate of 5℃ / min and calcine for 5h to obtain lithium iron phosphate positive electrode material.

[0071] Test Example 1

[0072] The first discharge specific capacity of each battery was measured respectively. The measurement results are shown in Table 1. The measurement method is as follows: the nominal specific capacity is 170 mAh / g, charged to 4.2 V at a constant current of 0.1 C, left to stand for 2 minutes, and then discharged to 2.5 V at a constant current of 0.1 C. The test was stopped and the value was recorded.

[0073] Table 1 Battery charge and discharge test results

[0074] Experimental protocol First discharge specific capacity mAh / g Example 1 165.4 Example 2 140.2 Example 3 144.2 Example 4 140.2 Example 5 158.3 Comparative Example 1 130.1 Comparative Example 2 135.5 Comparative Example 3 138.4

[0075] From the data in the table, it can be seen that when carbon nanotubes are added to coat lithium iron phosphate, the discharge specific capacity is significantly improved. This is because the carbon nanotubes can form a three-dimensional conductive network structure on the surface of LiFePO4 particles after coating, and the excellent conductivity of carbon nanotubes increases the electron transmission speed on the surface of LiFePO4 particles, the electronic conductivity of LiFePO4 is improved, the conductivity of the composite material is significantly improved, and the electrochemical reaction can proceed more quickly. Compared with the control examples 1 to 3, it can be shown that modifying the carbon nanotubes can further improve the conductivity, which may be because the modified carbon nanotubes can improve the dispersibility of the carbon nanotubes so that they are better wrapped on the surface of LiFePO4 when mixed with it and are not easy to agglomerate. Compared with Example 1, the electrochemical performance of the battery in Example 1 is significantly better in Control Example 3. This may be because the acidification of carbon nanotubes will destroy the structure of the surface of carbon nanotubes, while in Example 1, a non-covalent modification of carbon nanotubes is adopted, in which polyethylene glycol capped with oligofuran is mixed with carbon nanotubes. Since the polyethylene glycol capped with oligofuran is amphiphilic, and furan, as an aromatic ring with a π electron cloud, can form π-π interactions with the surface of carbon nanotubes, including van der Waals interactions and electrostatic interactions, the oligofuran end can be well adsorbed on the surface of carbon nanotubes, and the hydrophilic end of polyethylene glycol can enhance the dispersibility of carbon nanotubes in water. This non-covalent modification method not only improves the defect of easy agglomeration of carbon nanotubes during dispersion, but also improves the dispersibility of carbon nanotubes in solvents. The modified carbon nanotube dispersion is sintered with iron phosphate, lithium carbonate, etc. to obtain the positive electrode material. The oligofuran-terminated polyethylene glycol on the surface of the carbon nanotubes is cracked into a carbon network under high temperature, which plays the role of a conductive layer and a binder. The carbon network covers the surface of the lithium iron phosphate to form a mesh-like fast conductive network, which can better improve the Li + The diffusion rate in LiFePO4 is high, so the battery performance in Example 1 is the best. Compared with Examples 2 to 5, the addition amount of modified carbon nanotubes in Example 1 is different. From the test results, it can be found that the performance of Example 1 is relatively the best. This may be because when the carbon nanotubes form a three-dimensional conductive network structure on the surface of LiFePO4 particles, when the addition amount is too small, the network structure will not be dense enough, and when the addition amount is too large, it will affect Li + transmission, so the addition amount in Example 1 is optimal.

