Positive electrode material, preparation method thereof and electrochemical device

By forming the first cladding layer of cobalt element and solid electrolyte and the second cladding layer of boron element on the surface of the high nickel positive electrode material, the internal resistance and residual alkali problems of the high nickel positive electrode material are solved, and the specific capacity and high temperature performance are improved , suitable for large-scale production.

CN118919695APending Publication Date: 2024-11-08NANTONG RESHINE NEW MATERIAL CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411179635.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The high-nickel positive electrode material has problems such as high residual alkali content on the surface, large internal resistance, poor rate performance, low capacity, poor circulation performance and poor thermal stability. The existing modification methods are complex and difficult to produce on a large scale, and their performance is The improvement is not ideal.

Method used

Using a nickel-cobalt-manganese ternary positive electrode material, the first cladding layer and the second cladding layer are formed on the surface of the substrate. The first cladding layer contains solid electrolyte and cobalt elements, and the second cladding layer contains boron elements, which are passed through cobalt elements. Chemical reaction with the residual lithium on the substrate surface reduces internal resistance, solid electrolytes improve ion conductivity, and boron elements reduce the loss of active substances.

Benefits of technology

It effectively reduces the internal resistance and residual alkali of the cathode material, improves specific capacity and high temperature performance, improves rate performance and interface stability, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919695A_ABST
    Figure CN118919695A_ABST
Patent Text Reader

Abstract

The positive electrode material, the preparation method thereof and the electrochemical device are characterized in that the positive electrode material comprises a substrate, a first coating layer and a second coating layer, the surface of the substrate is sequentially coated with the first coating layer and the second coating layer, the substrate is a nickel-cobalt-manganese ternary positive electrode material, the molar content of a nickel element is larger than or equal to 0.6, the first coating layer contains a solid electrolyte and a cobalt element, and the second coating layer contains a boron element. The positive electrode material has double coating layers, so that the internal resistance and residual alkali of the positive electrode material are effectively reduced, the specific capacity of the positive electrode material is improved, and the high-temperature performance of the positive electrode material is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of new energy materials, and in particular to a positive electrode material and a preparation method thereof, and an electrochemical device. Background Art

[0002] In recent years, the continuous technological innovation of new energy vehicles has put forward higher requirements for battery safety and long-term performance. The energy of the battery structure is mainly provided by the positive electrode material. Compared with other low-nickel and medium-nickel ternary materials, high-nickel positive electrode materials (nickel content exceeds 60%) have the advantages of high energy density and low price, and are one of the most promising battery positive electrode materials.

[0003] However, high-nickel cathode materials still have problems such as high surface residual alkali content, large internal resistance, poor rate performance, low capacity, poor cycle performance and poor thermal stability. In view of the above problems, high-nickel cathode materials need to be modified to improve their comprehensive performance. However, the current modification methods are complex and use a large amount of organic solvents. The solvent residues in the product are difficult to remove, which is not conducive to large-scale production. In addition, the existing modification methods are still not ideal in terms of performance improvement. Summary of the invention

[0004] In view of this, in order to solve at least one of the above technical problems, an embodiment of the present application provides a positive electrode material.

[0005] In addition, the embodiments of the present application also provide a method for preparing the aforementioned positive electrode material, and an electrochemical device using the positive electrode material.

[0006] An embodiment of the present application provides a positive electrode material, which includes a substrate and a first coating layer and a second coating layer sequentially coated on the surface of the substrate, wherein the substrate is a nickel-cobalt-manganese ternary positive electrode material, the molar content of the nickel element is ≥0.6, the first coating layer contains a solid electrolyte and a cobalt element, and the second coating layer contains a boron element.

[0007] In some possible embodiments, at least a portion of the cobalt element is doped into the matrix; and at least a portion of the solid electrolyte is embedded in the matrix.

[0008] In some possible embodiments, the mass ratio of the matrix to the cobalt element is 1:(0.001-0.04);

[0009] The mass ratio of the matrix to the solid electrolyte is 1:(0.001-0.04).

[0010] In some possible embodiments, the solid electrolyte has at least one of the following characteristics:

[0011] (1) The solid electrolyte includes at least one of an oxide electrolyte, a sulfide electrolyte, a fluoride electrolyte, a phosphate electrolyte and a polymer electrolyte;

[0012] (2) The oxide electrolyte comprises lithium lanthanum zirconium oxide;

[0013] (3) The solid electrolyte includes lithium lanthanum zirconium oxide doped with a metal element M, and the metal element M includes at least one of Al, Ta, Nb, Sr, Mn, Ni, Ca, Ba, Mg, Ga, Se, Mo, Sn, Ge, V, Ta and Cu.

[0014] The present application also provides a method for preparing a positive electrode material, comprising:

[0015] The matrix of the nickel-cobalt-manganese ternary positive electrode material, the solid electrolyte and the cobalt source are mixed once to obtain a first mixed material;

[0016] sintering the first mixed material once to obtain a sintered material;

[0017] Mixing the sintered material and the boron source for a second time to obtain a second mixed material; and

[0018] The second mixed material is subjected to secondary sintering to obtain the positive electrode material.

[0019] In some possible embodiments, the mass ratio of the matrix, the solid electrolyte and the cobalt in the cobalt source is 1:(0.001-0.04):(0.001-0.04); and / or

[0020] The mass percentage of boron in the boron source to the second mixed material is 0.05% to 0.5%.

