Perovskite / crystalline silicon laminated cell and preparation method thereof

By introducing an amorphous germanium layer into the perovskite/crystalline silicon stacked battery, the problems of low carrier exchange rate and high interface contact resistance are solved, and the conversion efficiency and photoelectric performance of the battery are improved.

CN118922005AActive Publication Date: 2024-11-08CHUZHOU JIETAI NEW ENERGY TECH CO LTD

Patent Information

Application Number
CN202411163137.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-08
Estimated Expiration
2044-08-22

AI Technical Summary

Technical Problem

In perovskite/crystalline silicon laminated batteries, existing transparent conductive oxide film layers or n/p-type silicon-based tunneling composite junctions have low carrier exchange rate, high interface contact resistance, and battery conversion efficiency as intermediate series layers. Low problem.

Method used

In the perovskite/crystalline silicon stacked battery, an amorphous germanium layer is provided as the intermediate composite layer to enhance the tunneling conductivity between the second doped silicon layer and the intermediate composite layer and reduce the interface contact resistance.

Benefits of technology

The filling factor and conversion efficiency of the battery are improved, and the photoelectric performance of the perovskite/crystalline silicon stacked battery is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922005A_ABST
    Figure CN118922005A_ABST
Patent Text Reader

Abstract

The invention discloses a perovskite / crystalline silicon laminated cell and a preparation method thereof, and belongs to the field of perovskite / crystalline silicon lamination, the perovskite / crystalline silicon laminated cell comprises a bottom cell and a top cell, the bottom cell takes a crystalline silicon wafer as a substrate, and the back surface of the bottom cell is sequentially provided with an interface passivation layer, a first doped silicon layer, a first transparent conductive oxide film layer and a metal conductive film layer; an interface passivation layer, a second doped silicon layer and an intermediate composite layer are sequentially arranged on the front surface; the top cell takes a perovskite light absorption layer as a light absorption layer, the back surface is provided with a first carrier transport layer, and the front surface is sequentially provided with a second carrier transport layer, a second transparent conductive oxide film layer and a metal grid line electrode; and the amorphous germanium layer is arranged between the second doped silicon layer and the middle composite layer, so that the tunneling conductivity between the second doped silicon layer and the middle composite layer is enhanced, the interface contact resistance is reduced, and the FF and conversion efficiency of the cell are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of perovskite / crystalline silicon stacking, and in particular to a perovskite / crystalline silicon stacking cell and a preparation method thereof. Background Art

[0002] The highest laboratory conversion efficiency of single-crystal silicon cells has reached 27.09%, close to the theoretical limit of 29.4%, and there is little room for efficiency improvement in the future. In order to break through the efficiency ceiling, perovskite / crystalline silicon tandem cells have become one of the new directions for photovoltaic technology transformation. The theoretical conversion efficiency of perovskite / crystalline silicon tandem cells formed by stacking crystalline silicon cells and perovskite cells is 43%, and the current highest laboratory conversion efficiency has reached 33.9%. Both the theoretical efficiency and laboratory efficiency of perovskite / crystalline silicon tandem cells are significantly higher than those of single-crystal silicon cells.

[0003] The tandem cell requires an intermediate series layer to enable carrier exchange between the top and bottom cells. Therefore, its photoelectric performance will directly affect the photoelectric conversion efficiency of the tandem cell.

[0004] The intermediate series layer usually uses a transparent conductive oxide film or an n / p-type silicon-based tunneling composite junction. When an n / p-type silicon-based tunneling junction is used as the intermediate series layer, due to process conditions, the tunneling barrier of the n / p-type silicon-based tunneling junction is relatively high, which makes the probability of carrier tunneling low and the density of defect states at the interface low, resulting in a low carrier exchange rate and increased recombination losses of photogenerated carriers, thereby resulting in high electrical losses at the tunneling junction in the solar cell; when a TCO composite junction is used as the intermediate series layer, there is a Schottky barrier between the TCO film layer and the doped silicon layer. The barrier height is greatly affected by the effective doping concentration and bandgap width of the doped silicon layer, which easily leads to excessive interface contact resistance, resulting in an increase in the battery series resistance and a decrease in the fill factor; in addition, an excessively high barrier height will lead to an excessively large depletion layer thickness in the doped silicon layer, affecting the battery open circuit voltage, and ultimately resulting in a decrease in the battery conversion efficiency.

[0005] In view of this, the inventor conducted in-depth research on this demand, and thus the present case was produced. Summary of the invention

[0006] Aiming at a series of problems existing in the prior art of perovskite / crystalline silicon tandem cells using a transparent conductive oxide film layer or an n / p-type silicon-based tunneling composite junction as an intermediate series connection layer, the present invention provides a perovskite / crystalline silicon tandem cell, including a bottom cell and a top cell.

[0007] The bottom cell is based on a crystalline silicon wafer, and an interface passivation layer, a first doped silicon layer, a first transparent conductive oxide film layer and a metal conductive film layer are sequentially arranged on the back side, and an interface passivation layer, a second doped silicon layer and an intermediate composite layer are sequentially arranged on the front side;

[0008] The top cell uses a perovskite light-absorbing layer as the light absorption layer, a first carrier transport layer is arranged on the back, and a second carrier transport layer, a second transparent conductive oxide film layer and a metal grid electrode are arranged in sequence on the front; an amorphous germanium layer is arranged between the second doped silicon layer and the intermediate composite layer.

[0009] Preferably, the amorphous germanium layer is undoped, p-type doped or n-type doped amorphous, nanocrystalline or microcrystalline.

