Surface coated cutting tool

By using AlTiN and AlTiSiN layers alternately stacked in the cladding layer of the cutting tool and setting TiN layers on the surface, the problem of insufficient wear resistance in high-speed cutting of stainless steel is solved, and high speed cutting of steel or cast iron is achieved Wear resistance and excellent performance of high-speed cutting of stainless steel.

CN118922264AActive Publication Date: 2024-11-08MITSUBISHI MATERIALS CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202380029029.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-22
Filing Date
2023-03-16
Publication Date
2024-11-08
Estimated Expiration
2043-03-16

AI Technical Summary

Technical Problem

Existing cutting tools perform well when cutting steel or cast iron at high speed, but are not well-resistant in high-speed cutting of stainless steel and are prone to degradation of performance due to oxidative wear and boundary damage.

Method used

A clad layer structure is adopted, in which the lower layer A is composed of 0.5 to 4.0 nm AlTiN layer and AlTiSiN layer alternately stacked, and the upper layer B is composed of AlaTi1-a-bSibN, and the outermost TiN layer is provided on the substrate to improve oxidation resistance. and wear resistance.

Benefits of technology

While high-speed cutting of steel or cast iron is achieved, it also has excellent wear resistance to high-speed cutting of stainless steel, reducing oxidative wear and boundary damage, and extending tool life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922264A_ABST
    Figure CN118922264A_ABST
Patent Text Reader

Abstract

The coated tool is characterized in that the average thickness At of a lower layer A is 0.3-6.0 [mu] m, the average thickness Bt of an upper layer B is 0.1-3.0 [mu] m, 2.0 < = At / Bt < = 5.0, the lower layer A is an alternating laminated layer of A1 [alpha] layers having an average thickness [alpha] t and A1 [beta] layers having an average thickness [beta] t, 0.5 nm < = [alpha] t < = 4.0 nm, 0.5 nm < = [beta] t < = 4.0 nm, 0.7 < = [beta] t / [alpha] t < = 1.3, the composition of the A1 [alpha] layers is AlxTi1-xN (the average value xavg of x is 0.35 < = xavg < = 0.55), the composition of the A1 [beta] layers is AlyTi1-yN (the average value yavg The composition of the upper layer (B) is AlaTi1-a-bSibN (the average value of a is aavg, the average value of b is bavg, 0.35 < = aavg < = 0.60, and 0.00 < bavg < = 0.15).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a surface-coated cutting tool (hereinafter, sometimes referred to as a coated tool). This application claims priority based on Japanese patent application No. 2022-45633 filed on March 22, 2022. All the contents described in the Japanese patent application are incorporated into this specification by reference. Background Art

[0002] Conventionally, as a coated tool, there is known a coated tool in which a coating layer is formed on a base body such as tungsten carbide (hereinafter referred to as WC)-based cemented carbide.

[0003] Furthermore, it has been proposed to obtain a coated tool with further improved cutting performance by adjusting the composition and layer structure of the coating layer.

[0004] For example, Patent Document 1 describes a coating tool having a coating layer formed by coating Ti with a x Al 1-x N and Ti y Al 1- y N (0≤x<0.5, 0.5<y≤1) these two layers are repeated alternately to form a laminate and the overall composition of the laminate is stoichiometrically rich in aluminum. The coated tool has excellent wear resistance and defect resistance.

[0005] In addition, for example, Patent Document 2 describes a coated tool, wherein the coating layer of the coated tool includes alternating layers, each of which has a thickness of 2 nm or more and 100 nm or less, including one or more first layers and one or more second layers, wherein the composition of the first layer is Ti a Al b Si c N (0.25≤a≤0.45, 0.55≤b≤0.75, 0≤c≤0.1, a+b+c=1), the composition of the second layer is Ti d Al e Si f N(0.35≤d≤0.55, 0.45≤e≤0.65, 0≤f≤0.1, d+e+f=1), 0.05≤da≤0.2 and 0.05≤be≤0.2, the tool life of the coated tool is improved.

[0006] Furthermore, for example, Patent Document 3 describes a coated tool having a coating layer, wherein the nanobeam diffraction pattern index of the coating layer is a WC crystal structure, the coating layer having an a layer composed of a carbide containing W and Ti and an interlayer arranged on the a layer, the film thickness of the a layer is greater than 1 nm and less than 10 nm, the interlayer is alternately formed by a b layer and a c layer, the b layer is composed of a nitride or carbonitride of Al and Ti having an Al content ratio (atomic %) of greater than 50% and less than 70% relative to the total amount of the metal elements, the c layer is composed of a nitride or carbonitride of Al and Ti having an Al content ratio (atomic %) of greater than 70% relative to the total amount of the metal elements, the difference in the Al content ratio (atomic %) between the b layer and the c layer is greater than 10% and less than 30%, and the coated tool also has excellent durability in cutting stainless steel.

[0007] In addition, for example, Patent Document 4 describes a coated tool, the outermost layer of the coating of which is a coating composed of hexagonal nitride or carbonitride, wherein the hexagonal nitride or carbonitride contains only Al of 60% to 80% and Si of 5% to 10% in terms of atomic % of the metal components, and the remainder is composed of Ti, and the coated tool has durability.

[0008] Patent Document 1: Japanese Patent Publication No. 7-97679

[0009] Patent Document 2: Japanese Patent Publication No. 2017-193004

[0010] Patent Document 3: Japanese Patent Publication No. 2015-110259

[0011] Patent Document 4: Japanese Patent Publication No. 2017-18551 Summary of the invention

[0012] The present invention has been made in view of the above circumstances and the above solutions, and an object of the present invention is to provide a cutting tool having excellent wear resistance that can be used not only for high-speed cutting of steel or cast iron but also for high-speed cutting of stainless steel and the like.

