Silicon-carbon negative electrode material and preparation method thereof

By using a combination of spherical porous carbon matrix and nanosilicon in the negative electrode material of lithium-ion battery, combining the passivated carbon layer and the highly conductive outer carbon layer to form a conductive network, the problems of high resistivity and poor compressive resistance of the new silicon are solved. , improves the circulation and rate performance of the material.

CN118919688AActive Publication Date: 2024-11-08HEFEI GUOXUAN HIGH TECH POWER ENERGY

Patent Information

Application Number
CN202411009078.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-08
Estimated Expiration
2044-07-26

AI Technical Summary

Technical Problem

The new silicon carbon has high resistivity and poor compressive resistance, which leads to the material being easily broken under high pressure, affecting the circulation and rate performance of lithium-ion batteries.

Method used

Using spherical porous carbon matrix as the core, nanosilicon is distributed in its surface pores, and is coated by passivation carbon layer and high-conductive outer carbon layer, nanosilver is added to form a three-dimensional conductive network, reducing the material specific table, enhancing conductivity and structure strength.

Benefits of technology

The cycling performance and rate performance of the negative electrode material of lithium-ion battery is improved, the absolute volume expansion of the material during charging and discharging is reduced, the resistivity is reduced, and the cycle life of the battery is extended.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919688A_ABST
    Figure CN118919688A_ABST
Patent Text Reader

Abstract

The invention provides a silicon-carbon negative electrode material and a preparation method thereof, and relates to the technical field of lithium ion battery negative electrode material preparation. The silicon-carbon negative electrode material comprises an inner core and a coating layer, the inner core comprises one or more spherical porous carbon matrixes with surface pore channels, nanometer silicon is distributed in the surface pore channels of the spherical porous carbon matrixes, the coating layer coats the inner core and comprises a passivated carbon layer and a high-conductivity outer carbon layer, the passivated carbon layer coats the inner core, the high-conductivity outer carbon layer coats the passivated carbon layer, and the nanometer silicon is distributed in the surface pore channels of the spherical porous carbon matrixes. And nano-silver is dispersed and distributed in the high-conductivity outer carbon layer, so that the silicon-carbon negative electrode material is low in resistivity and excellent in rate capability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion battery negative electrode material preparation, and in particular to a silicon-carbon negative electrode material and a preparation method thereof. Background Art

[0002] Currently, lithium-ion batteries are widely used in various consumer electronic products, including mobile phones, laptops and power tools, due to their high energy, power density, fast charging capability and long cycle life. They are also used in electric vehicles, grid energy storage markets, aerospace and marine applications. Lithium-ion batteries include positive electrode materials, negative electrode materials, separators and electrolytes, among which negative electrode materials play a key role in the performance of lithium-ion batteries.

[0003] At present, the commonly reported negative electrode materials include silicon negative electrode materials, and the common types of silicon negative electrode materials are pre-lithium silicon oxygen and new silicon carbon. Among them, new silicon carbon has become a research and development hotspot for silicon negative electrode materials due to its good nano-scale cycle.

[0004] However, the resistivity of the new silicon carbon is between 10 and 30Ω·cm, and the powder resistivity is generally one order of magnitude higher than that of pre-lithium silicon oxygen (pre-lithium silicon oxygen powder resistance: 1Ω·cm). After compounding with graphite, the electrode membrane resistance is also high, which affects the rate performance of the battery cell. In addition, the multi-porous structure causes the material to have poor compressive resistance. Under high compaction, the material breaks and the silicon material is exposed, which reacts with the electrolyte and affects the battery cell cycle. Therefore, there are still many technical difficulties in the new silicon carbon technology that need to be solved. Summary of the invention

[0005] 1. Technical issues to be resolved

[0006] In view of the deficiencies of the prior art, the present invention provides a silicon-carbon negative electrode material and a preparation method thereof, which solves the technical problem of high resistivity of the existing new silicon-carbon.

[0007] (II) Technical solution

[0008] To achieve the above objectives, the present invention is implemented through the following technical solutions:

[0009] In one aspect, the present invention provides a silicon-carbon negative electrode material, the silicon-carbon negative electrode material comprising

[0010] The inner core comprises one or more spherical porous carbon matrices having surface pores, wherein nano-silicon is distributed in the surface pores of the spherical porous carbon matrix, and

[0011] The coating layer covers the inner core, and the coating layer comprises a passivated carbon layer and a highly conductive outer carbon layer. The passivated carbon layer covers the inner core, and the highly conductive layer covers the passivated carbon layer. Nanosilver is dispersed in the highly conductive outer carbon layer.

[0012] Preferably, the silicon-carbon negative electrode material is granular, and its particle size D50 is 6-10 μm; the mass ratio of the passivated carbon layer to the single-particle silicon-carbon negative electrode material is 3%-6%, and the mass ratio of the highly conductive outer carbon layer to the single-particle silicon-carbon negative electrode material is 2%-5%.

[0013] In another aspect, the present invention provides a method for preparing a silicon-carbon negative electrode material, comprising the following steps:

[0014] 1) dissolving n-hexane and ethanol in a mass ratio of 1:1 to 5 to obtain a mixed solution A;

[0015] A mixed solution of n-hexane and ethanol was used to remove soluble organic impurities.