[0076] Test Example 2

[0077] At 45°C, the lithium iron phosphate battery is charged to 4.35V at 1C constant current, then charged to 0.05C at constant voltage, and then discharged to 3.0V at 1C constant current. This is the first cycle, and 300 cycles of charge / discharge are performed according to the above conditions. The capacity retention rate of the lithium iron phosphate battery after 300 cycles at 45°C = (discharge capacity of 300 cycles / discharge capacity of the first cycle) × 100%. At 25°C, the lithium iron phosphate battery is charged to 4.35V at 1C constant current, then charged to a current of ≤0.05C at a constant voltage of 4.35V, and after 5 minutes of storage, discharged to a cut-off voltage of 3V at a constant current of 0.2C. At this time, the actual discharge capacity is recorded as D0. Then charge to 4.35V at 1C constant current, then charge to a current of ≤0.05C at a constant voltage of 4.35V, and finally discharge to a cut-off voltage of 3V at 2C. The actual discharge capacity at this time is recorded as D1. Rate performance = [(D1-D0) / D0] × 100%. See Table 2 for specific results.

[0078] Table 2 Battery rate performance and cycle test results

[0079] Experimental protocol Capacity retention rate / % Rate performance / % Example 1 99.1 95.3 Example 2 90.2 85.4 Example 3 92.3 88.1 Example 4 95.0 90.2 Example 5 96.7 91.1 Comparative Example 1 82.1 76.7 Comparative Example 2 85.3 80.2 Comparative Example 3 88.4 83.2

[0080] As can be seen from Table 2, compared with the control example and the embodiment, when carbon nanotubes are added to coat lithium iron phosphate, the electrochemical performance of the battery is obviously better, because the carbon nanotubes are coated on the surface of LiFePO4 to form a conductive network, thereby increasing the charge transfer rate of the positive electrode material, so the rate performance and cycle performance are improved. In Example 1, the polyethylene glycol terminated with oligofuran is mixed with carbon nanotubes. Since the polyethylene glycol terminated with oligofuran is amphiphilic, and furan, as an aromatic ring with a π electron cloud, can form π-π interactions with the surface of carbon nanotubes, including van der Waals interaction and electrostatic interaction, the oligofuran end can be well adsorbed on the surface of carbon nanotubes, and the polyethylene glycol hydrophilic end can enhance the dispersibility of carbon nanotubes in water. This non-covalent modification method not only improves the defect of easy agglomeration of carbon nanotubes when dispersed, but also improves the dispersibility of carbon nanotubes in solvents. The modified carbon nanotube dispersion is sintered with iron phosphate, lithium carbonate, etc. to obtain the positive electrode material. The oligofuran-terminated polyethylene glycol on the surface of the carbon nanotubes is cracked into a carbon network under high temperature, which plays the role of a conductive layer and a binder. The carbon network covers the surface of the lithium iron phosphate to form a mesh-like fast conductive network, which can better improve the Li + The diffusion rate in LiFePO4 is such that the battery in Example 1 has the best performance in various aspects. It improves the shortcomings of poor electronic conductivity and poor ionic conductivity of lithium iron phosphate materials, improves the charge and discharge capacity of the material under large current, improves the battery rate and cycle performance, and can meet the market's development needs for high-energy, high-power lithium-ion batteries.

[0081] The preferred specific embodiments of the present invention are described in detail above. It should be understood that a person skilled in the art can make many modifications and changes based on the concept of the present invention without creative work. Therefore, any technical solution that can be obtained by a person skilled in the art through logical analysis, reasoning or limited experiments based on the concept of the present invention on the basis of the prior art should be within the scope of protection determined by the claims.

Claims

1. A method for preparing an ultra-high current lithium iron phosphate battery, characterized in that: The steps include: S1. Add lithium iron phosphate positive electrode material, conductive material and binder into N-methylpyrrolidone and stir evenly to obtain slurry, evenly coat it on aluminum foil, bake and compact it to obtain positive electrode sheet; S2. Use the above-mentioned positive electrode sheet as the positive electrode, graphite as the negative electrode, and polypropylene film as the separator. After assembling, inject the electrolyte and seal it to obtain a battery.

2. The method for preparing the ultra-high current lithium iron phosphate battery according to claim 1, characterized in that: The conductive material is acetylene black.

3. The method for preparing the ultra-high current lithium iron phosphate battery according to claim 1, characterized in that: The binder is polyvinylidene fluoride.

