Low-temperature high-voltage sodium-ion battery electrolyte
By using carbonate solvents and flame-retardant and film-forming additives in sodium ion battery electrolyte, the electrode/electrolyte interface layer is constructed, and the performance attenuation and safety of sodium ion battery at low temperatures is solved, and high efficiency is achieved. Stable sodium ion battery runs.
Patent Information
- Application Number
- CN202411298120.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-18
- Publication Date
- 2024-11-08
AI Technical Summary
Sodium ion batteries exhibit problems such as increased electrolyte viscosity, reduced ion conductivity, and slow Na+ transmission kinetics under low temperature environments, resulting in significant attenuation of specific capacity, energy density, power density and cycle life, and ether-based electrolyte cannot To meet the needs of high voltage operation, carbonate-based electrolyte has low ionic conductivity and slow kinetics at low temperatures.
Adopt carbonate solvent system, add flame retardant and film-forming additives such as ethoxy pentafluorocyclophosphazene (PFPN) and sodium difluorooxalic acid borate (NaDFOB) to build an electrode rich in inorganic substances such as Na3N and NaF/ The electrolyte interface layer improves Na+ transmission efficiency and battery cycle stability, meets the needs of high voltage operation and reduces the risk of low-temperature spontaneous combustion.
It effectively reduces the internal resistance of sodium ion batteries at low temperatures, improves Na+ transmission efficiency and cycle stability, broadens the electrochemical stability window of electrolyte, and ensures the safe and efficient operation of sodium ion batteries under low temperature conditions.
Smart Images

Figure CN118919843A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electrochemistry, and in particular relates to a low-temperature and high-voltage sodium ion battery electrolyte. Background Art
[0002] Lithium-ion batteries (LIBs) have the advantages of high operating voltage, high energy density and long cycle life, which make them widely used in portable electronic products, electric vehicles and other fields. However, they are faced with problems such as uneven distribution of lithium resources and poor safety, which restrict the future large-scale use of LIBs. Sodium-ion batteries (SIBs) have a lower manufacturing cost than LIBs due to the abundant reserves of sodium resources in nature. In addition, SIBs have a higher internal resistance than LIBs, and generate less instantaneous heat and have a lower temperature rise in safety tests such as short circuits. Therefore, as an important supplement to LIBs, SIBs are expected to be used in large-scale energy storage, low-speed electric vehicles and other aspects. With the expansion of actual application scenarios, secondary batteries have gradually exposed problems such as performance degradation, safety, and poor endurance when used in low-temperature environments such as high latitudes, aerospace, and deep sea. SIBs have a similar working mechanism to LIBs, and sodium and lithium have similar physical and chemical properties. However, compared with Li + In comparison, Na + The Stokes radius is smaller, and the sodium ion-based electrolyte system has higher conductivity and lower desolvation energy at the same concentration, which gives SIBs better low-temperature performance, meaning that sodium ion batteries have broader development prospects.
[0003] At low temperatures, SIBs still face the problems of significantly increased electrolyte viscosity, decreased ionic conductivity, and Na + Desolvation energy is difficult, resulting in Na + Problems such as slow transfer kinetics cause a significant decline in the specific capacity, energy density, power density, and cycle life of SIBs, severe battery polarization, and even sodium precipitation at the negative electrode. The electrolyte is one of the important components of sodium-ion batteries. Ether-based electrolytes usually cannot meet the high-voltage operation requirements of SIBs. Most carbonate-based electrolytes are limited by their own high melting point and high viscosity, and have low ionic conductivity and sluggish kinetics at low temperatures. Therefore, researchers have focused their attention on optimizing the components of carbonate-based electrolytes, such as developing new solvents, using co-solvents, and introducing additives to improve the physical and chemical properties of the electrolyte and its compatibility with electrodes, thereby solving problems such as poor cycle stability, low energy density, and low safety of SIBs under low-temperature environments. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a low-temperature and high-pressure sodium ion battery electrolyte. The low-temperature and high-pressure sodium ion battery electrolyte proposed by the present invention adopts a carbonate solvent system, and by adding flame retardant additives and film-forming additives such as ethoxy pentafluorocyclophosphazene (PFPN) and sodium difluorooxalatoborate (NaDFOB), a Na-rich electrolyte is constructed. 3 The electrode / electrolyte interface layer of inorganic materials such as N and NaF effectively reduces the internal resistance of SIBs under low temperature conditions and improves the Na + The transmission efficiency and low-temperature cycle stability of the battery are improved. In addition, the electrolyte uses flame-retardant carbonate solvents, and the film-forming additives NaDFOB and flame-retardant phosphate additives PFPN are introduced, which not only meet the high-voltage operation requirements of SIBs, but also reduce the possibility of battery spontaneous combustion under low-temperature conditions.
