Solid-state battery and preparation method thereof
By in-situ polymerization in lithium batteries to form a dense electrode-electrolyte interface, the interface problem of solid electrolyte in lithium batteries is solved, the circulation and rate performance of the battery is improved, and compatible with the existing battery production lines, achieving large-scale production.
Patent Information
- Application Number
- CN202411213251.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-08
AI Technical Summary
Lithium battery polymer solid electrolyte faces interface problems in application, resulting in poor solid-solid interface compatibility, low ionic conductivity and high interface impedance, affecting cycling performance and rate performance, and at the same time, it does not match the existing battery production line, making it difficult to achieve scale. Chemical production.
By polymerizing the solid electrolyte precursor in situ during medium-temperature pressurization treatment, a good and dense electrode-electrolyte interface is formed. Combined with standstill and multiple curing treatments, the preparation process of the battery cell is optimized and it is carried out synchronously with battery assembly. Reduce costs and be compatible with existing industrial systems.
It improves the interface impedance of solid-state batteries, improves cycle performance and rate performance, achieves compatibility with existing battery production lines, reduces production costs, and has good application prospects.
Smart Images

Figure CN118919820A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of battery technology, and in particular, to a solid-state battery and a method for preparing the same. Background Art
[0002] Lithium batteries have always been the mainstream energy source in mobile devices, electric vehicles and other fields. However, traditional liquid electrolytes have concerns about safety and stability. In order to overcome these problems, research is now underway on new electrolyte materials, and one of the most anticipated technologies is lithium battery polymer solid electrolytes. Compared with liquid electrolytes, polymer solid electrolytes have higher safety and stability, and can effectively suppress the safety hazards of lithium batteries under high temperature or abnormal working conditions. This technological breakthrough is expected to promote lithium battery technology towards a safer and more efficient future.
[0003] However, lithium battery polymer solid electrolytes face a key challenge in their application, namely the interface problem. Traditional polymer solid electrolytes are usually prepared separately as self-supporting films, then sandwiched between electrodes and assembled into batteries, which undoubtedly leads to poor solid-solid interface compatibility and low ionic conductivity, and are not compatible with existing battery production lines, which is not conducive to further expansion of production. Moreover, the thickness of this separately prepared polymer solid electrolyte is mostly over 100μm, which is thicker than the current liquid electrolyte and separator thickness, further leading to an increase in the interface impedance between the electrode and the electrolyte, hindering ion transport and affecting the battery's cycle performance and rate performance. Summary of the invention
[0004] The present application provides a solid-state battery and a method for preparing the same, which can improve the technical problem of high interface impedance of the solid-state battery.
[0005] The embodiment of the present application is implemented as follows:
[0006] In a first aspect, the present application example provides a method for preparing a solid-state battery, which includes: subjecting the liquid-filled battery cell to a first curing treatment, the first curing treatment comprising charging to 40% SOC to 100% SOC at a current of 0.01C to 0.5C at a temperature of 40°C to 70°C and a pressure of 0.05MPa to 1MPa.
[0007] The liquid-injected battery cell includes a solid electrolyte precursor, and the solid electrolyte precursor includes a monomer and an initiator.
[0008] In the above technical scheme, in the preparation method of the solid-state battery of the present application, the solid electrolyte precursor has not yet solidified, and the liquid-filled battery cell is subjected to a medium-temperature pressurized treatment in a powered state. During this treatment process, the monomers in the solid electrolyte precursor are polymerized in situ under the action of the initiator. At the same time, the battery cell forms a good and dense electrode-electrolyte interface in situ, that is, an atomic-level interface transmission layer that is conducive to lithium ion transmission is formed in situ, which inherits the good interface contact between the liquid electrolyte and the electrode, improves the problem of high interface impedance of the solid-state battery, and is conducive to improving the cycle performance and rate performance of the prepared solid-state battery. At the same time, since the preparation of the solid electrolyte can be carried out simultaneously with the battery assembly, the cost is effectively reduced, and this preparation method can be well compatible with the existing battery industry system, and can achieve large-scale production, with good application prospects.