[0016] 2) adding the medium-temperature coal tar pitch to part of the mixed solution A, mixing and heating to 100-150° C. at a stirring speed of 90-120 r / min, keeping the temperature for 2-4 hours, and then filtering to obtain the insoluble substance B;

[0017] 3) Mixing dimethyl silicone oil with the insoluble substance B, heating the mixture to 300-400° C. under stirring at 100-300 r / min, and keeping the mixture warm for 3-6 hours to obtain a spherical carbon precursor C, wherein the particle size D50 of the spherical carbon precursor is 1-4 μm;

[0018] 4) mixing the spherical carbon precursor C with a mixed solution of n-hexane and ethanol, heating to 100-150° C. at a stirring speed of 90-120 r / min, keeping warm for 2-4 hours, filtering, washing with ethanol, and drying to obtain a spherical carbon matrix, the spherical carbon matrix and KOH are mixed in a mass ratio of 1:1-1:3, calcined at 600-900° C. in an inert atmosphere for 1-4 hours, then washed with 0.5-1M hydrochloric acid, then washed with deionized water, and dried to prepare a spherical porous carbon matrix D with uniform pore distribution;

[0019] Dimethyl silicone oil is used as a dispersant. Under continuous stirring conditions, dimethyl silicone oil and insoluble substance B generate a spherical small-particle carbon matrix with uniform particle size (particle size D50 is 1 to 4 μm, not fine powder) due to surface tension and pressure. Since the carbon matrix has a uniform particle size and a regular spherical shape, the pore size of the material is uniform after pore formation, and the pore distribution is uniform. After silane deposition, nano-silicon is easily deposited uniformly in the pores to form a material with uniform material structure and high material structure strength. In addition, the stress generated by the volume effect in the spherical material in the lateral direction during the charge and discharge process can be partially offset, thereby improving the material's cycle performance. The carbon volume material is small, which, on the one hand, reduces the lithium ion transmission path and improves the material's rate performance. In addition, it reduces the absolute volume expansion of the material during the charge and discharge process, thereby improving the material's expansion and circulation.

[0020] 5) introducing a first mixed gas into the spherical porous carbon matrix D, heating to 400-700° C. and keeping the temperature for 2-6 hours, replacing the mixture with a second mixed gas, and keeping the temperature at 650-750° C. for 1-3 hours to obtain product E;

[0021] 6) introducing a third mixed gas into the product E at a gas flow ratio of 2:1 to 1:2, heating to 650 to 750° C. and keeping the temperature for 1 to 4 hours to obtain a silicon-carbon material precursor F;

[0022] Step 5) After depositing the nano-silicon, a carbon coating is first performed to passivate the surface, and then a secondary carbon coating is performed in step 6) to reduce the material specific surface area, increase the conductivity, and also completely isolate and passivate the nano-silicon in the matrix pores from the outside.

[0023] 7) adding the medium temperature coal tar pitch to a 0.1M silver nitrate solution, stirring for 1 to 3 hours at a stirring speed of 900 to 1200 r / min to form a solution with a solid content of 40 to 60%, and then filtering and drying the solution to form a composite carbon source G;

[0024] 8) The composite carbon source G and the silicon-carbon material precursor F are stirred and mixed at a mass ratio of 5:95 to 10:90 and a stirring speed of 300 to 500 r / min, and heated to 350°C to 500°C, and kept warm for 1 to 3 hours to complete granulation, and then calcined at 650°C to 900°C for 2 to 4 hours in an inert atmosphere to obtain a silicon-carbon negative electrode material I.

[0025] In steps 7) and 8), silver nitrate solution is mixed with cheap medium-temperature asphalt, and then in step 9), the asphalt is carbonized into a highly conductive dense carbon layer, which improves the conductivity, reduces the specific surface area, and restrains the expansion of nano-silicon during charging and discharging. At the same time, silver ions are reduced to nano-silver particles by the hydroxyl and carboxyl groups of the asphalt, and are evenly dispersed in the highly conductive dense carbon layer to form a three-dimensional conductive network, thereby improving the conductivity of the material.

[0026] Preferably, in step 2), the softening point of medium-temperature coal tar pitch is 280°C, and the mass ratio of medium-temperature tar pitch to solution A is 1:1 to 1:3.

[0027] Preferably, in step 3), the mass ratio of dimethyl silicone oil to insoluble substance B is 1:2 to 1:5, which ensures that the insoluble substance B can be fully dispersed and the particle size of the spherical carbon precursor C can be controlled.

[0028] Preferably, in the step 4), the mass ratio of the spherical carbon precursor C to the solution A is 1:1 to 1:3, the drying temperature is 60°C to 80°C, and the particle size D50 of the spherical porous carbon matrix D is 1 to 4 μm, generating a spherical small-particle carbon matrix with uniform particle size (particle size D50 is 1 to 4 μm, not a fine powder). The small particle size shortens the lithium ion transmission particle size, so that the material has excellent cycle performance.

[0029] Preferably, in step 5), the first mixed gas comprises silane and hydrogen, and the volume ratio of silane to hydrogen is 10:1 to 2:1. This ratio provides a highly reducing atmosphere and ensures the silicon source required for nano-silicon.

[0030] Preferably, in step 5), the second mixed gas comprises acetylene and argon, and the volume ratio of acetylene to argon is 2:1 to 1:3. This ratio ensures that the second mixed gas maintains a fluid state and also ensures the amount of carbon source acetylene required for coating.

