Lithium ion battery containing carbon negative electrode material and low-temperature quantitative formation process of lithium ion battery

By using a low-temperature quantitative formation process in lithium-ion batteries, controlling the consumption of lithium-ion and the formation of SEI films, the problems of low charging and discharging efficiency of lithium-ion batteries and poor SEI films in traditional processes are solved, and high-efficiency lithium-ion is achieved Battery process.

CN118919867APending Publication Date: 2024-11-08MEIZHOU LIANGNENG NEW ENERGY SCI & TECHCO
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411077535.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Traditional high-temperature or high-alloy-current formation processes are difficult to effectively control the consumption of lithium ions, resulting in a reduction in the charging and discharging efficiency of lithium ion batteries and poor density and uniformity of SEI films.

Method used

The low-temperature quantitative formation process is adopted, including low-current constant current charging of 0.01C to 0.1C at a temperature of -30℃ to 5℃, and aging at a temperature of -20℃ to 45℃, combining the low-temperature, normal-temperature and high-temperature stand-off steps , controls lithium ion consumption and SEI film formation.

Benefits of technology

Effectively control the consumption of lithium ions, no more than 10%, to form a dense, uniform and thin SEI film, which improves the charging and discharging efficiency of lithium ion batteries and reduces the resistance of the SEI film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919867A_ABST
    Figure CN118919867A_ABST
Patent Text Reader

Abstract

The invention provides a lithium ion battery containing a carbon negative electrode material and a low-temperature quantitative formation process of the lithium ion battery. The low-temperature quantitative formation process of the lithium ion battery containing the carbon negative electrode material comprises the following steps: acquiring a lithium ion battery A which is filled with liquid and contains the carbon negative electrode material; carrying out constant-current charging on the lithium ion battery A containing the carbon negative electrode material to 8% SOC to 20% SOC by adopting a small current of 0.01 C to 0.1 C under the temperature condition of-30 DEG C to 5 DEG C, so as to obtain a lithium ion battery B containing the carbon negative electrode material; and aging the lithium ion battery B containing the carbon negative electrode material at the temperature of-20 DEG C to 45 DEG C for 12-48 hours to obtain the lithium ion battery containing the carbon negative electrode material. According to the formation process, the formation operation is carried out by adopting low-temperature small constant current, so that the consumption of lithium ions in the actual electrolyte is well controlled, and the aging operation is matched, so that the formation of a compact and thin SEI film is facilitated, and the lithium ion battery containing a carbon negative electrode material is ensured to have relatively high charge-discharge efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the technical field of lithium-ion batteries, and in particular to a lithium-ion battery containing a carbonaceous negative electrode material and a low-temperature quantitative formation process thereof. Background Art

[0002] There are many formation processes for lithium-ion batteries, such as negative pressure formation, open-mouth formation, closed-mouth formation, high-temperature formation, low-temperature formation, high-current formation, low-current formation, etc. As Chinese patent documents CN 113346156A and CN 115295905 A show, high-temperature formation or high-current formation is used to form a SEI film on the negative electrode surface.

[0003] In the actual application of lithium-ion batteries, since the negative electrode material of lithium-ion batteries is generally a carbon-based negative electrode material, and the first coulomb efficiency of carbon-based negative electrode materials after formation is generally 90% to 92%, this means that during the formation process, only about 10% of the lithium ions in the electrolyte need to be consumed to meet the formation of the negative electrode SEI film and the consumption of side reactions. However, since it is difficult to control the consumption of lithium ions in the actual electrolyte during traditional high-temperature formation or high-current formation, the consumption of lithium ions usually appears to be greater than 10%, which reduces the charge and discharge efficiency of lithium-ion batteries containing carbon-based negative electrode materials. In addition, traditional high-temperature formation or high-current formation will also cause the SEI film to be thick and uneven, that is, there is a problem of poor compactness. Summary of the invention

[0004] The purpose of the present disclosure is to overcome the shortcomings of the prior art and provide a lithium-ion battery containing carbon-based negative electrode materials and its low-temperature quantitative formation process, which can better control the consumption of lithium ions in the actual electrolyte and is conducive to forming a dense, uniform and thin SEI film, thereby ensuring that the lithium-ion battery containing carbon-based negative electrode materials has a higher charge and discharge efficiency.

[0005] The purpose of this disclosure is achieved through the following technical solutions:

[0006] A low-temperature quantitative formation process for a lithium-ion battery containing a carbonaceous negative electrode material, comprising the following steps:

[0007] Obtain a lithium-ion battery A filled with liquid and containing a carbonaceous negative electrode material;

[0008] Under the temperature condition of -30°C to 5°C, the lithium ion battery A containing the carbonaceous negative electrode material is charged to 8% SOC to 20% SOC with a small current of 0.01C to 0.1C to obtain a lithium ion battery B containing the carbonaceous negative electrode material;

[0009] The lithium ion battery B containing the carbonaceous negative electrode material is placed at a temperature of -20°C to 45°C for aging for 12h to 48h to obtain a lithium ion battery containing the carbonaceous negative electrode material.

[0010] In one embodiment, the small current is 0.01C to 0.05C.

[0011] In one embodiment, the lithium-ion battery A containing the carbonaceous negative electrode material is charged with a constant current to 8% SOC to 15% SOC.

