Organic-inorganic composite polymer solid electrolyte as well as preparation method and application thereof

By introducing Cu-based compounds into the organic-inorganic composite polymer solid electrolyte, the distribution of lithium salt anion electron cloud was regulated, solving the problems of ionic conductivity and interface stability of polyoxyethylene composite electrolyte, and achieving high energy density and long-term cycle stability of lithium battery performance.

CN118919834APending Publication Date: 2024-11-08UNIV OF CHINESE ACAD OF SCI
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410982008.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing polyoxyethylene organic-inorganic composite solid electrolytes have low ionic conductivity, low lithium-ion transference number, and poor interfacial stability at room temperature, which limits the high energy density and long-term cycle stability of all-solid-state batteries.

Method used

Introducing Cu-based compounds with electrocatalytic activity into organic-inorganic composite polymer solid electrolytes promotes the electronic processes of lithium salt anions at the interface by regulating the electron cloud distribution of lithium salt anions, generating products that are beneficial to the stability of lithium metal, and constructing a gradient interface rich in Li2O-Li3N-LiF inorganic phases.

Benefits of technology

It achieves high room temperature ionic conductivity, low interface resistance and high lithium stability, improves the long-term cycle stability and lithium-ion transference number of lithium batteries, and enhances the stable cycle time of symmetric batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919834A_ABST
    Figure CN118919834A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of energy storage materials, and discloses an organic-inorganic composite polymer solid electrolyte as well as a preparation method and application thereof. The organic-inorganic composite polymer solid electrolyte comprises the following components: polyoxyethylene, polyvinylidene fluoride, a lithium salt, an active filler and a Cu-based compound, the Cu-based compound contains cuprous ions. According to the organic-inorganic composite polymer solid electrolyte provided by the invention, the Cu-based compound targeting additive with electrocatalytic activity is introduced, anions are anchored, and the electronic structure of the anions at an interface is regulated, so that the lithium ion conductivity and the interface stability of the organic-inorganic composite polymer solid electrolyte are improved; the organic-inorganic polymer solid electrolyte provided by the invention has relatively high lithium ion conductivity and low interface impedance, and can greatly prolong the stable cycle time of a symmetric battery under the current density of 0.1 mA cm <-1 >.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of energy storage materials, and specifically relates to an organic-inorganic composite polymer solid electrolyte and a preparation method and application thereof. Background Art

[0002] In recent years, as one of the signs of electrification of transportation, the new energy vehicle industry has developed rapidly, but at the same time, it has also been given higher requirements. Objective problems such as range anxiety and safety anxiety have restricted its further market expansion. As the "heart" of new energy vehicles, power batteries with higher energy density and higher safety are in urgent need of development.

[0003] Compared with the currently widely used liquid lithium-ion batteries, solid-state batteries have significantly improved intrinsic safety because they do not use flammable and explosive liquid electrolytes, avoid leakage and volatilization of electrolytes. Compared with inorganic solid electrolytes such as oxides, sulfides, and halides, polymer solid electrolytes represented by polyethylene oxide have good flexibility and processability, production process compatibility, low cost, and good interface compatibility, and are considered to be the solid electrolytes with the most industrial prospects. However, polyethylene oxide polymer solid electrolytes have high crystallinity and slow lithium ion transfer kinetics, and usually can only work at high temperatures. The best solution is to reduce the crystallinity of the polymer by compounding with inorganic active fillers, constructing an organic-inorganic composite polymer solid electrolyte to achieve faster lithium ion transfer. However, polyethylene oxide organic-inorganic composite solid electrolytes still have the characteristics of low ionic conductivity, low lithium ion migration number, low critical current density, and poor interface stability at room temperature, and the stability of the time difference in matching with the ultra-high nickel positive electrode further limits its construction of high-energy-density all-solid-state batteries.

[0004] Therefore, there is an urgent need to develop an organic-inorganic composite solid electrolyte that can simultaneously achieve high room temperature ionic conductivity and interfacial stability with lithium metal, thereby improving the long-term cycle stability of lithium batteries. Summary of the invention

[0005] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention provides an organic-inorganic composite polymer solid electrolyte and a preparation method and application thereof. The organic-inorganic composite polymer solid electrolyte provided by the present invention can improve lithium ion conductivity, reduce interface resistance, and improve the long-term cycle stability of lithium batteries.

