Composite current collector and preparation method and application thereof

By using a three-layer co-extruded microporous membrane structure and polyolefin copolymer elastomer modification, the adhesion and mechanical properties of polypropylene-based membranes in composite current collectors were solved, resulting in improved adhesion, conductivity, and heat resistance, and improved internal resistance and fast charging performance of secondary batteries.

CN118970060APending Publication Date: 2024-11-15SHENZHEN SENIOR TECH MATERIAL
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410991915.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Traditional polypropylene-based films suffer from poor adhesion, low interfacial adhesion, weak mechanical properties, poor heat resistance, and uneven deposition of conductive metal layers during the preparation of composite current collectors, resulting in high internal resistance and poor fast-charging performance of secondary batteries.

Method used

A three-layer co-extruded microporous membrane structure is adopted, combined with polyolefin copolymer elastomer (POE) modification treatment, to regulate the pore structure and composition of the base membrane, improve the interfacial adhesion between the base membrane and the conductive metal layer, and enhance the mechanical strength and heat resistance through physical cross-linking network.

Benefits of technology

It improves the surface adhesion, conductivity, mechanical strength and heat resistance of the composite current collector, reduces internal resistance, and enhances the fast charging performance and safety of the secondary battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004959105210000191
    Figure BDA0004959105210000191
  • Figure BDA0004959105210000201
    Figure BDA0004959105210000201
  • Figure BDA0004959105210000211
    Figure BDA0004959105210000211
Patent Text Reader

Abstract

The invention provides a composite current collector and a preparation method and application thereof. The composite current collector comprises a three-layer co-extrusion microporous membrane and conductive metal layers arranged on the two sides of the three-layer co-extrusion microporous membrane, the three-layer co-extrusion microporous membrane comprises a core layer and surface layers arranged on the two sides of the core layer respectively, and the surface layers and the core layer are made of different materials. One of the surface layer and the core layer is made of polypropylene resin, the other one of the surface layer and the core layer is made of modified raw materials, and the modified raw materials comprise the polypropylene resin and a polyolefin copolymer elastomer. According to the invention, the pore structure and composition of the base film are regulated and controlled, and the three-layer co-extrusion microporous film is modified by using the polyolefin copolymer elastomer, so that the prepared composite current collector has good surface adhesion, conductivity, mechanical strength and heat resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of current collector materials, and in particular relates to a composite current collector and a preparation method and application thereof. Background Art

[0002] At present, composite current collectors based on polymer-based films have received extensive attention and application in the new energy industry. They can not only improve the energy density and power density of secondary batteries, but also reduce the production cost of secondary batteries. Therefore, composite current collectors have broad application prospects in the manufacture of secondary batteries.

[0003] On the one hand, polypropylene (PP) has become the mainstream material for the base film in the composite current collector due to its advantages of low cost and wide sources. However, in the process of preparing the composite current collector with the traditional polypropylene film as the base film, there are the following problems: ① The polarity of the polypropylene base film is weak, which makes the surface tension of the base film low and the adhesion performance is poor, which ultimately leads to poor affinity between the base film and the conductive metal layer with high surface tension, resulting in low adhesion at the interface between the two and the problem of weak bonding; ② The mechanical properties of the polypropylene base film are poor, which easily causes the composite current collector to break or perforate during the preparation process, thereby reducing the yield rate of the product, and the prepared composite current collector has the problem of poor mechanical properties and interface adhesion; ③ The heat resistance is poor. When the temperature is too high, the thermal shrinkage rate of the prepared base film is too large, which makes the base film and the conductive metal layer easily separated; ④ The conductive metal layer is deposited unevenly, and it is easy to form more pores, which makes the bonding force between the conductive metal layer and the base film poor and the contact is uneven, resulting in a large internal resistance of the secondary battery, which is not conducive to improving the fast charging performance of the secondary battery.

[0004] Therefore, in the art, there is an urgent need to modify the base film made of polypropylene to comprehensively improve the performance of the composite current collector. Summary of the invention

[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a composite current collector and its preparation method and application. The present invention modifies the pore structure and composition of the base film and uses a polyolefin copolymer elastomer to modify the three-layer co-extruded microporous membrane, so that the prepared composite current collector has good surface adhesion, conductivity, mechanical strength and heat resistance.

[0006] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0007] In the first aspect, the present invention provides a composite current collector, comprising a three-layer co-extruded microporous membrane and a conductive metal layer arranged on both sides of the three-layer co-extruded microporous membrane, the three-layer co-extruded microporous membrane comprising a core layer and surface layers respectively arranged on both sides of the core layer, the surface layer and the core layer are made of different materials, the material of one of the surface layer or the core layer comprises polypropylene resin, and the material of the other comprises a modified raw material, and the modified raw material comprises polypropylene resin and a polyolefin copolymer elastomer.

[0008] On the one hand, the present invention adopts a microporous film with a pore structure as a base film, and further regulates the base film to be a three-layer co-extruded multi-layer microporous film, so that it has an A / B / A structure. Due to the presence of micropores, the internal resistance of the base film is reduced, and its own conductivity and roughness are improved, and the interfacial adhesion between the base film and the conductive metal layer can also be improved. On the other hand, the present invention adds a polyolefin copolymer elastomer (POE) to the raw material of one of the surface layer or the core layer, which not only has good compatibility with the polypropylene resin, but also the α-olefin soft chain contained in the molecular structure can interact with the polyethylene chain crystal region to form a physical cross-linked network. This physical cross-linked network can play a connecting and buffering role between the components, thereby enhancing the mechanical strength, heat resistance and processing performance of the base film.

[0009] Preferably, the polyolefin copolymer elastomer comprises ethylene-octene copolymer elastomer.

[0010] In the present invention, the ethylene-octene copolymer elastomer (POE) is a polymer obtained by in-situ polymerization of ethylene and α-olefin using a metallocene catalyst, so that the polymer has a polyethylene chain crystalline region (resin phase) with typical plastic properties and an amorphous region (rubber phase) with rubber elasticity, thereby giving the POE material the dual characteristics of plastic and rubber. On the one hand, the polyethylene chain crystalline region can play the role of a physical crosslinking point, so that the polymer has typical plastic properties. On the other hand, the introduction of α-olefins (such as 1-butene, 1-hexene or 1-octene, etc.) can weaken the crystalline region of the polyethylene chain, thereby forming an amorphous region showing rubber elasticity, so that the polymer has the properties of an elastomer at the same time.

