Coated tool and cutting tool

By forming a hexagonal crystal structure and an alternating laminated structure on the coated tool that meets the specific X-ray diffraction spectrum, the problem of insufficient wear resistance and heat resistance of the existing coated tools is solved, and the tool life is significantly extended.

CN118922266AActive Publication Date: 2024-11-08KYOCERA CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202380030061.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2023-03-31
Publication Date
2024-11-08
Estimated Expiration
2043-03-31

AI Technical Summary

Technical Problem

There is room for improvement in the wear resistance and heat resistance of existing coated tools in cutting processing, resulting in a short tool life.

Method used

Using a coating layer composed of cubic crystals, a hexagonal crystal structure satisfies 1h(100)/Ih(002)≤0.9 was formed by heat treatment at a temperature of 1200°C under a non-oxidizing atmosphere, and the coating layer was formed. The Ta and Mo laminated structures are alternately arranged to improve bond resistance and collapse resistance.

Benefits of technology

It extends the life of coated tools, improves its wear and heat resistance in high-speed and low-speed machining, and reduces the risk of bond damage and collapse.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922266A_ABST
    Figure CN118922266A_ABST
Patent Text Reader

Abstract

The coated cutting tool according to the present invention is provided with: a base body; and a coating layer on the substrate and composed of cubic crystals. The X-ray diffraction spectrum measured for the coating layer after being held for 0.5 hour at a temperature of 1200 DEG C in a non-oxidizing atmosphere satisfies the relationship Ih (100) / Ih (002) < = 0.9. Ih (100) is an intensity of a diffraction peak corresponding to a (100) plane of a hexagonal crystal formed in the coating layer. Ih (002) is the intensity of a diffraction peak corresponding to the (002) plane of the hexagonal crystal.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a coated tool and a cutting tool. Background Art

[0002] As a tool used for cutting such as turning and milling, there is known a coated tool in which the surface of a base body such as cemented carbide, cermet, or ceramic is coated with a coating layer to improve wear resistance and the like.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2002-3284 Summary of the invention

[0006] A coated tool according to one embodiment of the present invention comprises: a substrate; and a coating layer, which is located on the substrate and is composed of cubic crystals. The X-ray diffraction spectrum measured for the coating layer after being kept at a temperature of 1200°C for 0.5 hours in a non-oxidizing atmosphere satisfies the relationship of Ih(100) / Ih(002)≤0.9. Ih(100) is the intensity of the diffraction peak corresponding to the (100) plane of the hexagonal crystal formed in the coating layer. Ih(002) is the intensity of the diffraction peak corresponding to the (002) plane of the hexagonal crystal. BRIEF DESCRIPTION OF THE DRAWINGS

[0007] Figure 1 This is a perspective view showing an example of a coated tool according to the embodiment.

[0008] Figure 2 This is a side sectional view showing an example of a coated tool according to the embodiment.

[0009] Figure 3 This is a diagram schematically showing an example of an X-ray diffraction spectrum measured for the coating layer according to the embodiment.

[0010] Figure 4 This is a cross-sectional view showing an example of a coating layer according to an embodiment.

[0011] Figure 5 It is a cross-sectional view showing an example of a Ta-containing stacked structure and a Mo-containing stacked structure constituting the coating layer of the embodiment.

[0012] Figure 6 It is a cross-sectional view showing an example of the first compound layer and the second compound layer constituting the Ta-containing stacked structure.

[0013] Figure 7 It is a cross-sectional view showing an example of the third compound layer and the fourth compound layer constituting the Mo-containing stacked structure.

[0014] Figure 8 This is a diagram schematically showing an example of a film forming apparatus for forming a coating layer on a substrate.

[0015] Fig. 9 This is a front view showing an example of a cutting tool according to an embodiment.

[0016] Fig.10 This is a table showing the production conditions of the coating layer formed on the substrate.

[0017] Fig.11 : is a table showing the structure of the coating layer formed on the substrate.

[0018] Fig. 12A This is a diagram showing an X-ray diffraction spectrum measured for the coating layer of the coated tool of Sample No. 1 after heat treatment.

[0019] Fig. 12B This is a diagram showing an X-ray diffraction spectrum measured for the coating layer of the coated tool of Sample No. 2 after heat treatment.

[0020] Fig. 12C This is a diagram showing an X-ray diffraction spectrum measured for the coating layer of the coated tool of Sample No. 3 after heat treatment.