[0013] Here, high-speed cutting refers to cutting in which the cutting speed is 30% or more faster than normal cutting.

[0014] Regarding the surface-coated cutting tool according to the embodiment of the present invention,

[0015] A substrate and a coating layer arranged on the substrate,

[0016] The covering layer comprises a lower layer A and an upper layer B on the lower layer A,

[0017] The average thickness At of the lower layer A is greater than or equal to 0.3 μm and less than or equal to 6.0 μm, the average thickness Bt of the upper layer B is greater than or equal to 0.1 μm and less than or equal to 3.0 μm, 2.0≤At / Bt≤5.0,

[0018] The lower layer A comprises an alternating stack of A1α layers with an average thickness of αt and A1β layers with an average thickness of βt,

[0019] 0.5nm≤αt≤4.0nm, 0.5nm≤βt≤4.0nm, 0.7≤βt / αt≤1.3,

[0020] The composition of the A1α layer is Al x Ti 1-x N(the average value of x avg 0.35≤x avg ≤0.55),

[0021] The composition of the A1β layer is Al y Ti 1-y N(the average value of y avg 0.60≤y avg ≤0.80),

[0022] Satisfy 1.2≤y avg / x avg ,

[0023] The composition of the upper layer B is Al a Ti 1-a-b Si b N(the average value of a avg , the average value of b avg 0.35≤a avg ≤0.60, 0.00<b avg ≤0.15).

[0024] The surface-coated cutting tool according to the above-mentioned embodiment may also satisfy the following matters.

[0025] The lower layer A is a lower layer A1 on the substrate side and a lower layer A2 on the upper layer B side.

[0026] The average thickness A1t of the lower layer A1 and the average thickness A2t of the lower layer A2 are 0.1 μm≤A1t≤4.5 μm, 0.2 μm≤A2t≤4.0 μm, 0.5≤A1t / A2t≤3.0,

[0027] The lower layer A1 is the alternating stack of the A1α layer and the A1β layer,

[0028] The lower layer A2 is an alternating stack of A2γ layers with an average thickness of γt and A2δ layers with an average thickness of δt.

[0029] 1.5nm≤γt≤8.0nm, 1.5nm≤δt≤8.0nm, 0.7≤δt / γt≤1.3,

[0030] 1.0<(γt+δt) / (αt+βt)≤6.0,

[0031] The composition of the A2γ layer is Al z Ti 1-z N(the average value of z avg 0.30≤z avg ≤0.50),

[0032] The composition of the A2δ layer is Al w Ti 1-w N(the average value of w avg 0.55≤w avg ≤0.75),

[0033] Satisfy 1.2≤w avg / z avg ,

[0034] And 0.02≤(x avg -z avg )≤0.30、0.02≤(y avg -w avg )≤0.30.

[0035] The surface-coated cutting tool is used not only for high-speed cutting of steel or cast iron but also for high-speed cutting of stainless steel, and exhibits excellent wear resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 This is an example of a schematic diagram of a longitudinal section of a coating layer in a surface-coated cutting tool according to an embodiment of the present invention.

[0037] Figure 2 This is an example of a schematic diagram of a longitudinal section of a coating layer in a surface-coated cutting tool according to another embodiment of the present invention. DETAILED DESCRIPTION

[0038] The present inventors have conducted intensive research on coating layers in order to obtain a cutting tool having excellent wear resistance for high-speed cutting of stainless steel, etc. while maintaining performance in cutting steel or cast iron. As a result, the following findings (1) to (3) were obtained.

[0039] (1) If a layer composed of a stack of an AlTiN layer with a high Al content and an AlTiN layer with a low Al content, each having an average thickness of 0.5 to 4.0 nm, is used as a coating layer, the hardness increases due to the decomposition of AlTiN during cutting (it is estimated that AlTiN decomposes into TiN and AlN), and a coated tool with excellent wear resistance for cutting steel or cast iron can be obtained. However, in the case where the coating layer produces oxidative wear, its performance may not be fully exerted. In other words, the AlTiN stack with different Al contents may sometimes reduce wear resistance due to oxidation damage.

[0040] (2) Therefore, it has been studied to provide a TiSiN layer on the upper part of the AlTiN stack to suppress the aforementioned oxidative wear of the coating layer. However, since the oxidation resistance of the TiSiN layer is low, it causes damage development due to boundary damage, for example, in the cutting of stainless steel. Furthermore, the lattice constant of the TiSiN layer is greatly different from that of the AlTiN layer, and the integration at the interface of the two layers is poor.

[0041] (3) On the other hand, even if a TiAlSiN stack having a different Si content is formed instead of the above-mentioned AlTiN stack, the wear resistance will be reduced because it is difficult to produce decomposition of TiAlSiN in the TiAlSiN stack (it is estimated that TiAlSiN decomposes into TiN, AlN and Si3N4) and the improvement in wear resistance is small.

[0042] Therefore, the present inventors have further studied and found that the above-mentioned object can be achieved by providing a layer in which two types of AlTiN layers with average thicknesses of 0.5 to 4.0 nm are alternately stacked and an AlTiN layer containing Si, i.e., an AlTiSiN layer, is provided on top.