4. The method for preparing the ultra-high current lithium iron phosphate battery according to claim 1, characterized in that: The mass ratio of the lithium iron phosphate positive electrode material to the conductive material and the binder is 100:3-5:2-6.

5. The method for preparing the ultra-high current lithium iron phosphate battery according to claim 1, characterized in that: The solid content of the positive electrode slurry is 40 wt %.

6. The method for preparing the ultra-high current lithium iron phosphate battery according to claim 1, characterized in that: The electrolyte includes lithium hexafluorophosphate, ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate, the concentration of lithium hexafluorophosphate is 1 mol / L, and the volume ratio of ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate is 1:1:

1.

7. The method for preparing the ultra-high current lithium iron phosphate battery according to claim 1, characterized in that: The method for preparing the lithium iron phosphate positive electrode material comprises the following steps: X1. Add 3-furanacetic acid to N,N-dimethylformamide, then add N-bromosuccinimide, stir at room temperature for 16-24 hours under nitrogen atmosphere, dilute with ethyl acetate, extract with water three times, dry and concentrate the organic phase after synthesis to obtain a residue, and recrystallize from ethanol for the next step; X2. The product of the previous step was mixed with methoxy polyethylene glycol-hydroxy, and the temperature was raised to remove moisture. After adding dichloromethane and 4-dimethylaminopyridine, a dichloromethane solution of 1 mol / L dicyclohexylcarbodiimide was added dropwise, and the mixture was stirred at room temperature for 40 to 60 hours and filtered. After adding ether to the filtrate, a precipitate appeared. The mixture was filtered, and the residue was dried and added to N,N-dimethylformamide together with 2-(tributyltinyl)furan. Bistriphenylphosphine palladium dichloride was added under a nitrogen atmosphere. After heating and stirring for 40 to 60 hours, ether was added to dilute the mixture. A precipitate appeared. The mixture was filtered, and the residue was dried to obtain oligofuran-terminated polyethylene glycol. The oligofuran-terminated polyethylene glycol was mixed with multi-walled carbon nanotubes at a mass ratio of 10:1 and added to water to obtain a 10 wt% modified carbon nanotube dispersion. X3. Li2CO3 and FePO4 are weighed and mixed in a molar ratio of 1:1, and 12wt% glucose is added. After ball milling and mixing evenly, a modified carbon nanotube dispersion is added to make the added amount of the modified carbon nanotubes 1-5wt%. After ball milling and spray drying, the mixture is heated to 700-800°C at a rate of 5°C / min and calcined for 4-6h to obtain a lithium iron phosphate positive electrode material.

8. The method for preparing the ultra-high current lithium iron phosphate battery according to claim 7, characterized in that: The molar ratio of the 3-furanacetic acid to N-bromosuccinimide is 3-5:8; in step X2, the molar ratio of the product of the previous step to methoxypolyethylene glycol-hydroxy, 4-dimethylaminopyridine, and dicyclohexylcarbodiimide is 5-15:5-10:1:

1.

9. The method for preparing a super-high current lithium iron phosphate battery according to claim 7, characterized in that: The temperature range of heating and stirring in step X2 is 50-60° C.; the molar ratio of the residue to 2-(tributylstannyl)furan and bistriphenylphosphine palladium dichloride in step X2 is 1:4-5:0.1-0.

25.

10. An ultra-high current lithium iron phosphate battery, characterized in that: Prepared by the method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Lithium iron phosphate anode material for power lithium ion battery and preparation method thereof

    CN102227024B

  • A method for in-situ synthesis of carbon / carbon nanotube-coated lithium iron phosphate composite materials

    CN106876705B

  • Method for preparing carbon nanometer-tube decorated with amphipathic nature polyalcohol

    CN101177255A

  • Hydroxyl group functionalization carbon nanotube for polyurethane chain-expanding agent and method for preparing same

    CN101332989A

  • Modified carbon nano tube and preparation method thereof

    CN102875844A