[0012] In one embodiment, the step of aging the lithium ion battery B containing the carbonaceous negative electrode material at a temperature of -20°C to 45°C for 12h to 48h includes the following specific steps:

[0013] The lithium ion battery B containing the carbonaceous negative electrode material is placed at low temperature for 0.5 h to 1 h, wherein the low temperature is -20°C to 2°C;

[0014] The lithium-ion battery B containing the carbonaceous negative electrode material which has been placed at low temperature is placed at room temperature for 8 hours to 35 hours; wherein the room temperature is 20° C. to 35° C.;

[0015] The lithium ion battery B containing the carbonaceous negative electrode material which has been left at room temperature is left at high temperature for 3.5 hours to 12 hours, wherein the high temperature is 40° C. to 45° C.

[0016] In one embodiment, under the temperature condition of -30°C to 5°C, the step of constant current charging the lithium ion battery A containing the carbonaceous negative electrode material to 8% SOC to 20% SOC with a small current of 0.01C to 0.1C includes the following specific steps:

[0017] The lithium ion battery A containing the carbonaceous negative electrode material is charged with a first constant current at a temperature of 0°C to 5°C and a current of 0.05C to 0.1C, and the lithium ion battery A containing the carbonaceous negative electrode material is charged to 1% SOC to 2% SOC;

[0018] The lithium ion battery A containing the carbonaceous negative electrode material is subjected to a second constant current charge at a temperature of -30°C to 0°C and a current of 0.01C to 0.03C, and the lithium ion battery A containing the carbonaceous negative electrode material is charged to 3% SOC to 20% SOC.

[0019] In one embodiment, the carbon-containing negative electrode material includes at least one of graphite, silicon-carbon negative electrode material, mesophase carbon microbeads, hard carbon and soft carbon.

[0020] In one embodiment, after the step of obtaining a lithium ion battery A containing a carbonaceous negative electrode material filled with liquid, and before the step of constant current charging the lithium ion battery A containing a carbonaceous negative electrode material to 8% SOC to 20% SOC using a small current of 0.01C to 0.1C at a temperature of -30°C to 5°C, the following steps are also included:

[0021] The lithium-ion battery A containing the carbonaceous negative electrode material which has been filled with electrolyte is placed at rest to allow the electrolyte to completely infiltrate the battery cell of the lithium-ion battery A containing the carbonaceous negative electrode material.

[0022] In one embodiment, the static operation conditions are a temperature of 40° C. to 60° C. and a time of 8 h to 12 h.

[0023] In one embodiment, before the step of obtaining the lithium ion battery A with the carbonaceous negative electrode material filled with liquid, the following steps are also included:

[0024] Obtaining a battery cell containing a carbonaceous negative electrode material;

[0025] The battery cell containing the carbonaceous negative electrode material is baked.

[0026] A lithium-ion battery containing a carbonaceous negative electrode material is prepared by using the low-temperature quantitative formation process for a lithium-ion battery containing a carbonaceous negative electrode material described in any of the above embodiments.

[0027] Compared with the prior art, the present invention has at least the following advantages:

[0028] 1) Under the temperature condition of -30°C to 5°C, a small current of 0.01C to 0.1C is used to perform constant current charging to 8% SOC to 20% SOC for the lithium ion battery A containing carbonaceous negative electrode materials, so that the polarization caused by the small current formation of the lithium ion battery A containing carbonaceous negative electrode materials by a small current of 0.01C to 0.1C is small, and in combination with the use of -30°C to 5°C and constant current charging to 8% SOC to 20% SOC, a low-temperature quantitative formation process for the lithium ion battery A containing carbonaceous negative electrode materials is realized, and the consumption of lithium ions in the actual electrolyte is better controlled, that is, the consumption of lithium ions is better controlled to be no more than 10%, thereby ensuring that the lithium ion battery containing carbonaceous negative electrode materials has a higher charge and discharge efficiency.

[0029] 2) Since the formation operation of the lithium-ion battery A containing carbon-based negative electrode materials is carried out at low temperature and low constant current, and the aging is carried out at a temperature of -20°C to 45°C for 12h to 48h, the kinetic diffusion of the SEI film is improved, which is conducive to the formation of a dense, uniform and thin SEI film on the negative electrode surface of the lithium-ion battery A containing carbon-based negative electrode materials, thereby effectively reducing the resistance of the SEI film. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the technical solutions of the embodiments of the present disclosure, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present disclosure and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0031] Figure 1 A flow chart of a low-temperature quantitative formation process for a lithium-ion battery containing a carbonaceous negative electrode material according to an embodiment of the present invention;

[0032] Figure 2 1 is the SEI diagram of the silicon-carbon negative electrode material used in each embodiment of the present invention. DETAILED DESCRIPTION

[0033] In order to facilitate the understanding of the present disclosure, the present disclosure will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present disclosure are given in the drawings. However, the present disclosure can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present disclosure more thoroughly and comprehensively understood.

[0034] It should be noted that when an element is referred to as being "fixed to" another element, it may be directly on the other element or there may be a central element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be a central element at the same time. The terms "vertical", "horizontal", "left", "right" and similar expressions used herein are for illustrative purposes only and do not represent the only implementation method.

[0035] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present disclosure. The terms used herein in the specification of the present disclosure are only for the purpose of describing specific embodiments and are not intended to limit the present disclosure. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0036] The present invention provides a low-temperature quantitative formation process for a lithium-ion battery containing a carbonaceous negative electrode material, comprising the following steps: obtaining a lithium-ion battery A containing a carbonaceous negative electrode material which is filled with liquid; performing constant-current charging on the lithium-ion battery A containing a carbonaceous negative electrode material to 8% SOC to 20% SOC using a small current of 0.01C to 0.1C under a temperature condition of -30°C to 5°C, to obtain a lithium-ion battery B containing a carbonaceous negative electrode material; and aging the lithium-ion battery B containing a carbonaceous negative electrode material at a temperature of -20°C to 45°C for 12h to 48h, to obtain a lithium-ion battery containing a carbonaceous negative electrode material.