[0043] In addition, it was found that if the lower layer is set as a lower layer A1 on the substrate side and a lower layer A2 on the upper side thereof, the lower layer A1 is a layer formed by alternatingly stacking AlTiN layers of the aforementioned average thickness and the two Al contents, and the lower layer A2 is a layer formed by alternatingly stacking AlTiN layers of the aforementioned average thickness and the two Al contents, respectively, and the Al content of the two AlTiN layers of the lower layer A1 is greater than the Al content of the two AlTiN layers of the lower layer A2, then the aforementioned purpose can be achieved more reliably.

[0044] The coated tool according to the embodiment of the present invention is described in more detail below. In addition, in the description of this specification and claims, when "L to M" is used to express a numerical range, it has the same meaning as "above L and below M", and the range includes the numerical values ​​of the upper limit M and the lower limit L. In addition, when only the unit of the upper limit M is described, the unit of the upper limit M and the lower limit L is the same.

[0045] I. First Implementation

[0046] Next, a coating tool according to the first embodiment will be described.

[0047] 1. Coating layer

[0048] The layer structure of the coating layer of the coated tool according to the first embodiment of the present invention is as follows: Figure 1 As one example is schematically shown in FIG. 1 , the coating layer 2 has a lower layer A (3) on the substrate 1, and an upper layer B (4) on the upper portion of the lower layer A (3). Figure 1 In the embodiment, the lower layer A (3) is preferably a stack of thin layers each having an average thickness of 0.5 to 4.0 nm, that is, an alternating stack of A1α layers 7 and A1β layers 8. Figure 1 In the white background portion of the lower layer A(3), A1α layers 7 and A1β layers 8 are alternately stacked.

[0049] Furthermore, the coating layer may have other layers described below in addition to these layers.

[0050] (1) The sum of the average thickness of the lower layer A and the average thickness of the upper layer B

[0051] The sum of the average thickness of the lower layer A and the average thickness of the upper layer B in this embodiment is preferably 0.4 μm or more and 9.0 μm or less. The reason is that if it is less than 0.4 μm, excellent wear resistance cannot be exerted in long-term use, and on the other hand, if it is greater than 9.0 μm, the grains are easily coarsened and the chipping resistance cannot be improved. The average thickness is more preferably 0.8 μm or more and 6.0 μm or less.

[0052] (2) Average thickness of lower layer A and upper layer B

[0053] Preferably, the average thickness At of the lower layer A is greater than or equal to 0.3 μm and less than or equal to 6.0 μm, the average thickness Bt of the upper layer B is greater than or equal to 0.1 μm and less than or equal to 3.0 μm, and 2.0≤At / Bt≤5.0. The reason is that if the average thickness At of the lower layer A and the average thickness Bt of the upper layer B are within this range, oxidation damage of the coating layer during cutting can be suppressed, and TiAlN in the lower layer A is decomposed into TiN and AlN, thereby improving wear resistance.

[0054] More preferably, the average thickness At of the lower layer A is 0.6 μm or more and 4.0 μm or less, and the average thickness Bt of the upper layer B is 0.2 μm or more and 2.0 μm or less. In addition, more preferably, 2.3≤At / Bt≤3.5.

[0055] Furthermore, by making the average thickness Bt of the upper layer B thinner than the average thickness At of the lower layer A, the lower layer A decomposes AlTiN (AlTiN decomposes into TiN and AlN) during cutting, thereby increasing the hardness and improving the wear resistance of the coating layer.

[0056] (3) Composition of lower layer A

[0057] The lower layer A is an alternating stack of A1α layers and A1β layers. It is preferred that the average thicknesses αt and βt of the A1α layer and the A1β layer, respectively, satisfy the following relationship: 0.5nm≤αt≤4.0nm, 0.5nm≤βt≤4.0nm, 0.7≤βt / αt≤1.3. It is more preferred that 0.8nm≤αt≤3.5nm, 0.8nm≤βt≤3.5nm, 0.8≤βt / αt≤1.2 be satisfied.

[0058] The reason for this is that if the relationship between these average thicknesses is satisfied, the aforementioned object can be achieved.

[0059] (3-1) Number of A1α and A1β layers

[0060] If the number of stacked layers of the A1α layer is m and the number of stacked layers of the A1β layer is n, |mn|≤1. There is no particular limitation on m+n, but it is preferably 50 to 2001. The reason is that if it is less than 50, the cracks generated during cutting cannot be sufficiently prevented from progressing, so the defect resistance may be reduced. If it is greater than 2001, the number of repetitions increases, so that the grains of the lower layer A are finely divided, which sometimes leads to a reduction in wear resistance. m+n is more preferably 100 to 1001.

[0061] In addition, the A1α layers and the A1β layers may be alternately stacked, and the layers on the substrate side and the tool surface side may be arbitrary layers.

[0062] (3-2) Composition of A1α layer and A2α layer

[0063] The compositions of the A1α layer and the A2α layer constituting the lower layer are preferably as follows:

[0064] A1α layer is Al x Ti 1- xN(the average value of x avg 0.35≤x avg ≤0.55),

[0065] A1β layer is Al y Ti 1-y N(the average value of y avg 0.60≤y avg ≤0.80),

[0066] Satisfy 1.2≤y avg / x avg .

[0067] When the composition of the A1α layer and the A2α layer is within this range, the wear resistance is improved. The reason for this is presumably because AlTiN is decomposed into TiN and AlN during cutting.

[0068] In addition, AlTiN constituting the lower layer is manufactured in a ratio of (AlTi) to N of 1:1 according to an example of a manufacturing method described later, but the ratio may inevitably (unintentionally) not be 1:1. This also applies to other nitrides described below.