[0021] In some possible embodiments, the primary sintering temperature is 400° C. to 800° C., and the primary sintering time is 5 h to 15 h;

[0022] The secondary sintering temperature is 200°C to 400°C, and the secondary sintering time is 5h to 15h;

[0023] The solid electrolyte, cobalt source and boron source are all nano-scale particles.

[0024] In some possible embodiments, the solid electrolyte has at least one of the following characteristics:

[0025] (1) The solid electrolyte includes at least one of an oxide electrolyte, a sulfide electrolyte, a fluoride electrolyte, a phosphate electrolyte and a polymer electrolyte;

[0026] (2) The oxide electrolyte comprises lithium lanthanum zirconium oxide;

[0027] (3) The solid electrolyte includes lithium lanthanum zirconium oxide doped with a metal element M, and the metal element M includes at least one of Al, Ta, Nb, Sr, Mn, Ni, Ca, Ba, Mg, Ga, Se, Mo, Sn, Ge, V, Ta and Cu.

[0028] In addition, an embodiment of the present application further provides an electrochemical device, which includes a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the positive electrode sheet includes a positive electrode material, and the positive electrode material is the aforementioned positive electrode material.

[0029] Compared with the prior art, the high-nickel ternary positive electrode material provided in the embodiment of the present application forms a first coating layer and a second coating layer on the surface of the substrate of the positive electrode material. The double coating layer effectively reduces the internal resistance and residual alkali of the positive electrode material on the one hand, improves the specific capacity of the positive electrode material, and improves the high temperature performance of the positive electrode material on the other hand. Among them, the cobalt element in the first coating layer can react chemically with the lithium remaining on the surface of the substrate to form lithium cobalt oxide, which effectively reduces the internal resistance and residual alkali of the positive electrode material; the solid electrolyte in the first coating layer has good ionic conductivity, increases the lithium ion deintercalation rate in the positive electrode material, reduces the electrochemical impedance of the positive electrode material, further improves the specific capacity of the positive electrode material at high rate, and improves the interface stability of the positive electrode material. The second coating layer is a uniform and dense boron coating layer, which effectively reduces the contact between the substrate and the electrolyte, avoids the loss of positive electrode active materials in the substrate, and further improves the specific capacity and stability of the positive electrode material. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 A process flow chart of the method for preparing the positive electrode material provided in an embodiment of the present application.

[0031] Figure 2 This is a schematic diagram of the structure of the electrochemical device provided in an embodiment of the present application.

[0032] Figure 3A This is a scanning electron microscope image of the positive electrode material of Example 2 of the present application.

[0033] Figure 3B This is a scanning electron microscope image of the positive electrode material of comparative example 3 of the present application.

[0034] Figure 4 This is a comparison chart of the room temperature DCIR of batteries prepared with the positive electrode materials in Examples 1-2 and Comparative Examples 1-3 of the present application.

[0035] Figure 5 This is a comparison chart of the 1C / 1C cycle capacity retention rate at 45°C of batteries prepared with the positive electrode materials in Example 2 and Comparative Example 3 of the present application. DETAILED DESCRIPTION

[0036] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments of the present application, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present application.

[0037] An embodiment of the present application provides a positive electrode material, which includes a substrate and a first coating layer and a second coating layer sequentially coated on the surface of the substrate, wherein the substrate is a nickel-cobalt-manganese ternary positive electrode material, the molar content of the nickel element is ≥0.6, the first coating layer contains a solid electrolyte and a cobalt element, and the second coating layer contains a boron element.

[0038] Specifically, the chemical formula of the matrix of the positive electrode material is LiNi α Co β Mn γ O2, wherein 1>α≥0.6, 0.4≥β>0, 0.4≥γ>0, and β+γ≤0.4, illustratively, it may be NCM613, NCM622, NCM712 or NCM811, etc. High nickel ternary cathode materials with a nickel content of more than 60% have the advantages of high energy density and low price.

[0039] The first coating layer in the positive electrode material is an inner coating layer, in which the solid electrolyte has good ionic conductivity, increases the lithium ion deintercalation rate, reduces the electrochemical impedance of the positive electrode material, and improves the specific capacity at high rates and the interface stability of the positive electrode material. However, a single solid electrolyte coating can cause problems such as a decrease in the specific surface area of ​​the positive electrode material, a decrease in the powder resistivity, or a decrease in the cycle performance. The cobalt element in the first coating layer can promote the embedding of the solid electrolyte into the matrix by optimizing the interface contact between the matrix and the solid electrolyte, improve the interface compatibility, and improve the structure and morphology of the surface of the positive electrode material, effectively solve the above problems, eliminate the negative effects of the solid electrolyte, and react chemically with the lithium remaining on the surface of the matrix (i.e., the high-nickel ternary positive electrode material) to generate lithium cobalt oxide, further reducing the internal resistance and residual alkali amount of the positive electrode material, and improving the conductivity of the positive electrode material. The cobalt element and the solid electrolyte in the first coating layer work together to synergistically improve the electrochemical performance of the positive electrode material.

[0040] The uniform and dense second coating layer containing boron as an outer coating layer can physically isolate the substrate from the electrolyte, reduce the reaction between the positive electrode active material and the electrolyte in the substrate, avoid the loss of the positive electrode active material, and thus improve the specific capacity of the positive electrode material. At the same time, the second coating layer can also isolate the reaction between the electrolyte and the first coating layer, reduce the dissolution of cobalt elements in the first coating layer, and at the same time, boron and solid electrolyte jointly build an effective lithium ion channel to improve the specific capacity of the positive electrode material. The first coating layer and the second coating layer also have a synergistic effect, which effectively improves the specific capacity and stability of the positive electrode material.