[0031] Preferably, in step 6), the third mixed gas includes acetylene and an inert atmosphere. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0033] Figure 1 This is the XRD diagram of the silicon-carbon negative electrode material in Example 3 of the present invention.

[0034] Figure 2 Schematic diagram of the structure of the silicon-carbon negative electrode material of the present invention.

[0035] Figure 3 This is the full battery cycle result of the silicon-carbon negative electrode material of Example 3 of the present invention. DETAILED DESCRIPTION

[0036] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention are clearly and completely described. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] The embodiments of the present application provide a silicon-carbon negative electrode material and a preparation method thereof, thereby solving the technical problems of high resistivity and poor compressive resistance of the existing new silicon-carbon.

[0038] The technical solution in the embodiment of the present application is to solve the above technical problems, and the overall idea is as follows:

[0039] 1. At present, new silicon carbon is usually made of biomass, petroleum coke or resin, which is crushed into irregular blocks, and then a block-shaped porous carbon matrix is ​​formed after pore formation. The carbon matrix prepared by this method usually has an uneven particle size distribution, and there are fine powders (particle size <1μm, large specific surface area, and many side reactions) or large particles (>20μm, long lithium ion transmission path, and poor rate performance). The structure itself is prone to macroporous defects inside or on the surface due to reaction side reactions or the preparation environment. At the same time, the difference in particle size and formation leads to different local surface energy, which will also lead to uneven pore formation, affecting the uniformity of deposition and the electrochemical performance of the material. In addition, after the nano-silicon is deposited in the pores of the above-mentioned carbon matrix, due to the volume effect of silicon during the charging and discharging process, the stress of each local area of ​​the irregular shape material is different, and the material is easy to break and pulverize, which affects the material cycle performance. The preparation method of the present invention uses cheap medium-temperature coal tar as raw material, step 1) uses a mixed solution of n-hexane and ethanol to remove soluble organic impurities, and step 3) uses dimethyl silicone oil as a dispersant, and continuously stirs in a reactor under the action of surface tension and pressure to generate a spherical small-particle carbon matrix (1-4 μm, non-fine powder) with uniform particle size. Since the carbon matrix has a uniform particle size and a regular spherical shape, the material has a uniform pore size and a uniform pore distribution after pore formation. After silane deposition, nano-silicon is easily uniformly deposited in the pores to form a material with uniform material structure and high material structure strength. In addition, the stress generated by the volume effect in the spherical material in the lateral direction during the charge and discharge process can be partially offset, thereby improving the material cycle performance. The carbon volume material is relatively small, which, on the one hand, reduces the lithium ion transmission path and improves the material rate performance, and in addition, reduces the absolute volume expansion of the material during the charge and discharge process, thereby improving the material expansion and circulation.

[0040] 2. In step 5) of the present invention, after depositing nano-silicon, a carbon coating is first performed to passivate the surface, and then a secondary carbon coating is performed in step 6) to reduce the material specific surface area and increase the conductivity, while also completely isolating and passivating the nano-silicon in the matrix pores from the outside.

[0041] 3. In steps 7) and 8) of the present invention, a silver nitrate solution is mixed with cheap medium-temperature asphalt, and then in step 9), the asphalt is carbonized into a highly conductive dense carbon layer, which improves the conductivity, reduces the specific surface area, and restrains the expansion of nano-silicon during charging and discharging. At the same time, silver ions are reduced by the hydroxyl and carboxyl groups of the asphalt to form nano-silver particles, which are evenly dispersed in the highly conductive dense carbon layer to form a three-dimensional conductive network, thereby improving the conductivity of the material.

[0042] 4. The design structure of the present invention is a spherical new silicon-carbon (nanosilicon deposited in the pores of a porous carbon matrix) composite material with a small core and uniform particle size, and then one or more cores are compounded by granulation to form a finished product with a slightly larger size. The structural advantages include:

[0043] 1) Due to the multi-porous structure of the carbon matrix of the new silicon-carbon material, ion transmission needs to bypass the pores, and the ion conductivity is poor. The use of a small-sized core can shorten the lithium ion transmission path and increase the lithium ion transmission rate.

[0044] 2) Using medium-temperature asphalt granulation and carbonization to compound multiple cores can reduce the specific surface area of ​​the material (increase in particle size), reduce negative reactions with the electrolyte, and improve the first effect (reduce SEI film). Better wrapping of the core further inhibits the volume change of the material during the charge and discharge process, and wraps the core in all directions to improve the exposure of fresh silicon to the electrolyte due to the volume change of the silicon-based material during the battery cell cycle, effectively reducing negative reactions and improving the material cycle performance.

[0045] In addition, the carbon layers after carbonization of asphalt have a larger interlayer spacing, which provides a fast channel for the transport of electrons and lithium ions. The nanosilver dispersed in it further enhances the conductivity of the material, improving the shortcomings of this type of material, such as high resistivity and poor rate performance.

[0046] 5. If Figure 2 The silicon-carbon negative electrode material of the present invention comprises an inner core, which comprises one or more spherical porous carbon matrices with surface pores, wherein nano-silicon is distributed in the surface pores of the spherical porous carbon matrix, and a coating layer, which coats the inner core, wherein the coating layer comprises a passivated carbon layer and a highly conductive outer carbon layer, wherein the passivated carbon layer coats the inner core, and the highly conductive layer coats the passivated carbon layer, wherein nano-silver is dispersed in the highly conductive outer carbon layer.