[0006] The invention provides an organic-inorganic composite polymer solid electrolyte.

[0007] Specifically, an organic-inorganic composite polymer solid electrolyte includes the following components: polyethylene oxide (PEO), polyvinylidene fluoride (PVDF), lithium salt, active filler and Cu-based compound; the Cu-based compound contains cuprous ions.

[0008] The present invention adds cuprous ions with electrocatalytic activity into an organic-inorganic composite polymer solid electrolyte to regulate the electron cloud distribution of lithium salt anions, thereby promoting the electron-acquisition process of lithium salt anions at the interface of the solid electrolyte, and efficiently reducing them to generate products that are beneficial to the stability of lithium metal, thereby achieving long-term cycle stability, high ionic conductivity and low interface resistance of the lithium battery.

[0009] Preferably, the Cu-based compound includes at least one of tetrafluoroborate copper tetraacetonitrile, hexafluorophosphate copper tetraacetonitrile, cuprous acetate, bis(phenylphosphine) copper nitrate, cuprous selenide, cuprous trifluoromethanesulfonate, bis(triphenylphosphine) borohydride, and cuprous diphenyl phosphate. Further preferably, the Cu-based compound is selected from at least one of tetrafluoroborate copper tetraacetonitrile, hexafluorophosphate copper tetraacetonitrile, cuprous selenide, and hexafluoromethanesulfonate. Especially tetrafluoroborate copper tetraacetonitrile and hexafluorophosphate copper tetraacetonitrile. The tetrafluoroborate copper tetraacetonitrile and the hexafluorophosphate copper tetraacetonitrile have stable anion groups, and the coordination groups are small. The anions are not easily decomposed during the lithium symmetric half-cell cycle, which is beneficial to improve the stability of the lithium metal interface and improve the stable cycle time of the lithium battery.

[0010] Preferably, the mass of the Cu-based compound accounts for 1% to 50% of the total mass of the polyethylene oxide and the polyvinylidene fluoride (hereinafter referred to as the polymer); further preferably, the mass of the Cu-based compound accounts for 5% to 30% of the total mass of the polyethylene oxide and the polyvinylidene fluoride; more preferably, the mass of the Cu-based compound accounts for 5% to 20% of the total mass of the polyethylene oxide and the polyvinylidene fluoride. For example, the mass of the Cu-based compound accounts for 5% to 15%, 8% to 15%, etc. of the total mass of the polyethylene oxide and the polyvinylidene fluoride.

[0011] Preferably, the lithium salt includes at least one of LiTFSI, LiFSI, LiBOB, LiODFB, LiPF6, LiClO4, LiNO3, LiDFP, LiAsF6, LiBF4, and LiOTF.

[0012] Preferably, the molar ratio of EO in the polyethylene oxide to Li in the lithium salt is (2-45):1; further preferably, the molar ratio of EO in the polyethylene oxide to Li in the lithium salt is (4-36):1; more preferably, the molar ratio of EO in the polyethylene oxide to Li in the lithium salt is (4-24):1. For example, the molar ratio of EO in the polyethylene oxide to Li in the lithium salt is (4-18):1, (4-12):1, etc.

[0013] Preferably, the active filler includes at least one of lithium lanthanum zirconium oxide (LLZO), lithium lanthanum zirconium tantalum oxide (LLZTO), lithium aluminum titanium phosphide (LATP), lithium phosphorus sulfur chloride (LPSCl), lithium aluminum germanium phosphate (LAGP), Li3InCl6, Li3YCl6, Li2ZrCl6, and LiPON.

[0014] Preferably, the mass of the active filler accounts for 1% to 50% of the total mass of the polyethylene oxide and the polyvinylidene fluoride; further preferably, the mass of the active filler accounts for 4% to 30% of the total mass of the polyethylene oxide and the polyvinylidene fluoride; more preferably, the mass of the active filler accounts for 5% to 20% of the total mass of the polyethylene oxide and the polyvinylidene fluoride.