[0009] In combination with the first aspect, in a first possible example of the first aspect of the present application, the above-mentioned first curing treatment includes first charging with a current of 0.01C to 0.05C for 50min to 120min, then charging with a current of 0.1C to 0.2C for 30min to 60min, and then charging with a current of 0.2C to 0.5C to 40% SOC to 100% SOC.
[0010] Optionally, the first curing treatment includes charging at a current of 0.01C to 0.19C for 25 to 60 min, then charging at a current of 0.02C to 0.05C for 25 to 60 min, then charging at 0.1C to 0.2C for 30 to 60 min, and then charging at a current of 0.2C to 0.5C to 40% SOC to 100% SOC.
[0011] In the above example, the first curing treatment includes first applying power with a smaller current, then applying power with a larger current, and then applying power with an even larger current, which is beneficial for forming a good and dense electrode-electrolyte interface in situ in the battery cell.
[0012] In combination with the first aspect, in a second possible example of the first aspect of the present application, before the above-mentioned first curing treatment, the method for preparing a solid-state battery also includes a first standing treatment, and the first standing treatment includes placing the liquid-filled battery cell at a temperature of 10°C to 50°C for 1h to 72h.
[0013] Optionally, the temperature of the first static treatment is 35°C to 50°C.
[0014] Optionally, the battery is turned over every 1 h to 5 h during the first static treatment.
[0015] In the above example, before the first curing treatment, the liquid-filled battery cell is subjected to the first static treatment, which is conducive to the solution formed by the solid electrolyte precursor to completely infiltrate the positive electrode, negative electrode and separator, so that the monomers and initiators in the solid electrolyte precursor are evenly dispersed, which is conducive to the subsequent in-situ curing reaction.
[0016] In combination with the first aspect, in a third possible example of the first aspect of the present application, after the above-mentioned first curing treatment, the method for preparing a solid-state battery also includes a second standing treatment, and the second standing treatment includes placing the battery cell that has completed the first curing treatment at a temperature of 35°C to 50°C for 3h to 5h.
[0017] Optionally, the battery is turned over every 0.5 h to 2 h during the second static treatment.
[0018] In the above example, after the first curing treatment, the battery cell that has completed the first curing treatment is subjected to a second static treatment, so that the monomers and initiators in the solid electrolyte precursor can further undergo a curing reaction in a medium temperature environment.
[0019] In combination with the first aspect, in a fourth possible example of the first aspect of the present application, after the above-mentioned second standing treatment, the method for preparing a solid-state battery also includes a second curing treatment, and the second curing treatment includes placing the battery cell that has completed the second standing treatment at a temperature of 70°C to 85°C and a pressure of 0.02MPa to 0.8MPa for curing for 2h to 5h.
[0020] In the above example, after the second standing treatment, the battery cell that has completed the second standing treatment is subjected to a second curing treatment, and the temperature of the second curing treatment is higher than the temperature of the second curing treatment and the temperature of the first standing treatment, so that the monomers and initiators in the solid electrolyte precursor further undergo a curing reaction in a high temperature and pressurized environment, thereby improving the overall curing degree of the solid electrolyte and discharging most of the non-solid components in the battery cell and the trace gases generated by the reaction.
[0021] In combination with the first aspect, in the fifth possible example of the first aspect of the present application, in the above-mentioned second curing process, first cure at a pressure of 0.02MPa to 0.05MPa for 5min to 10min, then cure at a pressure of 0.05MPa to 0.09MPa for 5min to 10min, then cure at a pressure of 0.1MPa to 0.8MPa for 5min to 10min, and then cure at a pressure of 0.1MPa to 0.8MPa for 150min to 165min.
[0022] In the above example, the second curing process adopts a process of slowly increasing pressure. The battery cell is first treated with a smaller pressure to adapt the battery cell to the smaller pressure, and then treated with a larger pressure to adapt the battery cell to the larger voltage. Then, the battery cell is treated with an even greater pressure to adapt the battery cell to the even greater pressure, thereby preventing the battery cell from directly bearing the large pressure and causing damage to its internal structure.