[0010] Preferably, the amorphous germanium layer includes at least one of hydrogenated amorphous germanium, hydrogenated amorphous germanium silicon or hydrogenated amorphous germanium carbon film, and has a thickness of 0.5-5.0 nm.

[0011] Preferably, the crystalline silicon wafer may be a Czochralski single crystal silicon wafer, a cast single crystal silicon wafer or a polycrystalline silicon wafer, may be N-type doped or P-type doped, have a resistivity of 0.1-10.0 Ωcm, and a thickness of 50-500 um.

[0012] Preferably, the intermediate composite layer is one of a transparent conductive oxide layer, n-type doped silicon or p-type doped silicon, and has a thickness of 10-30 nm.

[0013] Preferably, the first doped silicon layer is a low-temperature amorphous silicon film layer or a high-temperature polycrystalline silicon film layer, and is n-type doped or p-type doped, with a doping concentration of 10 17 -10 20 cm -3 ;

[0014] The second doped silicon layer is a low temperature amorphous silicon film layer or a high temperature polycrystalline silicon film layer, and is n-type doped or p-type doped, with a doping concentration of 10 17 -10 20 cm -3 , the second doped silicon layer has a conductivity type opposite to that of the first doped silicon layer;

[0015] The low-temperature amorphous silicon film layer is formed at a temperature of 100-300°C, and the high-temperature polysilicon film layer is formed at a temperature of 600-1000°C.

[0016] Preferably, the low temperature amorphous silicon film layer comprises at least one of a-Si:H, a-SiOx:H, a-SiCx:H, uc-Si:H, uc-SiOx:H, uc-SiCx:H, and has a thickness of 5-20 nm;

[0017] The high temperature polysilicon film layer includes at least one of poly-Si, poly-SiOx, poly-SiNx, and poly-SiCx, and has a thickness of 5-50 nm.

[0018] Preferably, the first transparent conductive oxide film layer comprises at least one of doped indium oxide, tin oxide, and zinc oxide-based films, with a thickness of 60-150 nm;

[0019] The second transparent conductive oxide film layer includes at least one of doped indium oxide, tin oxide, and zinc oxide-based films, with a thickness of 60-150 nm;

[0020] The metal conductive film layer includes at least one of Ag, Al, Ni, Cu, and Fe, and has a thickness of 100-1000 nm.

[0021] Preferably, the interface passivation layer includes at least one of an intrinsic amorphous silicon film layer or a tunneling dielectric film layer;

[0022] The intrinsic amorphous silicon film layer includes at least one of a-Si:H, a-SiOx:H, and a-SiCx:H, with a thickness of 4-8nm; the tunneling dielectric film layer includes at least one of SiOx, SiNx, and SiCx, with a thickness of 1-3nm.

[0023] Preferably, the general formula of the perovskite light-absorbing layer is ABX3, wherein A is a monovalent cation, including but not limited to any one of lithium, sodium, potassium, cesium, amine or amidine; B is a divalent cation, including but not limited to any one of lead and tin; X is a monovalent anion, including but not limited to any one of iodine, bromine and chlorine; the thickness of the perovskite light-absorbing layer is 500-1500nm.

[0024] Preferably, the first carrier transport layer comprises a stacked first inorganic carrier transport layer and a first organic carrier transport layer; the first carrier transport layer is a hole transport layer or an electron transport layer; the first carrier transport layer and the first doped silicon layer have the same conductivity type;

[0025] The second carrier transport layer includes a stacked second inorganic carrier transport layer and a second organic carrier transport layer; the second carrier transport layer is a hole transport layer or an electron transport layer; the second carrier transport layer has a conductivity type opposite to that of the first carrier transport layer and the same conductivity type as the second doped silicon layer.

[0026] Preferably, the first inorganic carrier transport layer includes an inorganic hole transport layer or an inorganic electron transport layer; the second inorganic carrier transport layer includes an inorganic hole transport layer or an inorganic electron transport layer, and the first inorganic carrier transport layer and the second inorganic carrier transport layer have opposite conductivity types;

[0027] The inorganic hole transport layer includes at least one of NiOx, V2O5, MoOx, WOx, and Cu2O, with a thickness of 0.5-50.0 nm; the inorganic electron transport layer preferably includes at least one of SnO2, TiO2, ZnO, Nb2O5, ZrO2, TiSnOx, SnZnOx, LiF, and MgFx, with a thickness of 0.5-50.0 nm;

[0028] The first organic carrier transport layer includes an organic hole transport layer or an organic electron transport layer, the second organic carrier transport layer includes an organic hole transport layer or an organic electron transport layer, and the first organic carrier transport layer and the second organic carrier transport layer have opposite conductivity types;

[0029] The organic hole transport layer preferably includes at least one of 2PACz, Me-4PACz, MeO-2PACz, PTAA, P3HT, Poly-TPD, PEDOT:PSS, Spiro-OMeTAD, m-MTDATA, Spiro-TTB, F4-TCNQ, F6-TCNNQ, and TAPC, and has a thickness of 0.5-50.0 nm;

[0030] The organic electron transport layer preferably includes at least one of fullerene C60, fullerene C70, and fullerene derivative PCBM, and has a thickness of 0.5-50.0 nm.

[0031] Preferably, the metal gate line electrode is at least one of Ag, Al, Ni, Cu, and Fe, and the gate line thickness is 0.1-20.0 um and the spacing is 0.5-5.0 mm.