[0047] In order to better understand the above technical solution, the above technical solution will be described in detail below in conjunction with the accompanying drawings and specific implementation methods.

[0048] Example 1

[0049] This embodiment provides a method for preparing a long-cycle silicon-carbon negative electrode material, which is as follows:

[0050] The mixed solution A was obtained by dissolving n-hexane and ethanol in a mass ratio of 1:3, and medium-temperature coal tar with a softening point of 280°C was added in a mass ratio of 1:1, placed in a reactor and heated to 100°C, stirred at 100r / min for 2h, and then filtered. The obtained insoluble substance B and dimethyl silicone oil were placed in a reactor in a mass ratio of 1:2, heated to 300°C, kept warm for 3h, stirred at 100r / min, and spherical carbon precursor C was obtained. The spherical carbon precursor C was mixed in a mass ratio of 1:1. : 1 is put into a mixed solution of n-hexane and ethanol, placed in a reactor and heated to 100°C, stirred at 100r / min for 2h, then filtered, washed with ethanol, and dried at 60°C to obtain a spherical carbon matrix. The spherical carbon matrix is ​​mixed with KOH in a mass ratio of 1:1, calcined at 600°C under an inert atmosphere for 1h, then washed with 0.5M hydrochloric acid, then washed with deionized water, and dried at 60°C to obtain a spherical porous carbon matrix D with a particle size D50 of 1μm and uniform pore distribution.

[0051] The spherical porous carbon matrix D is placed in a fluidized bed, and a mixture of silane and hydrogen is introduced at a gas flow ratio of 10:1, heated to 400°C and kept warm for 2 hours, and then a mixture of acetylene and argon is introduced at a gas flow ratio of 2:1, and kept warm at 650°C for 1 hour to obtain product E. Product E is placed in a CVD, and a mixture of acetylene and inert atmosphere is introduced at a gas flow ratio of 2:1, and kept warm at 650°C for 1 hour to obtain a long-cycle silicon-carbon material precursor F; medium-temperature coal tar is added to a 0.1M silver nitrate solution, stirred for 2 hours at a stirring speed of 1000r / min to form a solution with a solid content of 50%, which is then filtered and dried to form a composite carbon source G.

[0052] The composite carbon source G and the long-cycle silicon-carbon material precursor F are placed in a granulation kettle at a mass ratio of 5:95, stirred and heated to 350°C at 350r / min and kept warm for 1h to complete granulation, and then calcined at 650°C for 2h under an inert atmosphere to obtain a finished long-cycle silicon-carbon material I with a particle size D50 of 6μm, wherein the passivation layer accounts for 3% of the mass ratio of the single-particle long-cycle silicon-carbon negative electrode material, and the highly conductive outer carbon layer accounts for 2% of the mass ratio of the single-particle long-cycle silicon-carbon negative electrode material.

[0053] The obtained long-cycle silicon-carbon negative electrode material and metal lithium were used to form a half-cell for electrochemical performance testing, with a test rate of 0.1C (first time) + 0.5C (cycle) and a charge and discharge voltage of 0.005-0.8V. The results showed that the discharge capacity of the negative electrode sheet can reach 1650mAh / g, with an initial efficiency of 82.6%. After 50 cycles, it can still maintain 82.1% of the capacity.

[0054] The obtained long-cycle silicon-carbon negative electrode material was evenly mixed with graphite in a mass ratio of 5:95 as a composite negative electrode material. NCM622 was used as the positive electrode, and the processes of slurry mixing, coating, rolling, slitting, die-cutting, lamination, welding of pole ears, top and side sealing, baking, and liquid injection were carried out to assemble 7Ah soft-pack batteries. After fractionation, a room temperature cycle test was carried out at a current density of 1C / 1C. The initial efficiency of the battery cell was 88%. After 450 cycles of the full battery, the capacity retention rate was 94.8%.

[0055] Example 2

[0056] This embodiment provides a method for preparing a long-cycle silicon-carbon negative electrode material, which is as follows:

