Preparation method of in-situ crosslinking type electric coupling flame-retardant polymer electrolyte and preparation method of sodium metal battery

Through the preparation of in-situ crosslinked electrically coupled flame retardant polymer electrolyte, the safety and energy density of liquid electrolytes in sodium ion batteries are solved, and solid electrolytes with high mechanical strength and high ionic conductivity are achieved, which improves sodium Cycle stability and safety of metal batteries.

CN118943499AActive Publication Date: 2024-11-12GUANGDONG UNIV OF TECH

Patent Information

Application Number
CN202410968015.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-12
Estimated Expiration
2044-07-18

AI Technical Summary

Technical Problem

The liquid electrolytes used in existing sodium ion batteries have problems such as leakage, volatile, flammable, toxicity, uneven deposition of sodium metal negative electrodes, and poor mechanical properties of SEI membranes, resulting in insufficient battery safety and energy density.

Method used

The preparation method of in-situ crosslinking electrically coupled flame retardant polymer electrolyte is adopted, and the mechanical strength and ionic conductivity of solid polymer electrolyte are improved through multi-site crosslinking reaction and the addition of flame retardant, and a three-dimensional crosslinking hyperbranched structure is designed. , reduce the crystallinity of electrolytes, promote sodium ion transport, and add flame retardants to the battery to improve safety.

Benefits of technology

Significantly inhibit the growth of sodium dendrites, improve the conductivity of sodium ion, reduce the internal impedance of the battery, enhance the safety of the battery, and improve the cycle stability and energy density of sodium metal batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943499A_ABST
    Figure CN118943499A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of an in-situ crosslinking type electric coupling flame-retardant polymer electrolyte and a preparation method of a sodium metal battery. The in-situ cross-linking type electric coupling flame-retardant polymer electrolyte can capture anions and improve the sodium ion conductivity, and has excellent flame retardance. The method provided by the invention has the following outstanding advantages: the flame retardance of the designed polymer electrolyte is greatly improved by adding the flame retardant triethyl phosphate; in addition, additives fluoroethylene carbonate and 4-trifluoromethylphenylboronic acid are added, construction of an SEI layer and a CEI layer is promoted in the cycle process, the cycle stability of the battery is improved, and boron atoms in TFPBA serve as Lewis acid centers to capture anions; in addition, the excellent mechanical property of the electrolyte can inhibit the growth of sodium negative electrode dendrites, and the safety performance of the battery is ensured. The electrochemical performance, the cycle life and the safety of the sodium metal battery are remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of new energy electrochemical materials, and more specifically, to a method for preparing an in-situ cross-linked electrically coupled flame-retardant polymer electrolyte and a method for preparing a sodium metal battery. Background Art

[0002] With the large-scale application of mobile electronic devices, electric vehicles and the rapid development of smart grid technology, large-scale energy storage technology will play an important role in the development of power systems and energy transformation. As an indispensable energy storage tool in people's lives, lithium-ion batteries have been widely used as energy storage devices, but the demand for batteries has increased year by year, which has caused people to worry about the scarcity of lithium resources. Sodium-ion batteries are considered to be an ideal alternative to lithium-ion batteries due to their low cost and abundant sodium reserves.

[0003] However, currently commercial lithium and sodium ion batteries most commonly use organic liquid electrolytes. Although liquid electrolytes have great advantages such as high ionic conductivity and good electrode interface wettability, they have serious problems in nature: while sodium metal anodes have shown significant advantages in improving battery energy density, sodium metal anodes based on traditional liquid electrolytes also face severe challenges: (1) Traditional liquid electrolytes, including carbonate and ether electrolytes, are prone to leakage, volatility, flammability and toxicity, and are prone to oxidative decomposition in high voltage areas. (2) During the sodium deposition process, the metal sodium anode does not deposit evenly and smoothly, but tends to form tree-like irregular sodium "dendrites", leading to serious battery safety problems. (3) The solid electrolyte interface (SEI) has poor mechanical properties and is easy to rupture. Dendrite growth leads to the rupture of the SEI film, and the exposed active Na continues to react with the electrolyte. (4) Sodium dendrites grow to a certain stage and break to produce "dead sodium". The dead sodium in the sodium metal battery increases continuously in the later stages of the cycle, and the electrode changes from a dense structure to a loose and porous structure, with a significant increase in volume, which seriously affects the transmission of sodium ions and the coulombic efficiency. (5) Severe volume expansion. Compared with the volume change of traditional intercalation-type negative electrode materials (such as hard carbon), the "host-free" nature of the sodium metal negative electrode leads to an unlimited volume change, which further leads to an uneven SEI film and aggravates the growth of sodium dendrites.