[0023] In combination with the first aspect, in a sixth possible example of the first aspect of the present application, after the above-mentioned second curing treatment, the method for preparing a solid-state battery also includes a third standing treatment, and the third standing treatment includes placing the battery cell that has completed the second curing treatment at a temperature of 5°C to 25°C for 8h to 15h.
[0024] Optionally, the battery is turned over every 0.5 h to 3 h during the third static treatment.
[0025] In the above example, after the second curing treatment, the battery cell that has completed the second curing treatment is subjected to a third static treatment, which is beneficial to fully release the interface stress of the solid electrolyte-electrode / diaphragm, avoid interface failure problems caused by thermal stress, and improve production yield and service reliability.
[0026] In combination with the first aspect, in the seventh possible example of the first aspect of the present application, the above-mentioned monomer includes any one or more of methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, methacrylate carbonate, vinyl acetate, vinyl carbonate, methyl vinyl carbonate and ethyl vinyl carbonate.
[0027] In the above examples, when the monomers include any one or more of methyl methacrylate, ethyl methacrylate, propyl methpropionate, butyl methpropionate, methacrylate carbonate, vinyl acetate, vinyl carbonate, methyl vinyl carbonate and ethyl vinyl carbonate, through the first curing treatment, the above monomers can be in-situ polymerized under the action of the initiator, and at the same time, the battery cell can form a good and dense electrode-electrolyte interface in situ.
[0028] In combination with the first aspect, in an eighth possible example of the first aspect of the present application, the initiator includes azobisisobutyronitrile.
[0029] In the above example, when the initiator includes azobisisobutyronitrile, through the first curing treatment, the monomers in the solid electrolyte precursor can be polymerized in situ under the action of the above initiator, and at the same time, the battery cell can form a good and dense electrode-electrolyte interface in situ.
[0030] In a second aspect, the present application example provides a solid-state battery, which is manufactured according to the solid-state battery manufacturing method as described above.
[0031] In the above technical solution, the solid-state battery of the present application has good cycle performance and rate performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.
[0033] Figure 1 This is a flow chart of the preparation method of the solid-state battery of the present application.
[0034] Figure 2 The voltage-capacity curve diagram of the solid-state battery 1C discharge prepared in Example 1 and Comparative Example 1 of the present application.
[0035] Figure 3 The voltage-capacity curve diagram of the solid-state battery 1C during charge and discharge of Example 2 and Comparative Example 2 of the present application. DETAILED DESCRIPTION
[0036] The embodiments of the present application will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. In the examples, if specific conditions are not specified, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0037] At present, lithium batteries have been widely used in automotive electronics, mobile digital products and other fields due to their wide operating temperature range, high mass-to-energy ratio and volume-to-energy ratio.
[0038] However, traditional liquid electrolytes have concerns about safety and stability, and the use of solid electrolytes instead of liquid electrolytes has become a research direction. However, solid electrolytes face a key challenge in application, namely the interface problem. Traditional polymer solid electrolytes are usually prepared separately as self-supporting films, then sandwiched between electrodes, and then assembled into batteries, which undoubtedly leads to poor solid-solid interface compatibility and low ionic conductivity, and is not compatible with existing battery production lines, which is not conducive to further expansion of production.
[0039] The in-situ polymerization process for preparing solid-state lithium metal polymer batteries has been proposed to solve or improve the problems of solid electrolyte-electrode interface contact and solid electrolyte being too thick. As a new processing technology, it can generate polymer solid electrolytes by in-situ polymerization inside the battery, so that the polymer solid electrolyte has better interface compatibility with the electrode, and can be ultra-thin, significantly improving the performance of the battery. Abandoning the polymer dissolution, drying and film formation processes of existing polymer electrolytes, the preparation of polymer solid electrolytes and battery assembly can be carried out simultaneously, effectively reducing costs and being better compatible with the existing battery industry system, and has good application prospects.