[0011] Preferably, the molar percentage of α-octene structural units in the ethylene-octene copolymer elastomer is 15%-45%, preferably 20%-30%, for example, it can be 15%, 18%, 20%, 22%, 25%, 28%, 30%, 32%, 35%, 38%, 40%, 42%, 45%, etc.

[0012] In the present invention, the melt index of the ethylene-octene copolymer elastomer is maintained in a preferred numerical range by regulating the molar percentage of the α-octene structural unit in the ethylene-octene copolymer elastomer. If the melt index of the ethylene-octene copolymer elastomer is too low, it is not mixed evenly with the polypropylene resin, and the film-forming property of the modified base film is poor in the subsequent stretching process; if the melt index of the ethylene-octene copolymer elastomer is too high, its film-forming property is poor and the mechanical properties of the modified base film are poor.

[0013] Preferably, the density of the ethylene-octene copolymer elastomer is 0.85 g / cm 3 -0.90g / cm 3 , for example, it can be 0.85 g / cm 3 , 0.86g / cm 3 , 0.87g / cm 3 , 0.88g / cm 3 , 0.89g / cm 3 , 0.90g / cm 3 wait.

[0014] Preferably, the melt index of the ethylene-octene copolymer elastomer at 230°C and 2.16kg is 1.0g / 10.0min-10g / 10.0min, preferably 1.5g / 10.0min-5.0g / 10.0min, for example, it can be 1.0g / 10min, 1.5g / 10.0min, 2.0g / 10min, 3.0g / 10min, 4.0g / 10min, 5.0g / 10min, 6.0g / 10min, 7.0g / 10min, 8.0g / 10min, 9.0g / 10min, 10g / 10min, etc.

[0015] Preferably, the tear strength of the ethylene-octene copolymer elastomer is 20 KN / m-150 KN / m, preferably 30 KN / m-100 KN / m, for example, it can be 20 KN / m, 30 KN / m, 50 KN / m, 60 KN / m, 80 KN / m, 90 KN / m, 100 KN / m, 110 KN / m, 120 KN / m, 130 KN / m, 140 KN / m, 150 KN / m, etc.

[0016] Preferably, the elongation at break of the ethylene-octene copolymer elastomer is 500%-3000%, preferably 1500%-2500%, for example, it can be 500%, 600%, 800%, 900%, 1000%, 1200%, 1500%, 1800%, 2000%, 2200%, 2500%, 2800%, 3000%, etc.

[0017] Preferably, based on the total mass of the raw materials of the surface layer or the core layer as 100%, the modified raw material includes 80%-95% polypropylene resin and 5%-20% polyolefin copolymer elastomer, and more preferably 85%-95% polypropylene resin and 5%-15% polyolefin copolymer elastomer.

[0018] In the present invention, the mass percentage of the polypropylene resin is 80%-95%, for example, it can be 80%, 82%, 85%, 88%, 90%, 92%, 95%, etc.

[0019] In the present invention, the mass percentage of the polyolefin copolymer elastomer is 5%-20%, for example, it can be 5%, 8%, 10%, 12%, 15%, 18%, 20%, etc. If the content of the polyolefin copolymer elastomer in the raw material of any layer of the surface layer or the core layer is too low, the modification effect on the base film is not significantly improved; if the content of the polyolefin copolymer elastomer in the raw material of any layer of the surface layer or the core layer is too high, the polyolefin copolymer elastomer is easy to agglomerate in the polypropylene resin and form material defects, which ultimately makes the mechanical properties of the base film poor.

[0020] Preferably, based on the total mass of the raw materials of the surface layer or the core layer being 100%, the modified raw material further comprises 0%-2% of a dispersant, 0%-0.5% of a coupling agent and 0%-0.5% of a lubricant.

[0021] In the present invention, the mass percentage of the dispersant is 0%-2%, preferably 0.2%-1%, for example, it can be 0%, 0.2%, 0.5%, 0.8%, 1%, 1.2%, 1.5%, 1.8%, 2%, etc.

[0022] In the present invention, the mass percentage of the coupling agent is 0%-0.5%, preferably 0.2%-0.5%, for example, it can be 0%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, etc.

[0023] In the present invention, the mass percentage of the lubricant is 0%-0.5%, preferably 0.2%-0.5%, for example, it can be 0%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5% and the like.

[0024] In the present invention, the dispersant includes any one or a combination of at least two of polyvinyl pyrrolidone, sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, polyethylene glycol, hydroxypropyl methylcellulose, polyvinyl alcohol, N,N-dimethylformamide, N-methylpyrrolidone, sodium carboxymethyl cellulose, polyacrylic acid alkylhydroxylamine, ethylene oxide, ethylene glycol and isopropanol.

[0025] In the present invention, the coupling agent includes any one or a combination of at least two of a silane coupling agent, a titanate coupling agent, an aluminate coupling agent, a bimetallic coupling agent, a phosphate coupling agent, a borate coupling agent and a chromium complex.

[0026] In the present invention, the lubricant includes any one or a combination of at least two of titanium dioxide, silicon dioxide, calcium carbonate, talc, kaolin, diatomaceous earth, siloxane and acrylate.

[0027] Preferably, the modified raw material further includes any one of inorganic filler, epoxy resin and acrylic resin or a combination of at least two thereof, so as to further reduce the internal resistance of the base film or improve the mechanical strength of the base film.

[0028] Preferably, based on the total mass of the modified raw material as 100%, the content of any one or a combination of at least two of the inorganic filler, epoxy resin and acrylic resin is 0%-5%, for example, it can be 0%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, etc.

[0029] Preferably, the inorganic filler includes any one of nano oxides, nano carbides, metal single substance materials and nano carbon materials, or a combination of at least two of them, preferably nano carbon materials.

[0030] Preferably, the nano-oxide includes any one of silicon dioxide, titanium dioxide, boehmite, aluminum oxide and copper oxide, or a combination of at least two thereof, preferably at least one of silicon dioxide, boehmite or aluminum oxide.

[0031] Preferably, the nanocarbide comprises tungsten carbide.

[0032] Preferably, the metal single substance material includes nano copper.

[0033] Preferably, the nanocarbon material includes any one or a combination of at least two of graphene, conductive carbon black, carbon nanotubes, diamond, acetylene black, conductive fibers and carbon nanofibers, preferably graphene and / or carbon nanotubes, so as to improve the conductivity, heat resistance and surface roughness of the base film, and at the same time help to improve the interface adhesion between the base film and the conductive metal layer.

