Preparation method of lithium ion battery diaphragm, diaphragm prepared by preparation method and application of diaphragm

By using electrocatalytic etherification reaction and electrospinning technology in lithium-ion battery separators, the problem of insufficient porosity and wettability of existing separators is solved, and a separator with high thermal stability and mechanical strength is prepared, which improves lithium Electrochemical properties and cycle life of ion batteries.

CN118920018AActive Publication Date: 2024-11-08DALIAN INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411416630.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-11
Publication Date
2024-11-08
Estimated Expiration
2044-10-11

AI Technical Summary

Technical Problem

Existing lithium-ion battery separators have shortcomings in low porosity and low wettability, resulting in limited battery resistance and energy density, and the material will melt and shrink at high temperatures to cause short circuits.

Method used

By mixing the phase transfer catalyst with an aqueous solution of ultra-high polymerization polymer with acrylonitrile, electrocatalytic etherification reaction, precipitation, filtration, and drying, then preparing lithium-ion battery separators using electrospinning technology, adjusting the material ratio and Process conditions to improve the thermal stability and wettability of the diaphragm.

Benefits of technology

The prepared separator has high electrolyte wettability and excellent pore structure, which improves the transmission speed and migration of lithium ions, inhibits dendrites, enhances the rate discharge performance and cycle life of the battery, and is safe and environmentally friendly, reducing the Acrylonitrile self-polymerization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118920018A_ABST
    Figure CN118920018A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a lithium ion battery diaphragm, the diaphragm prepared by the preparation method and application, and belongs to the field of battery materials. Comprising the following steps: adding a phase transfer catalyst into an aqueous solution containing a polymer with an ultrahigh polymerization degree for reaction, then mixing with acrylonitrile to obtain a mixed system, and carrying out electrocatalytic etherification reaction, precipitation, filtration, drying, dissolution and spinning under the catalytic condition of a platinum-palladium catalytic electrode to obtain the lithium ion battery diaphragm. The prepared diaphragm has extremely strong electrolyte wettability, and the diaphragm prepared by an electrostatic spinning process has an excellent pore structure, so that the transmission speed and the transference number of lithium ions are increased, the lithium ions are induced to be uniformly deposited, dendritic crystal growth is effectively inhibited, and the rate discharge performance and the cycle performance under high rate of the battery are improved; the electrochemical performance and the cycle life of the lithium ion battery are improved, and the diaphragm has huge application potential in the field of lithium ion battery diaphragms.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a method for preparing a lithium-ion battery diaphragm, the diaphragm prepared therefrom and applications thereof, and belongs to the field of battery materials. Background Art

[0002] At present, most of the lithium-ion battery separators on the market focus on polyolefin separators such as polyethylene (PE) and polypropylene (PP). These polyolefin microporous membranes have good chemical stability and high mechanical strength. However, the low porosity and poor wettability of polyolefin membranes with polar liquid electrolytes seriously affect the battery resistance, energy density and rate capability of LIB. Polyolefin materials will melt and shrink at high temperatures, causing battery short circuits. The ideal separator should have low interfacial resistance, high electrolyte wettability and uniform pore distribution to meet the requirements of normal operation of batteries in different applications. The separator needs to have high thermal stability, high mechanical strength and high wettability to meet these requirements. Therefore, it is very important to prepare separators by adjusting the raw material ratio and copolymerization of different polymers for the development of lithium-ion batteries. It is very important to develop separators with high thermal stability, high mechanical strength and high wettability to replace traditional commercial separators to further improve the performance and safety of lithium-ion batteries.

[0003] Electrospinning technology can be used to continuously produce micron-scale nanofiber membranes. Nanofiber membranes have large specific surface area, high porosity, small pore size, and strong adsorption, which can improve the wettability and thermal stability of the membrane. With the development and commercial production of large-scale electrospinning equipment, mass production of nanofibers has become possible. For example, patent CN105428572A prepares lithium-ion battery separators by electrospinning; patent CN110565269A uses coaxial electrospinning to prepare lithium battery separators. Summary of the invention

[0004] According to one aspect of the present application, a method for preparing a lithium ion battery separator is provided, comprising the following steps: A phase transfer catalyst is added to an aqueous solution containing a polymer with an ultra-high degree of polymerization for reaction, and then mixed with acrylonitrile to obtain a mixed system, and then subjected to an electrocatalytic etherification reaction, precipitation, filtration, drying, dissolution, and spinning to obtain the lithium-ion battery separator.

[0005] The thickness of the lithium-ion battery separator is 12-45 μm.