[0037] The above-mentioned low-temperature quantitative formation process for lithium-ion batteries containing carbonaceous negative electrode materials uses a small current of 0.01C to 0.1C to perform constant current charging to 8% SOC to 20% SOC under a temperature condition of -30°C to 5°C, so that the polarization caused by the small current of 0.01C to 0.1C when the lithium-ion battery A containing carbonaceous negative electrode materials is formed by a small current is small, and the use of -30°C to 5°C and constant current charging to 8% SOC to 20% SOC realizes the low-temperature quantitative formation process for lithium-ion batteries A containing carbonaceous negative electrode materials, better controls the consumption of lithium ions in the actual electrolyte, that is, better controls the consumption of lithium ions to be no more than 10%, thereby ensuring that the lithium-ion battery containing carbonaceous negative electrode materials has a higher charge and discharge efficiency. Furthermore, since the formation operation of the lithium-ion battery A containing carbonaceous negative electrode materials is carried out at a low temperature and a small constant current, and the aging is carried out at a temperature of -20°C to 45°C for 12h to 48h, the kinetic diffusion of the SEI film is improved, which is conducive to the formation of a dense, uniform and thin SEI film on the negative electrode surface of the lithium-ion battery A containing carbonaceous negative electrode materials, thereby effectively reducing the resistance of the SEI film.

[0038] See also Figure 1 In order to better understand the technical solution and beneficial effects of the present disclosure, the present disclosure is further described in detail below in conjunction with specific embodiments. A low-temperature quantitative formation process for a lithium-ion battery containing a carbonaceous negative electrode material in one embodiment includes some or all of the following steps:

[0039] S101, obtaining a lithium-ion battery A containing a carbonaceous negative electrode material that has been filled with electrolyte, so that the electrolyte can infiltrate the battery cell of the lithium-ion battery A containing the carbonaceous negative electrode material.

[0040] In one embodiment, after the step of obtaining the lithium ion battery A containing carbonaceous negative electrode material filled with liquid, and before the step of constant current charging the lithium ion battery A containing carbonaceous negative electrode material to 8% SOC ~ 20% SOC with a small current of 0.01C ~ 0.1C under the temperature conditions of -30°C ~ 5°C, the following step is also included: the lithium ion battery A containing carbonaceous negative electrode material filled with liquid is allowed to stand still so that the electrolyte completely infiltrates the battery cell of the lithium ion battery A containing carbonaceous negative electrode material.

[0041] Specifically, in one of the embodiments, the static operation conditions are a temperature of 40° C. to 60° C. and a time of 8 h to 12 h to ensure that the electrolyte can completely infiltrate the battery cell of the lithium-ion battery A containing the carbonaceous negative electrode material.

[0042] In one embodiment, before the step of obtaining the lithium-ion battery A containing the carbonaceous negative electrode material filled with liquid, the following steps are also included: obtaining a battery cell containing the carbonaceous negative electrode material; and baking the battery cell containing the carbonaceous negative electrode material. It can be understood that by baking the battery cell containing the carbonaceous negative electrode material, the moisture in the battery cell can be effectively removed.

[0043] S102. Under the temperature condition of -30°C to 5°C, the lithium ion battery A containing the carbonaceous negative electrode material is charged with a small current of 0.01C to 0.1C to a constant current of 8% SOC to 20% SOC to obtain a lithium ion battery B containing the carbonaceous negative electrode material.

[0044] It can be understood that, under the temperature condition of -30℃~5℃, the lithium ion battery A containing carbonaceous negative electrode material is charged to 8%SOC~20%SOC by a small current of 0.01C~0.1C, so that the polarization caused by the small current formation of the lithium ion battery A containing carbonaceous negative electrode material by a small current of 0.01C~0.1C is small, and the use of -30℃~5℃ and constant current charging to 8%SOC~20%SOC is realized, and the low-temperature quantitative formation process of the lithium ion battery A containing carbonaceous negative electrode material is better controlled. The consumption of lithium ions in the actual electrolyte is better controlled, that is, the consumption of lithium ions is better controlled to be no more than 10%, thereby ensuring that the lithium ion battery containing carbonaceous negative electrode material has a high charge and discharge efficiency. In addition, the formation operation of the lithium ion battery A containing carbonaceous negative electrode material using a low-temperature small constant current is conducive to the formation of a dense, uniform and thin SEI film on the negative electrode surface of the lithium ion battery A containing carbonaceous negative electrode material, thereby effectively reducing the resistance of the SEI film.

[0045] In one embodiment, the small current is 0.01C to 0.05C to ensure that the small current of the formation operation is small, which is conducive to forming a dense, uniform and thin SEI film. Specifically, those skilled in the art can select the size of the small current according to actual conditions, such as 0.01C, 0.02C, 0.03C, 0.04C and 0.05C. In a preferred embodiment, the small current is 0.01C.

[0046] In one embodiment, the lithium-ion battery A containing the carbonaceous negative electrode material is charged with a constant current to 8% SOC to 15% SOC.