[0034] Preferably, the number of graphene layers is ≤10, for example, it can be 2 layers, 3 layers, 4 layers, 5 layers, 6 layers, 7 layers, 8 layers, 9 layers or 10 layers.

[0035] Preferably, the graphene sheet diameter is 3-15 μm, preferably 5-10 μm, for example, 3 μm, 5 μm, 8 μm, 10 μm, 12 μm, 15 μm, etc.

[0036] Preferably, the carbon nanotubes are single-walled carbon nanotubes.

[0037] Preferably, the length of the single-walled carbon nanotube is 5-30 μm, preferably 10-20 μm, for example, 5 μm, 8 μm, 10 μm, 12 μm, 15 μm, 18 μm, 20 μm, 22 μm, 25 μm, 28 μm, 30 μm, etc.

[0038] In the present invention, the molecular weight distribution index of the polypropylene resin is 3.8-5.0, for example, it can be 3.8, 4.0, 4.2, 4.5, 4.8, 5.0, etc. If the molecular weight distribution index of the polypropylene resin is too high, the content of the polypropylene resin with a small molecular weight is higher, resulting in poor mechanical properties and poor film-forming properties of the prepared base film; if the molecular weight distribution index of the polypropylene resin is too low, the content of the polypropylene resin with a small molecular weight is too low, which makes the film-forming properties of the modified base film worse in the subsequent stretching process, resulting in a decrease in the yield rate of the product.

[0039] In the present invention, the isotacticity of the polypropylene resin is ≥ 98%, for example, it can be 98%, 98.5%, 99%, 99.5%, etc. The higher the isotacticity of the polypropylene resin, the higher the regularity of the polypropylene resin. The present invention can improve the crystallinity and orientation of the polypropylene resin by appropriately improving the regularity of the polypropylene resin, thereby improving the mechanical properties of the prepared base film.

[0040] In the present invention, the melt index of the polypropylene resin at 230°C and 2.16kg is 0.5-3.0g / 10min, for example, it can be 0.5g / 10min, 0.8g / 10min, 1.0g / 10min, 1.5g / 10min, 2.0g / 10min, 2.5g / 10min, 3.0g / 10min, etc. The present invention selects a polypropylene resin with a specific melt index range, so that the modified base film is easy to form in the subsequent stretching process, and the prepared modified base film has good comprehensive properties. If the melt index of the polypropylene resin is too low, the molecular weight of the polypropylene resin is too large, resulting in poor film-forming properties of the modified base film in the subsequent stretching process; if the melt index of the polypropylene resin is too high, the molecular weight of the polypropylene resin is too low, and its film-forming properties are poor and the mechanical properties of the prepared modified base film are poor.

[0041] Preferably, the thickness of the three-layer co-extruded microporous membrane is 2-10 μm, for example, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, etc. The thickness of the three-layer co-extruded microporous membrane directly affects its own mechanical strength and the energy density of the prepared composite current collector. If the thickness of the three-layer co-extruded microporous membrane is larger, the energy density of the prepared composite current collector will also be smaller; if the thickness of the three-layer co-extruded microporous membrane is smaller, the base membrane is prone to shrinkage deformation and perforation during subsequent preparation and use, and even the conductive metal layer is prone to fall off, thereby greatly reducing the process yield and comprehensive performance of the composite current collector.

[0042] Preferably, the porosity of the three-layer co-extruded microporous membrane is 30-50%, preferably 35-45%, for example, it can be 30%, 32%, 35%, 38%, 40%, 42%, 45%, 48%, 50%, etc. In the present invention, the present invention improves the conductivity of the base film and the interfacial adhesion between the base film and the conductive metal layer by regulating the porosity of the three-layer co-extruded microporous membrane. If the porosity of the three-layer co-extruded microporous membrane is too high, the mechanical strength of the base film is too low, and deformation and perforation are prone to occur; if the porosity of the three-layer co-extruded microporous membrane is too low, the conductivity of the base film deteriorates, and the energy density of the prepared composite current collector is too low.

[0043] In the present invention, the heat-resistant temperature of the three-layer co-extruded microporous membrane is not less than 160°C, so that the transverse (TD) heat shrinkage rate and the longitudinal (MD) heat shrinkage rate of 1h at this temperature are both less than 5%. Since the heat-resistant temperature of the three-layer co-extruded microporous membrane directly affects the heat-resistant temperature of the prepared composite current collector, the present invention adjusts the three-layer co-extruded microporous membrane to have a higher heat-resistant temperature, so that the base film is not prone to shrinkage deformation and perforation during the preparation of the composite current collector, and the conductive metal layer is also less likely to fall off. However, if the heat-resistant temperature of the three-layer co-extruded microporous membrane is too high, the material performance requirements of the base film are high, and the production cost is greatly increased, which is not conducive to large-scale application.

[0044] In the present invention, the transverse (TD) tensile strength of the three-layer co-extruded microporous membrane is not less than 300MPa, the transverse elongation at break is not less than 60%, the longitudinal (MD) tensile strength is not less than 250MPa, the longitudinal elongation at break is not less than 80%, and the puncture strength is not less than 1N / μm. If the mechanical strength of the three-layer co-extruded microporous membrane is too low, the modified base film will be deformed and perforated when preparing the composite current collector, and even the conductive metal layer in the composite current collector will fall off, and the cycle life of the secondary battery finally assembled will be reduced.

[0045] In the present invention, the material of the conductive metal layer includes but is not limited to any one or more combinations of copper, aluminum, silver, gold, iron, titanium, cobalt, chromium, molybdenum and tungsten, preferably aluminum and / or copper.

[0046] In the present invention, the thickness of the conductive metal layer is 1-2 μm, for example, 1 μm, 1.2 μm, 1.5 μm, 1.8 μm, 2 μm, etc.

[0047] In the present invention, the conductive metal layer can be prepared exemplarily by coating, and the coating method includes but is not limited to vacuum magnetron sputtering, resistance heating vacuum evaporation coating, vacuum plasma sputtering, any one or more combinations of chemical plating and electroplating, preferably any one or more combinations of vacuum magnetron sputtering, resistance heating vacuum evaporation coating and electroplating.

[0048] In the present invention, when the material of the conductive metal layer is aluminum, the conductive metal layer is directly formed by the physical vapor deposition technology; when the material of the conductive metal layer is copper, the physical vapor deposition technology is first used to form a base copper layer, and then the base copper layer is thickened by water electroplating to form the conductive metal layer. Of course, when the material of the conductive metal layer is copper, the conductive metal layer can also be directly formed by using either the physical vapor deposition technology or the water electroplating process.

