Nano Pt-MBene positive electrode catalyst for lithium carbon dioxide battery and preparation method of nano Pt-MBene positive electrode catalyst

Through Pt-MBene nanocomposite materials as catalysts, the high cost and low cycle performance problems of the cathode catalyst of lithium carbon dioxide batteries are solved, and efficient lithium carbonate decomposition and electrochemical performance improvement are achieved.

CN118919749APending Publication Date: 2024-11-08BEIJING UNIV OF CHEM TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411236482.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The cathode catalysts of lithium carbon dioxide batteries have problems of high cost and low cycle performance, and it is difficult to effectively decompose lithium carbonate, which limits the practical application of the battery.

Method used

Using Pt-MBene nanocomposite as catalyst, nano Pt-MBene composite material is formed by ultrasonic mixing and stirring of molybdenum-based MBene powder with K2PtCl6 solution, retaining the slab structure of MBene and growing Pt particles on its surface to increase catalytic activity. loci.

Benefits of technology

The cycling performance and electrochemical kinetic performance of lithium carbon dioxide batteries are significantly improved, the overpotential is reduced, and the energy conversion efficiency is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919749A_ABST
    Figure CN118919749A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of electrochemistry and new energy, and relates to a lithium carbon dioxide battery positive electrode catalyst and a preparation method thereof, and the catalyst is a Pt-MBene nano composite material. The preparation process of the material is simple and efficient, special experimental equipment is not needed, and the prepared Pt-MBene nano composite material has excellent conductivity and excellent capability of catalyzing decomposition of discharge products, shows low overpotential and excellent cycling stability when being used as a positive electrode catalyst for a lithium carbon dioxide battery, and can be applied to the lithium carbon dioxide battery. And the possibility is provided for industrial production and practical application of the lithium carbon dioxide battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of electrochemistry and new energy technology, and relates to a method for preparing a Pt-MBene nanocomposite material, and application of a catalyst material prepared by the method as a positive electrode catalyst for a lithium carbon dioxide battery. Background Art

[0002] In the past few decades, the use of non-renewable resources such as oil and coal has promoted the booming global economy, but the rapid consumption of natural resources has caused these non-renewable energy sources to be quickly depleted, and the series of environmental problems caused by burning these energy sources are far beyond human imagination. It is predicted that according to the current consumption rate, fossil fuels will be completely exhausted by 2050. In order to achieve the "dual carbon" goal and solve problems such as global warming, the scientific community is committed to reducing carbon dioxide emissions and converting them into valuable chemical raw materials through capture and conversion. Simple and environmentally friendly energy storage technologies such as electrochemical reduction of carbon dioxide provide a potential sustainable method for reducing carbon dioxide emissions. It can not only effectively reduce the carbon dioxide content in the atmosphere, but also convert carbon dioxide into fuels or chemicals to achieve energy storage. Therefore, this technology has shown great application prospects in industrial production and daily life. It can not only store surplus electricity from fossil fuels, but also achieve a balance between electricity supply and carbon cycle. High-energy-density lithium carbon dioxide batteries have attracted much attention due to their "one stone two birds" characteristics in fixing greenhouse gas carbon dioxide and providing electrochemical energy storage. The working process of lithium carbon dioxide batteries is reversible, including carbon dioxide reduction reaction and carbon dioxide evolution reaction. These reactions occur through 4-electron transfer reactions, which can be expressed as . However, the discharge product lithium carbonate is a wide bandgap insulator with high thermodynamic stability and slow reaction kinetics, which leads to excessive potential and poor reversibility, and the accumulation of solid lithium carbonate on the positive electrode surface will cause the electrochemical performance of the battery to decline until the lithium carbon dioxide battery fails, which seriously limits the practical application of lithium carbon dioxide batteries. Therefore, it is urgent to design an efficient and stable positive electrode catalyst to promote the uniform nucleation and decomposition of lithium carbonate, thereby improving the electrochemical performance of lithium carbon dioxide batteries. At present, commonly used lithium carbon dioxide battery catalysts are mainly precious metals and carbon-based materials. The cost of precious metal catalysts is very high, which is not conducive to practical application, and although carbon-based materials are relatively low in price, when used as lithium carbon dioxide battery positive electrode catalysts, lithium carbonate cannot be effectively decomposed, and its cycle performance, rate capability and efficiency are still very limited. Therefore, finding a suitable positive electrode catalyst to reduce electrochemical polarization and improve energy conversion efficiency is one of the technical problems to be solved in the field of lithium carbon dioxide batteries. Summary of the invention