[0041] In some embodiments, at least part of the cobalt element can be doped into the matrix to react with lithium, thereby reducing the lithium-nickel mixing of the high-nickel ternary positive electrode material, stabilizing the layered oxide structure of the high-nickel ternary positive electrode material, and reducing the generation of rock salt phase. The lithium cobalt oxide formed during the doping process can also improve the electronic conductivity of the positive electrode material, thereby improving the high-temperature cycle performance and stability of the positive electrode material.

[0042] In some embodiments, at least part of the solid electrolyte can also be embedded in the matrix, which increases the interface contact between the solid electrolyte and the matrix, shortens the lithium ion transmission path, further increases the lithium ion deintercalation rate, and reduces the electrochemical impedance of the positive electrode material.

[0043] It is understandable that part of the cobalt element is doped into the matrix and part of the solid electrolyte is embedded in the matrix at the same time, which can also make the first coating layer more closely combined with the matrix, thereby enhancing the stability of the positive electrode material.

[0044] In some embodiments, the mass ratio of the substrate to the cobalt element can be 1:(0.001-0.04). Within the above range, cobalt can form a moderate coating on the substrate, which can not only improve the specific capacity and cycle stability of the positive electrode material, but also help improve the structural stability of the positive electrode material. The mass ratio of the substrate to the cobalt element can further be 1:(0.005-0.02), and can be exemplarily 1:0.001, 1:0.002, 1:0.005, 1:0.008, 1:0.01, 1:0.015, 1:0.02, 1:0.025, 1:0.03, 1:0.035 or 1:0.04, etc.

[0045] In some embodiments, the mass ratio of the substrate to the solid electrolyte may be 1:(0.001-0.04), and the mass ratio within the above range may balance the conductivity, structural stability and cost of the positive electrode material. The mass ratio of the substrate to the solid electrolyte may further be 1:(0.002-0.02), and may be 1:0.001, 1:0.002, 1:0.005, 1:0.008, 1:0.01, 1:0.015, 1:0.02, 1:0.025, 1:0.03, 1:0.035 or 1:0.04, etc.

[0046] In some embodiments, the solid electrolyte may include at least one of an oxide electrolyte, a sulfide electrolyte, a fluoride electrolyte, a phosphate electrolyte, and a polymer electrolyte, etc. Coating the positive electrode material with the above solid electrolyte is beneficial to improving the thermal stability and conductivity of the positive electrode material.

[0047] In some embodiments, the oxide electrolyte may be lithium lanthanum zirconium oxide (LLZO), which is a garnet-type solid electrolyte (cubic phase, c-LLZO, Li7La3Zr2O 12 Since LLZO has high ionic conductivity, high electrochemical stability, and good chemical stability to the positive electrode material and the lithium metal negative electrode, the first coating layer can effectively improve the conductivity and interface stability of the positive electrode material.

[0048] LLZO may also be doped with a metal element M, which may include at least one of Al, Ta, Nb, Sr, Mn, Ni, Ca, Ba, Mg, Ga, Se, Mo, Sn, Ge, V, Ta, and Cu, and may further include at least one of Al, Nb, and Ta. The metal element M may adjust the conductivity, chemical stability, structural characteristics, and interface stability of LLZO by replacing lithium, zirconium, or lanthanum, thereby significantly improving the performance of the solid electrolyte LLZO in cathode material applications.

[0049] Compared with the prior art, the positive electrode material provided in the embodiment of the present application has the following beneficial effects:

[0050] 1. The high-nickel ternary positive electrode material provided in the embodiment of the present application forms a first coating layer and a second coating layer on the surface of the substrate of the positive electrode material. The second coating layer not only effectively reduces the loss of positive electrode active material in the core, but also reduces the dissolution of cobalt in the first coating layer. At the same time, the boron in the second coating layer and the solid electrolyte in the first coating layer jointly build an effective lithium ion channel to improve the specific capacity of the positive electrode material. The synergistic effect of the double coating layer effectively reduces the internal resistance and residual alkali of the positive electrode material, improves the specific capacity of the positive electrode material, and improves the high temperature performance of the positive electrode material on the other hand.

[0051] 2. The first coating layer contains cobalt and solid electrolyte, wherein the solid electrolyte provides a fast ion channel for the substrate surface, reduces the internal resistance of the positive electrode material, improves the rate performance and interface stability of the positive electrode material, and the solid electrolyte can also be semi-embedded in the substrate to further improve the ionic conductivity and interface stability of the positive electrode material. At the same time, the cobalt element and the residual lithium on the substrate surface generate lithium cobalt oxide, which effectively reduces the internal resistance and residual alkali content of the positive electrode material. The cobalt element can also be doped into the substrate, reducing the lithium-nickel mixing, stabilizing the layered oxide structure, and reducing the generation of rock salt phase. The cobalt coating can also improve the problems of reduced specific surface area, reduced powder resistivity, and poor cycle performance introduced by the solid electrolyte coating. The two work together to improve the high-temperature cycle performance and stability of the positive electrode material.

[0052] 3. The second coating layer contains boron element, and the second coating layer is evenly and densely wrapped on the surface of the first coating layer, providing effective protection for the positive electrode material, reducing the reaction between the positive electrode active material and the electrolyte in the matrix, and improving the specific capacity of the positive electrode material.