[0006] Optionally, the thickness of the lithium-ion battery separator is any value of 12µm, 15µm, 20µm, 25µm, 30µm, 35µm, 40µm, 45µm, or a range between any two values.

[0007] The polymer with ultra-high polymerization degree is selected from at least one of vinyl acetate-ethylene copolymer (EVA), polyvinyl acetate (PVAC), and vinyl acetate-vinyl chloride copolymer (EVC).

[0008] The degree of polymerization of the ultra-high degree of polymerization polymer is 1800-2500.

[0009] Optionally, the degree of polymerization of the ultrahigh degree of polymerization polymer is any value among 1800, 1900, 2000, 2100, 2200, 2300, 2400, 2500 or a range value between any two of them.

[0010] In the mixed system, the mass fraction of each component is: Polymer with ultrahigh polymerization degree: 25~35wt%; optionally, any value among 25wt%, 26wt%, 27wt%, 28wt%, 29wt%, 30wt%, 31wt%, 32wt%, 33wt%, 34wt%, 35wt% or any range between two of them.

[0011] Water: 25-47 wt%; optionally, any value among 25 wt%, 30 wt%, 35 wt%, 40 wt%, 45 wt%, 47 wt% or any range therebetween.

[0012] Phase transfer catalyst: 2-5wt%; optionally, any value among 2wt%, 3wt%, 4wt%, 5wt% or any range between two of them.

[0013] Acrylonitrile: 25-35wt%. Optionally, any value among 25wt%, 26wt%, 27wt%, 28wt%, 29wt%, 30wt%, 31wt%, 32wt%, 33wt%, 34wt%, 35wt%, or any range between two of them.

[0014] The phase transfer catalyst is a quaternary ammonium salt, selected from tetrabutylammonium bromide, benzyltriethylammonium bromide, and dodecyltrimethylammonium chloride.

[0015] The reaction temperature is 30-60°C.

[0016] Optionally, the reaction temperature is any value among 30°C, 40°C, 50°C, 60°C, or any range therebetween.

[0017] The stirring rate of the reaction is 400-800 rpm.

[0018] Optionally, the stirring rate of the reaction is any value among 400 rpm, 500 rpm, 600 rpm, 700 rpm, 800 rpm, or any range value therebetween.

[0019] The reaction time is 1 to 3 hours.

[0020] Optionally, the reaction time is any value among 1 h, 2 h, 3 h, or any range between the two.

[0021] The mixing temperature is 30-60°C.

[0022] Optionally, the mixing temperature is any value among 30°C, 40°C, 50°C, 60°C, or any range therebetween.

[0023] The stirring rate of the mixing is 400-800 rpm.

[0024] Optionally, the stirring rate of the mixing is any value among 400 rpm, 500 rpm, 600 rpm, 700 rpm, 800 rpm, or any range value therebetween.

[0025] The mixing time is 1 to 3 hours.

[0026] Optionally, the mixing time is any value among 1 h, 2 h, 3 h, or any range between the two.

[0027] The temperature of the electrocatalytic etherification reaction is 25-30°C.

[0028] Optionally, the temperature of the electrocatalytic etherification reaction is any value among 25°C, 26°C, 27°C, 28°C, 29°C, 30°C, or a range between any two of them.

[0029] The current density of the electrocatalytic etherification reaction is 30-60 mA cm -2 .

[0030] Optionally, the current density of the electrocatalytic etherification reaction is 30 mA·cm -2 , 40mA·cm -2 , 50mA·cm -2 、60mA·cm -2 Any value in or any range between them.

[0031] The electrocatalytic etherification reaction time is 1 to 2 hours.

[0032] Optionally, the time of the electrocatalytic etherification reaction is any value among 1 h, 1.5 h, 2 h, or a range between any two values.

[0033] The electrocatalytic etherification reaction is carried out under the catalytic conditions of platinum-palladium catalytic electrode.

[0034] Optionally, the preparation method comprises the following steps: 1) Place the ultra-high degree of polymerization polymer and solvent in a four-necked flask equipped with a thermometer, a stirrer, a reflux condenser and a dropping funnel and place it in a constant temperature water area, heat it up and stir it evenly; the conditions are: 35~65℃, rotation speed 400~800 rpm, time 3~6h; 2) Cool down naturally to room temperature, add phase transfer catalyst, heat up and stir to react; 3) Add acrylonitrile and mix; 4) transferring the entire reaction system to an electrocatalytic device and performing an electrocatalytic etherification reaction under catalytic conditions of a platinum-palladium catalytic electrode; 5) Add deionized water, precipitate, filter and dry to obtain the product.