[0021] Fig.12D This is a diagram showing an X-ray diffraction spectrum measured for the coating layer of the coated tool of Sample No. 4 after heat treatment.

[0022] Fig.13 This is a table showing the results of X-ray diffraction spectrum measurement and cutting test on coated cutting tools of Samples No. 1 to No. 4. DETAILED DESCRIPTION

[0023] Hereinafter, the method for implementing the coated tool and cutting tool based on the present invention (hereinafter, recorded as "embodiment") is described in detail with reference to the accompanying drawings. The coated tool and cutting tool based on the present invention are not limited by this embodiment. The various embodiments can be appropriately combined within the scope that does not cause contradictions in the processing contents. In the following various embodiments, the same reference numerals are marked on the same parts, and repeated descriptions are omitted.

[0024] In the embodiments described below, there are cases where expressions such as "constant", "orthogonal", "perpendicular" or "parallel" are used, but these expressions do not need to be strictly "constant", "orthogonal", "perpendicular" or "parallel". That is, each of the above expressions allows deviations such as manufacturing accuracy or setting accuracy.

[0025] As a tool used for cutting such as turning and milling, there is known a coated tool in which the surface of a base body such as cemented carbide, cermet, or ceramic is coated with a coating layer to improve wear resistance and the like.

[0026] In the above-mentioned conventional techniques, there is room for further improvement in terms of extending the life of the tool.

[0027] Therefore, realization of a technology capable of overcoming the above-mentioned problems and extending the life of a tool is desired.

[0028] <Coated tools>

[0029] Figure 1 : is a perspective view showing an example of a coated tool according to an embodiment. Figure 2 1 is a side sectional view showing an example of a coated tool 1 according to an embodiment. Figure 1 As shown, a coated tool 1 according to the embodiment includes an insert body 2 .

[0030] (Blade body 2)

[0031] The blade body 2 has, for example, an upper surface and a lower surface ( Figure 1 The shape of the surface intersecting with the Z axis) is a hexahedron of a parallelogram.

[0032] A corner portion of the blade body 2 functions as a cutting edge portion. The cutting edge portion has a first surface (e.g., an upper surface) and a second surface (e.g., a side surface) connected to the first surface. In an embodiment, the first surface functions as a "front face" for scraping off chips generated by cutting, and the second surface functions as a "flank face". A cutting edge is disposed on at least a portion of the ridgeline where the first surface and the second surface intersect, and the coated tool 1 cuts the cutter by pressing the cutting edge against the cutter.

[0033] A through hole 5 is disposed in the center of the blade body 2, penetrating the blade body 2 from top to bottom. A screw 75 (see FIG. 1 ) for attaching the coated tool 1 to a tool holder 70 described later is inserted into the through hole 5. Fig. 9 ).

[0034] like Figure 2 As shown, the insert body 2 has a base body 10 and a coating layer 20 .

[0035] (Substrate 10)

[0036] The substrate 10 is formed of, for example, cemented carbide. Cemented carbide contains W (tungsten), specifically WC (tungsten carbide). Cemented carbide may also contain Ni (nickel) or Co (cobalt). Specifically, the substrate 10 is composed of a WC-based cemented carbide having WC particles as a hard phase component and Co as a main component of a bonding phase.

[0037] The base 10 may be formed of cermet. The cermet contains, for example, Ti (titanium), specifically, TiC (titanium carbide) or TiN (titanium nitride). The cermet may contain Ni or Co.

[0038] The substrate 10 may also be formed of a cubic boron nitride sintered body containing cubic boron nitride (cBN) particles. The substrate 10 is not limited to cubic boron nitride (cBN) particles, but may also contain particles of hexagonal boron nitride (hBN), rhombohedral boron nitride (rBN), or wurtzite boron nitride (wBN).

[0039] The substrate 10 may also be formed of ceramics. For example, the ceramics contain Al2O3 oxide (aluminum oxide), such as K-Al2O3 and α-Al2O3. The ceramics may also contain elements other than aluminum oxide. For example, the ceramics may also contain magnesium (Mg), calcium (Ca), strontium (Sr), silicon (Si) and at least one of the third group elements of the periodic table in addition to aluminum oxide.