[0053] See also Figure 1 As shown, the method for preparing the positive electrode material provided in the embodiment of the present application specifically comprises the following steps:

[0054] Step S1, mixing a matrix, a solid electrolyte and a cobalt source of a nickel-cobalt-manganese ternary positive electrode material to obtain a first mixed material.

[0055] Specifically, the chemical formula of the matrix of the nickel-cobalt-manganese ternary positive electrode material is LiNi α Co β Mn γ O2, wherein 1>α≥0.6, 0.4≥β>0, 0.4≥γ>0, and β+γ≤0.4, exemplarily, it can be NCM613, NCM622, NCM712 or NCM811, etc.

[0056] In some embodiments, the solid electrolyte may include at least one of an oxide electrolyte, a sulfide electrolyte, a fluoride electrolyte, a phosphate electrolyte, and a polymer electrolyte. Among them, the oxide electrolyte may be lithium lanthanum zirconium oxide. Lithium lanthanum zirconium oxide has high lithium ion conductivity, excellent chemical stability, low resistance, and good mechanical stability, which is beneficial to improving the electrochemical performance and stability of the positive electrode material.

[0057] In some embodiments, the preparation method of lithium lanthanum zirconium oxide may include: mixing lithium-containing oxide, lanthanum-containing oxide and zirconium-containing oxide uniformly by ball milling, sand milling, grinding, soy milk machine, etc. and calcining at 800°C to 1300°C for 5 to 20 hours, and then dispersing and refining the particles by ball milling, sand milling, grinding, soy milk machine, etc. to obtain lithium lanthanum zirconium oxide that meets the coating requirements, and the particle size of lithium lanthanum zirconium oxide is preferably D50 = 0.05 to 1.0 μm. It is understood that the mixing method and the dispersion method include but are not limited to the above methods, and any method that can meet the requirements of sufficient mixing or sufficient dispersion is acceptable.

[0058] Among them, the lithium-containing oxide may include at least one of lithium carbonate and lithium hydroxide; the lanthanum-containing oxide may include at least one of lanthanum oxide, lanthanum carbonate, lanthanum oxycarbonate and lanthanum hydroxide; the zirconium-containing oxide may include zirconium dioxide.

[0059] In some embodiments, lithium lanthanum zirconium oxide may also be doped with a metal element M, which may be mixed with a lithium oxide, a lanthanum oxide and a zirconium oxide in the form of a metal oxide and sintered to obtain lithium lanthanum zirconium oxide doped with the metal element M; wherein the metal element M may include at least one of Al, Ta, Nb, Sr, Mn, Ni, Ca, Ba, Mg, Ga, Se, Mo, Sn, Ge, V, Ta and Cu. The metal element M may adjust the conductivity, chemical stability, structural characteristics and interface stability of LLZO by replacing the lithium position, the zirconium position or the lanthanum position, thereby significantly improving the performance of the solid electrolyte LLZO in the application of positive electrode materials.

[0060] In some embodiments, the cobalt source may include at least one of cobalt hydroxide, cobalt oxide, cobalt trioxide, cobalt sulfate, cobalt nitrate, cobalt chloride, cobalt carbonate, and cobalt oxalate, etc., to provide cobalt elements for the positive electrode material.

[0061] In some embodiments, the solid electrolyte and the cobalt source can be nano-sized particles, which generally have a higher specific surface area and a shorter ion transport path, and can make the solid electrolyte and the cobalt source particles more evenly distributed in the coating layer, which can bring higher ion conductivity, better interface bonding effect, stronger mechanical stability and chemical stability to the coating layer. These advantages help to further improve the overall performance of the positive electrode material battery, including charge and discharge efficiency, energy density and life.

[0062] In some embodiments, the preparation method of the matrix may include: mixing the lithium source and the positive electrode material precursor according to Li (molar amount of lithium in the lithium source): Me (molar amount of metal in the positive electrode material precursor) = 1.04, mixing evenly, pre-sintering at 400℃~750℃ for 10h~15h, dispersing evenly again, calcining at a high temperature of 800℃~1000℃ for 15h~20h, then crushing and sieving on a roller to prepare the positive electrode material coated matrix material.

[0063] In some embodiments, the mass ratio of the matrix to the solid electrolyte can be 1:(0.001-0.04), and further can be 1:(0.005-0.02); the mass ratio of the matrix to the cobalt in the cobalt source can be 1:(0.001-0.04), and further can be 1:(0.002-0.02). The appropriate mixing ratio is conducive to controlling the content of cobalt element and solid electrolyte in the coating layer and optimizing the comprehensive performance of the positive electrode material.

[0064] Step S2, sintering the first mixed material once to obtain a sintered material.

[0065] In this step, after high-temperature sintering, the cobalt and solid electrolyte in the first mixed material form an inner coating layer on the surface of the substrate, that is, the first coating layer in the positive electrode material.

[0066] In some embodiments, the conditions for the primary sintering may be: sintering at a sintering temperature of 400°C to 800°C for 5h to 15h. The coating temperature regions of cobalt and solid electrolyte overlap, and within the above temperature range, both cobalt and solid electrolyte can be effectively coated while saving production costs. In addition, a higher coating temperature is also beneficial for at least part of the cobalt in the coating layer to be doped into the matrix and at least part of the solid electrolyte to be embedded in the matrix, further improving the structural stability and conductivity of the positive electrode material. The temperature of the primary sintering may further be 600°C to 800°C, and may be 400°C, 450°C, 500°C, 550°C, 600°C, 650°C, 700°C, 750°C or 800°C, etc., for example.