[0032] The present invention also provides a method for preparing the above-mentioned perovskite / crystalline silicon stacked cell, which has a simple process and is easy to implement, and specifically comprises the following steps:

[0033] S1, corroding and cleaning the surface of the crystalline silicon wafer;

[0034] S2, a first interface passivation layer and a first doped silicon layer are sequentially arranged on the back of the crystalline silicon wafer; a second interface passivation layer, a second doped silicon layer, an amorphous germanium layer and an intermediate composite layer are sequentially arranged on the front;

[0035] S3, disposing a first transparent conductive oxide film layer and a metal conductive film layer on the surface of the first doped silicon layer at the back side; and disposing a first carrier transport layer on the surface of the first doped silicon layer at the front side;

[0036] S4, depositing a perovskite light absorbing layer on the surface of the first carrier transport layer;

[0037] S5, depositing a second carrier transport layer on the surface of the perovskite light absorbing layer;

[0038] S6, depositing a second transparent conductive oxide film layer on the surface of the second carrier transport layer;

[0039] S7. Dispose a metal gate electrode on the surface of the second transparent conductive oxide film layer.

[0040] The beneficial effects produced by the technical solution of the present invention are as follows: an ultra-thin amorphous germanium layer is arranged between the second doped silicon layer and the intermediate composite layer, which enhances the tunneling conductivity between the second doped silicon layer and the intermediate composite layer, reduces the interface contact resistance, and improves the battery FF and conversion efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0042] Figure 1 It is a schematic diagram of the layer structure of the perovskite / crystalline silicon tandem battery in the present invention;

[0043] Figure 2 It is a process flow chart of the preparation of the perovskite / crystalline silicon tandem battery in the present invention;

[0044] Figure 3 is a schematic diagram of the layer structure of the perovskite / crystalline silicon tandem battery in Example 1 of the present invention;

[0045] Figure 4 is a schematic diagram of the layer structure of the perovskite / crystalline silicon tandem battery in Example 2 of the present invention;

[0046] Figure 5 It is a schematic diagram of the layer structure of the perovskite / crystalline silicon tandem battery in Comparative Example 1 of the present invention.

[0047] In the figure:

[0048] 1. Bottom cell; 11. Crystalline silicon wafer; 12. Interface passivation layer; 13. First doped silicon layer; 14. First transparent conductive oxide film layer; 15. Metal conductive film layer; 16. Second doped silicon layer; 17. Intermediate composite layer; 2. Top cell; 21. Perovskite light absorption layer; 22. First carrier transport layer; 23. Second carrier transport layer; 24. Second transparent conductive oxide film layer; 25. Metal grid electrode. DETAILED DESCRIPTION

[0049] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Therefore, the following detailed description of the embodiments of the present invention provided in the drawings is not intended to limit the scope of the claimed invention, but merely represents the selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0050] like Figure 1 As shown, a perovskite / crystalline silicon stacked cell includes a bottom cell 1 and a top cell 2.

[0051] The bottom cell 1 is based on a crystalline silicon wafer 11, and an interface passivation layer 12, a first doped silicon layer 13, a first transparent conductive oxide film layer 14 and a metal conductive film layer 15 are sequentially arranged on the back side, and an interface passivation layer 12, a second doped silicon layer 16 and an intermediate composite layer 17 are sequentially arranged on the front side;

[0052] The top cell 2 uses a perovskite light-absorbing layer 21 as a light-absorbing layer, a first carrier transport layer 22 is arranged on the back, and a second carrier transport layer 23, a second transparent conductive oxide film layer 24 and a metal grid electrode 25 are arranged in sequence on the front; an amorphous germanium layer 3 is arranged between the second doped silicon layer 16 and the intermediate composite layer 17.

[0053] As a preferred implementation, the amorphous germanium layer 3 is undoped, p-type doped or n-type doped amorphous, nanocrystalline or microcrystalline.

[0054] As a preferred implementation, the amorphous germanium layer 3 includes at least one of hydrogenated amorphous germanium, hydrogenated amorphous germanium silicon or hydrogenated amorphous germanium carbon film, and has a thickness of 0.5-5.0 nm.

[0055] As a preferred embodiment, the crystalline silicon wafer 11 may be a Czochralski single crystal silicon wafer, a cast single crystal silicon wafer or a polycrystalline silicon wafer, may be N-type doped or P-type doped, have a resistivity of 0.1-10.0Ωcm, and a thickness of 50-500um.

[0056] As a preferred implementation, the intermediate composite layer 18 is one of a transparent conductive oxide layer, n-type doped silicon or p-type doped silicon, and has a thickness of 10-30 nm.

[0057] As a preferred embodiment, the first doped silicon layer 13 is a low-temperature amorphous silicon film layer or a high-temperature polycrystalline silicon film layer, and is n-type doped or p-type doped, with a doping concentration of 10 17 -10 20 cm-3 ;

[0058] The second doped silicon layer 17 is a low temperature amorphous silicon film layer or a high temperature polycrystalline silicon film layer, and is n-type doped or p-type doped, with a doping concentration of 10 17 -10 20 cm -3 , the second doped silicon layer has a conductivity type opposite to that of the first doped silicon layer;

[0059] The low-temperature amorphous silicon film layer is formed at a temperature of 100-300°C, and the high-temperature polysilicon film layer is formed at a temperature of 600-1000°C.

[0060] As a preferred embodiment, the low temperature amorphous silicon film layer includes at least one of a-Si:H, a-SiOx:H, a-SiCx:H, uc-Si:H, uc-SiOx:H, and uc-SiCx:H, and has a thickness of 5-20 nm;

[0061] The high temperature polysilicon film layer includes at least one of poly-Si, poly-SiOx, poly-SiNx, and poly-SiCx, and has a thickness of 5-50 nm.