[0047] It can be understood that, during the formation process of the traditional lithium-ion battery with carbon-based negative electrode materials, the electrolyte will undergo a reduction reaction on the surface of the carbon-based negative electrode to generate various lithium-containing inorganic components on the surface of the carbon-based negative electrode, such as Li2CO3, LIF, Li2O, ROCO2Li, ROLi, (ROCO2Li)2, etc., and cover the surface of the carbon-based negative electrode to form a SEI film. Therefore, in the process of SEI film formation, part of the lithium ions of the electrolyte need to be consumed to increase the irreversible capacity of the first coulomb efficiency. If the constant current charging of the lithium-ion battery A containing carbon-based negative electrode materials is less than 8% SOC, it cannot be guaranteed that a dense SEI film will be formed in the lithium-ion battery containing carbon-based negative electrode materials. If the constant current charging of the lithium-ion battery A containing carbon-based negative electrode materials is higher than 20% SOC, it will cause the consumption of more lithium ions in the electrolyte, resulting in the problem of lower charging and discharging efficiency of the lithium-ion battery containing carbon-based negative electrode materials. Therefore, in the present disclosure, by controlling the constant current charging of the lithium ion battery A containing the carbonaceous negative electrode material to 8% SOC ~ 15% SOC, a dense, uniform and thin SEI film is ensured to be formed on the surface of the carbonaceous negative electrode, thereby effectively avoiding the problem of low charge and discharge efficiency of the lithium ion battery containing the carbonaceous negative electrode material due to excessive consumption of lithium ions in the electrolyte, and better controlling the consumption of lithium ions in the electrolyte, thereby better ensuring that the lithium ion battery containing the carbonaceous negative electrode material has a higher charge and discharge efficiency.

[0048] S103, aging the lithium ion battery B containing the carbonaceous negative electrode material at a temperature of -20°C to 45°C for 12h to 48h to obtain a lithium ion battery containing the carbonaceous negative electrode material, so as to ensure that a dense, uniform and thin SEI film is formed on the surface of the carbonaceous negative electrode.

[0049] In one embodiment, the step of aging the lithium ion battery B containing the carbonaceous negative electrode material at a temperature of -20°C to 45°C for 12h to 48h includes the following specific steps: subjecting the lithium ion battery B containing the carbonaceous negative electrode material to low-temperature standing for 0.5h to 1h, wherein the low temperature is -20°C to 2°C; subjecting the lithium ion battery B containing the carbonaceous negative electrode material that has been subjected to low-temperature standing to room temperature standing for 8h to 35h, wherein the room temperature is 20°C to 35°C; subjecting the lithium ion battery B containing the carbonaceous negative electrode material that has been subjected to room temperature standing to high-temperature standing for 3.5h to 12h, wherein the high temperature is 40°C to 45°C.

[0050] It can be understood that in S102, when the lithium ion battery A containing carbon-based negative electrode materials is subjected to the formation operation at low temperature and small constant current, it is beneficial to form a dense and uniform SEI film on the negative electrode surface of the lithium ion battery A containing carbon-based negative electrode materials. If high temperature standing is directly adopted at this time, the kinetic diffusion of the SEI film just formed at low temperature is too fast, and it is impossible to ensure the formation of a dense and uniform SEI film; if medium temperature standing or low temperature standing is directly adopted, it is impossible to ensure that the SEI film diffuses more comprehensively, and still affects the compactness and uniformity of the SEI film. Therefore, in the present disclosure, first, the lithium ion battery B containing carbon-based negative electrode materials is subjected to low temperature standing to achieve a better transition with the SEI film just formed at low temperature, which is conducive to the formation of a dense and uniform SEI film; then, normal temperature standing and high temperature standing are performed, so that the SEI film just formed at low temperature can achieve a slow step-by-step temperature rise, thereby ensuring that the SEI film can achieve full, comprehensive and stable diffusion in the slow step-by-step temperature rise, and then ensure the formation of a dense, uniform and thin SEI film.

[0051] In one embodiment, under the temperature condition of -30℃~5℃, the step of constant current charging the lithium ion battery A containing carbon-based negative electrode material to 8% SOC~20% SOC with a small current of 0.01C~0.1C includes the following specific steps: using a temperature of 0℃~5℃ and a current of 0.05C~0.1C to perform a first constant current charging on the lithium ion battery A containing carbon-based negative electrode material, and charging the lithium ion battery A containing carbon-based negative electrode material to 1% SOC~2% SOC; using a temperature of -30℃~0℃ and a current of 0.01C~0.03C to perform a second constant current charging on the lithium ion battery A containing carbon-based negative electrode material, and charging the lithium ion battery A containing carbon-based negative electrode material to 3% SOC~20% SOC.

[0052] It can be understood that if a small current is always used to perform constant current charging on the lithium ion battery A containing carbon-based negative electrode materials, although the density and uniformity of the SEI film are improved, it will affect the formation efficiency of the lithium ion battery containing carbon-based negative electrode materials. Therefore, in the present disclosure, the first constant current charging is performed on the lithium ion battery A containing carbon-based negative electrode materials at 0°C to 5°C and a current of 0.05C to 0.1C, and the lithium ion battery A containing carbon-based negative electrode materials is charged to 1% SOC to 2% SOC; on the one hand, the carbon-based negative electrode material will expand slightly at a relatively high temperature to provide a larger deposition area for the SEI film initially deposited on the surface of the carbon-based negative electrode material, thereby providing a better basic film layer for the SEI film formed subsequently; at the same time, the reaction energy of the lithium ion battery A containing carbon-based negative electrode materials can be quickly activated, which is conducive to the rapid formation of a dense and uniform SEI on the surface of the carbon-based negative electrode material. Then, the lithium ion battery A containing the carbonaceous negative electrode material is charged with a second constant current at a temperature of -30°C to 0°C and a current of 0.01C to 0.03C, and the lithium ion battery A containing the carbonaceous negative electrode material is charged to 3% SOC to 20% SOC, so as to ensure that the lithium ion battery A containing the carbonaceous negative electrode material can form a dense and uniform SEI film relatively quickly at a constant current of 0.01C to 0.03C and a temperature of -30°C to 0°C, which is beneficial to the rapid formation of a dense, uniform and thin SEI film on the one hand, and better controls the consumption of lithium ions in the electrolyte on the other hand, thereby ensuring that the lithium ion battery containing the carbonaceous negative electrode material has a higher charge and discharge efficiency.