[0004] Application Contents

[0005] In order to overcome at least one problem existing in the prior art, the present application provides a method for preparing an in-situ cross-linked electrically coupled flame-retardant polymer electrolyte. The method for preparing an in-situ cross-linked electrically coupled flame-retardant polymer electrolyte in the present application can improve the mechanical strength and ionic conductivity of the solid polymer electrolyte, and the structure is highly controllable, and the structure-activity relationship between the structural unit and polymerization degree of the hyperbranched polymer electrolyte and the mechanical properties is studied, and an electrolyte with superior mechanical properties is flexibly designed to protect the sodium metal negative electrode, and a flame retardant is added to improve the battery safety performance, and a flexible and bendable energy storage device is constructed.

[0006] In order to solve the above technical problems, the technical solution adopted in this application is:

[0007] A method for preparing an in-situ cross-linked electrically coupled flame-retardant polymer electrolyte, characterized in that it comprises the following steps:

[0008] S1. A monomer containing multiple double bonds, wherein the monomer is a polymer, is dissolved in a solvent to obtain a uniform and transparent polymer solution;

[0009] S2. adding a flame retardant to the polymer solution obtained in S1 to obtain a preliminary composite solution;

[0010] S3. The composite solution obtained in S2 is then added with an appropriate amount of thermal polymerization initiator and additives fluoroethylene carbonate and 4-trifluoromethylphenylboric acid, and sodium salt is added and stirred at room temperature to obtain a uniform and transparent polymer solution;

[0011] S4. The polymer solution obtained in S3 was evenly coated on a polytetrafluoroethylene plate by in-situ polymerization and placed in an oven at 60°C to initiate thermal polymerization;

[0012] S5. Peeling the dried sample obtained in step S4 off the polytetrafluoroethylene substrate, and cutting it into round pieces with a diameter of 16 to 19 mm.

[0013] Compared with the prior art, the beneficial effects of this application are:

[0014] ①Multi-crosslinking site structural model, precisely control the degree of crosslinking in polymerization reaction, prepare high-strength polymer network, and inhibit the growth of sodium dendrites;

[0015] ② Design a three-dimensional cross-linked hyperbranched structure to break the orderly arrangement of the straight chain part in the polymer, reduce the crystallinity of the electrolyte, increase the swing of the polymer chain segment at room temperature, and promote the improvement of room temperature sodium ion conductivity;

[0016] ③ The in-situ polymerization strategy can significantly reduce the interfacial impedance between the polymer electrolyte and the positive and negative electrodes, and reduce the internal resistance of the battery;

[0017] ④ Utilize the electrically coupled anion capture effect to capture anions, promote the dissolution of sodium salts, and improve the ionic conductivity of sodium ions;

[0018] ⑤ The sodium ion transmission path inside the solid polymer electrolyte is uniform and dense, which promotes the uniform deposition of sodium metal and effectively inhibits the growth of sodium dendrites;

[0019] ⑥ Flame retardants are added to solid polymer electrolytes to improve the flame retardancy of polymer electrolytes and increase the safety of battery use. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a physical picture of the polymer electrolyte prepared in Example 1.

[0021] Figure 2 Electron microscopy and elemental energy spectrum of the polymer electrolyte prepared in Example 2.

[0022] Figure 3 This is an open flame combustion test of the polymer electrolyte prepared in Example 1.