[0040] (Coating layer 20)

[0041] The coating layer 20 is coated on the substrate 10 for the purpose of improving the wear resistance and heat resistance of the substrate 10, for example. Figure 2 In the example of , the coating layer 20 covers the substrate 10 as a whole. The coating layer 20 only needs to be located at least on the substrate 10. When the coating layer 20 is located on the first surface (here, the upper surface) of the substrate 10, the wear resistance and heat resistance of the first surface are high. When the coating layer 20 is located on the second surface (here, the side surface) of the substrate 10, the wear resistance and heat resistance of the second surface are high.

[0042] Here, refer to Figure 3 Specific characteristics of the coating layer 20 will be described. Figure 3 Schematically shows an example of an X-ray diffraction spectrum measured for the coating layer 20 of the embodiment. The coating layer 20 of the embodiment is composed of cubic crystals at a temperature of room temperature to 1000°C. The coated tool 1 of the embodiment is subjected to a heat treatment in a non-oxidizing atmosphere at a temperature of 1200°C for 0.5 hours. In the heat treatment, for example, a closed heating furnace (atmosphere furnace) can be used. As the non-oxidizing atmosphere, for example, a neutral gas such as nitrogen or hydrogen, or an inert gas such as helium or argon can be used.

[0043] Such heat treatment causes phase transition from cubic crystals to hexagonal crystals constituting the coating layer 20 of the embodiment. That is, the coating layer 20 after the heat treatment contains not only cubic crystals but also hexagonal crystals.

[0044] Next, an X-ray diffractometer (XRD) is used to measure the X-ray diffraction spectrum of the heat-treated coating layer 20. Figure 3 As shown in FIG. 1 , the X-ray diffraction spectrum measured after heat treatment shows various diffraction peaks such as the diffraction peak corresponding to the (iii) face of the cubic crystal, the diffraction peak corresponding to the (200) face of the cubic crystal, the diffraction peak corresponding to the (100) face of the hexagonal crystal, and the diffraction peak corresponding to the (002) face of the hexagonal crystal. Figure 3 In the figure, c(111), c(200), h(100) and h(002) are used to show the diffraction peak corresponding to the (iii) plane of the cubic crystal, the diffraction peak corresponding to the (200) plane of the cubic crystal, the diffraction peak corresponding to the (100) plane of the hexagonal crystal, and the diffraction peak corresponding to the (002) plane of the hexagonal crystal.

[0045] Regarding the coating layer 20 of the embodiment, the X-ray diffraction spectrum measured for the coating layer 20 after heat treatment satisfies the relationship of Ih(100) / Ih(002)≤0.9. Here, Ih(100) is the intensity of the diffraction peak corresponding to the (100) plane of the hexagonal crystal formed in the coating layer 20, and Ih(002) is the intensity of the diffraction peak corresponding to the (002) plane of the hexagonal crystal.

[0046] When the X-ray diffraction spectrum measured for the coating layer 20 after heat treatment satisfies the relationship Ih(100) / Ih(002)≤0.9, the proportion of hexagonal crystals formed in the coating layer 20 that are oriented in a manner such that the (002) plane of the hexagonal crystal is parallel to the surface of the substrate 10 on which the coating layer 20 is provided (the direction of the c-axis of the hexagonal crystal is perpendicular to the surface of the substrate 10) (hereinafter referred to as "first-oriented hexagonal crystals") is greater than the proportion of hexagonal crystals that are oriented in a manner such that the (100) plane of the hexagonal crystal is parallel to the surface of the substrate 10 (the direction of the c-axis of the hexagonal crystal is parallel to the surface of the substrate 10) (hereinafter referred to as "second-oriented hexagonal crystals").

[0047] The hexagonal crystals of the first orientation are easy to slide on the (002) plane, and the hexagonal crystals of the second orientation are easy to slide on the (100) plane. Here, the (002) plane of the hexagonal crystal is easier to cause sliding between the planes than the (100) plane of the hexagonal crystal. Therefore, it is believed that when the proportion of the hexagonal crystals in the first orientation is larger than the proportion of the hexagonal crystals in the second orientation, sliding of the (002) plane is easy to cause. As a result, it is believed that the damage caused by the adhesion of the cut part (damage such as film peeling and collapse caused by the detachment of the adhesive part) can be suppressed to a minimum, and the adhesion resistance and collapse resistance of the coating layer 20 can be improved.