[0053] In a preferred embodiment, the first constant current charging is performed on the lithium ion battery A containing the carbonaceous negative electrode material at a temperature of 0°C to 5°C and a current of 0.05C to 0.1C, and the lithium ion battery A containing the carbonaceous negative electrode material is charged to 1% SOC to 2% SOC; the second constant current charging is performed on the lithium ion battery A containing the carbonaceous negative electrode material at a temperature of -30°C to 0°C and a current of 0.01C to 0.03C, and the lithium ion battery A containing the carbonaceous negative electrode material is charged to 3% SOC to 15% SOC, so as to control the lower limit consumption of lithium ions in the electrolyte to the greatest extent, so as to quickly form a dense, uniform and thin SEI film on the surface of the carbonaceous negative electrode material, while also ensuring that the lithium ion battery containing the carbonaceous negative electrode material has a higher charge and discharge efficiency.

[0054] In one embodiment, the carbon-containing negative electrode material includes at least one of graphite, silicon-carbon negative electrode material, mesophase carbon microbeads, hard carbon and soft carbon.

[0055] It can be understood that due to the characteristics of silicon-carbon negative electrode materials such as ultra-large specific capacity and low operating voltage platform, it has great potential as a new type of negative electrode active material for lithium-ion batteries. However, since each silicon atom of the silicon-carbon negative electrode material will capture or lose 4 lithium atoms during charging and discharging, this will cause a large change in the volume of the silicon-carbon negative electrode, making the SEI film with poor density and unevenness formed under traditional high temperature or high current conditions very easy to break. Therefore, in the present disclosure, the lithium-ion battery A containing the silicon-carbon negative electrode material is first charged with a first constant current at 0°C to 5°C and a current of 0.05C to 0.1C, and the lithium-ion battery A containing the silicon-carbon negative electrode material is charged to 1% SOC to 2% SOC; the silicon-carbon negative electrode material will expand slightly at a relatively high temperature to provide a larger deposition area for the SEI film initially deposited on the surface of the silicon-carbon negative electrode material, thereby providing a better basic film layer for the SEI film formed subsequently; at the same time, the reaction energy of the lithium-ion battery A containing the silicon-carbon negative electrode material can be quickly awakened, which is conducive to rapid A dense and uniform SEI film is formed on the surface of the silicon-carbon negative electrode material, and then the lithium-ion battery A of the silicon-carbon negative electrode material is subjected to a second constant current charging at a temperature of -30°C to 0°C and a current of 0.01C to 0.03C, and the lithium-ion battery A of the silicon-carbon negative electrode material is charged to 3% SOC to 20% SOC. When the silicon-carbon negative electrode material is at -30°C to 0°C, the silicon-carbon negative electrode material can shrink at low temperatures, and the use of a small current is helpful to form a dense and uniform SEI film on the silicon-carbon negative electrode material, so as to better adapt to the application of lithium-ion batteries of silicon-carbon negative electrode materials.

[0056] In a preferred embodiment, the lithium ion battery A containing the silicon-carbon negative electrode material is first charged with a first constant current at a temperature of 2°C to 5°C and a current of 0.05C to 0.1C, and the lithium ion battery A containing the silicon-carbon negative electrode material is charged to 1% SOC to 2% SOC; then, the lithium ion battery A containing the silicon-carbon negative electrode material is charged with a second constant current at a temperature of -30°C to 0°C and a current of 0.01C to 0.03C, and the lithium ion battery A containing the silicon-carbon negative electrode material is charged to 3% SOC to 15% SOC to ensure that a dense, uniform and thin SEI film is formed on the surface of the silicon-carbon negative electrode material.

[0057] It can be understood that, during the charging process of the silicon-carbon negative electrode material, each silicon atom will capture 4 lithium atoms, resulting in a large change in the volume of the silicon-carbon negative electrode. Therefore, in the present disclosure, the silicon-carbon negative electrode material used is a mixture of low-expansion graphite and vapor-deposited silicon carbon to ensure that the silicon-carbon negative electrode has a low expansion rate during charging and has good tear strength and elongation, thereby ensuring that the prepared lithium-ion battery has good capacity, high first efficiency and long cycle characteristics. It can also be understood that since the particle size of silicon carbon in the present invention is 5um to 45um, wherein the particle size distribution is: D10 ≥ 5.0um; D50, 13.0 ± 2.0um; D90 ≤ 30.0um; D99 ≤ 45.0um; in this way, it is ensured that the particle size distribution of silicon carbon is more suitable, thereby ensuring that the prepared lithium-ion battery has both high capacity, high first efficiency and long cycle characteristics.