[0023] Figure 4 Arrhenius plots of the polymer electrolytes prepared in Examples 1 and 2.

[0024] Figure 5 This is the electrochemical stability window of the polymer electrolyte prepared in Example 1.

[0025] Figure 6 is the sodium ion transference number of the polymer electrolyte prepared in Example 1.

[0026] Figure 7 The rate performance diagram of the sodium metal battery assembled with the polymer electrolyte prepared in Example 1 and Example 2.

[0027] Figure 8 Cycling performance diagram of sodium metal batteries assembled with polymer electrolytes prepared in Examples 1 and 3.

[0028] Fig. 9 High load cycle performance diagram of the sodium metal battery assembled with the polymer electrolyte prepared in Example 1. DETAILED DESCRIPTION

[0029] The embodiments of the present application will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If specific conditions are not specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0030] It should be noted that:

[0031] In this application, unless otherwise specified, all the embodiments and preferred implementation methods mentioned herein can be combined with each other to form a new technical solution.

[0032] In the present application, unless otherwise specified, each reaction or operation step can be carried out sequentially or in a sequential manner. Preferably, the reaction method herein is carried out sequentially.

[0033] Unless otherwise specified, the professional and scientific terms used herein are the same as those familiar to those skilled in the art. In addition, any method or material similar or equivalent to the described content can also be applied to this application.

[0034] As the next generation of high energy density mainstream technology solution, all-solid-state sodium metal batteries have attracted extensive attention from researchers. They are expected to fundamentally solve the inherent shortcomings of liquid electrolytes. Their high mechanical properties can inhibit dendrite growth and can be adapted to sodium metal negative electrodes to build all-solid-state sodium metal batteries with higher energy density. Solid electrolytes mainly include inorganic solid electrolytes and organic polymer electrolytes. Each has obvious advantages and disadvantages: 1) Inorganic solid electrolytes (such as oxide and sulfide solid electrolytes) have high ionic conductivity and thermal stability, but face severe mechanical brittleness and high solid / solid interface impedance of electrolyte / electrode, which hinders the transmission of sodium ions at the interface; 2) Polymer solid electrolytes are composed of organic polymer matrix and sodium salt. Polymer electrolytes have excellent flexibility and interface compatibility, low electrolyte / electrode interface impedance, can uniformly transmit sodium ions, have good electrode interface compatibility and other advantages, are easy to process devices, and have great application prospects in flexible wearable devices, becoming a research hotspot in recent years. However, they also face problems such as low room temperature ionic conductivity, poor mechanical strength, narrow electrochemical window and flammability.

[0035] On the one hand, the present application provides a method for preparing an in-situ cross-linked electrically coupled flame-retardant polymer electrolyte, characterized in that it comprises the following steps:

[0036] S1. A monomer containing multiple double bonds, wherein the monomer is a polymer, is dissolved in a solvent to obtain a uniform and transparent polymer solution;

[0037] S2. adding a flame retardant to the polymer solution obtained in S1 to obtain a preliminary composite solution;

[0038] S3. The composite solution obtained in S2 is then added with an appropriate amount of thermal polymerization initiator and additives fluoroethylene carbonate and 4-trifluoromethylphenylboric acid, and sodium salt is added and stirred at room temperature to obtain a uniform and transparent polymer solution;

[0039] S4. The polymer solution obtained in S3 was added with sodium salt, and in-situ polymerization was used to evenly coat the polymer on a polytetrafluoroethylene plate and placed in an oven at 60 ° C to initiate thermal polymerization;

[0040] S5. Peeling the dried sample obtained in step S4 off the polytetrafluoroethylene substrate, and cutting it into round pieces with a diameter of 16 to 19 mm.