[0040] The following is a detailed description of a solid-state battery and a method for preparing the same in accordance with an embodiment of the present application:
[0041] See also Figure 1 The present application provides a method for preparing a solid-state battery, which comprises the following steps:
[0042] S1. First static treatment
[0043] The liquid-filled battery cell is subjected to a first static treatment, and the first static treatment includes placing the liquid-filled battery cell at a temperature of 10° C. to 50° C. and leaving it to stand for 1 hour to 72 hours.
[0044] Among them, the liquid-injected battery cell includes a solid electrolyte precursor, and the solid electrolyte precursor includes a monomer and an initiator.
[0045] Liquid-filled cells are made by the following method:
[0046] The positive electrode sheet, the negative electrode sheet and the separator are assembled into a dry cell, a solid electrolyte precursor is injected into the dry cell, and the cell is pre-sealed to obtain a liquid-injected cell.
[0047] As an example, the temperature of the first standing treatment may be 10°C, 15°C, 20°C, 25°C, 30°C, 35°C, 40°C, 45°C or 50°C.
[0048] Optionally, the temperature of the first static treatment is 35°C to 50°C.
[0049] As an example, the time for the first static treatment can be 1h, 2h, 5h, 8h, 10h, 12h, 16h, 20h, 24h, 28h, 32h, 36h, 40h, 44h, 48h, 52h, 56h, 60h, 64h, 68h or 72h.
[0050] Optionally, the battery is turned over every 1 h to 5 h during the first static treatment.
[0051] Optionally, the monomer includes any one or more of methyl methacrylate, ethyl methacrylate, propyl methpropionate, butyl methpropionate, methacrylate carbonate, vinyl acetate, vinyl carbonate, methyl vinyl carbonate and ethyl vinyl carbonate.
[0052] Optionally, the initiator comprises azobisisobutyronitrile.
[0053] When the monomer includes any one or more of methyl methacrylate, ethyl methacrylate, propyl methpropionate, butyl methpropionate, methacrylate carbonate, vinyl acetate, vinyl carbonate, methyl vinyl carbonate and ethyl vinyl carbonate, and the initiator includes azobisisobutyronitrile, through the first curing treatment, the above-mentioned monomer can be in-situ polymerized under the action of the above-mentioned initiator, and at the same time, the battery cell can form a good and dense electrode-electrolyte interface in situ.
[0054] Optionally, the solid electrolyte precursor further comprises a functional additive.
[0055] S2. First curing treatment
[0056] The liquid-filled battery cell that has completed the first static treatment is subjected to the first curing treatment. The first curing treatment includes placing the liquid-filled battery cell at a temperature of 40°C to 70°C and a pressure of 0.05MPa to 1MPa, and charging the cell to 40% SOC to 100% SOC at a current of 0.01C to 0.5C.
[0057] As an example, the temperature of the first curing process may be 40°C, 45°C, 50°C, 55°C, 60°C, 65°C or 70°C.
[0058] As an example, the pressure of the first curing process may be 0.05 MPa, 0.1 MPa, 0.2 MPa, 0.3 MPa, 0.4 MPa, 0.5 MPa, 0.6 MPa, 0.7 MPa, 0.8 MPa, 0.9 MPa or 1 MPa.
[0059] Optionally, the first curing treatment includes charging at a current of 0.01C to 0.05C for 50 min to 120 min, then charging at a current of 0.1C to 0.2C for 30 min to 60 min, and then charging at a current of 0.2C to 0.5C to 40% SOC to 100% SOC.
[0060] Optionally, the first curing treatment includes charging at a current of 0.01C to 0.19C for 25 to 60 min, then charging at a current of 0.02C to 0.05C for 25 to 60 min, then charging at 0.1C to 0.2C for 30 to 60 min, and then charging at a current of 0.2C to 0.5C to 40% SOC to 100% SOC.
[0061] Optionally, the first curing treatment includes charging at a current of 0.01C for 25min to 60min, then charging at a current of 0.02C for 25min to 60min, then charging at 0.1C for 30min to 60min, and then charging at a current of 0.2C to 40% SOC to 100% SOC.