[0067] Step S3, mixing the sintered material and the boron source for a second time to obtain a second mixed material.

[0068] In some embodiments, the boron source may include at least one of boric acid, boron oxide, boron carbonate, and boron oxalate, and the boron source may illustratively be boron oxide.

[0069] In some embodiments, the boron source may be nano-sized particles, which can improve the uniformity of boron element distribution, optimize the interface bonding with the coating layer formed in step S2, and also help enhance the thermal stability, chemical stability and mechanical strength of the positive electrode material.

[0070] In some embodiments, the boron in the boron source may account for 0.05% to 0.5% of the second mixed material by mass percentage, and may further account for 0.1% to 0.3%, and may be 0.05%, 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, 0.45% or 0.5%, etc. The appropriate amount of boron mixed is conducive to controlling the boron content in the final positive electrode material.

[0071] Step S4, performing secondary sintering on the second mixed material to obtain a positive electrode material.

[0072] In this step, after low-temperature sintering, the boron in the second mixed material forms a dense outer coating layer on the surface of the sintered material, that is, the second coating layer in the positive electrode material.

[0073] In some embodiments, the secondary sintering conditions may be: sintering at a sintering temperature of 200°C to 400°C for 5h to 15h. Since the boron source has a lower melting point and the nano-scale boron source can achieve better inter-particle bonding at a lower temperature, it is beneficial to form a stable surface boron coating within the above sintering temperature range. The secondary sintering temperature may further be 300°C to 400°C, and may be 200°C, 250°C, 300°C, 350°C or 400°C, etc., for example.

[0074] Compared with the prior art, the method for preparing the positive electrode material provided in the embodiment of the present application has the following beneficial effects:

[0075] 1. Cobalt and solid electrolyte are first coated on the substrate surface at high temperature, and then boron is coated at low temperature to form a double coating layer. First, the coating temperature regions of cobalt and solid electrolyte overlap, and high-temperature sintering together can save production costs and optimize the process. High-temperature sintering is also beneficial for cobalt and solid electrolyte to dope the substrate. Second, low-temperature coating of boron is conducive to achieving uniform and stable boron coating.

[0076] 2. By adopting the dry preparation method, the adverse effect of solvent residue on the purity of the positive electrode material is avoided, which is conducive to further improving the performance of the positive electrode material.

[0077] 3. This preparation method is simple, efficient, and low-cost, which is conducive to the large-scale production of positive electrode materials and has excellent commercial prospects.

[0078] See also Figure 2As shown, the embodiment of the present application also provides an electrochemical device (such as a battery), the electrochemical device 100 includes a positive electrode sheet 10, a negative electrode sheet 20, a separator 30 and an electrolyte 40, wherein the positive electrode sheet 10 includes a positive electrode material, and the positive electrode material is the positive electrode material as described above. The electrochemical device 100 prepared using the above-mentioned positive electrode material can give full play to the advantages of high energy density of high-nickel ternary positive electrode materials, and at the same time has good high-temperature cycle performance and high-rate performance, and can be applied to fast charging, high power and long cycle fields.

[0079] The above-mentioned positive electrode material and its preparation method and electrochemical device are further described below through specific examples.

[0080] Example 1

[0081] Step 1: Weigh 7.72g lithium carbonate (battery grade), 16.96g lanthanum carbonate (99% purity), 7.47g zirconium dioxide (98% purity) and a small amount of alumina as a solvent, mix them evenly with a ball mill, and use pure water as the liquid medium. The ball-to-liquid ratio is 6:1:2, the speed is 250r / min, and the time is 10h. After drying in a vacuum drying oven, transfer it to a crucible and place it in a muffle furnace to calcine at 950℃ for 10h to obtain a sintered product of lithium lanthanum zirconium oxide. Disperse and refine the particles through alcohol ball milling, the speed is 250r / min, the time is 5h, and after drying, the D50 of lithium lanthanum zirconium oxide is 0.75, which meets the coating requirements.

[0082] Step 2: Select NCM622 (chemical formula LiNi 0.6 Co 0.2 Mn 0.2 O2) is used as a matrix, 2.5 kg of the matrix is ​​first put into a coating mixer, and then 2.5 kg of the matrix is ​​added after all the coating auxiliary materials (lithium lanthanum zirconium oxide and cobalt) are put in; 47.31 g (0.509 mol) of cobalt hydroxide and 22.42 g of micro-powdered lithium hydroxide (monohydrate) (0.534 mol) are weighed, mixed in a PE bag to obtain a cobalt compound additive, and put into the coating mixer; then 25 g of the lithium lanthanum zirconium oxide additive is put into the coating mixer; after the above materials are put in, they are premixed at 500 r / min for 5 minutes, and then the speed is increased to 1500 r / min and maintained for 15 minutes for mixing to obtain a first mixed material.

[0083] Step 3: The first mixed material is loaded into a crucible and transferred to a box furnace, and sintered once at 750° C. in an oxygen atmosphere for 12 hours to obtain a sintered material.

[0084] Step 4: put the sintered material and boron oxide into a coating mixer, premix at 500 r / min for 5 min, then increase the speed to 1500 r / min and maintain for 15 min for secondary mixing to obtain a second mixed material, in which boron oxide accounts for 0.15% of the total mass of the second mixed material.