[0062] As a preferred embodiment, the first transparent conductive oxide film layer 14 includes at least one of doped indium oxide, tin oxide, and zinc oxide-based films, with a thickness of 60-150 nm;

[0063] The second transparent conductive oxide film layer 24 includes at least one of doped indium oxide, tin oxide, and zinc oxide-based films, with a thickness of 60-150 nm;

[0064] The metal conductive film layer 15 includes at least one of Ag, Al, Ni, Cu, and Fe, and has a thickness of 100-1000 nm.

[0065] As a preferred embodiment, the interface passivation layer 16 includes at least one of an intrinsic amorphous silicon film layer or a tunnel dielectric film layer;

[0066] The intrinsic amorphous silicon film layer includes at least one of a-Si:H, a-SiOx:H, and a-SiCx:H, with a thickness of 4-8nm; the tunneling dielectric film layer includes at least one of SiOx, SiNx, and SiCx, with a thickness of 1-3nm.

[0067] As a preferred embodiment, the general formula of the perovskite light-absorbing layer 21 is ABX3, wherein A is a monovalent cation, including but not limited to any one of lithium, sodium, potassium, cesium, amine or amidine; B is a divalent cation, including but not limited to any one of lead and tin; X is a monovalent anion, including but not limited to any one of iodine, bromine and chlorine; the thickness of the perovskite light-absorbing layer is 500-1500nm.

[0068] As a preferred embodiment, the first carrier transport layer 22 includes a stacked first inorganic carrier transport layer and a first organic carrier transport layer; the first carrier transport layer is a hole transport layer or an electron transport layer; the first carrier transport layer and the first doped silicon layer have the same conductivity type;

[0069] The second carrier transport layer 23 includes a stacked second inorganic carrier transport layer and a second organic carrier transport layer; the second carrier transport layer is a hole transport layer or an electron transport layer; the second carrier transport layer has an opposite conductivity type to the first carrier transport layer and the same conductivity type as the second doped silicon layer.

[0070] As a preferred embodiment, the first inorganic carrier transport layer includes an inorganic hole transport layer or an inorganic electron transport layer; the second inorganic carrier transport layer includes an inorganic hole transport layer or an inorganic electron transport layer, and the first inorganic carrier transport layer and the second inorganic carrier transport layer have opposite conductivity types;

[0071] The inorganic hole transport layer includes at least one of NiOx, V2O5, MoOx, WOx, and Cu2O, with a thickness of 0.5-50.0 nm; the inorganic electron transport layer preferably includes at least one of SnO2, TiO2, ZnO, Nb2O5, ZrO2, TiSnOx, SnZnOx, LiF, and MgFx, with a thickness of 0.5-50.0 nm;

[0072] The first organic carrier transport layer includes an organic hole transport layer or an organic electron transport layer, the second organic carrier transport layer includes an organic hole transport layer or an organic electron transport layer, and the first organic carrier transport layer and the second organic carrier transport layer have opposite conductivity types;

[0073] The organic hole transport layer preferably includes at least one of 2PACz, Me-4PACz, MeO-2PACz, PTAA, P3HT, Poly-TPD, PEDOT:PSS, Spiro-OMeTAD, m-MTDATA, Spiro-TTB, F4-TCNQ, F6-TCNNQ, and TAPC, with a thickness of 0.5-50.0 nm;

[0074] The organic electron transport layer preferably includes at least one of fullerene C60, fullerene C70, and fullerene derivative PCBM, and has a thickness of 0.5-50.0 nm.

[0075] As a preferred implementation, the metal gate line electrode 25 is at least one of Ag, Al, Ni, Cu, and Fe, with a gate line thickness of 0.1-20.0 um and a spacing of 0.5-5.0 mm.

[0076] like Figure 2 As shown, this embodiment also provides a method for preparing the above-mentioned perovskite / crystalline silicon stacked cell, which has a simple process and is easy to implement, and specifically includes the following steps:

[0077] S1, corroding and cleaning the surface of the crystalline silicon wafer;

[0078] S2, a first interface passivation layer and a first doped silicon layer are sequentially arranged on the back of the crystalline silicon wafer; a second interface passivation layer, a second doped silicon layer, an amorphous germanium layer and an intermediate composite layer are sequentially arranged on the front;

[0079] S3, disposing a first transparent conductive oxide film layer and a metal conductive film layer on the surface of the first doped silicon layer at the back side; and disposing a first carrier transport layer on the surface of the first doped silicon layer at the front side;

[0080] S4, depositing a perovskite light absorbing layer on the surface of the first carrier transport layer;

[0081] S5, depositing a second carrier transport layer on the surface of the perovskite light absorbing layer;

[0082] S6, depositing a second transparent conductive oxide film layer on the surface of the second carrier transport layer;

[0083] S7. Dispose a metal gate electrode on the surface of the second transparent conductive oxide film layer.

[0084] The beneficial effects of the perovskite / crystalline silicon tandem cell and its preparation process in this embodiment are further reviewed through several groups of examples.

[0085] Embodiment 1:

[0086] like Figure 3 As shown, the perovskite / crystalline silicon stacked cell in this embodiment includes, from the back to the front, an Ag conductive film layer, an ITO layer, a pa-Si:H layer, an ia-Si:H layer, an n-CZ Si layer, an ia-Si:H layer, a na-Si:H layer, an a-GeCx:H layer, a p-uc-SiOx:H layer, a NiOx layer, a 2PACz layer, a PVK layer, a LiF layer, a C60 layer, a SnO2 layer, an IZO layer and an Ag gate line.