[0041] The preparation method of the in-situ cross-linked electrically coupled flame-retardant polymer electrolyte of the present application prepares a polymer with a hyperbranched structural unit by introducing a method of multi-site cross-linking reaction nodes to simultaneously improve the mechanical strength and ionic conductivity of the solid polymer electrolyte. The structure is highly controllable, and the structure-activity relationship between the structural unit and degree of polymerization of the hyperbranched polymer electrolyte and the mechanical properties is studied, and an electrolyte with superior mechanical properties is flexibly designed to protect the sodium metal negative electrode. In addition, a flame retardant is added to improve the battery safety performance and construct a flexible and bendable energy storage device. It can be matched with a high specific capacity sodium metal negative electrode and a sodium alum phosphate positive electrode to suppress the dissolution of transition metal ions in the positive electrode, continuous voltage decay, and oxygen release during the cycle, thereby improving the cycle stability and safety of the solid-state sodium metal battery.

[0042] In some preferred embodiments, in step S1, the high molecular polymer skeleton is a mixture of one or two of polyethylene glycol diacrylate, N,N-methylenebisacrylamide, tetrapentaerythritol tetraacrylate, trimethylolpropane triacrylate and triallylamine, and the ratio of the two polymers in the mixture is 1:1 to 1:4.

[0043] In some preferred embodiments, in step S2, the flame retardant may be selected from one of trimethyl phosphate, triethyl phosphate, triphenyl phosphate and toluene diphenyl phosphate, and the mass ratio of the high molecular polymer to the flame retardant is 1:0.2 to 1:3.

[0044] In some preferred embodiments, in step S3, the thermal polymerization initiator is AIBN, and additives such as fluoroethylene carbonate and 4-trifluoromethylphenylboric acid are added, the mass ratio of the additives to the high molecular polymer in step S1 is 1:0.002 to 1:0.05, and the stirring time at room temperature is 30 to 60 minutes.

[0045] In some preferred embodiments, in step S3, the sodium salt used can be selected from one or more of sodium bis(trifluoromethylsulfonyl)imide, sodium perchlorate, sodium bis(trifluoromethylsulfonyl)imide, and sodium perchlorate.

[0046] On the other hand, the present application provides a method for preparing a sodium metal battery, characterized in that: the sodium metal battery is prepared by directly assembling the polymer solution obtained in step S3 as claimed in claim 1 with a metal sodium sheet, a glass fiber separator, and a positive electrode, and then placing the polymer solution in an oven at 60° C. for 12 hours to initiate thermal polymerization.

[0047] In some preferred embodiments, in the above-mentioned method for preparing a nanometal battery, the weight percentage content of sodium salt in the obtained polymer electrolyte (sodium salt / polymer film) is controlled at 5 to 50 wt %.

[0048] In some preferred embodiments, in the above-mentioned method for preparing the nano-metal battery, the assembled sodium metal battery positive electrode material is sodium alum phosphate or sodium nickel iron manganese oxide.

[0049] In some more preferred embodiments, the mass percentage of the active material in the entire electrode is 80 wt% to 95 wt%, and the loading per unit area is 3 to 8 mg cm -2 .

[0050] In some more preferred embodiments, no additional liquid or electrolyte needs to be added when assembling the battery.

[0051] The sodium metal battery prepared by the above preparation method in this application has the following characteristics:

[0052] First, through the in-situ polymerization strategy, the interface impedance between the polymer electrolyte and the positive and negative electrodes can be significantly reduced, thereby reducing the internal resistance of the battery.

[0053] Secondly, the electrically coupled anion capture effect is used to capture anions, promote the dissolution of sodium salts, and improve the ionic conductivity of sodium ions;

[0054] Secondly, the sodium ion transmission path inside the solid polymer electrolyte is uniform and dense, which promotes the uniform deposition of sodium metal and effectively inhibits the growth of sodium dendrites;

[0055] Finally, flame retardants are added to the solid polymer electrolyte to improve the flame retardancy of the polymer electrolyte and increase the safety of battery use.

[0056] Next, the preparation method of the in-situ cross-linked electrically coupled flame-retardant polymer electrolyte and the preparation method of the nanometal electromagnetic of the present application are described in detail with specific examples.