[0069] (4) Composition of upper layer B

[0070] Preferably, the upper layer B is Al a Ti 1-a-b Si b N(the average value of a avg , the average value of b avg 0.35≤a avg ≤0.60, 0.00<b avg ≤0.15).

[0071] When the composition of the upper layer B is within the above range, the oxidation resistance and the wear resistance can be improved, but when it is outside the range, the oxidation resistance and the wear resistance are reduced. The reason for this is presumably due to the precipitation of an AlN phase with a hexagonal structure.

[0072] (5) Other layers

[0073] (5-1) Layer that can be intentionally formed into a film

[0074] Examples of the layer that can be intentionally formed into a film include the outermost layer and the base layer described below.

[0075] (5-1-1) Outermost layer

[0076] An outermost layer may be selectively provided on the upper layer B.

[0077] As the outermost layer, for example, a TiN layer may be provided (the atomic ratio of Ti to N in the TiN layer is not limited to stoichiometric). When the TiN layer is provided, since the TiN layer itself has a golden hue, it can be used as, for example, an identification layer that distinguishes whether the coated tool is unused or used based on the change in hue. In addition, the average layer thickness of the TiN layer as the identification layer may be, for example, 0.1 to 1.0 μm.

[0078] (5-1-2) Basal layer

[0079] A base layer may be optionally provided between the lower layer A and the base.

[0080] Examples of the base layer include TiC, TiN, TiCN, and TiCNO layers, and Ti compound layers and AlTiN layers, and the average thickness thereof can be 0.1 to 2.0 μm. If the average thickness is within this range, the adhesion between the lower layer A and the substrate may be further improved.

[0081] (5-2) Unintentionally formed layer (layer that may be inevitably formed)

[0082] In this embodiment, the film is formed in a manner that there is no layer other than the base layer, the lower layer A (A1α layer and A1β layer), the upper layer B, and the outermost layer, that is, the film is formed in a manner that these layers are in contact. However, when the type of layer to be formed is changed, changes in pressure and temperature in the film forming device are unintentionally generated, and unintentional layers different from these layers may be formed.

[0083] 3. Matrix

[0084] (1) Material

[0085] If the matrix used in the present embodiment is a material of a matrix known in the past, any material can be used as long as it does not hinder the achievement of the aforementioned purpose. If one example is given, it is preferably a WC-based cemented carbide (in addition to WC, it also includes Co, and further includes an alloy formed by adding carbides or carbonitrides of Ti, Ta, Nb, etc.), a cermet (ceramics with TiC, TiN, TiCN, etc. as the main component, etc.), a ceramic (titanium carbide, silicon carbide, silicon nitride, aluminum nitride, aluminum oxide), a cBN sintered body, or a diamond sintered body.

[0086] (2) Shape

[0087] The shape of the base body is not particularly limited as long as it is a shape used as a cutting tool, and examples thereof include the shape of an insert and the shape of a drill.

[0088] II. Second Implementation

[0089] The second embodiment will be described below, but descriptions of parts that overlap with the description of the first embodiment will be omitted.

[0090] 1. Coating layer

[0091] The layer structure of the coating layer of the coating tool according to the second embodiment is as shown in Figure 2 As one example is schematically shown in FIG. 1 , the coating layer 2 has a lower layer A (3) on the substrate 1, and an upper layer B (4) is provided on the upper portion of the lower layer A (3). In the lower layer A (3), a lower layer A1 (5) and a lower layer A2 (6) are stacked. Figure 2 In the embodiment, it is preferred that the lower layer A1 (5) is the same as the first embodiment, and the lower layer A2 (6) is an alternating stack of thin layers each having an average thickness of 1.5 to 8.0 nm, that is, the lower layer A1 (5) is an alternating stack of A1α layers 7 and A1β layers 8, and the lower layer A2 (6) is an alternating stack of A2γ layers 9 and A2δ layers 10. In addition, in Figure 2 In the white background portions of the lower layer A1 (5) and the lower layer A2 (6), A1α layers 7 and A1β layers 8, A2γ layers 9 and A2δ layers 10 are alternately stacked.

[0092] Moreover, similarly to the first embodiment, the coating layer may have other layers described later in addition to these layers.

[0093] (1) The sum of the average thickness of the lower layer A and the average thickness of the upper layer B

[0094] In the second embodiment, the sum of the average thickness of the lower layer A and the average thickness of the upper layer B is preferably in the same thickness range as that of the first embodiment (the more preferred thickness range is also the same).

[0095] (2) Average thickness of lower layer A and upper layer B

[0096] In the second embodiment, the average thickness of each of the lower layer A and the upper layer B is preferably in the same thickness range as that of the first embodiment (more preferably, the thickness range is also the same).

[0097] (3) Composition of lower layer A

[0098] In the second embodiment, the lower layer A is composed of the lower layer A1 and the lower layer A2. Preferably, the average thickness A1t of the lower layer A1 and the average thickness A2t of the lower layer A2 are 0.1 μm≤A1t≤4.5 μm, 0.2 μm≤A2t≤4.0 μm, and 0.5≤A1t / A2t≤3.0. When this relationship is satisfied, the aforementioned object is achieved.

[0099] Next, the lower layer A1 and the lower layer A2 will be described in detail.

[0100] (3-1) Lower layer A1

[0101] Preferably, the lower layer A1 is an alternately stacked layer of A1α layers and A2α layers similar to the lower layer A of the first embodiment, and satisfies the average thickness and average thickness relationship described in the description of the first embodiment and further satisfies the composition and composition relationship.