[0003] The technical problem to be solved by the present invention is: to design a simple and efficient positive electrode catalyst for lithium carbon dioxide batteries. In view of the above technical problems, the present invention provides a Pt-MBene high-efficiency catalyst. After the molybdenum-based MBene and the K2PtCl6 solution are uniformly mixed and stirred for 24 hours, the Pt-MBene composite material can be obtained after centrifugal washing. The preparation process of the present invention is simple and has great practical application prospects. The obtained nano Pt-MBene heterogeneous composite material retains the lamellar structure of MBene, and Pt particles are uniformly grown on the surface of MBene. The in-situ generated Pt particles can not only prevent the collapse and stacking of MBene layers, but also increase the catalytic active sites. Thanks to the reasonable morphology and structure, the heterogeneous composite material shows excellent cycle performance and ultra-low overpotential when used as a positive electrode catalyst for lithium carbon dioxide batteries.

[0004] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0005] The present invention provides a Pt-MBene cathode catalyst and a method for preparing an electrode sheet used in a lithium carbon dioxide battery, comprising the following steps:

[0006] (1) Mo-based MBene powder and K2PtCl6 solution are ultrasonically mixed in a certain mass ratio to achieve uniform mixing.

[0007] (2) The mixture of the molybdenum-based MBene powder and the K2PtCl6 solution in step (1) was placed on a stirring table and stirred for 24 hours to obtain a Pt-MBene composite material.

[0008] (3) The Pt-MBene composite material obtained in step (2) is prepared into pole pieces and assembled into batteries, and electrochemical tests are performed in a CO2-filled atmosphere.

[0009] Optionally, the molybdenum-based MBene in step (1) includes Mo2B2MBene containing transition metal molybdenum, MoAl 1-x BMBene, Mo2AlB2 MBene, i-MBene: Mo 1.33 Y 0.67 A mixture of one or more MBene materials such as B2.

[0010] Optionally, in step (1), the mass ratio of the molybdenum-based MBene powder to the K2PtCl6 solution is 100:1 to 100:50.

[0011] Optionally, in step (1), the ultrasonic time of MBene powder and K2PtCl6 solution is 10 min to 120 min.

[0012] Optionally, in step (1), the ultrasonic power of the MBene powder and the K2PtCl6 solution is 100W to 600W.

[0013] Optionally, the type of atmosphere in step (3) can be selected as 100% CO2 or a mixed gas of CO2 and O2, Ar, N2, etc.

[0014] The present invention also provides the use of the Pt-MBene composite material described in the above technical solution as a positive electrode catalyst for a lithium carbon dioxide battery.

[0015] The present invention provides a Pt-MBene cathode catalyst material and a preparation method thereof, which has the following characteristics:

[0016] Beneficial effects:

[0017] (1) In the method of the present invention, MBene powder and K2PtCl6 solution are ultrasonicated in an ultrasonic machine for 30 minutes to allow the two to fully contact, so that Pt 4+ The electronic state of the Pt-B interaction is formed with B with low electronegativity in MBene, thus giving the Pt particles a valence state close to zero, which can improve the cycling performance of the material and increase the active reaction sites.

[0018] (2) In the ultrasonic stirring reduction, the reduction degree of Pt particles can be controlled by controlling the ratio of MBene powder to K2PtCl6 solution, ultrasonic time and stirring time. In this technical solution, the two-dimensional layer structure of MBene is preferably retained as the conductive framework of the composite material, which is conducive to electron transmission, thereby ensuring that the composite material has excellent conductivity.