[0049] In the present invention, the water electroplating process includes clamping horizontal plating and / or roller horizontal plating.

[0050] In the present invention, protective layers may be respectively provided on both sides of the conductive metal layer away from the polymer base film layer.

[0051] In the present invention, the material of the protective layer includes but is not limited to any one or more combinations of nickel, chromium, nickel-based alloys, copper-based alloys, copper oxide, aluminum oxide, silicon dioxide, nickel oxide, chromium oxide, cobalt oxide, copper chromium oxide, formic acid-copper complex, nickel-chromium alloy, graphite, carbon black, acetylene black, Ketjen black, carbon nano-quantum dots, carbon nanotubes, carbon nanofibers and graphene.

[0052] In the present invention, the thickness of the protective layer is 20nm-150nm, preferably 50nm-100nm, for example, 20nm, 30nm, 50nm, 60nm, 70nm, 80nm, 90nm, 100nm, 120nm, 150nm, etc. If the thickness of the protective layer is too small, it cannot protect the conductive metal layer from being scratched or oxidized; if the thickness of the protective layer is too large, it will reduce the conductivity of the composite current collector and increase its own weight and internal resistance.

[0053] In the present invention, the preparation method of the protective layer includes but is not limited to any one or more combinations of physical vapor deposition, chemical vapor deposition, in-situ forming, coating, electroplating or chemical plating.

[0054] In a second aspect, the present invention provides a method for preparing the composite current collector according to the first aspect, the method comprising the following steps:

[0055] The modified raw material and the polypropylene resin are respectively put into different extruders, melt-extruded, and converged into the same hanger-shaped die to form a composite molten material;

[0056] The composite melt is subjected to casting and cooling treatment, and then subjected to stretching treatment to form micropores to obtain a three-layer co-extruded microporous membrane;

[0057] Conductive metal layers are arranged on both sides of the three-layer co-extruded microporous membrane to obtain the composite current collector.

[0058] In the composite current collector prepared by the present invention, the base film and the conductive metal layer are tightly bonded and the interface internal resistance is small. At the same time, the deposited conductive metal layer is evenly distributed and dense, and the stress between the conductive metal layers is small, thereby comprehensively improving the heat resistance, mechanical strength and conductivity of the composite current collector.

[0059] Preferably, the melt extrusion equipment comprises a single screw multi-extruder.

[0060] In the present invention, different extruders can supply different raw materials through a single-screw multi-extruder mode, and the raw materials of each extruder pass through a distributor section or a multi-cavity die head, and converge through different chambers to realize a hamburger-like multilayer structure, and the die head voltage stabilizing section is synchronously ejected to realize the interlayer distribution of different raw materials (the ratio of the extrusion amount of each extruder), and realize multi-layer co-extrusion. The present invention can prepare a three-layer co-extruded microporous membrane structure of polypropylene resin layer / composite material layer / polypropylene resin layer, or composite material layer / polypropylene resin layer / composite material layer through such an arrangement.

[0061] Preferably, the temperature of the melt extrusion is 200-250°C, for example, 200°C, 210°C, 220°C, 230°C, 240°C, 250°C, etc.

[0062] Preferably, the melt extrusion rate is 100-180 m / min, for example, 100 m / min, 110 m / min, 120 m / min, 130 m / min, 140 m / min, 150 m / min, 160 m / min, 170 m / min, 180 m / min, etc.

[0063] Preferably, the casting temperature is 200-240°C, for example, 200°C, 210°C, 220°C, 230°C, 240°C, etc.

[0064] Preferably, the cooling treatment temperature is 60-80°C, for example, 60°C, 65°C, 70°C, 75°C, 80°C, etc.

[0065] In the present invention, the cooling treatment rate is 100-180 m / min, for example, it can be 100 m / min, 110 m / min, 120 m / min, 130 m / min, 140 m / min, 150 m / min, 160 m / min, 170 m / min, 180 m / min, etc.

[0066] In a third aspect, the present invention provides an electrode, comprising a current collector and an active material layer disposed on at least one side of the current collector, wherein the current collector comprises the composite current collector according to the first aspect.

[0067] In a fourth aspect, the present invention provides a secondary battery, comprising an electrode, an electrolyte and a separator, wherein the electrode comprises the electrode according to the third aspect.

[0068] Compared with the prior art, the present invention has the following beneficial effects:

[0069] The present invention provides a composite current collector. On the one hand, the present invention adopts a microporous film with a pore structure as a base film, and further regulates the base film to be a three-layer co-extruded multi-layer microporous film, so that it has a structure similar to A / B / A. Due to the presence of micropores, the internal resistance of the base film is reduced, and its own conductivity and roughness are improved, and the interfacial adhesion between the base film and the conductive metal layer can also be improved. On the other hand, the present invention adds a polyolefin copolymer elastomer (POE) to the raw material of one of the surface layer or the core layer, which not only has good compatibility with the polypropylene resin, but also the α-olefin soft chain contained in the molecular structure can interact with the polyethylene chain crystal region to form a physical cross-linked network. This physical cross-linked network can play a connecting and buffering role between the components, thereby enhancing the mechanical strength, heat resistance and processing performance of the base film.

[0070] The composite current collector provided by the present invention has the advantages of simple preparation process, high production efficiency, low cost and high economic benefit, and is easy to carry out mass production. DETAILED DESCRIPTION

[0071] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0072] Unless otherwise specified, the substances involved in the specific embodiments of the present invention are all conventional materials in the art and can be purchased commercially. In particular, the information of some of the substances involved is as follows:

[0073] Polypropylene resin: LG Chem, South Korea;

[0074] Ethylene-octene copolymer elastomer: purchased from ExxonMobil Corporation, brand 6102.

[0075] Example 1

[0076] The present embodiment provides a copper composite current collector, comprising a three-layer co-extruded microporous membrane (thickness of 4.5 μm) and a conductive metal copper layer arranged on both sides of the three-layer co-extruded microporous membrane, the three-layer co-extruded microporous membrane comprising a core layer and surface layers respectively arranged on both sides of the core layer, the core layer comprising polypropylene resin and ethylene-octene copolymer elastomer, the surface layer comprising polypropylene resin, wherein the model of ethylene-octene copolymer elastomer (POE) is 6102, and the density is 0.862 g / cm 3 The melt index at 230°C and 2.16kg is 2.0g / 10min, the tear strength is 34.3KN / m, and the elongation at break is greater than 2000%.