[0035] According to another aspect of the present application, a lithium-ion battery separator is provided, which is prepared by the above-mentioned preparation method.

[0036] The dissolving solvent is selected from at least one of DMAC, DMF and DMSO.

[0037] The mass fraction of the dissolved spinning solution is 9-18wt%.

[0038] Optionally, the mass fraction of the dissolved spinning solution is any value of 9wt%, 10wt%, 11wt%, 12wt%, 13wt%, 14wt%, 15wt%, 16wt%, 17wt%, 18wt% or a range value between any two of them.

[0039] The spinning is electrostatic spinning.

[0040] According to another aspect of the present application, there is provided an application of the above-mentioned lithium-ion battery separator for use in a lithium-ion battery.

[0041] The beneficial effects of this application include: 1) The present application adopts an electrocatalytic device to replace the traditional alkaline catalytic system for the cyanoethylation reaction of the polymer, which is safe and environmentally friendly, avoids environmental pollution, and has extremely high electrocatalytic efficiency, greatly reduces the self-polymerization of acrylonitrile, and reduces the amount of acrylonitrile used.

[0042] 2) The modified ultra-high degree of polymerization polymer contains a strong polar cyano group, and the prepared diaphragm has extremely strong electrolyte wettability. The diaphragm prepared by the electrospinning process has an excellent pore structure, which improves the transmission speed and migration number of lithium ions, induces uniform deposition of lithium ions, effectively inhibits dendrite growth, improves battery rate discharge performance and high rate cycle performance, improves the electrochemical properties and cycle life of lithium-ion batteries, and has great application potential in the field of lithium-ion battery diaphragms.

[0043] 3) The modified ultra-high degree of polymerization polymer has an ultra-high dielectric constant and can be used for electrospinning membrane. The prepared membrane has excellent performance in lithium-ion batteries, which can improve the wettability of the membrane to the electrolyte, improve the mechanical strength of the membrane, enhance stability, and prevent dendrite puncture from causing battery short circuit. It is hoped that this will provide a reference for solving the shortcomings of existing materials and designing and developing high-performance materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 It is the long cycle curve of the lithium iron phosphate full battery assembled with the diaphragm of the embodiment of the present application and the comparative example at 1C. DETAILED DESCRIPTION

[0045] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.

[0046] Unless otherwise specified, the raw materials and catalysts in the examples of this application were purchased through commercial channels.

[0047] Example 1 1) Put 30g of polyvinyl acetate with a degree of polymerization of 1800 and 35g of water into a four-necked flask equipped with a thermometer, a stirrer, a reflux condenser and a dropping funnel and place it in a constant temperature water area, heat it to 45°C, and stir at 600 rpm for 3h until it is uniform; 2) Cool down naturally to room temperature, add 3g of tetrabutylammonium bromide as phase transfer catalyst, raise the temperature to 35°C, and react at 500 rpm for 2h; 3) Add 32 g of acrylonitrile and continue stirring and mixing at 35°C and 500 rpm for 2 h; 4) The entire reaction system was transferred to an electrocatalytic device at 25 °C and a current density of 60 mA cm -2 and electrocatalytic etherification reaction was carried out under the catalytic conditions of platinum-palladium electrode for 1 h; 5) Add deionized water, precipitate, filter and dry to obtain the product.

[0048] The polymer obtained above was dissolved in DMF with a spinning solution mass fraction of 15 wt %, and spun to obtain an electrospinning membrane with a thickness of 22 μm.

[0049] Example 2 1) Put 25g of vinyl acetate-ethylene copolymer with a degree of polymerization of 2500 and 47g of water into a four-necked flask equipped with a thermometer, a stirrer, a reflux condenser and a dropping funnel and place it in a constant temperature water area, heat it to 35°C, and stir at 800 rpm for 5h until it is uniform; 2) Cool down naturally to room temperature, add 2 g of phase transfer catalyst benzyltriethylammonium bromide, raise the temperature to 60°C, and react at 400 rpm for 1 h; 3) Add 26 g of acrylonitrile and continue mixing at 60°C and 400 rpm for 1 h; 4) The entire reaction system was transferred to an electrocatalytic device at 30 °C and a current density of 30 mA cm -2 and electrocatalytic etherification reaction was carried out under the catalytic conditions of platinum-palladium electrode for 2 h; 5) Add deionized water, precipitate, filter and dry to obtain the product.

[0050] The polymer obtained above was dissolved in DMAC with a spinning solution mass fraction of 18 wt %, and spun to obtain an electrospinning membrane with a thickness of 12 μm.