[0048] It is believed that when the coated tool 1 of the embodiment is used to cut a workpiece, the strain of the hexagonal crystals in the first orientation is smaller than the strain of the hexagonal crystals in the second orientation. Therefore, it is believed that when the proportion of the hexagonal crystals in the first orientation is larger than the proportion of the hexagonal crystals in the second orientation, the reduction in the hardness of the coating layer 20 can be reduced. As a result, it is believed that the wear resistance of the coating layer 20 can be improved.

[0049] In this way, when the X-ray diffraction spectrum measured for the coating layer 20 after the heat treatment satisfies the relationship of Ih(100) / Ih(002)≦0.9, the life of the coated tool 1 can be extended.

[0050] During high-speed machining, the temperature of the coated tool 1 becomes around 1200°C. Therefore, it is considered that heat treatment of the coating layer 20 at a temperature of 1200°C for 0.5 hours in a non-oxidizing atmosphere corresponds to high-speed machining (machining at a cutting speed of ~200m / min) performed by the coated tool 1. During high-speed machining, when the temperature of the coating layer 20 composed of cubic crystals rises to around 1200°C, hexagonal crystals are generated in the coating layer 20. Generally, there is a tendency for the hardness and wear resistance of the coating layer to decrease when the proportion of hexagonal crystals increases. As a result, there is a tendency for the life of the coated tool during high-speed machining to become shorter. However, in the coated tool 1 of the embodiment, the X-ray diffraction spectrum measured for the coating layer 20 after heat treatment satisfies the relationship of Ih(100) / Ih(002)≤0.9, so that during high-speed machining, the reduction in the wear resistance of the coating layer 20 can be reduced, and the adhesion resistance and fracture resistance of the coating layer 20 relative to the cut workpiece can be improved.

[0051] On the other hand, in low-speed machining, the temperature of the coated tool 1 is about room temperature to 1000°C. In this case, the coating layer 20 is composed of cubic crystals, so the hardness and wear resistance of the coating layer 20 are maintained. In addition, the hardness and toughness of the coating layer 20 can be improved by the structure of the coating layer 20 in which the X-ray diffraction spectrum measured for the coating layer 20 after heat treatment as described later satisfies the relationship of Ih(100) / Ih(002)≤0.9. As a result, the wear resistance of the coating layer 20 can be improved in low-speed machining.

[0052] In this way, when the X-ray diffraction spectrum measured for the coating layer 20 after the heat treatment satisfies the relationship of Ih(100) / Ih(002)≤0.9, the life of the coated tool 1 can be extended in both low-speed machining and high-speed machining.

[0053] The X-ray diffraction spectrum measured for the heat-treated coating layer 20 may satisfy the relationship of Ih(100) / Ih(002)≤0.3. In this case, the proportion of hexagonal crystals in the first orientation can be further increased. As a result, the life of the coated tool 1 can be further extended.

[0054] Here, refer to Figure 4 , Figure 5 , Figure 6 as well as Figure 7 A specific structure of the coating layer 20 in which an X-ray diffraction spectrum measured for the coating layer 20 after the heat treatment satisfies the relationship of Ih(100) / Ih(002)≤0.9 will be described. Figure 4 It is a cross-sectional view showing an example of the coating layer 20 according to the embodiment. Figure 5 It is a cross-sectional view showing an example of a Ta-containing stacked structure and a Mo-containing stacked structure constituting the coating layer 20 according to the embodiment. Figure 6 It is a cross-sectional view showing an example of the first compound layer and the second compound layer constituting the Ta-containing stacked structure. Figure 7 It is a cross-sectional view showing an example of the third compound layer and the fourth compound layer constituting the Mo-containing stacked structure.

[0055] like Figure 4 As shown, the coating layer 20 includes a plurality of Ta-containing stacked structures 22 and a plurality of Mo-containing stacked structures 23 located on the intermediate layer 21. Each of the plurality of Ta-containing stacked structures 22 is a stacked structure containing at least Ta. Each of the plurality of Mo-containing stacked structures 23 is a stacked structure containing at least Mo.

[0056] like Figure 4 As shown, a plurality of Ta-containing stacked structures 22 and a plurality of Mo-containing stacked structures 23 may be alternately stacked in the coating layer 20 .

[0057] In this case, the residual stress between the Ta-containing stacked structure 22 and the Mo-containing stacked structure 23 can be reduced. As a result, the peeling or cracking between the Ta-containing stacked structure 22 and the Mo-containing stacked structure 23 can be reduced. In addition, the effects of the Ta-containing stacked structure 22 and the Mo-containing stacked structure 23 described later can be improved. As a result, the life of the coated tool 1 can be extended.