[0077] This embodiment also provides a method for preparing the copper composite current collector, which comprises the following steps:

[0078] (1) Based on the total mass of the raw materials of the core layer being 100%, 92.5% by mass of polypropylene resin and 7.5% by mass of POE 6102 are blended to obtain a core layer raw material; the polypropylene resin is used as the surface layer raw material, wherein the molecular weight distribution index of the polypropylene resin is 4.1, the isotacticity is 98.6%, and the melt index at 230° C. and 2.16 kg is 2.0 g / 10 min;

[0079] (2) melting and three-layer co-extrusion of the surface layer raw material and the core layer raw material obtained in step (1) through a single-screw multi-extruder mode, the melting temperature is 230° C., the three-layer co-extrusion rate is 120 m / min, and the composite melt is converged into the same hanger-type die to obtain a composite melt; casting the composite melt onto a casting roll at a casting temperature of 210° C., and passing through a cooling roll to obtain a sheet, the temperature of the cooling roll is 70° C., and the speed of the cooling roll is 120 m / min;

[0080] (3) preheating the sheet obtained in step (2) at 130° C., and then sequentially subjecting the sheet to longitudinal stretching and heat setting treatment, wherein the longitudinal stretching temperature is 145° C., the longitudinal stretching ratio is 2.1 times, the heat setting temperature is 158° C., and cooling at 20° C. to obtain a three-layer co-extruded microporous membrane;

[0081] (4) rolling and slitting the three-layer co-extruded microporous membrane obtained in step (3) to obtain a base film;

[0082] (5) depositing a base copper layer on both sides of the base film by vacuum magnetron sputtering, wherein the thickness of the base copper layer on both sides is 50 nm and the surface resistance is 1Ω / □;

[0083] (6) thickening the base copper layer by a roller-type horizontal plating process, and depositing electroplated copper layers on both sides of the base copper layer, respectively, with the thickness of the electroplated copper layers on both sides being 1 μm;

[0084] (7) A 50 nm thick nano-silicon dioxide protective layer is deposited on both sides of the electroplated copper layer away from the base film by plasma enhanced chemical vapor deposition (PECVD) process to obtain a copper composite current collector.

[0085] This embodiment further provides a negative electrode sheet, which includes the copper composite current collector and a negative electrode active material layer located on one side of the copper composite current collector.

[0086] This embodiment also provides a lithium-ion battery, which includes a positive electrode sheet, the above-mentioned negative electrode sheet, an electrolyte and a diaphragm. The diaphragm is a polypropylene dry-process diaphragm (purchased from Shenzhen Xingyuan Material Technology Co., Ltd.).

[0087] Example 2

[0088] The difference between this embodiment and embodiment 1 is that in step (1): taking the total mass of the raw materials of the core layer as 100%, 90% by mass of polypropylene resin and 10% by mass of POE 6102 are blended to obtain the core layer raw material, and the rest is the same as embodiment 1.

[0089] Example 3

[0090] The difference between this embodiment and embodiment 1 is that in step (1): taking the total mass of the raw materials of the core layer as 100%, 85% by mass of polypropylene resin and 15% by mass of POE 6102 are blended to obtain the core layer raw material, and the rest is the same as embodiment 1.

[0091] Example 4

[0092] The difference between this embodiment and embodiment 1 is that in step (1): taking the total mass of the raw materials of the core layer as 100%, 80% by mass of polypropylene resin and 20% by mass of POE 6102 are blended to obtain the core layer raw material, and the rest is the same as embodiment 1.

[0093] Example 5

[0094] The difference between this embodiment and embodiment 1 is that in step (1): based on the total mass of the raw materials of the core layer as 100%, 85% by mass of polypropylene resin and 15% by mass of POE 6102 are blended to obtain the core layer raw material, and in step (3), a three-layer co-extruded microporous membrane with a thickness of 8 μm is obtained, and the rest is the same as in embodiment 1.

[0095] Example 6

[0096] The difference between this embodiment and embodiment 1 is that in step (1): taking the total mass of the raw materials of the surface layer as 100%, 95% by mass of polypropylene resin and 5% by mass of POE 6102 are blended to obtain the raw materials for the surface layer; the raw materials for the core layer include polypropylene resin, and the rest are the same as in embodiment 1.

[0097] Example 7

[0098] The difference between this embodiment and embodiment 1 is that in step (1): taking the total mass of the raw materials of the surface layer as 100%, 85% by mass of polypropylene resin and 15% by mass of POE 6102 are blended to obtain the raw materials for the surface layer; the raw materials for the core layer include polypropylene resin, and the rest are the same as in embodiment 1.

[0099] Example 8

[0100] The difference between this embodiment and embodiment 1 is that in step (1): taking the total mass of the raw materials of the surface layer as 100%, 80% by mass of polypropylene resin and 20% by mass of POE 6102 are blended to obtain the surface layer raw material; the raw material of the core layer includes polypropylene resin, and in step (3), a three-layer co-extruded microporous membrane with a thickness of 10 μm is obtained to obtain a copper composite current collector, and the rest is the same as in embodiment 1.

[0101] Example 9

[0102] The present embodiment provides an aluminum composite current collector, including a three-layer co-extruded microporous membrane (with a thickness of 8 μm) and a conductive aluminum metal layer arranged on both sides of the three-layer co-extruded microporous membrane, the three-layer co-extruded microporous membrane includes a core layer and surface layers respectively arranged on both sides of the core layer, the core layer includes polypropylene resin and ethylene-octene copolymer elastomer, and the surface layer includes polypropylene resin, wherein the model of ethylene-octene copolymer elastomer (POE) is 6102.