[0062] The first curing treatment includes firstly applying power with a smaller current, then applying power with a larger current, and then applying power with an even larger current, which is beneficial to forming a good and dense electrode-electrolyte interface in situ in the battery cell.
[0063] S3, second static treatment
[0064] The battery cell that has completed the second curing treatment is subjected to a second static treatment, and the second static treatment includes placing the battery cell at a temperature of 35° C. to 50° C. for 3 hours to 5 hours.
[0065] As an example, the temperature of the second standing treatment may be 35°C, 40°C, 45°C or 50°C.
[0066] As an example, the second static treatment time may be 3 h, 3.5 h, 4 h, 4.5 h or 5 h.
[0067] Optionally, the battery is turned over every 0.5 h to 2 h during the second static treatment.
[0068] S4. Second curing treatment
[0069] The battery cells that have completed the second static treatment are subjected to a second curing treatment, wherein the second curing treatment includes curing the battery cells at a temperature of 70° C. to 85° C. and a pressure of 0.02 MPa to 0.8 MPa for 2 h to 5 h.
[0070] As an example, the temperature of the second curing process may be 70°C, 75°C, 80°C or 85°C.
[0071] Optionally, during the second curing treatment, the material is first cured at a pressure of 0.02MPa to 0.05MPa for 5min to 10min, then cured at a pressure of 0.05MPa to 0.09MPa for 5min to 10min, then cured at a pressure of 0.1MPa to 0.8MPa for 5min to 10min, and then cured at a pressure of 0.1MPa to 0.8MPa for 150min to 165min.
[0072] The second curing process adopts a process of slowly increasing pressure. The battery cell is first treated with a smaller pressure to allow the battery cell to adapt to the smaller pressure. The battery cell is then treated with a larger pressure to allow the battery cell to adapt to the larger voltage. The battery cell is then treated with an even greater pressure to allow the battery cell to adapt to the even greater pressure, thereby preventing the battery cell from directly bearing large pressure and causing damage to its internal structure.
[0073] S5. The third static treatment
[0074] The battery cell that has completed the second curing treatment is subjected to a third static treatment, and the third static treatment is to place the battery cell at a temperature of 5°C to 25°C for 8h to 15h.
[0075] As an example, the temperature of the third standing treatment may be 5°C, 10°C, 15°C, 20°C or 25°C.
[0076] As an example, the time for the third static treatment can be 8 h, 9 h, 10 h, 11 h, 12 h, 13 h, 14 h or 15 h.
[0077] Optionally, the battery is turned over every 0.5 h to 3 h during the third static treatment.
[0078] The preparation method of the solid-state battery of the present application includes a first standing treatment, a first curing treatment, a second standing treatment, a second curing treatment and a third standing treatment, wherein the first standing treatment is conducive to the solution formed by the solid electrolyte precursor to completely infiltrate the positive electrode, the negative electrode and the diaphragm, so that the monomers and initiators in the solid electrolyte precursor are evenly dispersed; the first curing treatment can enable the monomers in the solid electrolyte precursor to achieve in-situ polymerization under the action of the initiator, and at the same time, the battery cell forms a good and dense electrode-electrolyte interface in situ; the second standing treatment allows the monomers and initiators in the solid electrolyte precursor to further undergo a curing reaction in a medium temperature environment; the second curing treatment allows the monomers and initiators in the solid electrolyte precursor to further undergo a curing reaction in a high temperature and pressurized environment, thereby improving the overall curing degree of the solid electrolyte and discharging most of the non-solid components in the battery cell and the trace gases generated by the reaction; the third standing treatment is conducive to fully releasing the interface stress of the solid electrolyte-electrode / diaphragm, avoiding interface failure problems caused by thermal stress, and improving production yield and service reliability.