[0019] (3) In addition, the Pt particles grown in situ on the MBene surface can not only prevent the MBene sheets from collapsing and stacking, but also increase the catalytic active sites and improve the catalytic performance of the composite material. In addition, there is electron transfer at the heterogeneous interface between MBene and Pt, which can form a built-in electric field, accelerate electron transport, and improve electrochemical kinetic performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0021] Figure 1 The X-ray diffraction pattern (XRD) of the Pt-MBene material prepared in Example 1 of the present invention;

[0022] Figure 2 This is a scanning electron microscope (SEM) image of the Pt-MBene material prepared in Example 1 of the present invention;

[0023] Figure 3 The Pt-MBene material prepared in Example 1 of the present invention is 0.2A g -1 The first discharge curve diagram below;

[0024] Figure 4 The Pt-MBene material prepared in Example 1 of the present invention is 0.2A g -1 Cycle performance under

[0025] Figure 5 The rate performance of the Pt-MBene material prepared in Example 1 of the present invention;

[0026] Figure 6 The Mo2B2 MBene material prepared in Comparative Example 1 of the present invention is 0.2A g -1 The cycle performance curve diagram below;

[0027] Figure 7 0.2A g of Mo2B2 MBene material prepared in Comparative Example 1 of the present invention -1 The first discharge curve diagram below;

[0028] Figure 8 This is the X-ray diffraction pattern (XRD) of the Pt-Mo2AlB2 material prepared in Example 2 of the present invention. DETAILED DESCRIPTION

[0029] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] Example 1

[0031] (1) Weigh 200 mg Mo2B2 MBene and 200 ul (10 mg ml -1 )Put the K2PtCl6 solution in a vial and mix it evenly under ultrasonication for 30 min.

[0032] (2) The mixture was transferred to a stirring platform and stirred at room temperature for 24 h to obtain a Pt-MBene heterogeneous composite material.

[0033] (3) The above materials were mixed in a mass ratio of active material: conductive carbon black: PVDF = 8:1:1, and then NMP solvent was added to prepare a slurry after stirring and homogenization. A certain volume of the slurry was drawn with a pipette and coated on a circular carbon paper with a diameter of 8 mm, and then placed in a vacuum oven for drying to prepare an electrode sheet.

[0034] The X-ray diffraction (XRD) pattern of Pt-MBene heterogeneous composites is shown in Figure 1 As shown, it exhibits the characteristic peaks of Pt element and Mo2B2MBene, indicating the successful preparation of the composite material. Figure 2 This is a scanning electron microscope (SEM) image of the Pt-MBene material prepared in Example 1 of the present invention, in which the layered structure of MXene is retained as a conductive matrix, and more stable Pt particles and clusters are grown in situ on its surface, which improves the stability of the composite material and increases the catalytic active sites. The electrode sheet in step (3) is used as the positive electrode, glass fiber is used as the separator, 1 mol / L LiTFSI DMSO system is used as the electrolyte, and lithium foil is used as the counter electrode. A button half-cell is assembled using a special perforated battery shell, and the battery is placed in a test tank filled with carbon dioxide gas for electrochemical testing.

[0035] The battery assembled in the corresponding use case 1 was tested for charge and discharge performance. The test conditions were: the charge and discharge mode was constant current charge and discharge; the current density was 0.2A g -1 ; The discharge cut-off voltage is 2.0V; The first constant current discharge curve of the battery assembled in Application Example 1 is as follows Figure 3 As shown. Figure 3 It can be seen that the first discharge capacity of the battery assembled in Application Example 1 is as high as 26049 mAhg -1 Compared with the Mo2B2 MBene material heterogeneous composite material in Comparative Example 1, the first discharge specific capacity is greatly improved.