[0015] Preferably, the mass ratio of the polyvinylidene fluoride (PVDF) to the polyethylene oxide (PEO) is 1:(1-50); further preferably, the mass ratio of the polyvinylidene fluoride (PVDF) to the polyethylene oxide (PEO) is 1:(1-36); more preferably, the mass ratio of the polyvinylidene fluoride (PVDF) to the polyethylene oxide (PEO) is 1:(1-24). For example, 1:(1-15), 1:(2-10), 1:(3-6).

[0016] Preferably, the organic-inorganic composite polymer solid electrolyte further includes vinylene carbonate and / or lithium nitrate.

[0017] Preferably, the mass of the vinylene carbonate accounts for 1% to 80% of the total mass of the polyethylene oxide and the polyvinylidene fluoride; further preferably, the mass of the vinylene carbonate accounts for 5% to 50% of the total mass of the polyethylene oxide and the polyvinylidene fluoride; more preferably, the mass of the vinylene carbonate accounts for 5% to 30% of the total mass of the polyethylene oxide and the polyvinylidene fluoride. For example, the mass of the vinylene carbonate accounts for 5% to 20%, 5% to 15%, 5% to 10% and the like of the total mass of the polyethylene oxide and the polyvinylidene fluoride.

[0018] Preferably, the mass of the lithium nitrate accounts for 1% to 40% of the total mass of the polyethylene oxide and the polyvinylidene fluoride; further preferably, the mass of the lithium nitrate accounts for 3% to 30% of the total mass of the polyethylene oxide and the polyvinylidene fluoride; more preferably, the mass of the lithium nitrate accounts for 5% to 20% of the total mass of the polyethylene oxide and the polyvinylidene fluoride. In some embodiments of the present invention, the mass of the lithium nitrate accounts for 5% to 10% of the total mass of the polyethylene oxide and the polyvinylidene fluoride.

[0019] The invention also provides a method for preparing the organic-inorganic composite polymer solid electrolyte.

[0020] Specifically, a method for preparing an organic-inorganic composite polymer solid electrolyte comprises the following steps:

[0021] The components are weighed, a solvent is added, and the mixture is mixed; then the mixture is cast and dried to obtain an organic-inorganic composite polymer solid electrolyte.

[0022] Preferably, the polyethylene oxide (PEO) is dried before use, and the drying process is drying at 30-120° C. for 4-30 hours; more preferably, the drying process is drying at 45-80° C. for 4-24 hours.

[0023] Preferably, the solvent includes at least one of benzene, toluene, ethylenediamine, acetone, acetonitrile, dimethylacetamide (DMAC), dimethyl sulfoxide (DMSO), N-methylpyrrolidone (NMP), and N,N-dimethylformamide (DMF).

[0024] Preferably, the mixing process is heating and stirring at 30-150° C. for 2-48 hours to obtain a uniformly mixed slurry; further preferably, the mixing process is heating and stirring at 45-100° C. for 8-20 hours to obtain a uniformly mixed slurry.

[0025] Preferably, the drying process is vacuum drying at 30-120°C for 4-72 hours; further preferably, the drying process is vacuum drying at 45-100°C for 8-36 hours; more preferably, the drying process is vacuum drying at 45-80°C for 8-36 hours, and then naturally drying under argon atmosphere for 5-15 hours.

[0026] The invention also provides an application of an organic-inorganic composite polymer solid electrolyte.

[0027] Specifically, the application of the above organic-inorganic composite polymer solid electrolyte in the preparation of lithium batteries.

[0028] The invention also provides a lithium battery.

[0029] Specifically, a lithium battery includes the above-mentioned organic-inorganic composite polymer solid electrolyte.

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] (1) The present invention introduces a Cu-based targeted additive with electrocatalytic activity into a polyoxyethylene organic-inorganic composite polymer solid electrolyte, anchors anions, regulates the electronic structure of anions at the interface, changes the priority of anion reduction chemistry, and accelerates electron transfer during anion reduction, thereby activating dynamic interface self-reconstruction of lithium metal and constructing a gradient interface rich in Li2O-Li3N-LiF inorganic phases, so that the solid electrolyte has higher ionic conductivity, high lithium ion migration number, high critical current density and lithium stability at room temperature.