[0079] The preparation method of the solid-state battery of the present application forms an atomic-level interface transmission layer in situ that is conducive to lithium ion transmission, inherits the good interface contact between the liquid electrolyte and the electrode, improves the problem of high interface impedance of the solid-state battery, and is conducive to improving the cycle performance and rate performance of the prepared solid-state battery. At the same time, since the preparation of the solid electrolyte can be carried out simultaneously with the battery assembly, the cost is effectively reduced, and this preparation method can be well compatible with the existing battery industrial system, and can realize large-scale production, and has good application prospects.
[0080] The present application also provides a solid-state battery, which is prepared according to the solid-state battery preparation method as described above.
[0081] The solid-state battery of the present application has good cycle performance and rate performance.
[0082] The following is a further detailed description of a solid-state battery and a method for preparing the same in conjunction with embodiments of the present invention.
[0083] Example 1
[0084] The present invention provides a solid-state battery and a method for preparing the same, which comprises the following steps:
[0085] S1. First static treatment
[0086] The positive electrode sheet, the negative electrode sheet and the separator are assembled into a dry cell, a solid electrolyte precursor is injected into the dry cell, and the cell is pre-sealed to obtain a liquid-injected cell.
[0087] The solid electrolyte precursor includes methyl methacrylate, azobisisobutyronitrile and lithium bistrifluoromethanesulfonyl imide (LiTFSI), and the mass ratio of methyl methacrylate, azobisisobutyronitrile and lithium bistrifluoromethanesulfonyl imide is 67:3:30.
[0088] The liquid-filled battery cell is subjected to the first static treatment, which includes placing the liquid-filled battery cell at a temperature of 45° C. for 72 hours and turning the battery over every 5 hours.
[0089] S2. First curing treatment
[0090] The liquid-filled battery cell that has completed the first static treatment is subjected to the first curing treatment. The first curing treatment is performed at a temperature of 45° C. and a pressure of 0.05 MPa, including the following steps:
[0091] S21, let stand for 3 minutes, charge at 0.01C current for 25 minutes;
[0092] S22, let stand for 3 minutes, charge at 0.02C current for 25 minutes;
[0093] S23, let stand for 3 minutes, charge at 0.1C current for 30 minutes;
[0094] S24: Let stand for 3 minutes and charge to 40% SOC at a current of 0.2C.
[0095] S3, second static treatment
[0096] The battery cell that has completed the second curing treatment is subjected to a second static treatment, which includes placing the battery cell at a temperature of 45° C. for 3 hours and turning the battery over every 1 hour.
[0097] S4. Second curing treatment
[0098] The battery cell that has completed the second static treatment is subjected to a second curing treatment, and the temperature of the second curing treatment is 80° C., including the following steps:
[0099] S41, increase the pressure to 0.04MPa, which takes 10min;
[0100] S42, increasing the pressure to 0.08 MPa, which takes 10 minutes;
[0101] S43, increasing the pressure to 0.1 MPa, which takes 10 minutes;
[0102] S44, increase the pressure to 0.2 MPa and maintain it at 0.2 MPa for 150 minutes.
[0103] S5. The third static treatment
[0104] The battery cell that has completed the second curing treatment is subjected to a third static treatment. The third static treatment is to place the battery cell at a temperature of 25° C. for 15 hours, and turn the battery over every 2 hours.
[0105] Example 2
[0106] The embodiments of the present application provide a solid-state battery and a method for preparing the same. Embodiment 2 is based on Embodiment 1, in which only the temperature of the first curing treatment is modified to 70° C., and the other aspects remain unchanged.
[0107] Example 3
[0108] The embodiments of the present application provide a solid-state battery and a method for preparing the same. Embodiment 2 is based on Embodiment 1, in which only the pressure of the first curing treatment is modified to 1 MPa, and the other aspects remain unchanged.
[0109] Comparative Example 1
[0110] The comparative example of the present application provides a solid-state battery and a method for preparing the same, which comprises the following steps:
[0111] S1. First static treatment
[0112] The positive electrode sheet, the negative electrode sheet and the separator are assembled into a dry cell, a solid electrolyte precursor is injected into the dry cell, and the cell is pre-sealed to obtain a liquid-injected cell.