[0058] It can also be understood that, in order to reduce the expansion performance of silicon-carbon negative electrode materials, some scholars have found that the expansion rate of silicon-carbon negative electrode materials can be reduced by reducing the particle size of silicon-carbon negative electrode materials, such as controlling the particle size of silicon-carbon negative electrode materials to 50nm to 150nm. However, if silicon-carbon negative electrode materials with smaller particle sizes are used, it is not conducive to the preparation of silicon-carbon negative electrode slurry, and it is easy to agglomerate and not conducive to coating to obtain a uniform silicon-carbon negative electrode layer. Therefore, in the present disclosure, by combining a plurality of silicon-carbon particles with different particle sizes, the problem of agglomeration of silicon-carbon negative electrode materials with smaller particle sizes can be effectively reduced to ensure that a uniform silicon-carbon negative electrode layer is obtained by coating, thereby ensuring that a uniform SEI film is obtained by subsequent formation.

[0059] It can be understood that due to the high expansion performance of the silicon-carbon negative electrode material, in order to ensure that the silicon-carbon negative electrode material can form a dense, uniform and thin SEI film at 15% SOC, in the present disclosure, a slow step-by-step temperature increase is achieved for the SEI film just formed at a low temperature. At this time, the carbon in the silicon-carbon negative electrode material of the lithium-ion battery with a 15% SOC that has just been charged can maintain a certain expansion effect during room temperature and high temperature standing, effectively avoiding the shrinkage of silicon in the silicon-carbon negative electrode material during lithium desorption, that is, the expansion rate of carbon at a higher temperature can better compensate for the shrinkage area of ​​silicon during lithium desorption, thereby ensuring that the shrinkage ratio of the silicon-carbon negative electrode material during the formation of the SEI film will not change significantly, and the kinetic diffusion force of the SEI film is guaranteed to the greatest extent, thereby ensuring that under the condition of charging to 15% SOC, the electrolyte can form a dense, uniform and thin SEI film on the surface of the silicon-carbon negative electrode material, which is conducive to the preparation of a SEI film with higher charge and discharge efficiency, higher capacity retention rate and lower resistance. It should be noted that in the process of charging and discharging a lithium-ion battery containing a silicon-carbon negative electrode material, the first lithium to be embedded is usually a small-particle silicon-carbon negative electrode material. If only a small-particle silicon-carbon negative electrode material is used, then under the same charge amount, that is, under the condition of charging to 80% SOC, its expansion rate is relatively high, so that the newly formed SEI film is easily destroyed. Therefore, the mixed use of multiple particle sizes adopted in the present disclosure and the quantitative SOC charging to 8% SOC~20% SOC can effectively reduce side reactions to effectively reduce electrolyte consumption, so that the particle size of the silicon-carbon negative electrode material is controlled at 5um~45um, so that silicon-carbon negative electrode materials of different particle sizes can be stacked to form a certain spatial structure, and at the same time, it is mixed with carbon with a small expansion rate. In this way, under the same charging conditions of the silicon negative electrode material, small particles of silicon are not easy to expand greatly during the lithium embedding process, effectively avoiding the phenomenon that the silicon-carbon negative electrode material destroys the newly formed SEI film due to excessive expansion rate during the lithium embedding process. Moreover, silicon-carbon negative electrode materials of different particle sizes can also effectively reduce the agglomeration problem of silicon-carbon negative electrode materials of smaller particle sizes, so as to ensure that a uniform silicon-carbon negative electrode layer is coated, thereby ensuring that a dense, uniform and thin SEI film is obtained in the subsequent formation.

[0060] It should be noted that the low-temperature formation method disclosed in the present invention is also helpful for stabilizing the positive electrode CEI film. This is mainly because the decomposition of LiPF6 on the surface of the positive electrode material is an exothermic reaction, and the low-temperature formation will shift the chemical equilibrium in the lithium-ion battery containing carbon-based negative electrode materials toward the formation of a CEI film rich in LIF, which is conducive to the formation of a CEI film with better density, thereby ensuring that the lithium-ion battery containing carbon-based negative electrode materials has good cycle performance.

[0061] The present disclosure also provides a lithium-ion battery containing a carbonaceous negative electrode material, which is prepared by the low-temperature quantitative formation process for lithium-ion batteries containing carbonaceous negative electrode materials described in any of the above embodiments. It can be understood that the lithium-ion battery containing a carbonaceous negative electrode material prepared by the low-temperature quantitative formation process for lithium-ion batteries containing carbonaceous negative electrode materials disclosed in the present disclosure can better control the consumption of lithium ions in the actual electrolyte, and is also conducive to the formation of a dense, uniform and thin SEI film, thereby ensuring that the lithium-ion battery containing a carbonaceous negative electrode material has a higher charge and discharge efficiency.

[0062] Compared with the prior art, the present invention has at least the following advantages:

[0063] 1) Under the temperature condition of -30°C to 5°C, a small current of 0.01C to 0.1C is used to perform constant current charging to 8% SOC to 20% SOC for the lithium ion battery A containing carbonaceous negative electrode materials, so that the polarization caused by the small current formation of the lithium ion battery A containing carbonaceous negative electrode materials by a small current of 0.01C to 0.1C is small, and in combination with the use of -30°C to 5°C and constant current charging to 8% SOC to 20% SOC, a low-temperature quantitative formation process for the lithium ion battery A containing carbonaceous negative electrode materials is realized, and the consumption of lithium ions in the actual electrolyte is better controlled, that is, the consumption of lithium ions is better controlled to be no more than 10%, thereby ensuring that the lithium ion battery containing carbonaceous negative electrode materials has a higher charge and discharge efficiency.