[0057] Example 1 Preparation of in-situ cross-linked electrically coupled flame-retardant polymer electrolyte

[0058] S1. Mix 0.35 g of polyethylene glycol diacrylate (PEGDA) and 0.15 g of trimethylolpropane triacrylate (TMPTA) and stir for 30 min to obtain a clear and transparent solution.

[0059] S2. Add 25 mg of initiator azobisisobutyronitrile (AIBN) to the above solution, dissolve at room temperature, and stir for 30 min;

[0060] S3. Introduce 0.1 g of additives fluoroethylene carbonate (FEC) and 0.004 g of 4-trifluoromethylphenylboronic acid (TFPBA) into the above polymer solution and continue stirring at room temperature for 1 h.

[0061] S4. Weigh 0.42 g of sodium bis(trifluoromethylsulfonyl)imide (NaTFSI) and dissolve it in 1.5 g of triethyl phosphate (TEP), add it to the solution obtained in step S3, and continue stirring for 30 min to obtain a clear and transparent solution.

[0062] S5. Assemble the sodium metal battery with the above polymer solution directly and sodium metal sheet, glass fiber separator and sodium alum phosphate positive electrode, put it into an oven at 60°C for thermal initiation polymerization for 12 hours, take it out of the oven, cool it down and test its electrochemical performance.

[0063] Example 2

[0064] Example 2 is the comparative example 1 of preparing the in-situ cross-linked flame-retardant polymer electrolyte in the present application. Compared with Example 1, this comparative example omits step S3, that is, the additives fluoroethylene carbonate (FEC) and 4-trifluoromethylphenylboronic acid (TFPBA) are not added to the solution obtained after step S2.

[0065] S1. Mix 0.35 g of polyethylene glycol diacrylate (PEGDA) and 0.15 g of trimethylolpropane triacrylate (TMPTA) and stir for 30 min to obtain a clear and transparent solution.

[0066] S2. Add 25 mg of initiator azobisisobutyronitrile (AIBN) to the above solution, dissolve at room temperature, and stir for 30 min;

[0067] S4. Weigh 0.42 g of sodium bis(trifluoromethylsulfonyl)imide (NaTFSI) and dissolve it in 1.5 g of triethyl phosphate (TEP), add it to the solution obtained after step S2, and continue stirring for 30 min to obtain a clear and transparent solution.

[0068] S5 directly assembles a sodium metal battery with the above polymer solution and a sodium metal sheet, a glass fiber separator, and a sodium alum phosphate positive electrode, and puts it into an oven at 60°C for thermal initiation of polymerization for 12 hours. After taking it out of the oven and cooling it, test its electrochemical performance.

[0069] Example 3

[0070] Example 3 is comparative example 2 of the preparation of in-situ cross-linked flame-retardant polymer electrolyte in the present application. Compared with Example 1, Example 3 does not add flame retardant TEP, but only adds electrolyte to the polymer.

[0071] S1. Mix 0.35 g of polyethylene glycol diacrylate (PEGDA) and 0.15 g of trimethylolpropane triacrylate (TMPTA) and stir for 30 min to obtain a clear and transparent solution.

[0072] S2. Add 25 mg of initiator azobisisobutyronitrile (AIBN) to the solution obtained after step S1, dissolve at room temperature, and stir for 30 min;

[0073] S3'. Introduce 1.5 g of 1.0 M NaPF6 in EC:DMC=1:1 Vol% with 5.0% FEC electrolyte into the polymer solution obtained after step S2, add it to the solution in the above step, and continue stirring for 30 minutes to obtain a clear and transparent solution.

[0074] S4'. The polymer solution obtained after step S3' is directly assembled with a sodium metal sheet, a glass fiber separator, and a sodium alum phosphate positive electrode into a sodium metal battery, and placed in a 60°C oven for thermal polymerization for 12 hours. After being removed from the oven and cooled, its electrochemical properties are tested.