[0085] Step 5: The second mixed material is loaded into a crucible and transferred to a box furnace, and sintered at 350° C. for 12 hours in air for secondary sintering. After being taken out, it is placed in a high-speed mixer for uniform dispersion, and the positive electrode material is obtained by sieving to remove iron.

[0086] Example 2

[0087] Step 1: Weigh 7.72g lithium carbonate (battery grade), 16.96g lanthanum carbonate (99% purity), 7.47g zirconium dioxide (98% purity) and a small amount of alumina as a solvent, mix them evenly with a ball mill, and use pure water as the liquid medium. The ball-to-liquid ratio is 6:1:2, the speed is 250r / min, and the time is 10h. After drying in a vacuum drying oven, transfer it to a crucible and place it in a muffle furnace to calcine at 950℃ for 10h to obtain a sintered product of lithium lanthanum zirconium oxide. Disperse and refine the particles through alcohol ball milling, the speed is 250r / min, the time is 5h, and after drying, the D50 of lithium lanthanum zirconium oxide is 0.75, which meets the coating requirements.

[0088] Step 2: Select NCM811 (chemical formula LiNi 0.8 Co 0.1 Mn 0.1 O2) is used as a matrix, 2.5 kg of the matrix is ​​first put into a coating mixer, and then 2.5 kg of the matrix is ​​added after all the coating auxiliary materials (lithium lanthanum zirconium oxide and cobalt) are put in; 47.31 g (0.509 mol) of cobalt hydroxide and 22.42 g of micro-powdered lithium hydroxide (monohydrate) (0.534 mol) are weighed, mixed in a PE bag to obtain a cobalt compound additive, and put into the coating mixer; then 25 g of the lithium lanthanum zirconium oxide additive is put into the coating mixer; after the above materials are put in, they are premixed at 500 r / min for 5 minutes, and then the speed is increased to 1500 r / min and maintained for 15 minutes for mixing to obtain a first mixed material.

[0089] Step 3: The first mixed material is loaded into a crucible and transferred to a box furnace, and sintered once at 720° C. in an oxygen atmosphere for 8 hours to obtain a sintered material.

[0090] Step 4: put the sintered material and boron oxide into a coating mixer, premix at 500 r / min for 5 min, then increase the speed to 1500 r / min and maintain for 15 min for secondary mixing to obtain a second mixed material, in which boron oxide accounts for 0.10% of the total mass of the second mixed material.

[0091] Step 5: Load the second mixed material into a crucible and transfer it to a box furnace. Sinter it at 300° C. for 10 hours in air for secondary sintering. Take it out and place it in a high-speed mixer to disperse it evenly. Sieve it to remove iron to obtain the positive electrode material.

[0092] Comparative Example 1

[0093] Step 1: Weigh 7.72g lithium carbonate (battery grade), 16.96g lanthanum carbonate (99% purity), 7.47g zirconium dioxide (98% purity) and a small amount of alumina as a solvent, mix them evenly with a ball mill, and use pure water as the liquid medium. The ball-to-liquid ratio is 6:1:2, the speed is 250r / min, and the time is 10h. After drying in a vacuum drying oven, transfer it to a crucible and place it in a muffle furnace to calcine at 950℃ for 10h to obtain a sintered product of lithium lanthanum zirconium oxide. Disperse and refine the particles through alcohol ball milling, the speed is 250r / min, the time is 5h, and after drying, the D50 of lithium lanthanum zirconium oxide is 0.75, which meets the coating requirements.

[0094] Step 2: Select NCM622 (chemical formula LiNi 0.6 Co 0.2 Mn 0.2 O2) is used as a matrix, 2.5 kg of the matrix is ​​first put into a coating mixer, and then 2.5 kg of the matrix is ​​added after all the coating auxiliary materials (lithium lanthanum zirconium oxide and cobalt) are put in; 47.31 g (0.509 mol) of cobalt hydroxide and 22.42 g of micro-powdered lithium hydroxide (monohydrate) (0.534 mol) are weighed, mixed in a PE bag to obtain a cobalt compound additive, and put into the coating mixer; then 25 g of the lithium lanthanum zirconium oxide additive is put into the coating mixer; after the above materials are put in, they are premixed at 500 r / min for 5 minutes, and then the speed is increased to 1500 r / min and maintained for 15 minutes for mixing to obtain a first mixed material.

[0095] Step 3: put the first mixed material into a crucible and transfer it to a box furnace, sinter it once at 750° C. with oxygen for 12 hours, take it out and place it in a high-speed mixer to disperse it evenly, and sieve it to remove iron to obtain the positive electrode material.

[0096] Comparative Example 2

[0097] Step 1: Select NCM622 (chemical formula LiNi 0.6 Co 0.2 Mn 0.2O2) is used as a matrix, 2.5 kg of the matrix is ​​first put into a coating mixer, and then 2.5 kg of the matrix is ​​added after all the coating auxiliary materials (cobalt) are put in; 47.31 g (0.509 mol) of cobalt hydroxide and 22.42 g of micro powder lithium hydroxide (monohydrate) (0.534 mol) are weighed, mixed in a PE bag to obtain a cobalt compound additive, and put into the coating mixer; after the above materials are put in, they are premixed at 500 r / min for 5 minutes, and then the speed is increased to 1500 r / min and maintained for 15 minutes for mixing to obtain a first mixed material.

[0098] Step 2: The first mixed material is loaded into a crucible and transferred to a box furnace, and sintered once at 750° C. in oxygen for 12 hours. After being taken out, it is placed in a high-speed mixer for uniform dispersion, and the positive electrode material is obtained by sieving to remove iron.