[0057] n-Hexane and ethanol are mutually soluble in a mass ratio of 1:1, medium-temperature coal tar with a softening point of 280°C is added in a mass ratio of 1:1.5, placed in a reactor and heated to 100°C, stirred at 90r / min for 2h, and then filtered. The obtained insoluble matter and dimethyl silicone oil are placed in a reactor in a mass ratio of 1:2.5, heated to 300°C, kept warm for 3h, stirred at 100r / min to obtain a spherical carbon precursor, the particle size D50 of the spherical carbon precursor is 3μm, the spherical carbon precursor is placed in a mixed solution of n-hexane and ethanol in a mass ratio of 1:1, placed in a reactor and heated to 100°C, stirred at 90r / min for 2h, then filtered, washed with ethanol, and dried at 65°C to obtain a spherical carbon matrix, the spherical carbon matrix and KOH are mixed in a mass ratio of 1:1, 600 The product was calcined at 400 °C for 1 h in an inert atmosphere, then washed with 0.5 M hydrochloric acid and then with deionized water, and dried at 70 °C to obtain a spherical porous carbon matrix with a particle size D50 of 2 μm and uniform pore distribution. The matrix was placed in a fluidized bed, and a mixture of silane and hydrogen was introduced at a gas flow ratio of 9:1. The matrix was heated to 450 °C and kept warm for 3 h. A mixture of acetylene and argon was introduced at a gas flow ratio of 1:1, and the matrix was kept warm at 680 °C for 1.5 h to obtain product E. The matrix was placed in a CVD, and a mixture of acetylene and inert atmosphere was introduced at a gas flow ratio of 1.5:1, and the matrix was kept warm at 680 °C for 1.5 h to obtain a long-cycle silicon-carbon material precursor. The medium-temperature coal tar was added to a 0.1 M silver nitrate solution and stirred for 2 h at a stirring speed of 1000 r / min to form a solution with a solid content of 40%, which was then filtered and dried to form a composite carbon source. The composite carbon source and the long cycle silicon-carbon material precursor are placed in a granulation kettle at a mass ratio of 6:90, stirred and heated to 380°C at 380r / min and kept warm for 1.5h to complete granulation, and then calcined at 680°C for 2.5h under an inert atmosphere to obtain a finished long cycle silicon-carbon negative electrode material with a particle size D50 of 7μm, wherein the passivation layer accounts for 4% of the mass ratio of the single-particle long cycle silicon-carbon negative electrode material, and the highly conductive outer carbon layer accounts for 3% of the mass ratio of the single-particle long cycle silicon-carbon negative electrode material.

[0058] The obtained long-cycle silicon-carbon negative electrode material and metal lithium were used to form a half-cell for electrochemical performance testing, with a test rate of 0.1C (first time) + 0.5C (cycle) and a charge and discharge voltage of 0.005-0.8V. The results showed that the discharge capacity of the negative electrode sheet can reach 1680mAh / g, with an initial efficiency of 82.9%, and after 50 cycles, it can still maintain 84.1% of the capacity.

[0059] The obtained long-cycle silicon-carbon negative electrode material was evenly mixed with graphite in a mass ratio of 5:95 as a composite negative electrode material. NCM622 was used as the positive electrode, and the processes of slurry mixing, coating, rolling, slitting, die-cutting, lamination, electrode ear welding, top and side sealing, baking, and liquid injection were carried out to assemble a 7Ah soft-pack battery. After the battery was divided into capacities, a room temperature cycle test was carried out at a current density of 1C / 1C. The initial efficiency of the battery cell was 88%. After 450 cycles of the full battery, the capacity retention rate was 95.2%.

[0060] Example 3

[0061] This embodiment provides a method for preparing a long-cycle silicon-carbon negative electrode material, which is as follows:

[0062] n-Hexane and ethanol are mutually soluble in a mass ratio of 1:5, medium-temperature coal tar with a softening point of 280°C is added in a mass ratio of 1:3, placed in a reactor and heated to 150°C, stirred at 120r / min for 4h, and then filtered. The obtained insoluble matter and dimethyl silicone oil are placed in a reactor in a mass ratio of 1:2.5, heated to 380°C, kept warm for 4h, stirred at 150r / min to obtain a spherical carbon precursor, and the spherical carbon precursor is placed in a mixed solution of n-hexane and ethanol in a mass ratio of 1:2, placed in a reactor, heated to 130°C, stirred at 100r / min for 3h, then filtered, washed with ethanol, and dried at 70°C to obtain a spherical carbon matrix. The spherical carbon matrix is ​​mixed with KOH in a mass ratio of 1:2 and heated at 800°C under an inert atmosphere. The product was calcined for 3 hours, then washed with 0.9M hydrochloric acid and then with deionized water, and dried at 70°C to obtain a spherical porous carbon matrix with a particle size D50 of 3 μm and uniform pore distribution. The matrix was placed in a fluidized bed, and a mixture of silane and hydrogen was introduced at a gas flow ratio of 8:1. The matrix was heated to 500°C and kept warm for 4 hours. A mixture of acetylene and argon was introduced at a gas flow ratio of 1:1.5, and the matrix was kept warm at 700°C for 2 hours. The product was placed in a CVD, and a mixture of acetylene and inert atmosphere was introduced at a gas flow ratio of 1:1. The matrix was kept warm at 700°C for 2 hours to obtain a long-cycle silicon-carbon material precursor. The medium-temperature coal tar was added to a 0.1M silver nitrate solution and stirred for 2 hours at a stirring speed of 1000 r / min to form a solution with a solid content of 50%, which was then filtered and dried to form a composite carbon source. The composite carbon source and the long-cycle silicon-carbon material precursor are placed in a granulation kettle at a mass ratio of 7:90, stirred and heated to 400°C at 400r / min for 2h to complete granulation, and then calcined at 700°C for 3h under an inert atmosphere to obtain a finished long-cycle silicon-carbon negative electrode material with a particle size D50 of 8μm, in which the passivation layer accounts for 4.5% of the mass ratio of the single-particle long-cycle silicon-carbon negative electrode material, and the high-conductivity outer carbon layer accounts for 4% of the mass ratio of the single-particle long-cycle silicon-carbon negative electrode material. Figure 1 As shown, the XRD spectrum of the material has no obvious silicon characteristic peak, indicating that the internal structure of the material is uniform and has good cycle performance.