[0113] The solid electrolyte precursor includes methyl methacrylate, azobisisobutyronitrile and lithium bistrifluoromethanesulfonyl imide (LiTFSI), and the mass ratio of methyl methacrylate, azobisisobutyronitrile and lithium bistrifluoromethanesulfonyl imide is 67:3:30.
[0114] The liquid-filled battery cell is subjected to the first static treatment, which includes placing the liquid-filled battery cell at a temperature of 45° C. for 72 hours and turning the battery over every 5 hours.
[0115] S2. First curing treatment
[0116] The liquid-filled battery cell that has completed the first standing treatment is subjected to the first curing treatment, and the first curing treatment includes standing at 45° C. and 0.05 MPa for 100 minutes.
[0117] S3, second static treatment
[0118] The battery cell that has completed the second curing treatment is subjected to a second static treatment, which includes placing the battery cell at a temperature of 45° C. for 3 hours and turning the battery over every 1 hour.
[0119] S4. Second curing treatment
[0120] The battery cell that has completed the second static treatment is subjected to a second curing treatment, and the temperature of the second curing treatment is 80° C., including the following steps:
[0121] S41, increase the pressure to 0.04MPa, which takes 10min;
[0122] S42, increasing the pressure to 0.08 MPa, which takes 10 minutes;
[0123] S43, increasing the pressure to 0.1 MPa, which takes 10 minutes;
[0124] S44, increase the pressure to 0.2 MPa and maintain it at 0.2 MPa for 150 minutes.
[0125] S5. The third static treatment
[0126] The battery cell that has completed the second curing treatment is subjected to a third static treatment. The third static treatment is to place the battery cell at a temperature of 25° C. for 15 hours, and turn the battery over every 2 hours.
[0127] S6, Formation
[0128] The battery cell that has completed the third static treatment is subjected to a formation treatment, and the formation treatment includes the following steps:
[0129] S61, let stand for 3 minutes, charge at 0.01C current for 25 minutes;
[0130] S62, let stand for 3 minutes, charge at 0.02C current for 25 minutes;
[0131] S63, let stand for 3 minutes, charge at 0.1C current for 30 minutes;
[0132] S64. Let stand for 3 minutes and charge to 40% SOC at a current of 0.2C.
[0133] Comparative Example 2
[0134] The embodiment of the present application provides a solid-state battery and a method for preparing the same. Comparative Example 2 is based on Comparative Example 1, in which only the temperature of the first curing treatment is modified to 70° C., while the other aspects remain unchanged.
[0135] Test Example 1
[0136] The solid-state batteries prepared in Example 1 and Comparative Example 1 were charged to 3.65V at a constant current of 0.33C (198A), and charged at a constant voltage until the current dropped to 30A; left to stand for 30 minutes; discharged at a constant current of 1C to a cut-off voltage of 2.5V; left to stand for 5 minutes. The voltage-capacity curves of the solid-state batteries prepared in Example 1 and Comparative Example 1 at 1C discharge were measured, as shown in FIG. Figure 2 shown.
[0137] Depend on Figure 2 It can be seen that when discharging at a current of 1C, the discharge capacity of the solid-state battery prepared in Example 1 is 650Ah, while the discharge capacity of the solid-state battery prepared in Comparative Example 1 is only 560Ah. The discharge capacity of the solid-state battery prepared in Example 1 is higher than the discharge capacity of the solid-state battery prepared in Comparative Example 1.
[0138] Test Example 2
[0139] The solid-state batteries prepared in Example 2 and Comparative Example 2 were charged to 3.65V at a constant current of 0.33C (198A), and charged at a constant voltage until the current dropped to 30A; left to stand for 30 minutes; discharged at a constant current of 1C to a cut-off voltage of 2.5V; left to stand for 5 minutes. The voltage-capacity curves of the solid-state batteries prepared in Example 2 and Comparative Example 2 at 1C discharge were measured, as shown in FIG. Figure 3 shown.