[0099] Step 3: put the sintered material and boron oxide into a coating mixer, premix at 500 r / min for 5 min, then increase the speed to 1500 r / min and maintain for 15 min for secondary mixing to obtain a second mixed material, in which boron oxide accounts for 0.15% of the total mass of the second mixed material.

[0100] Step 4: The second mixed material is loaded into a crucible and transferred to a box furnace, and sintered at 350° C. for 12 hours in air for secondary sintering. After being taken out, it is placed in a high-speed mixer for uniform dispersion, and the positive electrode material is obtained by sieving to remove iron.

[0101] Comparative Example 3

[0102] Step 1: Weigh 7.72g lithium carbonate (battery grade), 16.96g lanthanum carbonate (99% purity), 7.47g zirconium dioxide (98% purity) and a small amount of alumina as a solvent, mix them evenly with a ball mill, and use pure water as the liquid medium. The ball-to-liquid ratio is 6:1:2, the speed is 250r / min, and the time is 10h. After drying in a vacuum drying oven, transfer it to a crucible and place it in a muffle furnace to calcine at 950℃ for 10h to obtain a sintered product of lithium lanthanum zirconium oxide. Disperse and refine the particles through alcohol ball milling, the speed is 250r / min, the time is 5h, and after drying, the D50 of lithium lanthanum zirconium oxide is 0.75, which meets the coating requirements.

[0103] Step 2: Select NCM811 (chemical formula LiNi 0.8 Co 0.1 Mn 0.1 O2) as the matrix, first put 2.5kg of the matrix into the coating mixer, and then add 2.5kg of the matrix after all the coating auxiliary materials (lithium lanthanum zirconium oxide) are put in; put 25g of lithium lanthanum zirconium oxide additive into the coating mixer; after the above materials are put in, premix at 500r / min for 5min, then increase the speed to 1500r / min and keep mixing for 15min to obtain the first mixed material.

[0104] Step 3: The first mixed material is loaded into a crucible and transferred to a box furnace, and sintered once at 720° C. in an oxygen atmosphere for 8 hours to obtain a sintered material.

[0105] Step 4: put the sintered material and boron oxide into a coating mixer, premix at 500 r / min for 5 min, then increase the speed to 1500 r / min and maintain for 15 min for secondary mixing to obtain a second mixed material, in which boron oxide accounts for 0.15% of the total mass of the second mixed material.

[0106] Step 5: Load the second mixed material into a crucible and transfer it to a box furnace. Sinter it at 300° C. for 10 hours in air for secondary sintering. Take it out and place it in a high-speed mixer to disperse it evenly. Sieve it to remove iron to obtain the positive electrode material.

[0107] The positive electrode materials obtained in Examples 1-2 and Comparative Examples 1-3 were subjected to the following tests.

[0108] 1. The positive electrode materials prepared in Example 2 and Comparative Example 3 were observed and tested by scanning electron microscope. The results of Example 2 are as follows: Figure 3A As shown, the results of Comparative Example 3 are as follows Figure 3B As shown. Figure 3A and Figure 3B By comparison, it can be seen that the positive electrode material of Example 2 has a regular spherical morphology, there is no agglomeration of particles on the surface, the solid electrolyte is distributed in an island shape, and is semi-embedded in the matrix particles. However, in Comparative Example 3, the positive electrode material lacks cobalt coating, the particles on the surface of the positive electrode material are agglomerated, the solid electrolyte is distributed on the surface of the positive electrode material, and the embedding effect is reduced.

[0109] 2. The electrical performance of the battery prepared by the positive electrode materials obtained in Examples 1-2 and Comparative Examples 1-3 was tested. The rate performance test results of Examples 1-2 and Comparative Examples 1-3 are shown in Table 1. The DC internal resistance (DCIR) test results of Examples 1-2 and Comparative Examples 1-3 at room temperature (25°C) are shown in Table 1. Figure 4 As shown, the test results of the 1C / 1C cycle capacity retention rate of Example 2 and Comparative Example 3 at 45°C are as follows Figure 5 shown.

[0110] The electrical performance test conditions are as follows: the prepared positive electrode material, conductive agent SP, and mixed liquid NMP are mixed at a ratio of 90:5:5, and the slurry pulling speed is 2000rpm for 90min; after coating and cutting, vacuum drying at 120℃ for 12h, and transferred to the glove box, the metal lithium sheet is the negative electrode, the battery shell is CR2032, and the test voltage is 2.8V~4.3V.

[0111] The first discharge capacity at different rates and the DC internal resistance at 25° C. of the batteries prepared using the positive electrode materials of Examples 1-2 and Comparative Examples 1-3 were measured.

[0112] The 1C / 1C cycle capacity retention rate of the batteries prepared using the positive electrode materials obtained in Example 2 and Comparative Example 3 at 45° C. was measured.

[0113] Table 1

[0114]

[0115] The rate performance test results show that compared with Example 1 (lack of second coating layer) of the same substrate, the discharge capacity of the battery prepared by the double-coating positive electrode material in Example 1 is significantly improved, and the battery has better rate performance. Compared with Example 2 (lack of solid electrolyte in the first coating layer) of the same type of substrate, the rate performance of the battery prepared by the positive electrode material in Example 1 is also better, with a discharge capacity of 155.4 mAh / g at 4C, while the discharge capacity of Comparative Example 2 at 4C is only 150.4 mAh / g. Comparing Example 2 and Comparative Example 3 (lack of cobalt in the first coating layer) with the same substrate, the discharge capacity of Example 2 at different rates is better than that of Comparative Example 3.