[0032] (2) The organic-inorganic composite polymer solid electrolyte provided by the present invention improves the lithium ion conductivity and interface stability of the organic-inorganic composite polymer solid electrolyte by introducing a Cu-based compound targeted additive with electrocatalytic activity, anchoring anions, and regulating the electronic structure of anions at the interface; and by controlling the amount of polyvinylidene fluoride (PVDF), lithium salt, active filler and Cu-based compound added to PEO to adjust its lithium ion conductivity and interface stability, so that the organic-inorganic composite polymer solid electrolyte provided by the present invention has high lithium ion conductivity, low interface impedance, and can greatly improve the symmetric battery at 0.1 mA cm -1 The time for stable cycling at a given current density. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 The lithium ion conductivity diagram of the organic-inorganic composite polymer solid electrolyte prepared in Example 1;

[0034] Figure 2 The interfacial impedance diagram of the lithium symmetric half-cell assembled in Example 1;

[0035] Figure 3 The lithium symmetric half-cell assembled for Example 1 was -1 Cyclic performance test diagram under current density;

[0036] Figure 4 The lithium ion conductivity diagram of the organic-inorganic composite polymer solid electrolyte prepared in Example 2;

[0037] Figure 5 The interfacial impedance diagram of the lithium symmetric half-cell assembled in Example 2;

[0038] Figure 6 The lithium symmetric half-cell assembled for Example 2 was-1 Cyclic performance test diagram under current density;

[0039] Figure 7 The lithium ion conductivity diagram of the organic-inorganic composite polymer solid electrolyte prepared in Example 3;

[0040] Figure 8 The interfacial impedance diagram of the lithium symmetric half-cell assembled in Example 3;

[0041] Fig. 9 The lithium symmetric half-cell assembled for Example 3 was -1 Cyclic performance test diagram under current density;

[0042] Fig.10 The lithium ion conductivity diagram of the organic-inorganic composite polymer solid electrolyte prepared in Example 4;

[0043] Fig.11 The interfacial impedance diagram of the lithium symmetric half-cell assembled in Example 4;

[0044] Fig.12 The lithium symmetric half-cell assembled for Example 4 was tested at 0.1 mA cm -1 Cyclic performance test diagram under current density;

[0045] Fig.13 This is a graph of lithium ion conductivity of the organic-inorganic composite polymer solid electrolyte prepared in Example 5;

[0046] Fig.14 The interfacial impedance diagram of the lithium symmetric half-cell assembled in Example 5;

[0047] Fig.15 The lithium symmetric half-cell assembled for Example 5 was tested at 0.1 mA cm -1 Cyclic performance test diagram under current density;

[0048] Fig.16 The lithium ion conductivity diagram of the organic-inorganic composite polymer solid electrolyte prepared in Example 6;

[0049] Fig.17 The interfacial impedance diagram of the lithium symmetric half-cell assembled in Example 6;

[0050] Fig.18 The lithium symmetric half-cell assembled for Example 6 was -1 Cyclic performance test diagram under current density;

[0051] Fig.19 The lithium ion conductivity diagram of the organic-inorganic composite polymer solid electrolyte prepared in Comparative Example 1;

[0052] Fig. 20 The interfacial impedance diagram of the lithium symmetric half-cell assembled in Comparative Example 1;

[0053] Fig.21 The lithium symmetric half-cell assembled for Comparative Example 1 was -1 Cyclic performance test diagram under current density. DETAILED DESCRIPTION

[0054] In order to make the technical scheme of the present invention more clearly understood by those skilled in the art, the following embodiments are listed for illustration. It should be pointed out that the following embodiments do not limit the protection scope of the present invention.

[0055] Unless otherwise specified, the raw materials, reagents or devices used in the following examples and comparative examples can be obtained from conventional commercial sources or by existing known methods.