[0058] The average value of the thickness of each of the plurality of Ta-containing stacked structures 22 and the plurality of Mo-containing stacked structures 23 may be 300 nm or more and 500 nm or less.

[0059] In this case, the residual stress between the Ta-containing stacked structure 22 and the Mo-containing stacked structure 23 can be reduced. As a result, the peeling or cracking between the Ta-containing stacked structure 22 and the Mo-containing stacked structure 23 can be reduced. In addition, the effects of the Ta-containing stacked structure 22 and the Mo-containing stacked structure 23 described later can be improved. As a result, the life of the coated tool 1 can be extended.

[0060] (Middle layer 21)

[0061] An intermediate layer 21 may be disposed between the substrate 10 and the coating layer 20. Specifically, the intermediate layer 21 contacts the upper surface of the substrate 10 at one surface (here, the lower surface), and contacts the lower surface of the coating layer 20 (e.g., the Ta-containing stacked structure 22) at the other surface (here, the upper surface).

[0062] The intermediate layer 21 has a higher bonding property with the substrate 10 than the coating layer 20. Examples of metal elements having such properties include Zr, Hf, V, Nb, Ta, Cr, Mo, W, Al, Si, Y, and Ti. The intermediate layer 21 contains at least one of the above metal elements. For example, the intermediate layer 21 may also contain Ti. Si is a semi-metal element, but in this specification, it is assumed that the semi-metal element is also included in the metal element.

[0063] When the intermediate layer 21 contains Ti, the content of Ti in the intermediate layer 21 may be 1.5 atomic % or more. For example, the content of Ti in the intermediate layer 21 may be 2.0 atomic % or more.

[0064] The intermediate layer 21 may also contain components other than the above-mentioned metal elements (Zr, Hf, V, Nb, Ta, Cr, Mo, W, Al, Si, Y and Ti). However, from the viewpoint of bonding with the substrate 10, the intermediate layer 21 may also contain at least 95 atomic % or more of the above-mentioned metal elements in total. The intermediate layer 21 may also contain 98 atomic % or more of the above-mentioned metal elements in total. The proportion of the metal components in the intermediate layer 21 can be determined by analysis using, for example, an EDS (energy dispersive X-ray spectrometer) attached to a STEM (scanning transmission electron microscope).

[0065] In this way, the bonding between the substrate 10 and the coating layer 20 can be improved by arranging the intermediate layer 21 having higher wettability with the substrate 10 than the coating layer 20. The bonding between the intermediate layer 21 and the coating layer 20 is also high, so it is difficult to produce a situation where the coating layer 20 peels off from the intermediate layer 21.

[0066] The thickness of the intermediate layer 21 may be, for example, not less than 0.1 nm and less than 20 nm.

[0067] (Ta-containing stacked structure 22)

[0068] like Figure 5 As shown, each of the plurality of Ta-containing stacked structures 22 includes a first compound layer 22a and a second compound layer 22b. The first compound layer 22a contains Ta in a first composition ratio. The second compound layer 22b contains Ta in a second composition ratio different from the first composition ratio. It should be noted that one of the first composition ratio and the second composition ratio may be 0.

[0069] In this way, the plurality of Ta-containing stacked structures 22 each include a first compound layer 22a containing Ta in a first composition ratio and a second compound layer 22b containing Ta in a second composition ratio different from the first composition ratio, thereby improving the thermal shock resistance, oxidation resistance and hardness at high temperatures of the coating layer 20. As a result, the life of the coated tool 1 can be extended.

[0070] The first compound layer 22a and the second compound layer 22b may each contain Al, Ti, and Ta. In this case, the Al content Al(1) contained in the first compound layer 22a, the Ti content Ti(1) contained in the first compound layer 22a, the Ta content Ta(1) contained in the first compound layer 22a, the Al content Al(2) contained in the second compound layer 22b, the Ti content Ti(2) contained in the second compound layer 22b, and the Ta content Ta(2) contained in the second compound layer 22b may have a relationship of Al(1)<Al(2), Ti(1)<Ti(2), and Ta(1)>Ta(2). Ta(2) may be 0.