[0087] The method for preparing the perovskite / crystalline silicon tandem cell in this embodiment comprises the following steps:

[0088] S1, using a wet process to perform texturing and cleaning on the surface of an N-type silicon wafer; using acid and alkali chemicals to eliminate organic contamination and metal impurities on the surface of the silicon wafer, forming a surface pyramid texture on the surface of the single crystal silicon wafer to increase the absorption of sunlight and reduce reflection; the single crystal silicon wafer is a phosphorus-doped N-type single crystal silicon wafer with a resistivity of 1Ωcm and a thickness of 150um.

[0089] S2, using PECVD method, deposit an i / p-type amorphous silicon layer on the back of the silicon wafer, and deposit an i / n-type amorphous silicon layer on the front of the silicon wafer; the thickness of the i layer on the back is 4-8nm, the thickness of the p layer is 5-10nm, and the boron doping concentration is 0.5%; the thickness of the i layer on the front is 4-8nmn, the thickness of the n layer is 5-10nm, and the phosphorus doping concentration is 1%; the deposition temperature is 200℃.

[0090] S3, using PECVD process, deposited a 0.5-1nm thick n-type doped amorphous germanium layer on the surface of the front n-type non-silicon film layer. The reaction gases are PH3, GeH4 and H2, where the flow ratio of PH3 to GeH4 is 0.01, the flow ratio of H2 to GeH4 is 5, and the power density of the PECVD equipment is 15mW / cm 2 , pressure of 50Pa, substrate temperature of 200℃; then deposit a p-type doped microcrystalline silicon oxide layer p-uc-SiOx:H on the surface of the amorphous germanium layer, the deposition temperature is 180℃, the thickness is 15nm, SiH4, CO2, H2, and B2H6 are used as reaction gases, the CO2 / SiH4 gas flow ratio is 0.5, the H2 / SiH4 flow ratio is 200:1, and the B2H6 / SiH4 gas flow ratio is 0.5%.

[0091] S4, using PVD method, ITO / Ag is deposited on the surface of the back p amorphous silicon layer, ITO target material is 90wt% In2O3+10wt% SnO, sputtering atmosphere is 0.2% O2 / Ar, ITO thickness is 100nm, Ag target material purity is 99.99wt%, Ag thickness is 500nm; then NiOx is deposited on the surface of the front p-type doped microcrystalline silicon oxide layer, using RF sputtering process, the target material is NiO target material with a purity of 99.99%, the sputtering atmosphere is pure Ar, and the thickness is 20nm.

[0092] S5, using spin coating + drying method, deposit 2PACz and PVK layer on NiOx surface. First, use 1mg / mL 2PACz ethanol solution, spin coating at 4000 rpm for 30s, and then dry at 100℃ for 10min; spin coating process deposits 1.7mol / LCs 0.05 FA 0.8 MA 0.15Pb(I 0.755 Br 0.255 )3 DMF and DMSO mixed solution (volume ratio 4:1) perovskite precursor solution, rotation speed 3500 rpm, time 40 s, and then dried at 100 ° C / N2 conditions for 30 min, the resulting perovskite band gap width is 1.69 eV.

[0093] S6, depositing LiF / C60 on the surface of the PVK layer by evaporation. 1 nm LiF is thermally evaporated on the PVK surface, and 18 nm C60 is thermally evaporated on the LiF surface.

[0094] S7, using ALD process to deposit SnO2 on the surface of C60. TDMASn and H2O are used as reaction gases, N2 is used as carrier gas, the deposition temperature is 80°C, and SnO2 with a thickness of 20nm is deposited.

[0095] S8, using PVD method to deposit IZO on the surface of SnO2. The IZO target composition is 90wt% In2O3+10wt% ZnO, the sputtering atmosphere is 0.2% O2 / Ar, the IZO thickness is 100nm, the Ag target purity is 99.99wt%, and the Ag thickness is 500nm.

[0096] S9, using printing + curing method, a low-temperature Ag paste gate electrode is formed on the IZO surface. The gate width is 30um, the spacing is 2mm; the curing temperature is 120℃, and the time is 10min.

[0097] Embodiment 2:

[0098] like Figure 4 As shown, the perovskite / crystalline silicon stacked cell in this embodiment includes, from the back to the front, an Ag conductive film layer, an ITO layer, a p-poly-Si layer, a SiO2 layer, an n-CZ Si layer, a SiO2 layer, an n-poly-Si layer, an a-GeCx:H layer, a p-uc-SiOx:H layer, a NiOx layer, a 2PACz layer, a PVK layer, a LiF layer, a C60 layer, a SnO2 layer, an IZO layer and an Ag gate line.

[0099] The method for preparing the perovskite / crystalline silicon tandem cell in this embodiment comprises the following steps:

[0100] S1, using a wet process to texturize and clean the surface of the N-type silicon wafer. Using acid and alkali chemicals to remove organic contamination and metal impurities on the surface of the silicon wafer, a surface pyramid texture is formed on the surface of the single crystal silicon wafer to increase the absorption of sunlight and reduce reflection; the single crystal silicon wafer is a phosphorus-doped N-type single crystal silicon wafer with a resistivity of 1Ωcm and a thickness of 150um.