[0056] Example 1

[0057] A method for preparing an organic-inorganic composite polymer solid electrolyte comprises the following steps:

[0058] 2.4 g PEO and 0.1 g PVDF were weighed in a mass ratio of 24:1 and set aside. 0.75 g vinylene carbonate and LiTFSI (EO:Li + The molar ratio was 24:1) and then dissolved in acetonitrile solvent. -1 The mixture was stirred at a speed of 300 r min for 10 min to obtain a mixed solution. Subsequently, 0.5 g of LiNO3 (polymer weight percentage 20%) was weighed and added to the above solution, and the mixture was stirred at 300 r min -1 After the LiNO3 is completely dissolved, add 0.5g of cuprous acetate (20% by weight of polymer) and stir for 5min. After the cuprous acetate is completely dissolved, add 0.5g of LLZTO (20wt% polymer) and stir at 250r min. -1 The prepared PVDF and PEO were slowly dispersed and dissolved in the solution, and then stirred at 200 r min -1 The mixture was stirred at 60°C for 24 hours to obtain a uniform slurry, and then dried at 60°C for 20 hours under vacuum, and then naturally dried for 8 hours under argon atmosphere to obtain a polymer electrolyte membrane. The lithium ion conductivity was tested to be 1.9x10 -4 S cm -1 (like Figure 1 ). Metal lithium sheets were used as electrodes on both sides of the polymer electrolyte membrane to assemble a lithium symmetric half-cell. The interface impedance of the assembled lithium symmetric half-cell was 170Ω (e.g. Figure 2), and at 0.1 mA cm -1 The current density can be stably cycled for 900h (such as Figure 3 ).

[0059] Example 2

[0060] A method for preparing an organic-inorganic composite polymer solid electrolyte comprises the following steps:

[0061] 1.8 g PEO and 0.1 g PVDF were weighed in a mass ratio of 18:1 and set aside. 0.38 g vinylene carbonate and LiTFSI (EO:Li + The molar ratio was 20:1) and the mixture was dissolved in toluene solvent. Then, the mixture was stirred at 230 rpm min at RT. -1 The mixture was stirred at a speed of 400 r min for 15 min to obtain a mixed solution. Subsequently, 0.285 g of LiNO3 (15% by weight of polymer) was added to the above solution and stirred at 400 r min -1 After the LiNO3 is completely dissolved, add 0.285g of 2-phenyl copper nitrate (polymer weight percentage is 20%) and stir for 5min. After the 2-phenyl copper nitrate is completely dissolved, add 0.285g of LLZTO (15wt% polymer) and stir at 350r min. -1 The prepared PVDF and PEO were slowly dispersed and dissolved in the solution, and then stirred at 300 r min -1 The mixture was stirred at 100 °C for 6 hours to obtain a uniform slurry, which was then dried at 60 °C for 20 hours under vacuum and then dried naturally in an argon atmosphere for 8 hours to obtain a polymer electrolyte membrane. The lithium ion conductivity was tested to be 2.2x10 -4 Scm -1 (like Figure 3 ). Metal lithium sheets were used as electrodes on both sides of the polymer electrolyte membrane to assemble a lithium symmetric half-cell. The interface impedance of the assembled lithium symmetric half-cell was 149Ω (e.g. Figure 2 ), and at 0.1 mA cm -1 The current density can be stably cycled for 1100h (such as Figure 6 ).

[0062] Example 3

[0063] A method for preparing an organic-inorganic composite polymer solid electrolyte comprises the following steps:

[0064] 1.2 g PEO and 0.1 g PVDF were weighed in a mass ratio of 12:1 and set aside. 0.195 g vinylene carbonate and LiTFSI (EO:Li +The mixture was stirred at 360 rpm min-1 for 45 min at RT to obtain a mixed solution. Then, 0.13 g of LiNO3 (10% by weight of the polymer) was added to the above solution and stirred at 400 r min-1 for 15:1 molar ratio) in turn in NMP solvent. -1 After the LiNO3 is completely dissolved, add 0.156g of bis(triphenylphosphine) cuprous borohydride (12% by weight of polymer) and stir for 10min. After the bis(triphenylphosphine) cuprous borohydride is completely dissolved, add 0.156g of LLZTO (12% by weight of polymer) and stir at 350r min. -1 The prepared PVDF and PEO were slowly dispersed and dissolved in the solution, and then stirred at 300 r min -1 The mixture was stirred at 75°C for 18 hours to obtain a uniform slurry, which was then dried at 60°C for 20 hours under vacuum and then dried naturally in an argon atmosphere for 8 hours to obtain a polymer electrolyte membrane. The lithium ion conductivity was 2.3x10 -4 S cm -1 (like Figure 7 ). Metal lithium sheets were used as electrodes on both sides of the polymer electrolyte membrane to assemble a lithium symmetric half-cell. The interface impedance of the assembled lithium symmetric half-cell was 124Ω (e.g. Figure 8 ), and at 0.1 mA cm -1 The current density can be stably cycled for 1500h (such as Fig. 9 ).

[0065] Example 4

[0066] A method for preparing an organic-inorganic composite polymer solid electrolyte comprises the following steps:

[0067] 0.8g PEO and 0.1g PVDF were weighed in a mass ratio of 8:1 and set aside. 0.09g vinylene carbonate and LiTFSI (EO:Li + The molar ratio was 10:1) and then dissolved in DMSO solvent. -1 The mixture was stirred at a speed of 500 r min for 60 min to obtain a mixed solution. Subsequently, 0.045 g of LiNO3 (5% by weight of polymer) was added to the above solution and stirred at 500 r min -1 After the LiNO3 is completely dissolved, add 0.09g of cuprous diphenyl phosphate (10% by weight of polymer) and stir for 25min. After the cuprous diphenyl phosphate is completely dissolved, add 0.072g of LLZTO (8wt% polymer) and stir at 450r min.-1 The prepared PVDF and PEO were slowly dispersed and dissolved in the solution, and then stirred at 400 r min -1 The mixture was stirred at 45°C for 20 hours to obtain a uniform slurry, which was then dried at 60°C for 20 hours under vacuum and then dried naturally in an argon atmosphere for 8 hours to obtain a polymer electrolyte membrane. The lithium ion conductivity was tested to be 2.8x10 -4 Scm -1 (like Fig.10 ). Metal lithium sheets were used as electrodes on both sides of the polymer electrolyte membrane to assemble a lithium symmetric half-cell. The interface impedance of the assembled lithium symmetric half-cell was 114Ω (e.g. Fig.11 ), and at 0.1mAcm -1 The current density can be stably cycled for 1800h (such as Fig.12 ).

[0068] Example 5

[0069] A method for preparing an organic-inorganic composite polymer solid electrolyte comprises the following steps:

[0070] 0.5 g PEO and 0.1 g PVDF were weighed in a mass ratio of 5:1 and set aside. 0.03 g vinylene carbonate and LiTFSI (EO:Li + The molar ratio was 4:1) and then dissolved in ethylenediamine solvent. -1 The mixture was stirred at a speed of 500 r min for 10 min to obtain a mixed solution. Subsequently, 0.045 g of LiNO3 (5% by weight of polymer) was added to the above solution and stirred at 500 r min -1 After the LiNO3 is completely dissolved, add 0.072g of copper tetraacetonitrile hexafluorophosphate (12% by weight of polymer) and stir for 60min. After the copper tetraacetonitrile hexafluorophosphate is completely dissolved, add 0.03g of LLZTO (5wt% polymer) and stir at 300r min. -1 The prepared PVDF and PEO were slowly dispersed and dissolved in the solution, and then stirred at 350 r min-1 for 30 hours at 30 ° C to obtain a uniform slurry, which was then dried at 60 ° C for 20 hours under vacuum and then naturally dried for 8 hours in an argon atmosphere to obtain a polymer electrolyte membrane. The lithium ion conductivity was tested to be 5x10 -4 Scm -1 (like Fig.13 ). Metal lithium sheets are used as electrodes on both sides of the polymer electrolyte membrane to assemble a lithium symmetric half-cell. The interface impedance of the assembled lithium symmetric half-cell is 101Ω (such as Fig.14), and at 0.1 mA cm -1 The current density can be stably cycled for 2000h (such as Fig.15 ).