[0005] The present invention provides a low-temperature and high-voltage sodium ion battery electrolyte, which is characterized by being realized by the following technical solutions:
[0006] The electrolyte comprises a carbonate solvent, a sodium salt, a flame retardant additive and a film-forming additive, wherein the carbonate solvent is selected from one or more combinations of ethylene carbonate (EC), propylene carbonate (PC), dimethyl carbonate (DMC), diethyl carbonate (DEC) and ethyl methyl carbonate (EMC).
[0007] The sodium salt is sodium perchlorate (NaClO 4 ), sodium hexafluorophosphate (NaPF 6 ), sodium bis(fluorosulfonyl)imide (NaFSI), sodium bis(trifluoromethylsulfonyl)imide (NaTFSI), sodium tetrafluoroborate (NaBF 4 ), sodium trifluoromethanesulfonate (NaOTF), and the concentration in the electrolyte is 0.5 to 2 mol / L.
[0008] The flame retardant additive is one or more combinations of phosphate solvents, such as ethoxypentafluorocyclophosphazene (PFPN), phenoxypentafluorocyclotriphosphazene (FPPN), and tris(2,2,2-trifluoroethyl) phosphate (FTEP), and accounts for 1% to 10% by volume in the electrolyte.
[0009] The film-forming additive is at least one of sodium difluorooxalatoborate (NaDFOB) and sodium dioxalatoborate (NaBOB), which is used in combination with a flame-retardant phosphate additive and accounts for 0.1% to 5% by mass in the electrolyte.
[0010] As a preferred technical solution of the present invention, when the carbonate solvent is selected from ethylene carbonate (EC) and propylene carbonate (PC), the volume ratio is 1:1.
[0011] As a preferred technical solution of the present invention, the sodium salt is sodium perchlorate (NaClO 4 ), the concentration in the electrolyte is 1 mol / L.
[0012] As a preferred technical solution of the present invention, the flame retardant additive, ethoxy pentafluorocyclophosphazene (PFPN), accounts for 5% by volume in the electrolyte, and the film-forming additive, sodium difluorooxalatoborate (NaDFOB), accounts for 0.5% by mass in the electrolyte.
[0013] The present invention uses a sodium ion battery assembled with the above electrolyte, and the sodium ion battery comprises a positive electrode sheet, a negative electrode sheet, a separator and the above low-temperature and high-pressure sodium ion battery electrolyte.
[0014] In the above sodium ion battery, the positive electrode sheet comprises a positive electrode current collector, a positive electrode active material, a conductive agent and a binder.
[0015] Furthermore, the positive electrode active material is a layered oxide with a structural formula of NaM x O y , M is selected from any one or more of iron, copper, nickel, cobalt and manganese, and the value ranges of x and y are: 0.8≤x≤1.5, 1.5≤y≤2.5.
[0016] As a preferred technical solution of the present invention, the positive electrode active material is O3 type Na[Ni 1 / 3 Fe 1 / 3 Mn 1 / 3 ]O 2 (NNFMO), single-sided coated on an aluminum foil current collector.
[0017] The conductive agent is selected from any one or a combination of at least two of Super P, acetylene black, Ketjen black, conductive graphite, carbon nanotubes, graphene or carbon fiber, preferably Super P conductive agent.
[0018] The binder is selected from any one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyacrylic acid (PCA), sodium alginate (SA), carboxymethyl cellulose (CMC), sodium carboxymethyl cellulose (CMC-Na), styrene-butadiene rubber (SBR), or a combination of at least two thereof, preferably polyvinylidene fluoride (PVDF) binder.
[0019] In the above sodium ion battery, the negative electrode plate is mainly composed of negative electrode active material.