[0071] When Al(1), Ti(1), Ta(1), Al(2), Ti(2), and Ta(2) have the relationship of Al(1)<Al(2), Ti(1)<Ti(2), and Ta(1)>Ta(2), the residual stress between the first compound layer 22a and the second compound layer 22b can be reduced, and the hardness and bonding of the first compound layer 22a and the second compound layer 22b can be maintained. As a result, the peeling or cracking between the first compound layer 22a and the second compound layer 22b can be reduced and the strength of the coating layer 20 can be improved. As a result, the life of the coated tool 1 can be extended.

[0072] The first compound layer 22a and the second compound layer 22b may each include a compound having the formula

[0073] (Al a Ti b Ta c )N (1)

[0074] (In the formula, a, b and c satisfy the relationship of 0.35≤a≤0.65, 0.3≤b≤0.5, 0.02≤c≤0.2 and a+b+c=1)

[0075] Represents Ta-containing compounds.

[0076] When a satisfies the relationship of 0.35≤a≤0.65, the hardness and wear resistance of the coating layer 20 can be maintained. When b and c satisfy the relationship of 0.3≤b≤0.5 and 0.02≤c≤0.2, the oxidation resistance of the coating layer 20 can be maintained and the strength of the coating layer 20 at high temperature can be improved. As a result, the life of the coated tool 1 can be extended.

[0077] like Figure 6 As shown in FIG. 1 , c for the Ta-containing compound included in the first compound layer 22a may also change continuously in the thickness direction of the first compound layer 22a. c for the Ta-containing compound included in the second compound layer 22b may also change continuously in the thickness direction of the second compound layer 22b. For example, Figure 6 As shown in FIG. 1 , c for the Ta-containing compound included in the first compound layer 22a may be maximized near the center of the distance in the thickness direction of the first compound layer 22a. c for the Ta-containing compound included in the second compound layer 22b may be minimized near the center of the distance in the thickness direction of the second compound layer 22b.

[0078] In this case, the residual stress between the first compound layer 22a and the second compound layer 22b can be further reduced. Thus, the peeling or cracking between the first compound layer 22a and the second compound layer 22b can be reduced. As a result, the life of the coated tool 1 can be extended.

[0079] (Mo-containing stacked structure 23)

[0080] like Figure 5 As shown, each of the plurality of Mo-containing stacked structures 23 includes a third compound layer 23a and a fourth compound layer 23b. The third compound layer 23a contains Mo at a third composition ratio. The fourth compound layer 23b contains Mo at a fourth composition ratio different from the third composition ratio. One of the third composition ratio and the fourth composition ratio may be 0.

[0081] In this way, each of the plurality of Mo-containing stacked structures 23 includes a third compound layer 23a containing Mo at a third composition ratio and a fourth compound layer 23b containing Mo at a fourth composition ratio different from the third composition ratio, thereby improving the toughness and strength of the coating layer 20. In addition, the lubricity of the coating layer 20 can be maintained even at high temperatures. As a result, the life of the coated tool 1 can be extended.

[0082] The third compound layer 23a and the fourth compound layer 23b may each contain Al, Cr, and Mo. In this case, the content of Al contained in the third compound layer 23a, the content of Cr contained in the third compound layer 23a, the content of Mo contained in the third compound layer 23a, the content of Al contained in the fourth compound layer 23b, the content of Cr contained in the fourth compound layer 23b, and the content of Mo contained in the fourth compound layer 23b, Mo(4), may have a relationship of Al(3) < Al(4), Cr(3) > Cr(4), and Mo(3) > Mo(4). Mo(4) may be 0.

[0083] When Al(3), Cr(3), Mo(3), Al(4), Cr(4) and Mo(4) have the relationship of Al(3)<Al(4), Cr(3)>Cr(4) and Mo(3)>Mo(4), the residual stress between the third compound layer 23a and the fourth compound layer 23b can be reduced. As a result, the peeling or cracking between the third compound layer 23a and the fourth compound layer 23b can be reduced. In addition, the lubricity of the coating layer 20 can be maintained at high temperatures, and the heat shock resistance, strength, oxidation resistance and hardness at high temperatures of the coating layer 20 can be further improved. As a result, the life of the coated tool 1 can be extended.

[0084] The third compound layer 23a and the fourth compound layer 23b may each include a compound having the formula

[0085] (Al d Cr e Si f Mo g )N (2)

[0086] (In the formula, d, e, f and g satisfy the relationship of 0.35≤d≤0.65, 0.2≤e≤0.45, 0.03≤f≤0.15, 0.02≤g≤0.2 and d+e+f+g=1)

[0087] Represents Mo-containing compounds.