[0075] Performance Characterization

[0076] The applicant also performed corresponding characterization on the performance of the polymer electrolytes prepared in Examples 1, 2 and 3 and the sodium metal batteries assembled with the polymer electrolytes prepared in the above three Examples. The characterization results are as follows:

[0077] The cross-linked electrically coupled flame-retardant polymer electrolyte and the cross-linked flame-retardant polymer electrolyte obtained in step S4 have an optical image as shown in Figure 1 As shown. Figure 1 It can be seen that the cross-linked electrically coupled flame-retardant polymer electrolyte can maintain its original morphology after folding and pulling, indicating that the cross-linked polymer electrolyte has excellent mechanical properties.

[0078] SEM image of cross-linked electrically coupled flame-retardant polymer electrolyte Figure 2 As shown. Figure 2 It can be seen that the electrolyte can penetrate into the glass fiber membrane and polymerize, and the Na, P, and F elements are distributed in the electrolyte.

[0079] The present application conducts an ignition test on the cross-linked electrically coupled flame-retardant polymer electrolyte prepared in step S4. The test results are as follows: Figure 3As shown in the figure, the cross-linked electrically coupled flame-retardant polymer electrolyte was not ignited after being exposed to an open flame for 5 seconds, which proves that the cross-linked electrically coupled flame-retardant polymer electrolyte has excellent flame retardancy.

[0080] By testing the ionic conductivity of the cross-linked electrically coupled flame-retardant polymer electrolyte prepared in this example at different temperatures, the following results are obtained: Figure 4 The Arrhenius diagram shown. Figure 4 It can be seen that the activation energies of ion migration in Example 1 and Example 2 are 0.1535 eV and 0.1941 eV, respectively, proving that the sodium ions in the cross-linked electrically coupled flame-retardant polymer electrolyte prepared in Example 1 have a high degree of freedom and a low migration energy barrier.

[0081] The cross-linked electrically coupled flame-retardant polymer electrolyte of Example 1 was subjected to LSV test. Figure 5 As shown. Figure 5 It can be seen that the electrochemical window of the cross-linked electrically coupled flame-retardant polymer electrolyte reaches 4.8 V. This shows that the electrolyte formed by the cross-linked network has higher electrochemical stability.

[0082] Figure 6 Chronoamperometric tests were performed for cross-linked electrically coupled flame-retardant polymer electrolytes. Figure 6 It can be seen that the sodium ion migration number of the cross-linked electrically coupled flame-retardant polymer electrolyte prepared in this application is as high as 0.51, indicating that TFPBA is added to the cross-linked electrically coupled flame-retardant polymer electrolyte prepared in this application, which captures anions, promotes the dissociation of sodium salts and selectively transports sodium ions. In addition, the cross-linked polymer can provide more sodium ion transmission channels, further improving the electrolyte's ability to transport sodium ions.

[0083] Button sodium ion batteries (the batteries assembled in Example 1 and Example 2) were assembled in an argon atmosphere glove box for testing. The test conditions were: the charge and discharge cut-off voltage was 2.5V to 3.8V, the charge and discharge current density was 0.1C, 0.3C, 0.5C, 1C, 0.1C (1C = 117.6 mA / g), and the rate charge and discharge diagram obtained by the test was shown in Figure 7 .like Figure 7 As shown, Example 1 exhibits specific capacities of 113.5 mAh / g, 113.9 mAh / g, 113.3 mAh / g, 112.3 mAh / g, 111.0 mAh / g, and 111.5 mAh / g, and Example 2 exhibits specific capacities of 107.0 mAh / g, 102.3 mAh / g, 98.2 mAh / g, 89.8 mAh / g, 55.7 mAh / g, and 102.6 mAh / g, respectively. This indicates that the cross-linked electrically coupled flame-retardant polymer electrolyte prepared in Example 1 has good cycle performance.

[0084] The cycle performance of the cross-linked electrically coupled flame-retardant polymer electrolyte prepared in this application is shown in the figure Figure 8 As shown. Figure 8 It can be seen that the charge and discharge current density of the cross-linked electrically coupled flame-retardant polymer electrolyte prepared in this application is 2C (1C = 117.6 mA / g). The composite material prepared in this embodiment showed a capacity retention rate of 94.28% and good cycle stability after 2200 cycles. This shows that the prepared cross-linked electrically coupled flame-retardant polymer electrolyte has excellent electrochemical properties, and good mechanical properties can inhibit the growth of sodium dendrites and adapt to the volume change of the electrode during the charge and discharge process.