[0020] Further negative electrode active materials include one or more combinations of metal sodium sheets, hard carbon, soft carbon, sodium titanate, and sodium alloys, preferably metal sodium negative electrodes.
[0021] In the above sodium ion battery, the separator is selected from any one of Celgard 2500 separator, Celgard 2325 separator or glass fiber separator or a combination of at least two thereof, preferably a glass fiber separator.
[0022] The advantages and positive effects of the present invention are:
[0023] The present invention obtains a low-temperature and high-voltage sodium ion battery electrolyte by introducing flame retardant additives and film-forming additives into a carbonate-based electrolyte. Compared with an electrolyte without additives, the flame retardant and film-forming additives introduced into the carbonate-based electrolyte not only improve the electrode / electrolyte interface microstructure, reduce the battery internal resistance, and improve the low-temperature cycle performance, but also broaden the electrochemical stability window of the electrolyte to meet the high-voltage operation requirements, thereby ensuring that the sodium ion battery can be used safely, stably and efficiently under low-temperature conditions. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 The O3 type Na[Ni 1 / 3 Fe 1 / 3 Mn 1 / 3 ]O 2 X-ray diffraction (XRD) pattern of (NNFMO);
[0025] Figure 2 It is the linear sweep voltammetry (LSV) curve of the Na / / Al battery based on different electrolytes in Example 1 and Example 2 at room temperature and 0.1 mV / s.
[0026] Figure 3 1 is the cycle performance curve of Na / / NNFMO battery based on different electrolytes at -20°C and 0.1C in Example 1 and Example 2;
[0027] Figure 4 The charge and discharge curves of the Na / / NNFMO battery based on different electrolytes in Example 1 and Example 2 at -20°C and 0.1C. DETAILED DESCRIPTION
[0028] The present invention is further described in detail below through specific examples. The following examples can enable those skilled in the art to more fully understand the present invention, but do not limit the present invention in any way.
[0029] Embodiment 1:
[0030] (1) Preparation of electrolyte based on PFPN additive, the specific process is as follows: In a glove box with high-purity argon atmosphere (O 2 <0.01ppm,H 2O<0.01ppm), the composition is 1.0M NaClO 4 5% PFPN was added to the blank electrolyte (purchased from Duoduo Reagent) of / EC-PC (solvent volume ratio 1:1), and after fully stirring, The molecular sieve was used to remove water, and the obtained electrolyte was recorded as blank + 5% PFPN.
[0031] (2) Preparation of NNFMO positive electrode, the specific process is as follows: 1 part by weight of PVDF binder is added to N-methyl-2-pyrrolidone (NMP), and stirred thoroughly until dissolved. At the same time, 7 parts by weight of NNFMO and 2 parts by weight of Super P are mixed and ground for 30 minutes. The mixture is then added to NMP dissolved with PVDF and stirred thoroughly for 36 hours until there is no particle feeling to obtain a mixed slurry, which is evenly coated on aluminum foil, dried, and cut into a diameter of 8 mm and an average loading of 3 mg / cm 2 NNFMO positive electrode plate;
[0032] (3) Na / / Al battery assembly and LSV testing. The specific process is as follows: In a glove box with a high-purity argon atmosphere (O 2 <0.01ppm, H 2 O<0.01ppm), a sodium metal sheet was used as the negative electrode, an aluminum foil with a diameter of 10mm was used as the positive electrode, a glass fiber separator was used, and the above blank and blank + 5% PFPN electrolytes were used to assemble Na / / Al batteries. The assembled battery was taken out of the glove box and left at room temperature for 12 hours. The LSV test was performed on the Autolab multi-channel electrochemical workstation to examine its electrochemical stability window, with a scan rate of 0.1mV / s.
[0033] (4) Na / / NNFMO battery assembly and cycle performance test. The specific process is as follows: In a glove box with a high-purity argon atmosphere (O 2 <0.01ppm, H 2O<0.01ppm), using sodium metal as the negative electrode, using the above-mentioned NNFMO positive electrode, glass fiber separator, blank electrolyte or blank + 5% PFPN electrolyte to assemble Na / / NNFMO battery. The assembled battery was taken out of the glove box, placed in a constant temperature box at 25°C, left for 12h, charged to 4.0V at a current density of 0.4C (1C = 130mA / g) on a Neware CT-4008 battery tester, and then discharged to 2.0V at the same current density, pre-cycled for 5 weeks, and then transferred to a constant temperature box at -20°C, left for 4h, charged to 4.0V at a current density of 0.1C (1C = 130mA / g) on a Neware CT-4008 battery tester, then charged to 0.05C cutoff at a constant voltage of 4.0V, and then discharged to 2.0V at 0.1C, and low-temperature cycling was performed in this way.