[0102] (3-2) Lower layer A2

[0103] The lower layer A2 is an alternating stack of A2γ layers and A2δ layers. Preferably, the average thicknesses γt and δt of the A2γ layer and the A2δ layer, respectively, satisfy the following relationship: that is, 1.5nm≤γt≤8.0nm, 1.5nm≤δt≤8.0nm, 0.7≤δt / γt≤1.3, and relative to the average thicknesses of the A1α layer and the A2α layer constituting the lower layer A1, respectively, satisfy 1.0<(γt+δt) / (αt+βt)≤6.0.

[0104] The reason for this is that if this relational expression is satisfied, the aforementioned object is achieved. More preferably, (γt+δt) / (αt+βt) satisfies 1.2≤(γt+δt) / (αt+βt)≤3.0.

[0105] (3-2) Composition of A2γ layer and A2δ layer

[0106] The composition of the A2γ layer is preferably Al z Ti 1-z N(the average value of z avg 0.30≤z avg ≤0.50),

[0107] The composition of the A2δ layer is Al w Ti 1-w N(the average value of w avg 0.55≤w avg ≤0.75),

[0108] Satisfy 1.2≤w avg / z avg .

[0109] In addition, it is preferred that the composition of the A1α layer and the A2α layer and the composition of the A2γ layer and the A2δ layer satisfy 0.02≤(x avg -z avg )≤0.30、0.02≤(y avg -w avg )≤0.30.

[0110] If the composition of the A1α layer and the A2α layer and the composition of the A2γ layer and the A2δ layer are within this range, the wear resistance will be improved. It is speculated that the reason is that if the composition of these layers is within this range, a lower layer A with a higher Al content can be formed, and AlTiN is decomposed into TiN and AlN during cutting. However, when it is out of this range, the difference in Al content between the lower layer A1 and the lower layer A2 becomes smaller, the decomposition is insufficient, and the strain reduction of the lower layer A1 is insufficient, and an AlN phase with a hexagonal crystal structure is precipitated, resulting in a decrease in the wear resistance of the coating layer.

[0111] (4) Average thickness and number of layers of A1α, A1β, A2γ, and A2δ

[0112] It is preferred that the average thickness of the A1α layer and the A1β layer constituting the lower layer A1 and the lower layer A2 is 0.5 to 4.0 nm, and the average thickness of the A2γ layer and the A2δ layer is 1.5 to 8.0 nm. The number of layers p of the A1α layer and the number of layers q of the A1β layer in the lower layer A1, the number of layers r of the A2γ layer and the number of layers s of the A2δ layer in the lower layer A2 are |pq|≤1, |rs|≤1, and p+q and r+s are not particularly limited, but preferably p+q is 50 to 901 and r+s is 20 to 551. The reason is that if p+q is less than 50 and r+s is less than 20, the cracks generated during cutting cannot be sufficiently prevented from progressing, so the defect resistance may be reduced. On the other hand, if p+q is greater than 901 and r+s is greater than 551, the number of repetitions increases, so that the grains of the lower layer A are finer, which sometimes leads to reduced wear resistance. More preferably, p+q is 100-451, and r+s is 50-180.

[0113] The A1α layer and the A1β layer, and the A2γ layer and the A2δ layer may be alternately stacked, and the layers on the substrate side and the tool surface side may be arbitrary layers.

[0114] 3. Upper layer

[0115] The upper layer is the same as described in the first embodiment.

[0116] 4. Other layers

[0117] Regarding the outermost layer and the base layer, they are the same as described in the first embodiment.

[0118] Regarding the unintentionally formed layers (layers that may be inevitably produced), it is the same as the case where the lower layer A (A1α layer and A1β layer) is replaced by the lower layer A1 (A1α layer and A1β layer) and the lower layer A2 (A2γ layer and A2δ layer).

[0119] 5. Matrix

[0120] The material and shape of the base may be the same as those in the first embodiment.

[0121] III. Determination Method

[0122] 1. Average composition and average thickness of lower layer A, upper layer B and other layers

[0123] The average thickness of the lower layer A, lower layer A1, lower layer A2, upper layer B and other layers constituting the coating layer can be determined by observing a longitudinal section (in the case of a blade, when the micro-concavities and convexities on the substrate surface are ignored and the substrate is treated as a flat surface, the section is perpendicular to the surface; in the case of an axial tool such as a drill, the section is perpendicular to the axis) using an energy dispersive X-ray spectrometer (EDS) attached to a scanning electron microscope (SEM) or a transmission electron microscope (TEM) to identify each layer and determine its average thickness. The average content ratio of each component in each layer can be determined by performing five TEM-EDS line analyses in the thickness direction.

[0124] Here, regarding the surface of the substrate, its longitudinal section is observed, and the interface between the substrate and the lower layer A (or lower layer A1) is determined by element mapping. The average straight line of the roughness curve of the interface obtained in this way is arithmetically calculated and is taken as the surface of the substrate.

[0125] 2. Average thickness of A1α layer, A1β layer, A2γ layer and A2δ layer

[0126] In the thickness direction of the coating layer, a line scan is performed with a length of at least 10 layers, preferably more than 50 layers, including these layers, and the average values ​​of the maximum and minimum values ​​of the intensity of the adjacent Ti EDS spectrum are calculated respectively. The position on the line segment where the line scan was performed is found, and the position gives the average value of the calculated adjacent maximum and minimum values ​​of the intensity. In addition, the distance between the positions containing a maximum value and giving the adjacent average value and the distance between the positions containing a minimum value and giving the adjacent average value become the thickness of each layer, and the average thickness can be obtained by averaging them.