[0036] The cycle performance test of the battery assembled in Example 1 is carried out under the following test conditions: the charge and discharge mode is constant current charge and discharge, and the current density is 0.2A g -1 , up to a specific capacity of 1000 mAh g -1 The cycle curve of the battery prepared in Application Example 1 is as follows: Figure 4 As shown. Figure 4 It can be seen that the battery prepared in Application Example 1 can be stably cycled for 1580 h, which is much better than the cycle performance of pure MBene in Comparative Example 1.

[0037] The rate performance test of the battery prepared in Example 1 was carried out under the following conditions: the charge and discharge mode was constant current charge and discharge, and the charge and discharge rates were 0.1, 0.2, 0.5, 0.8, and 0.1 A g -1The specific capacity was 1000 mAh g -1 The rate performance of the battery prepared in Application Example 1 is as follows: Figure 5 As shown. Figure 5 It can be seen that the battery made in Application Example 1 has the following characteristics: -1 The overpotentials are 1.37, 1.45, 1.56, and 1.63 V, respectively, with excellent rate performance.

[0038] Comparative Example 1

[0039] Mo2B2 MBene: conductive carbon black: PVDF were mixed in a mass ratio of 8:1:1, and then NMP solvent was added to prepare a slurry after stirring and homogenization. A certain volume of slurry was applied to a circular carbon paper with a diameter of 8 mm using a pipette, and then placed in a vacuum oven for drying to prepare a Mo2B2MBene electrode sheet. The Mo2B2 MBene electrode sheet was used as the positive electrode, glass fiber as the separator, 1 mol / L LiTFSI DMSO system as the electrolyte, and lithium foil as the counter electrode. A button half-cell was assembled using a special perforated battery shell, and the battery was placed in a test tank filled with carbon dioxide gas for electrochemical testing.

[0040] The battery assembled in Comparative Example 1 was tested for charge and discharge performance under the following test conditions: the charge and discharge mode was constant current charge and discharge; the current density was 0.2A g -1 ; The discharge cut-off voltage is 2.0V; The first constant current discharge curve of the battery assembled in Comparative Example 1 is as shown Figure 6 As shown. Figure 6 It can be seen that the first discharge capacity of the battery assembled in Application Example 1 is 2960 mAh g -1 .

[0041] The battery assembled in Comparative Example 1 was subjected to a cycle performance test under the following test conditions: the charge and discharge mode was constant current charge and discharge, and the current density was 0.2A g -1 , up to a specific capacity of 1000 mAh g -1 The cycle curve of the battery prepared in Application Example 1 is as follows: Figure 7 As shown. Figure 7 It can be seen that the battery prepared in Application Example 1 can be stably cycled for 230 hours.

[0042] Example 2

[0043] (1) Weigh 200 mg Mo2AlB2 MBene and 200 ul (10 mg ml -1 )Put the K2PtCl6 solution in a vial and mix it evenly under ultrasonication for 30 min.

[0044] (2) The above mixture was transferred to a stirring table and stirred at room temperature for 24 hours to obtain a Pt-Mo2AlB2 heterogeneous composite material.

[0045] (3) The above materials were mixed in a mass ratio of active material: conductive carbon black: PVDF = 8:1:1, and then NMP solvent was added to prepare a slurry after stirring and homogenization. A certain volume of the slurry was drawn with a pipette and coated on a circular carbon paper with a diameter of 8 mm, and then placed in a vacuum oven for drying to prepare an electrode sheet.

[0046] The X-ray diffraction (XRD) pattern of Pt-Mo2AlB2MBene heterogeneous composite material is shown in Figure 8 As shown, it exhibits characteristic peaks of Pt and Mo2AlB2 MBene, indicating the successful preparation of the composite material. Using the electrode sheet in step (3) as the positive electrode, glass fiber as the separator, 1 mol / L LiTFSI DMSO system as the electrolyte, lithium foil as the counter electrode, and a button half-cell assembled using a special perforated battery shell, the battery was placed in a test tank filled with carbon dioxide gas for electrochemical testing.