[0034] Embodiment 2:
[0035] (1) Preparation of electrolyte based on PFPN and NaDFOB additives. The specific process is as follows: In a glove box with high-purity argon atmosphere (O 2 <0.01ppm,H 2 O<0.01ppm), add 5% by volume of PFPN to the blank electrolyte, stir well, weigh the mixed solution, add 0.5% by volume of NaDFOB, and then add The molecular sieve was used to remove water, and the obtained electrolyte was recorded as blank + 5% PFPN + 0.5% NaDFOB electrolyte.
[0036] (2) Prepare the NNFMO positive electrode, the specific process is the same as in Example 1.
[0037] (3) Na / / Al battery assembly and LSV testing: In a glove box with high-purity argon atmosphere (O 2 <0.01ppm, H 2 O<0.01ppm), a Na / / Al battery was assembled with blank+5%PFPN+0.5%NaDFOB electrolyte, and an LSV test was performed on it. The specific process is the same as in Example 1.
[0038] (4) Na / / NNFMO battery assembly and cycle performance testing: In a glove box with a high-purity argon atmosphere (O 2 <0.01ppm, H 2 O<0.01ppm), a Na / / NNFMO battery was assembled with blank+5%PFPN+0.5%NaDFOB as the electrolyte, and the cycle performance was tested, the specific process is as in Example 1.
[0039] (5) Na / / NNFMO battery rate performance test, the specific process is as follows: first, the Na / / NNFMO battery based on blank + 5% PFPN + 0.5% NaDFOB electrolyte assembled in the above step (4) was placed at 25°C for 12 hours, and then pre-circulated for 5 weeks at a current density of 0.4C in the voltage range of 2.0-4.0V. Then the battery was transferred to a -20°C incubator, and the battery was charged and discharged at different current densities. The current was gradually increased from 0.1C to 1C (1C = 130mA / g) in steps of 0.1C, and the battery rate performance at -20°C was obtained as shown in Table 1:
[0040] Table 1
[0041]
[0042] According to the data in Table 1, the Na / / NNFMO battery based on blank + 5% PFPN + 0.5% NaDFOB electrolyte can achieve a discharge specific capacity of 100.52 mAh / g at -20°C and 0.1C, and has a discharge specific capacity of 40.47 mAh / g at -20°C and 1C, showing excellent low-temperature rate performance.
[0043] Figure 1 The O3 type Na[Ni 1 / 3 Fe 1 / 3 Mn 1 / 3 ]O 2 XRD spectrum of (NNFMO). Figure 1 As shown in the figure, the NNFMO powder diffraction peak in the XRD pattern is basically consistent with the standard card PDF#25-0819, indicating that this ternary material is a pure phase transition metal oxide type with an O3 stacking sequence (O3-NaTMO 2 ), corresponding to the R3m space group.
[0044] Figure 2 The LSV curves of Na / / Al batteries obtained in Example 1 and Example 2 based on electrolytes with different additives at room temperature and 0.1 mV / s. Figure 2 As shown, the starting voltages of the oxidative decomposition reactions of the blank + 5% PFPN and blank + 5% PFPN + 0.5% NaDFOB electrolytes are 4.80 V and 4.89 V, respectively, both of which are higher than the blank electrolyte with an oxidation potential of 4.68 V, indicating that the sodium ion electrolytes containing additives in Examples 1 and 2 of the present invention have excellent antioxidant capacity and can enable SIBs to operate at high voltage.