[0103] This embodiment also provides a method for preparing the aluminum composite current collector, which comprises the following steps:

[0104] (1) Based on the total mass of the raw materials of the core layer being 100%, 85% by mass of polypropylene resin and 15% by mass of POE 6102 are blended to obtain a core layer raw material; the polypropylene resin is used as the surface layer raw material, wherein the molecular weight distribution index of the polypropylene resin is 4.1, the isotacticity is 98.6%, and the melt index at 230° C. and 2.16 kg is 2.0 g / 10 min;

[0105] (2) melting and three-layer co-extrusion of the surface layer raw material and the core layer raw material obtained in step (1) through a single-screw multi-extruder mode, the melting temperature is 230° C., the three-layer co-extrusion rate is 120 m / min, and the composite melt is converged into the same hanger-type die to obtain a composite melt; casting the composite melt onto a casting roll at a casting temperature of 210° C., and passing through a cooling roll to obtain a sheet, the temperature of the cooling roll is 70° C., and the speed of the cooling roll is 120 m / min;

[0106] (3) preheating the sheet obtained in step (2) at 130° C., and then sequentially subjecting the sheet to longitudinal stretching and heat setting treatment, wherein the longitudinal stretching temperature is 145° C., the longitudinal stretching ratio is 2.1 times, the heat setting temperature is 158° C., and cooling at 20° C. to obtain a three-layer co-extruded microporous membrane;

[0107] (4) rolling and slitting the three-layer co-extruded microporous membrane obtained in step (3) to obtain a base film;

[0108] (5) depositing a metal aluminum layer on both sides of the base film by vacuum evaporation process, wherein the thickness of the metal aluminum layer on both sides is 1 μm respectively, and the surface resistance is 1 Ω / □;

[0109] (6) A nano-aluminum oxide protective layer with a thickness of 50 nm is deposited on both sides of the metal aluminum layer away from the base film through a resistance heating vacuum deposition process (PVD) to obtain an aluminum composite current collector.

[0110] This embodiment further provides a positive electrode sheet, which includes the aluminum composite current collector and a positive electrode active material layer located on one side of the aluminum composite current collector, wherein the positive electrode active material layer includes NCM811, a polyacrylate binder and conductive carbon black.

[0111] This embodiment also provides a lithium-ion battery, which includes the above-mentioned positive electrode sheet, negative electrode sheet, electrolyte and diaphragm, and the diaphragm is a polypropylene dry-process diaphragm (purchased from Shenzhen Xingyuan Material Technology Co., Ltd.).

[0112] Example 10

[0113] The present embodiment provides an aluminum composite current collector, including a three-layer co-extruded microporous membrane (with a thickness of 10 μm) and a conductive aluminum metal layer arranged on both sides of the three-layer co-extruded microporous membrane, the three-layer co-extruded microporous membrane includes a core layer and surface layers respectively arranged on both sides of the core layer, the core layer includes polypropylene resin, the surface layer includes polypropylene resin and ethylene-octene copolymer elastomer, wherein the model of ethylene-octene copolymer elastomer (POE) is 6102.

[0114] This embodiment also provides a method for preparing the aluminum composite current collector, which comprises the following steps:

[0115] (1) Based on the total mass of the raw materials of the surface layer being 100%, 80% by mass of a polypropylene resin and 20% by mass of POE 6102 are blended to obtain a surface layer raw material; the polypropylene resin is used as a core layer raw material, wherein the molecular weight distribution index of the polypropylene resin is 4.1, the isotacticity is 98.6%, and the melt index at 230° C. and 2.16 kg is 2.0 g / 10 min;

[0116] (2) melting and three-layer co-extrusion of the surface layer raw material and the core layer raw material obtained in step (1) through a single-screw multi-extruder mode, the melting temperature is 230° C., the three-layer co-extrusion rate is 120 m / min, and the composite melt is converged into the same hanger-type die to obtain a composite melt; casting the composite melt onto a casting roll at a casting temperature of 210° C., and passing through a cooling roll to obtain a sheet, the temperature of the cooling roll is 70° C., and the speed of the cooling roll is 120 m / min;

[0117] (3) preheating the sheet obtained in step (2) at 130° C., and then sequentially subjecting the sheet to longitudinal stretching and heat setting treatment, wherein the longitudinal stretching temperature is 145° C., the longitudinal stretching ratio is 2.1 times, the heat setting temperature is 158° C., and cooling at 20° C. to obtain a three-layer co-extruded microporous membrane;

[0118] (4) rolling and slitting the three-layer co-extruded microporous membrane obtained in step (3) to obtain a base film;

[0119] (5) depositing a metal aluminum layer on both sides of the base film by vacuum evaporation process, wherein the thickness of the metal aluminum layer on both sides is 1 μm respectively, and the surface resistance is 1 Ω / □;

[0120] (6) A nano-aluminum oxide protective layer with a thickness of 50 nm is deposited on both sides of the metal aluminum layer away from the base film through a resistance heating vacuum deposition process (PVD) to obtain an aluminum composite current collector.

[0121] This embodiment further provides a positive electrode sheet, which includes the aluminum composite current collector and a positive electrode active material layer located on one side of the aluminum composite current collector, wherein the positive electrode active material layer includes NCM811, a polyacrylate binder and conductive carbon black.

[0122] This embodiment also provides a lithium-ion battery, which includes the above-mentioned positive electrode sheet, negative electrode sheet, electrolyte and diaphragm, and the diaphragm is a polypropylene dry-process diaphragm (purchased from Shenzhen Xingyuan Material Technology Co., Ltd.).

[0123] Embodiment 11

[0124] The difference between this embodiment and embodiment 6 is that in step (1): based on the total mass of the raw materials of the surface layer as 100%, 80% by mass of polypropylene resin, 15% by mass of POE 6102, 2% by mass of few-layer graphene, 1% by mass of single-walled carbon nanotubes, 1% by mass of polyvinyl pyrrolidone dispersant, 0.5% by mass of silane coupling agent KH-560 and 0.5% by mass of calcium carbonate lubricant are blended to obtain the raw materials for the surface layer; the raw materials for the core layer include polypropylene resin, and in step (3), a three-layer co-extruded microporous membrane with a thickness of 4.5 μm is obtained, and the rest is the same as in embodiment 6.

[0125] Example 12

[0126] The difference between this embodiment and embodiment 11 is that in step (1): based on the total mass of the raw materials for the surface layer as 100%, 85% by mass of polypropylene resin, 10% by mass of POE 6102, 2% by mass of few-layer graphene, 1% by mass of single-walled carbon nanotubes, 1% by mass of polyvinyl pyrrolidone dispersant, 0.5% by mass of silane coupling agent KH-560 and 0.5% by mass of calcium carbonate lubricant are blended to obtain the raw materials for the surface layer; the raw materials for the core layer include polypropylene resin, and the rest are the same as in embodiment 11.

[0127] Comparative Example 1

[0128] The difference between this comparative example and Example 1 is that the three-layer co-extruded microporous membrane is replaced by a conventional biaxially oriented polypropylene base film (BOPP) with a thickness of 4.5 μm, and the rest is the same as Example 1.

[0129] Comparative Example 2

[0130] The difference between this comparative example and Example 1 is that in step (1): based on the total mass of the raw materials of the core layer being 100%, 98% by mass of polypropylene resin and 2% by mass of POE 6102 are blended to obtain the core layer raw material, and the rest is the same as Example 1.