[0127] IV. Manufacturing Method

[0128] The coating layer of the coated tool of the first embodiment and the second embodiment can be manufactured using, for example, an AIP device (arc ion plating device). In addition, the film can be formed by using an AiTi target having a composition corresponding to the composition of the lower layer A, the lower layer A1, and the lower layer A2 as the target, and using an AlTiSi target having a composition corresponding to the composition of the upper layer B as the target for forming the film of the upper layer B.

[0129] The above description includes the following additional features.

[0130] (Note 1)

[0131] A surface-coated cutting tool comprises a substrate and a coating layer arranged on the substrate, characterized in that:

[0132] The covering layer comprises a lower layer A and an upper layer B on the lower layer A,

[0133] The average thickness At of the lower layer A is greater than or equal to 0.3 μm and less than or equal to 6.0 μm, the average thickness Bt of the upper layer B is greater than or equal to 0.1 μm and less than or equal to 3.0 μm, 2.0≤At / Bt≤5.0,

[0134] The lower layer A comprises an alternating stack of A1α layers with an average thickness of αt and A1β layers with an average thickness of βt,

[0135] 0.5nm≤αt≤4.0nm, 0.5nm≤βt≤4.0nm, 0.7≤βt / αt≤1.3,

[0136] The composition of the A1α layer is Al x Ti 1-x N(the average value of x avg 0.35≤x avg ≤0.55),

[0137] The composition of the A1β layer is Al y Ti 1-y N(the average value of y avg 0.60≤y avg ≤0.80),

[0138] Satisfy 1.2≤y avg / x avg ,

[0139] The composition of the upper layer B is Al a Ti 1-a-b Si b N(the average value of a avg , the average value of b avg 0.35≤a avg ≤0.60, 0.00<b avg ≤0.15).

[0140] (Note 2)

[0141] The surface coated cutting tool according to Supplementary Note 1 is characterized in that:

[0142] The lower layer A is a lower layer A1 on the substrate side and a lower layer A2 on the upper layer B side.

[0143] The average thickness A1t of the lower layer A1 and the average thickness A2t of the lower layer A2 are 0.1 μm≤A1t≤4.5 μm, 0.2 μm≤A2t≤4.0 μm, 0.5≤A1t / A2t≤3.0,

[0144] The lower layer A1 is the alternating stack of the A1α layer and the A1β layer,

[0145] The lower layer A2 is an alternating stack of A2γ layers with an average thickness of γt and A2δ layers with an average thickness of δt.

[0146] 1.5nm≤γt≤8.0nm, 1.5nm≤δt≤8.0nm, 0.7≤δt / γt≤1.3,

[0147] 1.0<(γt+δt) / (αt+βt)≤6.0,

[0148] The composition of the A2γ layer is Al z Ti 1-z N(the average value of z avg 0.30≤z avg ≤0.50),

[0149] The composition of the A2δ layer is Al w Ti 1-w N(the average value of w avg 0.55≤w avg ≤0.75),

[0150] Satisfy 1.2≤w avg / z avg ,

[0151] And 0.02≤(x avg -z avg )≤0.30、0.02≤(y avg -w avg )≤0.30.

[0152] (Note 3)

[0153] The surface-coated cutting tool according to Supplementary Note 1 or 2 is characterized in that the upper layer B has an outermost layer.

[0154] (Note 4)

[0155] The surface-coated cutting tool according to any one of Supplementary Notes 1 to 3, characterized in that a base layer is provided between the lower layer A and the base body.

[0156] Example

[0157] Next, examples are described.

[0158] Here, as an embodiment of the coated tool of the present invention, a coated tool whose substrate is WC-based cemented carbide and has a blade shape is described, but the substrate can be any of the aforementioned materials. In addition, as mentioned above, its shape can also be a drill, end mill, etc.

[0159] First, as raw material powders, Co powder, TiC powder, VC powder, TaC powder, NbC powder, Cr3C2 powder, and WC powder were prepared, and these raw material powders were mixed according to the mixing ratio shown in Table 1, and wax was further added and wet mixed with a ball mill for 72 hours, and after reduced pressure drying, they were pressed at a pressure of 100 MPa. Their green compacts were sintered at 1400° C. for 1 hour under a vacuum atmosphere of 6 Pa, processed into a specified size, and WC-based cemented carbide substrates 1 to 3 having a blade shape of ANSI standard SEEN42AFTN1 were manufactured.

[0160] Next, the substrates 1 to 3 were ultrasonically cleaned in acetone and dried. In order to form a coating layer using an AIP device, the substrates 1 to 3 were installed along the periphery at a position separated from the central axis of the rotating table in the device in the radial direction by a predetermined distance. In addition, a target of a predetermined composition was arranged as a cathode electrode (evaporation source).

[0161] Next, while the AIP device is evacuated and maintained at a vacuum below 0.1 Pa, the device is heated to 600°C with a heater, a DC bias voltage of -1000V is applied to the substrate rotating on the turntable, and a current of 100A is passed between the cathode electrode and the anode electrode to bombard the surface of the substrate.

[0162] <Example corresponding to the first embodiment>

[0163] The reaction gas in the AIP device is set to a nitrogen atmosphere with a partial pressure of 2.6 to 7.5 Pa as shown in Table 2, and the furnace temperature is maintained as shown in Table 2. Then, a DC voltage of -40 to -125 V as shown in Table 2 is applied to the substrate rotating on the above-mentioned turntable, and a current of 125 to 210 A flows between the AlTi alloy electrode for forming the lower layer A (A1α layer, A1β layer) and the anode electrode to generate arc discharge, thereby forming the A1α layer and the A1β layer of a specified thickness.