[0116] Figure 4 The DCIR bar graphs of Examples 1-2 and Comparative Examples 1-3 at room temperature are shown. By comparing Example 2 with Comparative Example 3, it can be seen that the DCIR performance of the battery prepared with the positive electrode material of high-temperature coated cobalt and LLZO in Example 2 is better than that of the battery prepared with the positive electrode material of only high-temperature coated LLZO. By comparing Example 1 with Comparative Examples 1-2, it can be seen that the DCIR performance in Example 1 is significantly better than that in Comparative Examples 1-2. This is because compared with Comparative Examples 1-2, Example 1 has a complete first coating layer and a second coating layer, which can synergistically reduce the internal resistance of the positive electrode material, thereby improving the DCRI performance of the battery.

[0117] Figure 5 The 1C / 1C cycle capacity retention rate diagram of the battery prepared with the positive electrode materials in Example 2 and Comparative Example 3 at 45 degrees. It can be seen that the structure of simultaneously coating cobalt and LLZO at high temperature during the first sintering in Example 2 can improve the cycle performance of the positive electrode material at high temperature, while the cycle performance of Comparative Example 3 is significantly reduced because only LLZO is coated during the first sintering and the cobalt element is lacking.

[0118] It can be seen that the synergistic effect of the two coatings enables LLZO, cobalt and boron elements to greatly improve the high-temperature cycle stability and high-rate performance of the positive electrode material.

[0119] It is to be understood that the above embodiments are merely exemplary embodiments used to illustrate the principles of the present invention, but the present invention is not limited thereto. For those skilled in the art, various modifications and improvements can be made without departing from the spirit and essence of the present invention, and these modifications and improvements are also considered to be within the scope of protection of the present invention.

Claims

1. A positive electrode material, characterized in that: It includes a substrate and a first coating layer and a second coating layer sequentially coated on the surface of the substrate, wherein the substrate is a nickel-cobalt-manganese ternary positive electrode material, the molar content of the nickel element is ≥0.6, the first coating layer contains a solid electrolyte and a cobalt element, and the second coating layer contains a boron element.

2. The positive electrode material according to claim 1, characterized in that At least a portion of the cobalt element is doped into the matrix.

3. The positive electrode material according to claim 1, characterized in that At least a portion of the solid electrolyte is embedded in the matrix.

4. The positive electrode material according to claim 1, characterized in that The mass ratio of the matrix to the cobalt element is 1:(0.001-0.04); The mass ratio of the matrix to the solid electrolyte is 1:(0.001-0.04).

5. The positive electrode material according to claim 1, characterized in that The solid electrolyte has at least one of the following characteristics: (1) The solid electrolyte includes at least one of an oxide electrolyte, a sulfide electrolyte, a fluoride electrolyte, a phosphate electrolyte and a polymer electrolyte; (2) The solid electrolyte comprises lithium lanthanum zirconium oxide; (3) The solid electrolyte includes lithium lanthanum zirconium oxide doped with a metal element M, and the metal element M includes at least one of Al, Ta, Nb, Sr, Mn, Ni, Ca, Ba, Mg, Ga, Se, Mo, Sn, Ge, V, Ta and Cu.

6. A method for preparing a positive electrode material, characterized in that: include: The matrix of the nickel-cobalt-manganese ternary positive electrode material, the solid electrolyte and the cobalt source are mixed once to obtain a first mixed material; sintering the first mixed material once to obtain a sintered material; Mixing the sintered material and the boron source for a second time to obtain a second mixed material; and The second mixed material is subjected to secondary sintering to obtain the positive electrode material.

7. The method for preparing the positive electrode material according to claim 6, characterized in that: The mass ratio of the substrate, the solid electrolyte and the cobalt in the cobalt source is 1:(0.001-0.04):(0.001-0.04); and / or The mass percentage of boron in the boron source to the second mixed material is 0.05% to 0.5%.

8. The method for preparing the positive electrode material according to claim 6, characterized in that: The primary sintering temperature is 400°C to 800°C, and the primary sintering time is 5h to 15h; The secondary sintering temperature is 200°C to 400°C, and the secondary sintering time is 5h to 15h; The solid electrolyte, cobalt source and boron source are all nano-scale particles.

9. The method for preparing the positive electrode material according to claim 6, characterized in that: The solid electrolyte has at least one of the following characteristics: (1) The solid electrolyte includes at least one of an oxide electrolyte, a sulfide electrolyte, a fluoride electrolyte, a phosphate electrolyte and a polymer electrolyte; (2) The solid electrolyte comprises lithium lanthanum zirconium oxide; (3) The solid electrolyte includes lithium lanthanum zirconium oxide doped with a metal element M, and the metal element M includes at least one of Al, Ta, Nb, Sr, Mn, Ni, Ca, Ba, Mg, Ga, Se, Mo, Sn, Ge, V, Ta and Cu.

10. An electrochemical device, characterized in that: The electrochemical device comprises a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the positive electrode sheet comprises a positive electrode material, and the positive electrode material is the positive electrode material as described in any one of claims 1 to 5 or the positive electrode material prepared by the preparation method of the positive electrode material as described in any one of claims 6 to 9.

Citation Information

Cited By

  • Battery monomer, battery device, power utilization device and energy storage device