[0063] The obtained long-cycle silicon-carbon negative electrode material and metal lithium were used to form a half-cell for electrochemical performance testing, with a test rate of 0.1C (first time) + 0.5C (cycle) and a charge and discharge voltage of 0.005-0.8V. The results showed that the discharge capacity of the negative electrode sheet can reach 1648mAh / g, with an initial efficiency of 83.0%, and after 50 cycles, it can still maintain 85.2% of the capacity.

[0064] The obtained long-cycle silicon-carbon negative electrode material was evenly mixed with graphite in a mass ratio of 5:95 as a composite negative electrode material. NCM622 was used as the positive electrode, and the processes of slurry mixing, coating, rolling, slitting, die-cutting, lamination, welding of pole ears, top and side sealing, baking, and liquid injection were carried out to assemble 7Ah soft-pack batteries. After the batteries were divided into capacities, they were subjected to room temperature cycle tests at a current density of 1C / 1C. The first efficiency of the battery cell was 88% (depending on the first efficiency of the positive electrode). After 895 cycles of the full battery, the capacity retention rate was 93.7%.

[0065] Example 4

[0066] This embodiment provides a method for preparing a long-cycle silicon-carbon negative electrode material, which is as follows:

[0067] n-Hexane and ethanol are mutually soluble in a mass ratio of 1:3, medium-temperature coal tar with a softening point of 280°C is added in a mass ratio of 1:3, placed in a reactor and heated to 140°C, stirred at 100r / min for 3h, and then filtered, the obtained insoluble matter and dimethyl silicone oil are placed in a reactor in a mass ratio of 1:4, heated to 390°C, kept warm for 5h, stirred at 200r / min to obtain a spherical carbon precursor, the spherical carbon precursor is placed in a mixed solution of n-hexane and ethanol in a mass ratio of 1:2.5, placed in a reactor, heated to 140°C, stirred at 100r / min for 3.5h, then filtered, washed with ethanol, and dried at 75°C to obtain a spherical carbon matrix, the spherical carbon matrix is ​​mixed with KOH in a mass ratio of 1:2, and calcined at 850°C under an inert atmosphere The product was calcined for 3.5 hours, then washed with 0.9M hydrochloric acid and then with deionized water, and dried at 75°C to obtain a spherical porous carbon matrix with a particle size D50 of 3.5 μm and uniform pore distribution. The matrix was placed in a fluidized bed, and a mixture of silane and hydrogen was introduced at a gas flow ratio of 5:1. The matrix was heated to 600°C and kept warm for 5 hours. A mixture of acetylene and argon was introduced at a gas flow ratio of 1:2, and the matrix was kept warm at 700°C for 2 hours to obtain product E. The matrix was placed in a CVD, and a mixture of acetylene and inert atmosphere was introduced at a gas flow ratio of 1:1, and the matrix was kept warm at 730°C for 3 hours to obtain a long-cycle silicon-carbon material precursor. The medium-temperature coal tar was added to a 0.1M silver nitrate solution and stirred for 2 hours at a stirring speed of 1000r / min to form a solution with a solid content of 50%, which was then filtered and dried to form a composite carbon source. The composite carbon source and the long cycle silicon-carbon material precursor are placed in a granulation kettle at a mass ratio of 8:90, stirred and heated to 450°C at 450r / min and kept warm for 2.5h to complete granulation, and then calcined at 800°C for 3.5h in an inert atmosphere to obtain a finished long cycle silicon-carbon negative electrode material with a particle size D50 of 9μm, wherein the passivation layer accounts for 5% of the mass ratio of the single-particle long cycle silicon-carbon negative electrode material, and the highly conductive outer carbon layer accounts for 4.5% of the mass ratio of the single-particle long cycle silicon-carbon negative electrode material.

[0068] The obtained long-cycle silicon-carbon negative electrode material and metal lithium were used to form a half-cell for electrochemical performance testing, with a test rate of 0.1C (first time) + 0.5C (cycle) and a charge and discharge voltage of 0.005-0.8V. The results showed that the discharge capacity of the negative electrode sheet can reach 1600mAh / g, with an initial efficiency of 82.8%, and after 50 cycles, it can still maintain 84.9% of the capacity.

[0069] The obtained long-cycle silicon-carbon negative electrode material was evenly mixed with graphite in a mass ratio of 5:95 as a composite negative electrode material. NCM622 was used as the positive electrode, and the processes of slurry mixing, coating, rolling, slitting, die-cutting, lamination, welding of pole ears, top and side sealing, baking, and liquid injection were carried out to assemble 7Ah soft-pack batteries. After fractionation, a room temperature cycle test was carried out at a current density of 1C / 1C. The initial efficiency of the battery cell was 88%. After 450 cycles of the full battery, the capacity retention rate was 94.1%.