[0131] Comparative Example 3

[0132] The difference between this comparative example and Example 1 is that in step (1): based on the total mass of the raw materials of the core layer being 100%, 70% by mass of polypropylene resin and 30% by mass of POE 6102 are blended to obtain the core layer raw material, and the rest is the same as Example 1.

[0133] Comparative Example 4

[0134] The difference between this comparative example and Example 1 is that the POE 6102 in the core layer is replaced with an equal content of calcium carbonate, and the rest is the same as Example 1.

[0135] Test conditions

[0136] The base films and composite current collectors provided in Examples 1 to 12 and Comparative Examples 1 to 4 were tested respectively, and the testing methods were as follows:

[0137] The porosity is tested using the Best BSD-660 high-performance specific surface area and pore size analyzer in accordance with the national standard GB / T36363-2018.

[0138] The surface tension is measured according to GB / T 14216-2008 on the modified polypropylene base film layer.

[0139] The surface square resistance was tested using a four-probe resistance tester at five locations around and in the center of the composite current collector, and the average value was taken.

[0140] The high temperature test is to keep the composite current collector in an oven at 130±5℃ for 24h, and observe the deformation degree of the composite current collector and the peeling of the conductive metal layer. The sum of the length change rate of the composite current collector in the TD direction and the length change rate in the MD direction is set as the deformation degree. If the deformation degree of the composite current collector is ≤10% and there is no peeling of any metal layer, it passes the high temperature test, otherwise it fails.

[0141] The acid and alkali resistance test is to completely immerse the composite current collector sample in 5% sulfuric acid or sodium hydroxide solution for 24 hours at room temperature and pressure, and observe the expansion, peeling, corrosion and shedding of the sample. The sum of the length change rate of the composite current collector in the TD direction and the length change rate in the MD direction is set as the deformation degree. If the deformation degree of the composite current collector is ≤10%, there is no corrosion, and no conductive metal layer falls off, it passes the acid and alkali resistance test, otherwise it fails.

[0142] The peel strength was tested on a universal tensile testing machine and analyzed according to the national standard GB / T 2792-2014.

[0143] The puncture resistance strength was measured using a puncture tester (model CMT8102) produced by Meters Industrial Systems (China) Co., Ltd. The specimen clamp opening diameter was about 12 mm, the needle tip curvature radius was 0.5 mm, the temperature was 22-24°C, and the puncture speed was 5 mm / sec.

[0144] The tensile strength and elongation at break were tested on a tensile testing machine (model EM6.202) of MTS Industrial Systems (China) Co., Ltd. according to the national standard GB / T 16492-2008. The greater the elongation at break, the less likely the composite current collector is to be broken and the better the extensibility.

[0145] The test results of the base films provided by Examples 1 to 12 and Comparative Examples 1 to 4 are shown in Table 1:

[0146] Table 1

[0147]

[0148]

[0149] As can be seen from Table 1, it can be concluded from Comparative Examples 1-5, Examples 6-8 and Comparative Example 1 that the base film provided by the present invention is modified from the core layer or the surface layer. On the one hand, since a polyolefin copolymer elastomer (POE) is added to the raw material of one of the surface layer or the core layer, it not only has good compatibility with the polypropylene resin, but the α-olefin soft chain contained in the molecular structure can interact with the crystalline region of the polyethylene chain to form a physical cross-linked network. This physical cross-linked network can play a connecting and buffering role between the components, thereby enhancing the surface tension, mechanical strength, heat resistance and puncture strength of the base film.

[0150] Comparing Examples 1-4 and Comparative Examples 2-3, it can be seen that except for the different contents of PP and POE, the other compositions of Comparative Example 2, Examples 1-4 and Comparative Example 3 are the same. The various properties of the base film show a trend of first increasing and then decreasing, and the comprehensive performance of the base film provided by Example 3 is the best, which further shows that the present invention improves the modification effect of the base film by regulating the content of the polyolefin copolymer elastomer in the raw materials of any layer of the surface layer or the core layer.

[0151] By comparing Example 9 and Example 10, it can be seen that the base film provided by the present invention can also be applied to aluminum current collectors.

[0152] Comparing Example 11 with Example 12, the present invention further improves the comprehensive performance of the prepared base film by preferably adding other types of modified raw materials and additives to the raw materials due to the synergistic effect between the few-layer graphene and the single-walled carbon nanotubes.

[0153] By comparing Example 1 with Comparative Example 4, it can be seen that only adding inorganic filler components such as calcium carbonate to the core layer raw material cannot achieve all the technical effects of the present invention.

[0154] The test results of the composite current collectors provided in Examples 1 to 12 and Comparative Examples 1 to 4 are shown in Table 2:

[0155] Table 2

[0156]

[0157] As can be seen from Table 2, the comparison of Examples 1-5, Examples 6-8 and Comparative Example 1 shows that whether the modification is made from the core layer or the surface layer, the composite current collector finally prepared therefrom has excellent surface adhesion, conductivity, mechanical strength, heat resistance, high temperature resistance and corrosion resistance. In the composite current collector prepared by the present invention, the base film and the conductive metal layer are tightly bonded and the interface internal resistance is small. At the same time, the deposited conductive metal layer is evenly and densely distributed, and the stress between the conductive metal layers is small, thereby comprehensively improving the heat resistance, mechanical strength and conductivity of the composite current collector.

[0158] By comparing Examples 1-4 and Comparative Examples 2-3, it can be seen that since the various properties of the corresponding base films in Comparative Example 2, Examples 1-4, and Comparative Example 3 show a trend of first increasing and then decreasing, the various properties of the prepared composite current collector also show a trend of first increasing and then decreasing, and the composite current collector prepared in Example 3 has the best comprehensive performance, which further shows that the present invention has the best modification effect by regulating the base film, thereby further improving the comprehensive performance of the composite current collector.

[0159] By comparing Example 9 and Example 10, it can be seen that the aluminum current collector prepared by the base film provided by the present invention has good surface adhesion, conductivity, mechanical strength, heat resistance, high temperature resistance and corrosion resistance.

[0160] Comparing Example 11 with Example 12, the present invention further improves the comprehensive performance of the prepared base film by preferably adding other types of modified raw materials and additives to the raw materials, thereby comprehensively improving the overall performance of the prepared composite current collector.