[0101] S2, using PECVD method, deposits ultra-thin SiO2 film and p-type amorphous silicon film on the back of silicon wafer; ultra-thin SiO2 film and n-type amorphous silicon film are first deposited on the front of silicon wafer. The ultra-thin SiO2 film is formed by plasma discharge oxidation with N2O as the reaction gas, the deposition temperature is 250℃, and the thickness is 2nm; the n-type amorphous silicon film is deposited at 250℃, the thickness is 20nm, SiH4, H2, PH3 are used as reaction gases, and the PH3 / SiH4 gas flow ratio is 1.5%; the p-type amorphous silicon film is deposited at 250℃, the thickness is 20nm, SiH4, H2, B2H6 are used as reaction gases, and the B2H6 / SiH4 gas flow ratio is 1%.

[0102] S3, using furnace tube high temperature annealing to activate p-type and n-type amorphous silicon film layers, annealing temperature 850℃, time 30min, annealing atmosphere N2, after annealing, p-type and n-type amorphous silicon film layers are converted into p-type and n-type polysilicon film layers, doping concentration 1E20~1E21cm -3 .

[0103] S4, using HF solution to remove the parasitic oxide layer on the surface of the p-type and n-type polysilicon film layers after annealing, the HF concentration is 1wt%, the temperature is 20-30°C, and the time is 1-3min.

[0104] S5, using PECVD process, depositing a 0.5-1.0nm thick n-type doped amorphous germanium carbon layer on the front n-type polysilicon film layer, the reaction gases are PH3, GeH4, CH4 and H2, where the flow ratio of PH3 to GeH4 is 0.01, the flow ratio of CH4 / GeH4 is 4, the flow ratio of H2 to GeH4 is 5, and the power density of the PECVD equipment is 75mW / cm 2 , pressure of 50Pa, substrate temperature of 180℃; then deposit a p-type doped microcrystalline silicon oxide layer p-uc-SiOx:H on the surface of the amorphous germanium carbon layer, the deposition temperature is 180℃, the thickness is 15nm, SiH4, CO2, H2, and B2H6 are used as reaction gases, the CO2 / SiH4 gas flow ratio is 0.5, the H2 / SiH4 flow ratio is 200:1, and the B2H6 / SiH4 gas flow ratio is 0.5%.

[0105] S6, using PVD method, ITO / Ag is deposited on the surface of the back p-type amorphous silicon layer, the ITO target material is 90wt% In2O3+10wt% SnO, the sputtering atmosphere is 0.2% O2 / Ar, the ITO thickness is 100nm, the Ag target material purity is 99.99wt%, and the Ag thickness is 500nm; NiOx is deposited on the surface of the front p-type doped microcrystalline silicon oxide layer, the sputtering target material is NiO with a purity of 99.99%, the sputtering atmosphere is pure Ar, and the thickness is 20nm;

[0106] S7, using spin coating + drying method, deposit 2PACz and PVK layer on NiOx surface. First, use 1mg / mL 2PACz ethanol solution, spin coating at 4000 rpm for 30s, and then dry at 100℃ for 10min; the spin coating process deposits 1.7mol / LCs 0.05 FA 0.8 MA 0.15 Pb(I 0.755 Br 0.255 )3 DMF and DMSO mixed solution (volume ratio 4:1) perovskite precursor solution, rotation speed 3500 rpm, time 40 s, and then dried at 100 ° C / N2 conditions for 30 min, the resulting perovskite band gap width is 1.69 eV.

[0107] S8, depositing LiF / C60 on the surface of the PVK layer by evaporation, thermally evaporating 1 nm LiF on the PVK surface, and thermally evaporating 18 nm C60 on the LiF surface.

[0108] S9, using ALD process to deposit SnO2 on the surface of C60. TDMASn and H2O are used as reaction gases, N2 is used as carrier gas, the deposition temperature is 80°C, and SnO2 with a thickness of 20nm is deposited.

[0109] S10, depositing IZO on the surface of SnO2 by PVD, the composition of IZO target is 90wt% In2O3+10wt% ZnO, the sputtering atmosphere is 0.2% O2 / Ar, the thickness of IZO is 100nm, the purity of Ag target is 99.99wt%, and the thickness of Ag is 500nm.

[0110] S11, using printing + curing method, a low-temperature Ag paste gate electrode is formed on the IZO surface. The gate width is 30um, the spacing is 2mm; the curing temperature is 120℃, and the time is 10min.

[0111] Comparative Example 1:

[0112] like Figure 5 As shown, the perovskite / crystalline silicon stacked cell in this comparative example includes, from the back to the front, an Ag conductive film layer, an ITO layer, a pa-Si:H layer, an ia-Si:H layer, an n-CZ Si layer, an ia-Si:H layer, a na-Si:H layer, a p-uc-SiOx:H layer, a NiOx layer, a 2PACz layer, a PVK layer, a LiF layer, a C60 layer, a SnO2 layer, an IZO layer and an Ag gate line.

[0113] The preparation method of the perovskite / crystalline silicon tandem battery in this comparative example comprises the following steps:

[0114] S1, using a wet process to etch and clean the surface of the N-type silicon wafer. Using acid and alkali chemicals to remove organic contamination and metal impurities on the surface of the silicon wafer, a surface pyramid texture is formed on the surface of the single crystal silicon wafer to increase the absorption of sunlight and reduce reflection; the single crystal silicon wafer is a phosphorus-doped N-type single crystal silicon wafer with a resistivity of 1Ωcm and a thickness of 150um.