[0064] 2) Since the formation operation of the lithium-ion battery A containing carbon-based negative electrode materials is carried out at a low temperature and a small constant current, and the aging is carried out at a temperature of -20°C to 45°C for 12h to 48h, the kinetic diffusion of the SEI film is improved, which is conducive to the formation of a dense, uniform and thin SEI film on the negative electrode surface of the lithium-ion battery A containing carbon-based negative electrode materials, thereby effectively reducing the resistance of the SEI film.

[0065] Some specific examples are given below, and if % is mentioned, it means percentage by weight. It should be noted that the following examples do not exhaust all possible situations, and the materials used in the following examples can be obtained from commercial sources unless otherwise specified.

[0066] Example 1

[0067] S1. Obtain a battery cell containing silicon-carbon negative electrode material (silicon-carbon G420H, provided by Ling Technology (Dongguan) Co., Ltd.);

[0068] S2. Bake the battery cell containing silicon-carbon negative electrode material to remove moisture from the battery cell;

[0069] S3, injecting the electrolyte into the battery cell, and then standing it at a temperature of 45°C for 8 hours to obtain a lithium-ion battery A containing a silicon-carbon negative electrode material with electrolyte injected;

[0070] S4, performing a first constant current charge on the lithium ion battery A containing the silicon-carbon negative electrode material to 1% SOC at 5°C and 0.05C;

[0071] S5, performing a second constant current charge on the lithium ion battery A containing the silicon-carbon negative electrode material at -5°C and 0.01C to 15% SOC to obtain a lithium ion battery B containing the carbon negative electrode material;

[0072] S6, placing the lithium-ion battery B containing the silicon-carbon negative electrode material at a temperature of -5°C for 0.5h;

[0073] S7, placing the lithium ion battery B containing the silicon-carbon negative electrode material in step S6 at a temperature of 25° C. for 7 hours at room temperature;

[0074] S8. Place the lithium-ion battery B containing the silicon-carbon negative electrode material in step S7 at a temperature of 45° C. for 4.5 hours to obtain a lithium-ion battery containing the silicon-carbon negative electrode material.

[0075] Embodiment 2:

[0076] The difference from Example 1 is that in Example 2, the -5°C in step S5 is changed to 20°C, and the rest remains unchanged.

[0077] Embodiment 3:

[0078] The difference from Example 1 is that Example 3 omits step S4, and the rest remains unchanged.

[0079] Embodiment 4:

[0080] The difference from Example 1 is that Example 4 omits step S5, and the rest remains unchanged.

[0081] Embodiment 5:

[0082] The difference from Example 1 is that in Example 5, 0.01C in step S5 is changed to 0.20C, and the rest remains unchanged.

[0083] Embodiment 6:

[0084] The difference from Example 1 is that in Example 6, 15% SOC in step S5 is changed to 75% SOC.

[0085] Embodiment 7:

[0086] The difference from Example 1 is that Example 7 omits step S6, and the rest remains unchanged.

[0087] Embodiment 8:

[0088] The difference from Example 1 is that Example 8 omits step S7, and the rest remains unchanged.

[0089] Embodiment 9:

[0090] The difference from Example 1 is that Example 9 omits step S8, and the rest remains unchanged.

[0091] Embodiment 10:

[0092] The difference from Example 1 is that Example 10 omits steps S6 to S8, and directly places the lithium ion battery B containing silicon-carbon negative electrode material obtained in S5 at 45° C. for aging for 12 hours.

[0093] The lithium ion batteries containing silicon-carbon negative electrode materials of the above-mentioned Examples 1 to 10 were tested for charge and discharge efficiency and resistance of SEI film, and the following data were obtained:

[0094] project Charge and discharge efficiency 300 cycles capacity retention rate (%) SEI film resistance detection Example 1 89.3% 85.4% 29.5 Example 2 87.8% 84.6% 30.8 Example 3 87.5% 83.2% 32.3 Example 4 84.5% 78.4% 23.8 Example 5 88.3% 84.3% 30.3 Example 6 85.1% 81.5% 34.6 Example 7 86.4% 82.3% 32.6 Example 8 84.7% 80.1% 36.8 Example 9 84.9% 80.4% 35.6 Example 10 87.6% 84.6% 31.3

[0095] From the comparison between Example 1 and Example 2, it can be seen that since Example 2 adopts a higher temperature of 20°C to form the SEI film, the resistance is higher than the resistance of the SEI film formed at a lower temperature in Example 1, and the charge and discharge efficiency of Example 2 is also slightly worse than that of Example 1.

[0096] From the comparison between Example 1 and Example 3, it can be seen that since Example 3 omits the S4 step, the resistance and charge-discharge efficiency of the SEI film of Example 3 are slightly worse than those of Example 1.

[0097] From the comparison between Example 1 and Example 4, it can be seen that since Example 4 omits the S5 step, the SEI film formed in Example 4 is incomplete, so that the SEI film resistance is small, but it is not conducive to improving the charge and discharge efficiency and capacity retention rate of Example 4, so that the charge and discharge efficiency and capacity retention rate of Example 4 are worse than those of Example 1.

[0098] From the comparison between Example 1 and Example 5, it can be seen that since Example 5 adopts a higher current of 0.20C to obtain a larger SE I film resistance, the charge and discharge efficiency and capacity retention rate of Example 5 are slightly inferior to those of Example 1.

[0099] From the comparison between Example 1 and Example 6, it can be seen that when Example 6 performs a second constant current charge on the lithium ion battery A containing silicon-carbon negative electrode material to 75% SOC, the SE I film resistance formed is relatively large, and more electrolyte is consumed, which affects the capacity retention rate and charge and discharge efficiency of Example 6, making the comprehensive indicators of Example 6 worse than those of Example 1.