[0085] The cross-linked electrically coupled flame-retardant polymer electrolyte prepared in this application has good performance under high positive electrode loading (8-10 mg / cm 2 )'s charge-discharge cycle diagram is shown in Fig. 9 As shown by Fig. 9 It can be seen that the electrolyte prepared in this example still has good cycle performance under the condition of 0.5C (1C=117.6mA / g).

[0086] In summary, the present application provides, on one hand, a method for preparing an in-situ cross-linked electrically coupled flame-retardant polymer electrolyte, comprising the following steps:

[0087] S1. A monomer containing multiple double bonds, wherein the monomer is a polymer, is dissolved in a solvent to obtain a uniform and transparent polymer solution;

[0088] S2. adding a flame retardant to the polymer solution obtained in S1 to obtain a preliminary composite solution;

[0089] S3. The composite solution obtained in S2 is then added with an appropriate amount of a thermal polymerization initiator and a plasticizer, fluoroethylene carbonate and 4-trifluoromethylphenylboric acid, and stirred at room temperature to obtain a uniform and transparent polymer solution;

[0090] S4. The polymer solution obtained in S3 was added with sodium salt, and in-situ polymerization was used to evenly coat the polymer on a polytetrafluoroethylene plate and placed in an oven at 60 ° C to initiate thermal polymerization;

[0091] S5. Peeling the dried sample obtained in step S4 off the polytetrafluoroethylene substrate, and cutting it into round pieces with a diameter of 16 to 19 mm.

[0092] On the other hand, the present application also provides a method for preparing a sodium metal battery: the polymer solution obtained in the above step S3 is directly assembled with a metal sodium sheet, a glass fiber separator, and a positive electrode, and then placed in an oven at 60° C. for thermal initiation polymerization for 12 hours to prepare the sodium metal battery.

[0093] The present application provides a method for preparing a polymer with a hyperbranched structural unit by introducing a multi-site cross-linking reaction node to simultaneously improve the mechanical strength and ionic conductivity of a solid polymer electrolyte. The structure is highly controllable, and the structure-activity relationship between the structural unit and degree of polymerization of the hyperbranched polymer electrolyte and the mechanical properties is studied, and an electrolyte with superior mechanical properties is flexibly designed to protect the sodium metal negative electrode. In addition, a flame retardant is added to improve the battery safety performance and construct a flexible and bendable energy storage device. It can be matched with a high specific capacity sodium metal negative electrode and a sodium alum phosphate positive electrode to suppress the dissolution of transition metal ions in the positive electrode, continuous voltage decay, and oxygen release during the cycle, thereby improving the cycle stability and safety of solid-state sodium metal batteries.

[0094] The method provided in this application has the following outstanding advantages: the designed polymer electrolyte greatly improves the flame retardancy of the polymer electrolyte by adding the flame retardant triethyl phosphate; by adding additives fluoroethylene carbonate and 4-trifluoromethylphenylboric acid, the SEI layer and CEI layer are promoted to be constructed during the cycle process, the battery cycle stability is improved, and the boron atoms in TFPBA capture anions as Lewis acid centers; in addition, the excellent mechanical properties of the electrolyte can inhibit the growth of sodium negative electrode dendrites and ensure the safety performance of the battery. This application significantly improves the electrochemical performance, cycle life and safety of sodium metal batteries.

[0095] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials, or characteristics described in conjunction with the embodiments or examples are included in at least one embodiment or example of the present application. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials, or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.

[0096] Although several embodiments of the present application have been shown and described, those skilled in the art will appreciate that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present application, and that the scope of the present application is defined by the claims and their equivalents.