[0115] S2, using PECVD method, depositing i / p type amorphous silicon layer on the back of silicon wafer, and i / n type amorphous silicon layer on the front of silicon wafer. The thickness of i layer on the back is 4-8nm, the thickness of p layer is 5-10nm, and the boron doping concentration is 0.5%; the thickness of i layer on the front is 4-8nmn, the thickness of n layer is 5-10nm, and the phosphorus doping concentration is 1%; the deposition temperature is 200℃.

[0116] S3, using PECVD process, deposited p-type doped microcrystalline silicon oxide layer p-uc-SiOx:H on the surface of the front n-type polysilicon film layer, the deposition temperature was 180℃, the thickness was 15nm, SiH4, CO2, H2, B2H6 were used as reaction gases, CO2 / SiH4 gas flow ratio was 0.5, H2 / SiH4 flow ratio was 200:1,

[0117] B2H6 / SiH4 gas flow ratio 0.5%.

[0118] S4, using PVD method, ITO / Ag is deposited on the surface of the back p amorphous silicon layer, ITO target material is 90wt% In2O3+10wt% SnO, sputtering atmosphere is 0.2% O2 / Ar, ITO thickness is 100nm, Ag target material purity is 99.99wt%, Ag thickness is 500nm; NiOx is deposited on the front p-type doped microcrystalline silicon oxide layer, NiOx adopts RF sputtering process, NiOx target material with purity of 99.99%, sputtering atmosphere is pure Ar, NiOx thickness is 20nm.

[0119] S5, using spin coating + drying method, deposit 2PACz and PVK layer on NiOx surface. First, use 1mg / mL 2PACz ethanol solution, spin coating at 4000 rpm for 30s, and then dry at 100℃ for 10min; spin coating process deposits 1.7mol / LCs 0.05 FA 0.8 MA 0.15 Pb(I 0.755 Br 0.255 )3 DMF and DMSO mixed solution (volume ratio 4:1) perovskite precursor solution, rotation speed 3500 rpm, time 40 s, and then dried at 100 ° C / N2 conditions for 30 min, the resulting perovskite band gap width is 1.69 eV.

[0120] S6, depositing LiF / C60 on the surface of the PVK layer by evaporation. 1 nm LiF is thermally evaporated on the PVK surface, and 20 nm C60 is thermally evaporated on the LiF surface.

[0121] S7, using ALD process to deposit SnO2 on the surface of C60. TDMASn and H2O are used as reaction gases, N2 is used as carrier gas, the deposition temperature is 80°C, and SnO2 with a thickness of 20nm is deposited.

[0122] S8, using PVD method, IZO is deposited on the surface of SnO2. The IZO target material composition is 90wt% In2O3+10wt% ZnO, the sputtering atmosphere is 0.2% O2 / Ar, and the IZO thickness is 100nm; the Ag target material purity is 99.99wt%, the sputtering atmosphere is pure Ar, and the Ag thickness is 500nm.

[0123] S9, using printing + curing method, a low-temperature Ag paste gate electrode is formed on the IZO surface. The gate width is 30um, the spacing is 2mm; the curing temperature is 120℃, and the time is 10min.

[0124] The performance of the batteries obtained in the above two groups of embodiments and one group of comparative example was tested. The parameters of the solar cell were measured using an IV tester. The results are shown in Table 1.

[0125] Table 1 Battery performance test results in each group of examples

[0126]

[0127] As shown in Table 1, the perovskite / crystalline silicon tandem cell in Comparative Example 1 uses an n / p-type silicon-based tunnel junction as the intermediate series layer. Due to process conditions, the tunneling barrier of the n / p-type silicon-based tunnel junction is relatively high, which makes the carrier tunneling probability low and the density of defect states at the interface low, resulting in a low carrier exchange rate and increased recombination losses of photogenerated carriers, thereby resulting in high electrical losses at the tunnel junction in the solar cell and low FF and efficiency of the tandem cell.

[0128] In Example 1, an ultra-thin amorphous germanium layer a-Ge:H is arranged between the bottom battery na-Si:H and the middle composite layer p-uc-SiOx:H to enhance the tunneling conductivity between na-Si:H and p-uc-SiOx:H, reduce the interface tunneling barrier, and improve the battery FF and conversion efficiency.

[0129] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A perovskite / crystalline silicon tandem cell, characterized in that: Including bottom battery and top battery, The bottom cell is based on a crystalline silicon wafer, and an interface passivation layer, a first doped silicon layer, a first transparent conductive oxide film layer and a metal conductive film layer are sequentially arranged on the back side, and an interface passivation layer, a second doped silicon layer and an intermediate composite layer are sequentially arranged on the front side; The top cell uses a perovskite light-absorbing layer as the light absorption layer, a first carrier transport layer is arranged on the back, and a second carrier transport layer, a second transparent conductive oxide film layer and a metal grid electrode are arranged in sequence on the front; an amorphous germanium layer is arranged between the second doped silicon layer and the intermediate composite layer.

2. A perovskite / crystalline silicon tandem cell according to claim 1, characterized in that: The amorphous germanium layer is undoped, p-type doped or n-type doped amorphous, nanocrystalline or microcrystalline.

3. A perovskite / crystalline silicon tandem cell according to claim 1, characterized in that: The amorphous germanium layer includes at least one of hydrogenated amorphous germanium, hydrogenated amorphous germanium silicon or hydrogenated amorphous germanium carbon film, and has a thickness of 0.5-5.0 nm.

4. The perovskite / crystalline silicon tandem cell according to claim 1, characterized in that: The intermediate composite layer is one of a transparent conductive oxide layer, n-type doped silicon or p-type doped silicon, and has a thickness of 10-30 nm.