[0100] From the comparison between Example 1 and Examples 7 to 10, it can be seen that when Example 1 is sequentially subjected to the low-temperature standing of S6, the room-temperature standing of S7, and the high-temperature standing of S8, the kinetic diffusion of the SEI film is improved, which is beneficial to the formation of a dense, uniform and thin SEI film on the negative electrode surface of the lithium-ion battery A containing a carbonaceous negative electrode material, thereby effectively reducing the resistance of the SEI film, so that the comprehensive indicators of Example 1 are better than those of Examples 7 to 10.

[0101] The above-mentioned embodiments only express several implementation methods of the present disclosure, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the disclosed patent. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present disclosure, and these all belong to the protection scope of the present disclosure. Therefore, the protection scope of the disclosed patent shall be subject to the attached claims.

Claims

1. A low-temperature quantitative formation process for lithium-ion batteries containing carbonaceous negative electrode materials, characterized in that: The steps include: Obtain a lithium-ion battery A filled with liquid and containing a carbonaceous negative electrode material; Under the temperature condition of -30°C to 5°C, the lithium ion battery A containing the carbonaceous negative electrode material is charged to 8% SOC to 20% SOC with a small current of 0.01C to 0.1C to obtain a lithium ion battery B containing the carbonaceous negative electrode material; The lithium ion battery B containing the carbonaceous negative electrode material is placed at a temperature of -20°C to 45°C for aging for 12h to 48h to obtain a lithium ion battery containing the carbonaceous negative electrode material.

2. The low-temperature quantitative formation process for lithium-ion batteries containing carbonaceous negative electrode materials according to claim 1, characterized in that: The small current is 0.01C to 0.05C.

3. The low-temperature quantitative formation process for lithium-ion batteries containing carbonaceous negative electrode materials according to claim 1, characterized in that: The lithium ion battery A containing the carbonaceous negative electrode material is charged with a constant current to 8% SOC to 15% SOC.

4. The low-temperature quantitative formation process for lithium-ion batteries containing carbonaceous negative electrode materials according to claim 1, characterized in that: The step of aging the lithium ion battery B containing the carbonaceous negative electrode material at a temperature of -20°C to 45°C for 12h to 48h includes the following specific steps: The lithium ion battery B containing the carbonaceous negative electrode material is placed at low temperature for 0.5 h to 1 h, wherein the low temperature is -20°C to 2°C; The lithium-ion battery B containing the carbonaceous negative electrode material which has been placed at low temperature is placed at room temperature for 8 hours to 35 hours; wherein the room temperature is 20° C. to 35° C.; The lithium ion battery B containing the carbonaceous negative electrode material which has been left at room temperature is left at high temperature for 3.5 hours to 12 hours, wherein the high temperature is 40° C. to 45° C.

5. The low-temperature quantitative formation process for lithium-ion batteries containing carbonaceous negative electrode materials according to claim 1, characterized in that: Under the temperature condition of -30°C to 5°C, the step of constant current charging the lithium ion battery A containing the carbonaceous negative electrode material to 8% SOC to 20% SOC with a small current of 0.01C to 0.1C includes the following specific steps: The lithium ion battery A containing the carbonaceous negative electrode material is charged with a first constant current at a temperature of 0°C to 5°C and a current of 0.05C to 0.1C, and the lithium ion battery A containing the carbonaceous negative electrode material is charged to 1% SOC to 2% SOC; The lithium ion battery A containing the carbonaceous negative electrode material is subjected to a second constant current charge at a temperature of -30°C to 0°C and a current of 0.01C to 0.03C, and the lithium ion battery A containing the carbonaceous negative electrode material is charged to 3% SOC to 20% SOC.

6. The low-temperature quantitative formation process for lithium-ion batteries containing carbonaceous negative electrode materials according to claim 1, characterized in that: The carbon-containing negative electrode material includes at least one of graphite, silicon-carbon negative electrode material, mesophase carbon microbeads, hard carbon and soft carbon.

7. The low-temperature quantitative formation process for lithium-ion batteries containing carbonaceous negative electrode materials according to claim 1, characterized in that: The step of obtaining a lithium-ion battery A containing a carbonaceous negative electrode material having been injected with liquid includes the following specific steps: The lithium-ion battery A containing the carbonaceous negative electrode material which has been filled with electrolyte is placed at rest to allow the electrolyte to completely infiltrate the battery cell of the lithium-ion battery A containing the carbonaceous negative electrode material.

8. The low-temperature quantitative formation process for lithium-ion batteries containing carbonaceous negative electrode materials according to claim 7, characterized in that: The static operation conditions are a temperature of 40° C. to 60° C. and a time of 8 h to 12 h.

9. The low-temperature quantitative formation process for lithium-ion batteries containing carbonaceous negative electrode materials according to claim 1, characterized in that: Before the step of obtaining the lithium-ion battery A with the carbonaceous negative electrode material filled with liquid, the following steps are also included: Obtaining a battery cell containing a carbonaceous negative electrode material; The battery cell containing the carbonaceous negative electrode material is baked.

10. A lithium ion battery containing a carbonaceous negative electrode material, characterized in that: The carbonaceous negative electrode material is prepared by the low-temperature quantitative formation process for lithium-ion batteries according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Formation method of lithium ion battery

    CN113346156A

  • Formation method of lithium titanate battery and lithium titanate battery

    CN115295905A