[0070] Example 5

[0071] This embodiment provides a method for preparing a long-cycle silicon-carbon negative electrode material, which is as follows:

[0072] n-Hexane and ethanol are mutually soluble in a mass ratio of 1:3, medium-temperature coal tar with a softening point of 280°C is added in a mass ratio of 1:3, placed in a reactor and heated to 150°C, stirred at 100r / min for 4h, and then filtered, the obtained insoluble matter and dimethyl silicone oil are placed in a reactor in a mass ratio of 1:5, heated to 400°C, kept warm for 6h, stirred at 300r / min to obtain a spherical carbon precursor, the spherical carbon precursor is placed in a mixed solution of n-hexane and ethanol in a mass ratio of 1:3, placed in a reactor and heated to 150°C, stirred at 100r / min for 4h, then filtered, washed with ethanol, and dried at 75°C to obtain a spherical carbon matrix, the spherical carbon matrix is ​​mixed with KOH in a mass ratio of 1:3, and dried at 900°C under an inert atmosphere Calcinate for 4 hours, then wash with 1M hydrochloric acid, then wash with deionized water, and dry at 80°C to obtain a spherical porous carbon matrix product with a particle size D50 of 4μm and uniform pore distribution. Put it into a fluidized bed, introduce a mixture of silane and hydrogen at a gas flow ratio of 2:1, heat to 700°C and keep it warm for 6 hours, then introduce a mixture of acetylene and argon at a gas flow ratio of 1:3, and keep it warm at 750°C for 3 hours. The product is placed in a CVD, and acetylene and an inert atmosphere mixture are introduced at a gas flow ratio of 1:2, and kept warm at 750°C for 4 hours to obtain a long-cycle silicon-carbon material precursor. Add medium-temperature coal tar to 0.1M silver nitrate solution and stir for 2 hours at a stirring speed of 1000r / min to form a solution with a solid content of 50%, which is then filtered and dried to form a composite carbon source. The composite carbon source and the long cycle silicon-carbon material precursor are placed in a granulation kettle at a mass ratio of 10:90, stirred and heated to 500°C at 500r / min and kept warm for 3 hours to complete granulation, and then calcined at 900°C for 4 hours under an inert atmosphere to obtain a finished long cycle silicon-carbon negative electrode material with a particle size D50 of 10μm, wherein the passivation layer accounts for 6% of the mass ratio of the single-particle long cycle silicon-carbon negative electrode material, and the highly conductive outer carbon layer accounts for 5% of the mass ratio of the single-particle long cycle silicon-carbon negative electrode material.

[0073] The obtained long-cycle silicon-carbon negative electrode material and metal lithium were used to form a half-cell for electrochemical performance testing, with a test rate of 0.1C (first time) + 0.5C (cycle) and a charge and discharge voltage of 0.005-0.8V. The results showed that the discharge capacity of the negative electrode sheet can reach 1580mAh / g, with an initial efficiency of 82.0%, and after 50 cycles, it can still maintain 83.1% of the capacity.

[0074] The obtained long-cycle silicon-carbon negative electrode material was evenly mixed with graphite in a mass ratio of 5:95 as a composite negative electrode material. NCM622 was used as the positive electrode, and 7Ah soft-pack batteries were assembled through processes such as slurry mixing, coating, rolling, slitting, die-cutting, lamination, welding of pole ears, top and side sealing, baking, and liquid injection. After fractionation, a room temperature cycle test was carried out at a current density of 1C / 1C. The initial efficiency of the battery cell was 88%. After 450 cycles of the full battery, the capacity retention rate was 92.5%.

[0075] Comparative Example 1

[0076] The porous carbon matrix with a D50 of 8 μm was placed in a fluidized bed, and a mixture of silane and hydrogen was introduced at a gas flow ratio of 2:1, heated to 700°C and kept warm for 6 hours, and then a mixture of acetylene and argon was introduced at a gas flow ratio of 1:3, and kept warm at 750°C for 3 hours to obtain a silicon-carbon negative electrode material. The obtained silicon-carbon negative electrode material and metal lithium were used to form a half-cell for electrochemical performance testing. The test rate was 0.1C (first time) + 0.5C (cycle), and the charge and discharge voltage was 0.005~0.8V. The results show that the discharge specific capacity of the negative electrode sheet can reach 1580mAh / g, the first efficiency is 82.0%, and after 50 cycles, the capacity can still be maintained at 51.1%.

[0077] It can be seen from the performance results of the embodiments that the long-cycle silicon-carbon negative electrode material of the present invention is a spherical new silicon-carbon (nanosilicon deposited in the pores of a porous carbon matrix) composite material with a small-sized core and uniform particle size, and then one or more cores are compounded by granulation to form a slightly larger finished product. The structural advantages include: due to the multi-porous structure of the carbon matrix of the new silicon-carbon material, ion transmission needs to bypass the pores, and the ion conductivity is poor. The use of a small-sized core can shorten the lithium ion transmission path and improve the lithium ion transmission rate. The use of medium-temperature asphalt granulation and carbonization to compound multiple cores can reduce the specific surface area of ​​the material (the particle size becomes larger), reduce the negative reaction with the electrolyte, and improve the first effect (SEI film reduction). The coating layer better wraps the core, further suppresses the volume change of the material during the charge and discharge process, and wraps the core in all directions, improving the situation in which the silicon-based material is exposed to the electrolyte due to its own volume change during the battery cycle, effectively reducing negative reactions and improving the material cycle performance. In addition, the interlayer spacing of the carbon layer after asphalt carbonization is larger, providing a fast channel for the transport of electrons and lithium ions. The nanosilver dispersed in it further enhances the conductivity of the material, improving the shortcomings of this type of material, such as high resistivity and poor rate performance.

[0078] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the presence of other identical elements in the process, method, article or device including the elements.

[0079] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit them; although the present invention is described in detail with reference to the above embodiments, it should be understood by those skilled in the art that the technical solutions described in the above embodiments can still be modified, or some of the technical features can be replaced by equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the spirit and scope of the technical solutions of the embodiments of the present invention. Anything not described in detail in the present invention is a well-known technology to those skilled in the art.