[0164] Then, the number of layers of the lower layer A is determined by repeating the film formation of the A1α layer and the A1β layer a predetermined number of times.

[0165] Next, in a nitrogen atmosphere with a partial pressure of 0.4 to 0.6 Pa as shown in Table 2, a DC voltage of -40 to -120 V as shown in Table 2 is applied to the substrate, and a current of 120 to 220 A is passed between the AiTiSi alloy used to form the upper layer B and the anode electrode to generate arc discharge, thereby forming an upper layer B of a specified thickness to obtain the coated tools of the embodiments (hereinafter referred to as embodiments) 1 to 9.

[0166] <Example corresponding to the second embodiment>

[0167] The reaction gas in the AIP device is set to a nitrogen atmosphere with a partial pressure of 1.0 to 8.2 Pa as shown in Table 4, and the furnace temperature is maintained as shown in Table 4. Then, a DC voltage of -30 to -120 V as shown in Table 2 is applied to the substrate rotating on the above-mentioned turntable, and a current of 100 to 230 A flows between the AlTi alloy electrode for forming the lower layer A1 (A1α layer, A1β layer) and the anode electrode to generate arc discharge, thereby forming the A1α layer and A1β layer of a specified thickness.

[0168] Then, the film formation of the A1α layer and the A1β layer is repeated a predetermined number of times to obtain a predetermined number of stacked layers of the lower layer A1.

[0169] Next, in a nitrogen atmosphere with a partial pressure of 3.2 to 7.5 Pa as shown in Table 4, a DC voltage of -60 to -135 V is applied, and a current of 115 to 250 A is passed between the AlTi alloy electrode used to form the lower layer A2 (A2γ layer, A2δ layer) and the anode electrode to generate arc discharge, thereby forming A2γ layer and A2δ layer of specified thickness.

[0170] Then, the film formation of the A2γ layer and the A2δ layer is repeated a predetermined number of times to obtain a predetermined number of stacked layers of the lower layer A2.

[0171] Next, in a nitrogen atmosphere with a partial pressure of 2.5 to 7.7 Pa as shown in Table 4, a DC voltage of -45 to -180 V as shown in Table 2 is applied to the substrate, and a current of 125 to 200 A is passed between the AiTiSi alloy used to form the upper layer B and the anode electrode to generate arc discharge, and an upper layer B of a specified thickness is formed to obtain Examples 11 to 19.

[0172] Furthermore, in several examples corresponding to the first embodiment and the second embodiment, a nitrogen atmosphere with a partial pressure of 0.5 to 9.0 Pa is used as the reaction gas in the AIP device, and the temperature in the furnace is maintained at 300 to 600° C. Then, a DC voltage of -20 to -500 V is applied to the substrate rotating on the above-mentioned turntable, and a current of 50 to 250 A flows between the Ti electrode for forming the outermost layer and the anode electrode to generate arc discharge, and the outermost layer, i.e., the TiN layer, of a predetermined thickness is formed (the film forming conditions of the outermost layer are shown in Table 6). These examples are shown in Tables 7 and 8.

[0173] On the other hand, for the purpose of comparison, the same film-forming apparatus as that described above was used for the above-mentioned substrates 1 to 3, and a coating layer of a comparative example corresponding to the first embodiment was formed by vapor deposition according to the conditions shown in Table 3. A coating layer of a comparative example corresponding to the second embodiment was formed by vapor deposition according to the conditions shown in Table 5. Coated tools (hereinafter referred to as "comparative examples") 1 to 9 and 11 to 19 of the comparative examples shown in Tables 7 and 8 were prepared.

[0174] In some comparative examples corresponding to the first embodiment and the second embodiment, the TiN layer as the outermost layer was formed in the same manner as in the examples.

[0175] Regarding the average thickness and average composition of the coating layer, the average thickness and average composition of the coating layer were determined by observing the longitudinal section of the coating layer perpendicular to the surface of the substrate of Examples 1 to 9, 11 to 19 and Comparative Examples 1 to 9, 11 to 19 prepared as described above, with a field of view having a width of 10 μm in a direction parallel to the surface of the substrate and set to include the entire thickness region of the coating layer, using a scanning electron microscope (SEM), a transmission electron microscope (TEM), and an energy dispersive X-ray spectrometer (EDS).

[0176] Specifically, regarding the average thickness of the lower layer A and the upper layer B, the longitudinal section as the observation section was magnified 5000 times, the film thickness at five points was obtained, and the average thickness was calculated. In addition, when the average thickness of the lower layer A and the upper layer B was less than 1 μm, the longitudinal section as the observation section was magnified 10000 times, the film thickness at five points was obtained, and the average thickness was calculated. In addition, the average thickness of each layer constituting the alternately stacked layer and the average content of each component in each layer were measured by the above method.

[0177] [Table 1]

[0178]

[0179]

[0180]

[0181]

[0182]

[0183] [Table 6]

[0184]

[0185]

[0186]

[0187] Next, about Examples 1 to 9, 11 to 19 and Comparative Examples 1 to 9, 11 to 19, cutting tests 1 to 3 were performed under the following cutting conditions.

[0188] Cutting test 1

[0189] Cutting conditions:

[0190] Workpiece: Block material (SUS304) with a width of 60 mm and a length of 200 mm

[0191] Cutting speed: 160m / min.