[0140] Depend on Figure 3It can be seen that the charge capacity of comparative example 2 is 550.8Ah, the discharge capacity is 422.1Ah, and the first efficiency is 76.6%. The charge capacity of embodiment 2 is 618.5Ah, the discharge capacity is 561.0Ah, and the first efficiency is 90.7%. The discharge capacity and first efficiency of the solid-state battery prepared in embodiment 2 are higher than those of the solid-state battery prepared in comparative example 2.
[0141] The above description is only a specific embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.
Claims
1. A method for preparing a solid-state battery, characterized in that: The preparation method of the solid-state battery comprises: subjecting the liquid-filled battery cell to a first curing treatment, wherein the first curing treatment comprises charging to 40% SOC to 100% SOC at a current of 0.01C to 0.5C at a temperature of 40°C to 70°C and a pressure of 0.05MPa to 1MPa; The liquid-injected battery cell includes a solid electrolyte precursor, and the solid electrolyte precursor includes a monomer and an initiator.
2. The method for preparing a solid-state battery according to claim 1, characterized in that: The first curing treatment includes charging at a current of 0.01C to 0.05C for 50min to 120min, then charging at a current of 0.1C to 0.2C for 30min to 60min, and then charging at a current of 0.2C to 0.5C to 40% SOC to 100% SOC; Optionally, the first curing treatment includes charging at a current of 0.01C to 0.19C for 25 to 60 min, then charging at a current of 0.02C to 0.05C for 25 to 60 min, then charging at 0.1C to 0.2C for 30 to 60 min, and then charging at a current of 0.2C to 0.5C to 40% SOC to 100% SOC.
3. The method for preparing a solid-state battery according to claim 1, characterized in that: Before the first curing treatment, the method for preparing the solid-state battery further includes a first standing treatment, wherein the first standing treatment includes placing the liquid-filled battery cell at a temperature of 10° C. to 50° C. for 1 hour to 72 hours; Optionally, the temperature of the first static treatment is 35° C. to 50° C.; Optionally, during the first static treatment, the battery is turned over every 1 hour to 5 hours.
4. The method for preparing a solid-state battery according to claim 1, characterized in that: After the first curing treatment, the method for preparing the solid-state battery further includes a second standing treatment, wherein the second standing treatment includes placing the battery cell that has completed the first curing treatment at a temperature of 35° C. to 50° C. for 3 h to 5 h; Optionally, during the second static treatment, the battery is turned over every 0.5 h to 2 h.
5. The method for preparing a solid-state battery according to claim 4, characterized in that: After the second standing treatment, the method for preparing the solid-state battery also includes a second curing treatment, and the second curing treatment includes placing the battery cell that has completed the second standing treatment at a temperature of 70°C to 85°C and a pressure of 0.02MPa to 0.8MPa for curing for 2h to 5h.
6. The method for preparing a solid-state battery according to claim 5, characterized in that: During the second curing treatment, the material is first cured at a pressure of 0.02MPa to 0.05MPa for 5min to 10min, then cured at a pressure of 0.05MPa to 0.09MPa for 5min to 10min, then cured at a pressure of 0.1MPa to 0.8MPa for 5min to 10min, and then cured at a pressure of 0.1MPa to 0.8MPa for 150min to 165min.
7. The method for preparing a solid-state battery according to claim 5, characterized in that: After the second curing treatment, the method for preparing the solid-state battery further includes a third standing treatment, wherein the third standing treatment includes placing the battery cell that has completed the second curing treatment at a temperature of 5° C. to 25° C. for 8 h to 15 h; Optionally, during the third static treatment, the battery is turned over every 0.5 h to 3 h.
8. The method for preparing a solid-state battery according to any one of claims 1 to 7, characterized in that: The monomers include any one or more of methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, methacrylic carbonate, vinyl acetate, vinyl carbonate, methyl vinyl carbonate and ethyl vinyl carbonate.
9. The method for preparing a solid-state battery according to claim 8, characterized in that: The initiator includes azobisisobutyronitrile.
10. A solid-state battery, characterized in that: The solid-state battery is prepared according to the method for preparing a solid-state battery according to any one of claims 1 to 9.