[0071] Example 6

[0072] A method for preparing an organic-inorganic composite polymer solid electrolyte comprises the following steps:

[0073] 1.6 g PEO and 0.4 g PVDF were weighed in a mass ratio of 4:1 and set aside. 0.16 g vinylene carbonate and LiTFSI (EO:Li + The molar ratio was 12:1) and the mixture was dissolved in DMAC solvent. -1 The mixture was stirred at a speed of 300 r min for 10 min to obtain a clear solution. Subsequently, 0.2 g of LiNO3 (10% by weight of polymer) was added to the above solution and stirred at 300 r min -1 After the LiNO3 is completely dissolved, add 0.2 g of tetrafluoroborate copper tetraacetonitrile (10% by weight of polymer) and stir for 5 min. After the tetrafluoroborate copper tetraacetonitrile is completely dissolved and the solution begins to change color, add 0.2 g of LLZTO (10 wt% polymer) and stir at 250 r min. -1 The prepared PVDF and PEO were slowly dispersed and dissolved in the solution, and then stirred at 200 r min -1 The mixture was stirred at 60°C for 24 hours to obtain a uniform slurry, and then dried at 60°C for 20 hours under vacuum, and then naturally dried for 8 hours under argon atmosphere to obtain a polymer electrolyte membrane. The lithium ion conductivity was tested to be 5.5x10 -4 Scm -1 (like Fig.16 ). Metal lithium sheets were used as electrodes on both sides of the polymer electrolyte membrane to assemble a lithium symmetric half-cell. The interface impedance of the assembled lithium symmetric half-cell was 43.2Ω (e.g. Fig.17 ), and at 0.1 mA cm -1 The current density can be stably cycled for 2600h (such as Fig.18 The organic-inorganic composite polymer solid electrolyte provided in this embodiment adjusts its lithium ion conductivity and interface stability by adding a specific proportion of polyvinylidene fluoride (PVDF), lithium salt, active filler and Cu-based targeted additive to PEO, so that the lithium ion conductivity of the organic-inorganic composite polymer solid electrolyte reaches 5.5x10-4 S cm -1 The interface impedance is only 43.2, and the symmetrical battery is 0.1 mA cm -1 The current density can be stably cycled for more than 2600h.

[0074] Comparative Example 1

[0075] A method for preparing an organic-inorganic composite polymer solid electrolyte comprises the following steps:

[0076] 1.6 g PEO and 0.4 g PVDF761 were weighed in a mass ratio of 4:1 and set aside. 0.16 g vinylene carbonate and LiTFSI (EO:Li + The molar ratio was 12:1) and the mixture was dissolved in DMAC solvent. -1 The mixture was stirred at 250 r min for 10 min to obtain a clear solution. Subsequently, 0.2 g LLZTO (10 wt% polymer) was added to the above solution and the mixture was stirred at 250 r min for 10 min to obtain a clear solution. -1 The prepared PVDF and PEO were slowly dispersed and dissolved in the solution, and then stirred at 200 r min -1 The mixture was stirred at 60°C for 24 hours to obtain a uniform slurry, which was then dried at 60°C for 20 hours under vacuum and then dried naturally in an argon atmosphere for 8 hours to obtain a polymer electrolyte membrane. The lithium ion conductivity was tested to be 1.4x10 -4 Scm -1 (like Fig.19 ). Metal lithium sheets were used as electrodes on both sides of the polymer electrolyte membrane to assemble a lithium symmetric half-cell. The interface impedance of the assembled lithium symmetric half-cell was 225.8Ω (e.g. Fig. 20 ), and at 0.1 mA cm -1 The current density can be stably cycled for 700h (such as Fig.21 ).