[0192] Cutting depth: 1.5mm

[0193] Feed rate: 0.10mm / tooth.

[0194] Cutting was continued until the cutting length reached 2.0 m, and the flank wear width was measured to observe the wear state of the tool tip. Since the flank wear width also includes the wear width caused by oxidation damage and boundary damage, it is also possible to evaluate whether oxidation damage and boundary damage are suppressed.

[0195] The results of the cutting test are shown in Tables 9 and 10.

[0196] Cutting test 2

[0197] Cutting conditions:

[0198] Workpiece: Block material with a width of 60 mm and a length of 200 mm (FC■450)

[0199] Cutting speed: 180m / min.

[0200] Cutting depth: 1.2mm

[0201] Feed rate: 0.10mm / tooth.

[0202] Cut to a cutting length of 10.0 m, measure the wear width of the flank face, and observe the wear condition of the tool tip.

[0203] The results of the cutting test are shown in Tables 11 and 12.

[0204] Cutting test 3

[0205] Cutting conditions:

[0206] Workpiece: Block material (SNCM435) with a width of 60 mm and a length of 200 mm

[0207] Cutting speed: 200m / min.

[0208] Cutting depth: 1.2mm

[0209] Feed rate: 0.10mm / tooth.

[0210] Cut to a cutting length of 10.0 m, measure the wear width of the flank face, and observe the wear condition of the tool tip.

[0211] The results of the cutting test are shown in Tables 13 and 14.

[0212] [Table 9]

[0213]

[0214] In Table 9, “※” indicates that the service life is reached before the maximum cutting length is reached, and “※” indicates the time (seconds) to reach the service life.

[0215] [Table 10]

[0216]

[0217] [Table 11]

[0218]

[0219] [Table 12]

[0220]

[0221] [Table 13]

[0222]

[0223] [Table 14]

[0224]

[0225] According to the results of Tables 9 to 14, Examples 1 to 9 and 11 to 19 did not suffer from abnormal damage such as chipping and peeling, and were excellent in wear resistance and chipping resistance.

[0226] On the other hand, it is clear that the blades of Comparative Examples 1 to 9 and 11 to 19 reach the end of their life in a short time due to the occurrence of chipping or the progress of flank wear.

[0227] The embodiments disclosed above are merely illustrative in all aspects and are not restrictive. The scope of the present invention is expressed by the claims rather than the embodiments described above, and is intended to include all modifications within the meaning and scope equivalent to the claims.

[0228] Description of Reference Numerals

[0229] 1 Matrix

[0230] 2. Coating

[0231] 3Lower Layer A

[0232] 4Upper layer B

[0233] 5Lower layer A1

[0234] 6 Lower layer A2

[0235] 7A1α layer

[0236] 8A1β layer

[0237] 9A2γ layer

[0238] 10A2δ layer

Claims

1. A surface-coated cutting tool comprising a substrate and a coating layer disposed on the substrate, characterized in that: The covering layer comprises a lower layer A and an upper layer B on the lower layer A, The average thickness At of the lower layer A is greater than or equal to 0.3 μm and less than or equal to 6.0 μm, the average thickness Bt of the upper layer B is greater than or equal to 0.1 μm and less than or equal to 3.0 μm, 2.0≤At / Bt≤5.0, The lower layer A comprises an alternating stack of A1α layers with an average thickness of αt and A1β layers with an average thickness of βt, 0.5nm≤αt≤4.0nm, 0.5nm≤βt≤4.0nm, 0.7≤βt / αt≤1.3, The composition of the A1α layer is Al x Ti 1-x N, Among them, the average value of x avg 0.35≤x avg ≤0.55, The composition of the A1β layer is Al y Ti 1-y N, where the mean value of y is y avg 0.60≤y avg ≤0.80, Satisfy 1.2≤y avg / x avg , The composition of the upper layer B is Al a Ti 1-a-b Si b N, where the average value of a is a avg , the average value of b avg 0.35≤a avg ≤0.60, 0.00<b avg ≤0.

15.

2. The surface-coated cutting tool according to claim 1, characterized in that: The lower layer A is a lower layer A1 on the substrate side and a lower layer A2 on the upper layer B side. The average thickness A1t of the lower layer A1 and the average thickness A2t of the lower layer A2 are 0.1 μm≤A1t≤4.5 μm, 0.2 μm≤A2t≤4.0 μm, 0.5≤A1t / A2t≤3.0, The lower layer A1 is the alternating stack of the A1α layer and the A1β layer, The lower layer A2 is an alternating stack of A2γ layers with an average thickness of γt and A2δ layers with an average thickness of δt. 1.5nm≤γt≤8.0nm, 1.5nm≤δt≤8.0nm, 0.7≤δt / γt≤1.3, 1.0<(γt+δt) / (αt+βt)≤6.0, The composition of the A2γ layer is Al z Ti 1-z N, where the average value of z is z avg 0.30≤z avg ≤0.50, The composition of the A2δ layer is Al w Ti 1-w N, where the average value of w is w avg 0.55≤w avg ≤0.75, Satisfy 1.2≤w avg / z avg , And 0.02≤(x avg -z avg )≤0.30、0.02≤(y avg -w avg )≤0.30.

Citation Information

Patent Citations

  • Coated cutting tool

    JP2015110259A

  • Flower vase comprising transparent needle-point holder

    JP2017018551A

  • Surface coated cutting tool

    JP2017193004A

  • Surface-coated cutting tool

    CN104582881A

  • Surface-coated cutting tool

    JP2014091169A