[0045] Figure 3The cycle performance curves of the Na / / NNFMO battery based on different electrolytes in Example 1 and Example 2 under the conditions of 2.0-4.0V voltage range, -20℃ temperature and 0.1C current density. Figure 3 It can be seen that in Examples 1 and 2 of the present invention, the Na / / NNFMO batteries assembled with blank + 5% PFPN and blank + 5% PFPN + 0.5% NaDFOB electrolytes have a high coulombic efficiency close to 100% at -20°C and 0.1C, and the specific capacity is basically maintained at 91 mAh / g and 86 mAh / g in 3 to 25 cycles and 1 to 25 cycles, respectively, while the Na / / NNFMO battery assembled with the blank electrolyte shows a more obvious capacity decay, proving that the low-temperature and high-pressure sodium ion electrolyte obtained by introducing NaDFOB and PFPN additives in the present invention can construct a stable, uniform and strong SEI on the electrode surface, inhibiting the further decomposition of the electrolyte during the cycle, and showing good compatibility with the NNFMO positive electrode, so that the Na / / NNFMO battery has better low-temperature cycle stability.
[0046] Figure 4 The charge and discharge curves of the Na / / NNFMO battery based on different electrolytes in Example 1 and Example 2 at the 25th cycle under the conditions of 2.0-4.0V voltage range, -20℃ temperature and 0.1C current density. Figure 4 As shown in the figure, the charge and discharge curves corresponding to the Na / / NNFMO batteries assembled with blank, blank + 5% PFPN, blank + 5% PFPN + 0.5% NaDFOB electrolytes in Example 1 and Example 2, the discharge voltage platforms are 2.76, 2.83, and 2.77 V, respectively. Among them, the electrolyte after the introduction of flame retardant and film-forming additives makes the Na / / NNFMO battery show a greater platform capacity contribution, indicating that the PFPN and NaDFOB additives introduced in the present invention can improve the Na + Transport dynamics.
Claims
1. A low-temperature and high-voltage sodium ion battery electrolyte, characterized in that: Based on the flame-retardant carbonate solvent system, flame retardant additives and film-forming additives are introduced to broaden the antioxidant capacity and safety of the electrolyte, and a solid electrolyte interface film rich in inorganic substances such as Na3N and NaF is constructed, which effectively reduces the internal resistance of the battery and improves the Na + transfer efficiency and low-temperature cycling performance of sodium-ion batteries.
2. A low-temperature and high-voltage sodium ion battery electrolyte, characterized in that The steps include: (1) In a glove box filled with high-purity argon (O2<0.01ppm, H2O<0.01ppm), a certain volume percentage of a flame retardant phosphate additive is added to an electrolyte consisting of a carbonate solvent and a certain concentration of sodium salt, and the mixture is stirred thoroughly; (2) In a glove box filled with high-purity argon (O2<0.01ppm, H2O<0.01ppm), weigh the mass of the mixed solution in step (1), add a film-forming additive accounting for a certain mass percentage of the mixed solution, and then add The molecular sieve removes water to obtain a low-temperature and high-pressure sodium ion battery electrolyte.
3. A low-temperature and high-pressure sodium ion battery electrolyte according to claim 2, characterized in that: The carbonate solvent described in step (1) is selected from one or more combinations of ethylene carbonate (EC), propylene carbonate (PC), dimethyl carbonate (DMC), diethyl carbonate (DEC), and ethyl methyl carbonate (EMC).
4. The low-temperature and high-pressure sodium ion battery electrolyte according to claim 2, characterized in that: The sodium salt described in step (1) is one or more combinations of sodium perchlorate (NaClO4), sodium hexafluorophosphate (NaPF6), sodium bis(fluorosulfonyl)imide (NaFSI), sodium bis(trifluoromethylsulfonyl)imide (NaTFSI), sodium tetrafluoroborate (NaBF4), and sodium trifluoromethanesulfonate (NaOTF), and the concentration in the electrolyte is 0.5 to 2 mol / L.
5. The low-temperature and high-pressure sodium ion battery electrolyte according to claim 2, characterized in that: The flame retardant phosphate additive described in step (1) is one or more combinations of ethoxy pentafluorocyclophosphazene (PFPN), phenoxy pentafluorocyclotriphosphazene (FPPN), and tris(2,2,2-trifluoroethyl) phosphate (FTEP), and the volume proportion in the electrolyte is 1% to 10%.
6. The low-temperature and high-pressure sodium ion battery electrolyte according to claim 2, characterized in that: The film-forming additive in step (2) is at least one of sodium difluorooxalatoborate (NaDFOB) and sodium dioxalatoborate (NaBOB), and its mass proportion in the electrolyte is 0.1% to 5%.