Claims

1. A method for preparing an in-situ cross-linked electrically coupled flame-retardant polymer electrolyte, characterized in that: The following steps are involved: S1. A monomer containing multiple double bonds, wherein the monomer is a polymer, is dissolved in a solvent to obtain a uniform and transparent polymer solution; S2. adding a flame retardant to the polymer solution obtained in S1 to obtain a preliminary composite solution; S3. The composite solution obtained in S2 is then added with a thermal polymerization initiator and additives fluoroethylene carbonate and 4-trifluoromethylphenylboric acid, and sodium salt is added, and stirred at room temperature to obtain a uniform and transparent polymer precursor solution; S4. The polymer precursor solution obtained in S3 is evenly coated on a polytetrafluoroethylene plate by in-situ polymerization and placed in a 60°C oven to initiate thermal polymerization; S5. Peeling the dried sample obtained in step S4 off the polytetrafluoroethylene substrate, and cutting it into round pieces with a diameter of 16 to 19 mm.

2. The method for preparing the in-situ cross-linked electrically coupled flame-retardant polymer electrolyte according to claim 1, characterized in that: In step S1, the polymer skeleton is a mixture of one or two of polyethylene glycol diacrylate, N,N-methylenebisacrylamide, tetrapentaerythritol tetraacrylate, trimethylolpropane triacrylate and triallylamine, and the ratio of the two polymers in the mixture is 1:1 to 1:

4.

3. The method for preparing the in-situ cross-linked electrically coupled flame-retardant polymer electrolyte according to claim 1, characterized in that: In step S2, the flame retardant may be selected from one of trimethyl phosphate, triethyl phosphate, triphenyl phosphate and toluene diphenyl phosphate, and the mass ratio of the high molecular polymer to the flame retardant is 1:0.2 to 1:

3.

4. The method for preparing the in-situ cross-linked electrically coupled flame-retardant polymer electrolyte according to claim 1, characterized in that: In step S3, the thermal polymerization initiator is azobisisobutyronitrile, the mass ratio of the additive to the high molecular polymer in step S1 is 1:0.002 to 1:0.05, and the stirring time at room temperature is 30 to 60 minutes.

5. The method for preparing the in-situ cross-linked electrically coupled flame-retardant polymer electrolyte according to claim 1, characterized in that: In step S3, the sodium salt used can be selected from one or more of sodium bis(trifluoromethylsulfonyl)imide, sodium perchlorate, sodium bis(trifluoromethylsulfonyl)imide, and sodium perchlorate.

6. A method for preparing a sodium metal battery, characterized in that: The sodium metal battery is prepared by directly assembling the polymer solution obtained in step S3 of claim 1 with a metal sodium sheet, a glass fiber separator, and a positive electrode, and then placing the polymer solution in an oven at 60° C. for 12 hours to initiate thermal polymerization.

7. The method for preparing a sodium metal battery according to claim 6, characterized in that: The weight percentage content of sodium salt in the obtained polymer electrolyte is 5-50wt%.

8. The method for preparing a sodium metal battery according to claim 6, characterized in that: The assembled sodium metal battery positive electrode material is sodium alum phosphate or sodium nickel iron manganese oxide.

9. The method for preparing a sodium metal battery according to claim 8, characterized in that: The mass percentage of active material in the whole electrode is 80wt% to 95wt%, and the loading per unit area is 3 to 10mg / cm 2 .

10. The method for preparing a sodium metal battery according to claim 9, characterized in that: No additional liquid or electrolyte needs to be added when assembling the battery.

Citation Information

Patent Citations

  • Polymer electrolyte prepared by in-situ thermal initiation and all-solid sodium ion battery

    CN110459802A

  • Polymerized organic-inorganic composite solid electrolyte and in-situ assembled all-solid-state battery

    CN110556586A

  • Polymer solid electrolyte containing soluble additive and all-solid-state metal lithium battery

    CN115020831A

  • In-situ preparation and application of solid polymer electrolyte

    WO2023109659A1

Cited By

  • Flame-retardant polyester solid electrolyte membrane and preparation method thereof

    CN122494800A

  • Flame-retardant polyester solid electrolyte membrane and preparation method thereof

    CN122494800B