[0051] Example 3 1) Put 35g of vinyl acetate-vinyl chloride copolymer with a degree of polymerization of 2000 and 25g of water into a four-necked flask equipped with a thermometer, a stirrer, a reflux condenser and a dropping funnel and place it in a constant temperature water area, heat it to 65°C, and stir at 400 rpm for 6h until it is uniform; 2) Cool down naturally to room temperature, add 5 g of dodecyltrimethylammonium chloride as a phase transfer catalyst, raise the temperature to 30°C, and react at 800 rpm for 1 h; 3) Add 35 g of acrylonitrile and continue mixing at 30°C and 800 rpm for 3 h; 4) The entire reaction system was transferred to an electrocatalytic device at 30 °C and a current density of 40 mA cm -2 and electrocatalytic etherification reaction was carried out under the catalytic conditions of platinum-palladium electrode for 2 h; 5) Add deionized water, precipitate, filter and dry to obtain the product.

[0052] The polymer obtained above was dissolved in DMSO with a spinning solution mass fraction of 9 wt %, and spun to obtain an electrospinning membrane with a thickness of 45 μm.

[0053] Comparative Example 1 Comparative Example 1 is an electrospun PAN nanofiber membrane with a thickness of 22 μm.

[0054] Test Example 1 The separators in Example 1 and Comparative Example 1 were cut into 19 mm discs, and lithium iron phosphate full batteries were assembled. The polarization long cycle curves at 1C were tested. The results are as follows: Figure 1 The batteries assembled with the separators of Examples 1 to 3 can be stably cycled for 200 hours, while the battery assembled with the separator of Comparative Example 1 short-circuited after 150 hours of cycling, and its stability and discharge specific capacity were lower than those of the Examples.

[0055] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.

Claims

1. A method for preparing a lithium ion battery separator, characterized in that: The following steps are involved: Adding a phase transfer catalyst to an aqueous solution containing a polymer with an ultrahigh degree of polymerization to react, then mixing with acrylonitrile to obtain a mixed system, performing an electrocatalytic etherification reaction, precipitating, filtering, drying, dissolving, and spinning to obtain the lithium-ion battery separator; The thickness of the lithium-ion battery separator is 12-45 μm.

2. The preparation method according to claim 1, characterized in that: The polymer with ultra-high polymerization degree is selected from at least one of vinyl acetate-ethylene copolymer, polyvinyl acetate, and vinyl acetate-vinyl chloride copolymer; The degree of polymerization of the ultra-high degree of polymerization polymer is 1800-2500.

3. The preparation method according to claim 1, characterized in that: In the mixed system, the mass fraction of each component is: Ultra-high degree of polymerization polymer: 25~35wt%; Water: 25~47wt%; Phase transfer catalyst: 2~5wt%; Acrylonitrile: 25~35wt%.

4. The preparation method according to claim 1, characterized in that: The phase transfer catalyst is selected from one of tetrabutylammonium bromide, benzyltriethylammonium bromide and dodecyltrimethylammonium chloride.

5. The preparation method according to claim 1, characterized in that: The reaction temperature is 30-60°C; The stirring rate of the reaction is 400-800 rpm; The reaction time is 1 to 3 hours.

6. The preparation method according to claim 1, characterized in that: The mixing temperature is 30-60°C; The stirring rate of the mixing is 400-800 rpm; The mixing time is 1 to 3 hours.

7. The preparation method according to claim 1, characterized in that: The temperature of the electrocatalytic etherification reaction is 25-30°C; The current density of the electrocatalytic etherification reaction is 30-60 mA cm -2 ; The electrocatalytic etherification reaction time is 1 to 2 hours.

8. The preparation method according to claim 1, characterized in that: The electrocatalytic etherification reaction is carried out under the catalytic conditions of platinum-palladium catalytic electrode; The spinning is electrostatic spinning.

9. A lithium ion battery separator, characterized in that: Prepared by the preparation method according to any one of claims 1 to 8.

10. An application of the lithium ion battery separator according to claim 9, characterized in that: Used in lithium-ion batteries.

Citation Information

Patent Citations

  • Method for producing 2-cyanoethyl group-containing organic compound

    CN102731665A

  • Polyvinyl acetate-cyanoethyl etherate and synthesis method thereof

    CN105153336A

  • Electrolyte and electrolysis method for preparing adiponitrile from acrylonitrile through electro-catalysis

    CN116555786A

  • Lithium battery diaphragm as well as preparation method and application thereof

    CN117175141A

  • Method for preparing adiponitrile by electrocatalytic reduction of acrylonitrile

    CN118063330A