5. The perovskite / crystalline silicon tandem cell according to claim 1, characterized in that: The first doped silicon layer is a low temperature amorphous silicon film layer or a high temperature polycrystalline silicon film layer, and is n-type doped or p-type doped, with a doping concentration of 10 17 -10 20 cm -3 ; The second doped silicon layer is a low temperature amorphous silicon film layer or a high temperature polycrystalline silicon film layer, and is n-type doped or p-type doped, with a doping concentration of 10 17 -10 20 cm -3 , the second doped silicon layer has a conductivity type opposite to that of the first doped silicon layer; The low-temperature amorphous silicon film layer is formed at a temperature of 100-300°C, and the high-temperature polysilicon film layer is formed at a temperature of 600-1000°C.

6. A perovskite / crystalline silicon tandem cell according to claim 5, characterized in that: The low temperature amorphous silicon film layer comprises at least one of a-Si:H, a-SiOx:H, a-SiCx:H, uc-Si:H, uc-SiOx:H, and uc-SiCx:H, and has a thickness of 5-20 nm; The high temperature polysilicon film layer includes at least one of poly-Si, poly-SiOx, poly-SiNx, and poly-SiCx, and has a thickness of 5-50 nm.

7. The perovskite / crystalline silicon tandem cell according to claim 1, characterized in that: The interface passivation layer includes at least one of an intrinsic amorphous silicon film layer or a tunneling dielectric film layer; The intrinsic amorphous silicon film layer includes at least one of a-Si:H, a-SiOx:H, and a-SiCx:H, with a thickness of 4-8nm; the tunneling dielectric film layer includes at least one of SiOx, SiNx, and SiCx, with a thickness of 1-3nm.

8. The perovskite / crystalline silicon tandem cell according to claim 1, characterized in that: The first carrier transport layer comprises a stacked first inorganic carrier transport layer and a first organic carrier transport layer; the first carrier transport layer is a hole transport layer or an electron transport layer; the first carrier transport layer and the first doped silicon layer have the same conductivity type; The second carrier transport layer includes a stacked second inorganic carrier transport layer and a second organic carrier transport layer; the second carrier transport layer is a hole transport layer or an electron transport layer; the second carrier transport layer has a conductivity type opposite to that of the first carrier transport layer and the same conductivity type as the second doped silicon layer.

9. The perovskite / crystalline silicon tandem cell according to claim 8, characterized in that: The first inorganic carrier transport layer includes an inorganic hole transport layer or an inorganic electron transport layer; the second inorganic carrier transport layer includes an inorganic hole transport layer or an inorganic electron transport layer, and the first inorganic carrier transport layer and the second inorganic carrier transport layer have opposite conductivity types; The inorganic hole transport layer includes at least one of NiOx, V2O5, MoOx, WOx, and Cu2O, with a thickness of 0.5-50.0 nm; the inorganic electron transport layer preferably includes at least one of SnO2, TiO2, ZnO, Nb2O5, ZrO2, TiSnOx, SnZnOx, LiF, and MgFx, with a thickness of 0.5-50.0 nm; The first organic carrier transport layer includes an organic hole transport layer or an organic electron transport layer, the second organic carrier transport layer includes an organic hole transport layer or an organic electron transport layer, and the first organic carrier transport layer and the second organic carrier transport layer have opposite conductivity types; The organic hole transport layer preferably includes at least one of 2PACz, Me-4PACz, MeO-2PACz, PTAA, P3HT, Poly-TPD, PEDOT:PSS, Spiro-OMeTAD, m-MTDATA, Spiro-TTB, F4-TCNQ, F6-TCNNQ, and TAPC, and has a thickness of 0.5-50.0 nm; The organic electron transport layer preferably includes at least one of fullerene C60, fullerene C70, and fullerene derivative PCBM, and has a thickness of 0.5-50.0 nm.

10. A method for preparing a perovskite / crystalline silicon tandem cell according to any one of claims 1 to 9, characterized in that: The steps include: S1, corroding and cleaning the surface of the crystalline silicon wafer; S2, a first interface passivation layer and a first doped silicon layer are sequentially arranged on the back of the crystalline silicon wafer; a second interface passivation layer, a second doped silicon layer, an amorphous germanium layer and an intermediate composite layer are sequentially arranged on the front; S3, disposing a first transparent conductive oxide film layer and a metal conductive film layer on the surface of the first doped silicon layer at the back side; and disposing a first carrier transport layer on the surface of the first doped silicon layer at the front side; S4, depositing a perovskite light absorbing layer on the surface of the first carrier transport layer; S5, depositing a second carrier transport layer on the surface of the perovskite light absorbing layer; S6, depositing a second transparent conductive oxide film layer on the surface of the second carrier transport layer; S7. Dispose a metal gate electrode on the surface of the second transparent conductive oxide film layer.

Citation Information

Patent Citations

  • Crystalline silicon heterojunction lamination solar cell and manufacture method thereof

    CN102136517A

  • Composite layer-containing flexible substrate silicon-base multi-junction laminated solar battery

    CN102945886A

  • Perovskite / crystalline silicon laminated cell and preparation method thereof

    CN113206123A

  • Laminated photovoltaic device and production method

    CN113257940A

  • Ionized mineral composition for promoting shellfish growth and method for producing the same

    KR1020200119992A

Cited By

  • Perovskite / crystalline silicon laminated solar cell and preparation method thereof

    CN122497261A