[0047] The battery assembled in Example 2 was tested for charge and discharge performance. The test conditions were: the charge and discharge mode was constant current charge and discharge; the current density was 0.2A g -1 ; The discharge cut-off voltage is 2.0V; Its first discharge capacity is 13508mAh g -1 The cycle performance test of the battery assembled in Example 2, the test conditions are: the charge and discharge mode is constant current charge and discharge, the current density is 0.2A -1 , up to a specific capacity of 1000 mAh g -1 The battery prepared in this application example can be stably cycled for 870 hours.

[0048] Example 3

[0049] (1) Weigh 200 mg MoAl 1-x B MBene and 200ul (10mg ml -1 )Put the K2PtCl6 solution in a vial and mix it evenly under ultrasonication for 30 min.

[0050] (2) The above mixture was transferred to a stirring table and stirred at room temperature for 24 h to obtain Pt-MoAl 1-x B Heterogeneous composite materials.

[0051] (3) The above materials were mixed in a mass ratio of active material: conductive carbon black: PVDF = 8:1:1, and then NMP solvent was added to prepare a slurry after stirring and homogenization. A certain volume of the slurry was drawn with a pipette and coated on a circular carbon paper with a diameter of 8 mm, and then placed in a vacuum oven for drying to prepare an electrode sheet.

[0052] The electrode sheet in step (3) was used as the positive electrode, glass fiber was used as the separator, 1 mol / L LiTFSI in DMSO system was used as the electrolyte, and lithium foil was used as the counter electrode. A button half-cell was assembled using a special perforated battery shell, and the battery was placed in a test tank filled with carbon dioxide gas for electrochemical testing.

[0053] The battery assembled in the corresponding use case 3 was tested for charge and discharge performance. The test conditions were: the charge and discharge mode was constant current charge and discharge; the current density was 0.2A g -1 ; The discharge cut-off voltage is 2.0V; Its first discharge specific capacity is 14878mAh g -1 .

[0054] The cycle performance test of the battery assembled in Example 3 is carried out under the following test conditions: the charge and discharge mode is constant current charge and discharge, and the current density is 0.2A g -1 , up to a specific capacity of 1000 mAh g -1 The battery prepared in this application example can be stably cycled for 1780 hours.

Claims

1. A Pt-MBene composite material and a method for preparing a pole piece used in a lithium carbon dioxide battery, comprising the following steps: (1) mixing the molybdenum-based MBene powder and the K2PtCl6 solution uniformly after ultrasonic treatment at a certain mass ratio; (2) placing the mixture of the molybdenum-based MBene powder and the K2PtCl6 solution in step (1) on a stirring table and stirring for 24 hours to obtain a Pt-MBene composite material; (3) The Pt-MBene composite material obtained in step (2) is prepared into pole pieces and assembled into batteries, and electrochemical tests are performed in a CO2-filled atmosphere.

2. The preparation method according to claim 1, characterized in that: The molybdenum-based MBene in step (1) includes Mo2B2 MBene containing transition metal molybdenum, MoAl 1-x B MBene, Mo2AlB2 MBene, i-MBene: Mo 1.33 Y 0.67 A mixture of one or more MBene materials such as B2.

3. The preparation method according to claim 1, characterized in that In the step (1), the mass ratio of the molybdenum-based MBene powder to the K2PtCl6 solution is 100:1 to 100:

50.

4. The preparation method according to claim 1, characterized in that In the step (1), the ultrasonic time of MBene powder and K2PtCl6 solution is 10 min to 120 min.

5. The preparation method according to claim 1, characterized in that In the step (1), the ultrasonic power of the MBene powder and the K2PtCl6 solution is 100W to 600W.

6. The preparation method according to claim 1, characterized in that The type of atmosphere in step (4) can be selected from 100% CO2 or a mixture of CO2 and O2, Ar, N2, etc.

7. The Pt-MBene composite material and lithium carbon dioxide test electrode obtained according to the preparation method according to any one of claims 1 to 6.

8. A lithium carbon dioxide battery, characterized in that: The Pt-MBene composite material described in claim 7 is used as a positive electrode catalyst.