Claims

1. A silicon-carbon negative electrode material, characterized in that: The silicon-carbon negative electrode material comprises: A core, which comprises one or more spherical porous carbon matrices with surface pores, wherein nano-silicon is distributed in the surface pores of the spherical porous carbon matrix, and, The coating layer covers the inner core, and the coating layer comprises a passivated carbon layer and a highly conductive outer carbon layer. The passivated carbon layer covers the inner core, and the highly conductive layer covers the passivated carbon layer. Nanosilver is dispersed in the highly conductive outer carbon layer.

2. The silicon-carbon negative electrode material according to claim 1, characterized in that: The silicon-carbon negative electrode material is granular, with a particle size D50 of 6 to 10 μm, the passivated carbon layer accounts for 3% to 6% of the mass ratio of the single-particle silicon-carbon negative electrode material, and the highly conductive outer carbon layer accounts for 2% to 5% of the mass ratio of the single-particle silicon-carbon negative electrode material.

3. A method for preparing the silicon-carbon negative electrode material according to any one of claims 1 and 2, characterized in that: The steps include: 1) dissolving n-hexane and ethanol in a mass ratio of 1:1 to 5 to obtain a mixed solution A; 2) adding the medium-temperature coal tar pitch into the mixed solution A, mixing and heating to 100-150° C. at a stirring speed of 90-120 r / min, keeping the temperature for 2-4 hours, and then filtering to obtain the insoluble substance B; 3) Mixing dimethyl silicone oil with the insoluble substance B, heating the mixture to 300-400° C. under stirring at 100-300 r / min, and keeping the mixture warm for 3-6 hours to obtain a spherical carbon precursor C, wherein the particle size D50 of the spherical carbon precursor is 1-4 μm; 4) mixing the spherical carbon precursor C with a mixed solution of n-hexane and ethanol, heating to 100-150° C. at a stirring speed of 90-120 r / min, keeping warm for 2-4 hours, filtering, washing with ethanol, and drying to obtain a spherical carbon matrix, the spherical carbon matrix and KOH are mixed in a mass ratio of 1:1-1:3, calcined at 600-900° C. in an inert atmosphere for 1-4 hours, then washed with 0.5M-1M hydrochloric acid, then washed with deionized water, and dried to prepare a spherical porous carbon matrix D with uniform pore distribution; 5) introducing a first mixed gas into the spherical porous carbon matrix D, heating to 400-700° C. and keeping the temperature for 2-6 hours, then replacing the mixture with a second mixed gas, keeping the temperature at 650-750° C. for 1-3 hours, and obtaining product E; 6) introducing a third mixed gas into the product E at a gas flow ratio of 2:1 to 1:2, heating to 650 to 750° C. and keeping the temperature for 1 to 4 hours to obtain a silicon-carbon material precursor F; 7) adding the medium temperature coal tar pitch to a 0.1M silver nitrate solution, stirring for 1 to 3 hours at a stirring speed of 900 to 1200 r / min to form a solution with a solid content of 40 to 60%, and then filtering and drying the solution to form a composite carbon source G; 8) The composite carbon source G and the silicon-carbon material precursor F are stirred and mixed at a mass ratio of 5:95 to 10:90 and a stirring speed of 300 to 500 r / min, and heated to 350°C to 500°C, and kept warm for 1 to 3 hours to complete granulation, and then calcined at 650°C to 900°C for 2 to 4 hours in an inert atmosphere to obtain a silicon-carbon negative electrode material.

4. The preparation method according to claim 3, characterized in that: In the step 2), the softening point of the medium-temperature coal tar pitch is 280° C., and the mass ratio of the medium-temperature tar pitch to the solution A is 1:1 to 1:

3.

5. The preparation method according to claim 3, characterized in that: In the step 3), the mass ratio of dimethyl silicone oil to insoluble substance B is 1:2 to 1:

5.

6. The preparation method according to claim 3, characterized in that: In the step 4), the mass ratio of the spherical carbon precursor C to the solution A is 1:1 to 1:3, the drying temperature is 60° C. to 80° C., and the particle size D50 of the spherical porous carbon matrix D is 1 to 4 μm.

7. The preparation method according to claim 3, characterized in that: In the step 5), the first mixed gas includes silane and hydrogen, and the volume ratio of silane to hydrogen is 10:1 to 2:

1.

8. The preparation method according to claim 3, characterized in that: In the step 5), the second mixed gas includes acetylene and argon, and the volume ratio of acetylene to argon is 2:1 to 1:

3.

9. The preparation method according to claim 3, characterized in that: In the step 6), the third mixed gas includes acetylene and an inert atmosphere.

Citation Information

Patent Citations

  • Multi-core core-shell-structure silicon carbon composite negative pole material and preparation method thereof

    CN103094533A

  • Preparation method of silver doped carbon-silicon composite negative electrode material

    CN103151504A

  • Silver-particle-doped silicon carbon negative electrode material preparation method

    CN108336311A

  • Method for preparing pitch-based spherical activated carbon

    CN109399632A

  • Carbon-silicon negative electrode material and preparation method thereof

    CN112054171A

Cited By

  • Silicon-carbon material with multi-layer coating structure and preparation method and application of silicon-carbon material

    CN119627090A

  • Silicon-carbon composite negative electrode material and preparation method and application thereof

    CN120933326A