[0077] Comparative Example 2

[0078] A method for preparing an organic-inorganic composite polymer solid electrolyte comprises the following steps:

[0079] 1.6 g PEO and 0.4 g PVDF761 were weighed in a mass ratio of 4:1 and set aside. 0.16 g vinylene carbonate and LiTFSI (EO:Li + The molar ratio was 12:1) and the mixture was dissolved in DMAC solvent. -1 The mixture was stirred at a speed of 300 r min for 10 minutes to obtain a clear solution. Subsequently, 0.1 g of LiNO3 (5% by weight of polymer) was added to the above solution and stirred at 300 r min -1 Then, 0.2 g LLZTO (10 wt% polymer) was added to the solution and stirred at 250 r min.-1 The prepared PVDF and PEO were slowly dispersed and dissolved in the solution, and then stirred at 200 r min -1 The mixture was stirred at 60°C for 24 hours to obtain a uniform slurry, which was then dried at 60°C for 20 hours under vacuum and then dried naturally in an argon atmosphere for 8 hours to obtain a polymer electrolyte membrane. The lithium ion conductivity was 3.61x10 -4 S cm -1 Metal lithium sheets were used as electrodes on both sides of the polymer electrolyte membrane to assemble a lithium symmetric half-cell. The interfacial impedance of the assembled lithium symmetric half-cell was 83.3Ω, and the -1 The current density can be stably cycled for 1000h.

[0080] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. An organic-inorganic composite polymer solid electrolyte, characterized in that: The invention comprises the following components: polyethylene oxide, polyvinylidene fluoride, lithium salt, active filler and Cu-based compound; the Cu-based compound contains cuprous ions.

2. The organic-inorganic composite polymer solid electrolyte according to claim 1, characterized in that: The Cu-based compound includes at least one of tetraacetonitrile copper tetrafluoroborate, tetraacetonitrile copper hexafluorophosphate, cuprous acetate, bis(phenylphosphine) copper nitrate, cuprous selenide, cuprous trifluoromethanesulfonate, cuprous bis(triphenylphosphine) borohydride, and cuprous diphenyl phosphate.

3. The organic-inorganic composite polymer solid electrolyte according to claim 1 or 2, characterized in that: The mass of the Cu-based compound accounts for 1% to 50% of the total mass of the polyethylene oxide and the polyvinylidene fluoride; preferably, the mass of the Cu-based compound accounts for 5% to 30% of the total mass of the polyethylene oxide and the polyvinylidene fluoride.

4. The organic-inorganic composite polymer solid electrolyte according to claim 1 or 2, characterized in that: The lithium salt includes at least one of LiTFSI, LiFSI, LiBOB, LiODFB, LiPF6, LiClO4, LiNO3, LiDFP, LiAsF6, LiBF4, and LiOTF.

5. The organic-inorganic composite polymer solid electrolyte according to claim 4, characterized in that: The molar ratio of EO in the polyethylene oxide to Li in the lithium salt is (2-45):

1.

6. The organic-inorganic composite polymer solid electrolyte according to claim 1 or 2, characterized in that: The active filler includes at least one of lithium lanthanum zirconium oxide, lithium lanthanum zirconium tantalum oxide, lithium aluminum titanium phosphorus, lithium phosphorus sulfur chlorine, lithium germanium aluminum phosphate, Li3InCl6, Li3YCl6, Li2ZrCl6, and LiPON.

7. The organic-inorganic composite polymer solid electrolyte according to claim 1 or 2, characterized in that: The organic-inorganic composite polymer solid electrolyte further comprises vinylene carbonate and / or lithium nitrate.

8. The method for preparing the organic-inorganic composite polymer solid electrolyte according to any one of claims 1 to 7, characterized in that: The following steps are involved: The components are weighed, a solvent is added, and the mixture is mixed; then the mixture is cast and dried to obtain an organic-inorganic composite polymer solid electrolyte.

9. Use of the organic-inorganic composite polymer solid electrolyte according to any one of claims 1 to 7 in the preparation of lithium batteries.

10. A lithium battery, characterized in that: The invention comprises the organic-inorganic composite polymer solid electrolyte according to any one of claims 1 to 7.

Citation Information

Cited By

  • Chloride enhanced polymer electrolyte, preparation method and application thereof

    CN121035317A

  • Chloride-enhanced polymer electrolytes, methods of making, and uses thereof