[0161] By comparing Example 1 with Comparative Example 4, it can be seen that when only inorganic filler components such as calcium carbonate are added to the core layer raw material, the performance of the composite current collector obtained is poor.

[0162] The composite current collectors provided in Examples 1 to 12 and Comparative Examples 1 to 4 were assembled to obtain lithium-ion soft-pack batteries for testing. The testing method is as follows:

[0163] The battery internal resistance is tested using a battery internal resistance tester (model: Wuhan Guoshi, GSNR-1000).

[0164] The hot box test is to fully charge the single battery, put it into the temperature box, raise the temperature from room temperature to 150±2℃ at a rate of 5℃ / min, maintain this temperature for 30 minutes, then stop heating and observe for 1 hour.

[0165] The puncture test is to use a Φ3mm high-temperature resistant steel needle (the cone angle of the needle tip is 45-60°, the needle surface is smooth, free of rust, oxide layer and oil) to penetrate the battery plate at a speed of (25±5)mm / s from a direction perpendicular to the battery plate after the single battery is fully charged. The penetration position should be close to the geometric center of the punctured surface. The steel needle stays in the battery and is observed for 1h.

[0166] The specific test results are shown in Table 3:

[0167] Table 3

[0168]

[0169] As can be seen from Table 3, whether it is modified from the core layer or the surface layer, the composite current collector prepared from the final base film has excellent surface adhesion, conductivity, mechanical strength, heat resistance, high temperature resistance and corrosion resistance. Therefore, the assembled lithium-ion battery has a low internal resistance and does not catch fire under the 130°C test condition, which is consistent with the high-temperature test results of the composite current collector. The ignition time point under the 150°C test and the needle puncture test is also relatively delayed. The delay in the ignition time point fully demonstrates that the modification of the base film can comprehensively improve the safety of the composite current collector and the lithium-ion battery. It should be noted that the lithium-ion battery only caught fire but did not explode in the 150°C high temperature test and the needle puncture test.

[0170] The applicant declares that the present invention illustrates the process method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned process steps, that is, it does not mean that the present invention must rely on the above-mentioned process steps to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A composite current collector, characterized in that: The invention comprises a three-layer co-extruded microporous membrane and a conductive metal layer arranged on both sides of the three-layer co-extruded microporous membrane. The three-layer co-extruded microporous membrane comprises a core layer and surface layers respectively arranged on both sides of the core layer. The surface layers and the core layer are made of different materials. The material of one of the surface layers or the core layer comprises polypropylene resin, and the material of the other comprises a modified raw material. The modified raw material comprises polypropylene resin and a polyolefin copolymer elastomer.

2. The composite current collector according to claim 1, characterized in that: The polyolefin copolymer elastomer includes ethylene-octene copolymer elastomer; The molar percentage of α-octene structural units in the ethylene-octene copolymer elastomer is 15%-45%, preferably 20%-30%; The density of the ethylene-octene copolymer elastomer is 0.85 g / cm 3 -0.90g / cm 3 ; The melt index of the ethylene-octene copolymer elastomer at 230° C. and 2.16 kg is 1.0 g / 10.0 min to 10 g / 10.0 min, preferably 1.5 g / 10.0 min to 5.0 g / 10.0 min; The tear strength of the ethylene-octene copolymer elastomer is 20KN / m-150KN / m, preferably 30KN / m-100KN / m; The elongation at break of the ethylene-octene copolymer elastomer is 500%-3000%, preferably 1500%-2500%.

3. The composite current collector according to claim 1, characterized in that: Taking the total mass of the raw materials of the surface layer or the core layer as 100%, the modified raw materials include 80%-95% of polypropylene resin and 5%-20% of polyolefin copolymer elastomer; Preferably, based on the total mass of the raw materials of the surface layer or the core layer being 100%, the modified raw material further comprises 0%-2% of a dispersant, 0%-0.5% of a coupling agent and 0%-0.5% of a lubricant.

4. The composite current collector according to claim 1, characterized in that: The modified raw material further comprises any one or a combination of at least two of an inorganic filler, an epoxy resin and an acrylic resin; Based on the total mass of the modified raw material being 100%, the content of any one or a combination of at least two of the inorganic filler, epoxy resin and acrylic resin is 0%-5%; The inorganic filler includes any one of nano oxides, nano carbides, metal single substance materials and nano carbon materials or a combination of at least two thereof, preferably nano carbon materials.

5. The composite current collector according to claim 4, characterized in that: The nano-oxide comprises any one of silicon dioxide, titanium dioxide, boehmite, aluminum oxide and copper oxide, or a combination of at least two thereof, preferably at least one of silicon dioxide, boehmite or aluminum oxide; Preferably, the nanocarbide comprises tungsten carbide; Preferably, the metal single substance material comprises nano copper; Preferably, the nano-carbon material includes any one or a combination of at least two of graphene, conductive carbon black, carbon nanotubes, diamond, acetylene black, conductive fibers and carbon nanofibers, preferably graphene and / or carbon nanotubes.

6. The composite current collector according to claim 1, characterized in that: The thickness of the three-layer co-extruded microporous membrane is 2-10 μm; The porosity of the three-layer co-extruded microporous membrane is 30-50%, preferably 35-45%.

7. A method for preparing a composite current collector according to any one of claims 1 to 6, characterized in that: The method comprises the following steps: The modified raw material and the polypropylene resin are respectively put into different extruders, melt-extruded, and converged into the same hanger-shaped die to form a composite molten material; The composite melt is subjected to casting and cooling treatment, and then subjected to stretching treatment to form micropores to obtain a three-layer co-extruded microporous membrane; Conductive metal layers are arranged on both sides of the three-layer co-extruded microporous membrane to obtain the composite current collector.

8. The method according to claim 7, characterized in that The temperature of the melt extrusion is 200-250°C; The melt extrusion rate is 100-180m / min; The casting temperature is 200-240°C; The temperature of the cooling treatment is 60-80°C.

9. An electrode, characterized in that: The electrode comprises a current collector and an active material layer disposed on at least one side of the current collector, and the current collector comprises the composite current collector according to any one of claims 1 to 6.

10. A secondary battery, characterized in that: The secondary battery includes an electrode, an electrolyte, and a separator, and the electrode includes the electrode according to claim 9.

Citation Information

Cited By

  • BOPP (biaxially-oriented polypropylene) ultralow-temperature high-speed heat-sealing film and preparation method thereof

    CN120396471A

  • Composite current collector, manufacturing method therefor, battery and electrical apparatus

    WO2026148920A1