[0088] When d satisfies the relationship of 0.35≤d≤0.65, the hardness and wear resistance of the coating layer 20 can be maintained. When e, f and g satisfy the relationships of 0.2≤e≤0.45, 0.03≤f≤0.15 and 0.02≤g≤0.2, the lubricity of the coating layer 20 at high temperature can be maintained and the thermal shock resistance, strength and oxidation resistance of the coating layer 20 can be improved. As a result, the life of the coated tool 1 can be extended.

[0089] like Figure 7 As shown in FIG. 1 , g for the Mo-containing compound included in the third compound layer 23a may also change continuously in the thickness direction of the third compound layer 23a. g for the Mo-containing compound included in the fourth compound layer 23b may also change continuously in the thickness direction of the fourth compound layer 23b. For example, Figure 7 As shown in FIG. 2 , g for the Mo-containing compound included in the third compound layer 23a may be maximum near the center of the distance in the thickness direction of the third compound layer 23a. g for the Mo-containing compound included in the fourth compound layer 23b may be minimum near the center of the distance in the thickness direction of the fourth compound layer 23b.

[0090] In this case, the residual stress between the third compound layer 23a and the fourth compound layer 23b can be further reduced. Thus, the peeling or cracking between the third compound layer 23a and the fourth compound layer 23b can be reduced. As a result, the life of the coated tool 1 can be extended.

[0091] The average value of the thicknesses of the first compound layer 22 a , the second compound layer 22 b , the third compound layer 23 a , and the fourth compound layer 23 b may be greater than or equal to 3 nm and less than or equal to 15 nm.

[0092] In this case, the Ta-containing stacked structure 22 including the first compound layer 22a and the second compound layer 22b is a stacked structure having a plurality of layers with a thickness of the nanometer level. The Mo-containing stacked structure 23 including the third compound layer 23a and the fourth compound layer 23b is a stacked structure having a plurality of layers with a thickness of the nanometer level. Thus, the strength of the coating layer 20 with respect to external forces can be improved. In addition, the oxidation resistance and hardness at high temperatures of the coating layer 20 can be improved. As a result, the life of the coated tool 1 can be extended.

[0093] <Method for manufacturing coated tool>

[0094] Next, refer to Figure 8 An example of a method of manufacturing the coated tool 1 according to the embodiment will be described. Figure 81 is a diagram schematically showing an example of a film forming apparatus for forming a coating layer on a substrate. It should be noted that the method for manufacturing the coated tool 1 is not limited to the method shown below.

[0095] First, a substrate 10 having the shape of the coated tool 1 is prepared by a conventionally known method. Next, a coating layer 20 is formed on the surface of the substrate 10. As a film forming method of the coating layer 20, a physical vapor deposition (PVD) method such as an ion plating method or a sputtering method can be used. As an example, when the coating layer 20 is prepared by the ion plating method, for example, Figure 8 An arc ion plating film forming apparatus (hereinafter referred to as an AIP apparatus) 1000 as shown.

[0096] Figure 8 The AIP device 1000 shown introduces a gas such as N2 or Ar into a vacuum chamber 101 from a gas inlet 102, and applies a high voltage between a cathode electrode 103 and an anode electrode 104 disposed in the AIP device 1000, thereby generating a gas plasma. Under the action of such plasma, a desired metal or ceramic is evaporated and ionized from a target material 105, thereby generating metal or ceramic ions in a high energy state. The ionized metal or ceramic is attached to the surface of a substrate 10 as a sample, and a coating layer 20 is covered on the surface of the substrate 10.

[0097] like Figure 8 As shown in FIG. 1 , a plurality of substrates 10 may be placed on a tower 107 and placed on a sample support table 106. A plurality of sets (two sets in the figure) of sample support tables 106 may also be placed on a workbench not shown. Figure 8 As shown, a heater 108 for heating the substrate 10 , a gas exhaust port 109 for exhausting gas to the outside of the system, and a bias power supply 110 for applying a bias voltage to the substrate 10 are provided.

[0098] As the target material 105, for example, a metal target material that independently contains metal tantalum (Ta), metal molybdenum (Mo) and one or more metals selected from the fifth group elements or the sixth group elements of the periodic table, Si, Y and Ce, an alloy target material that is a composite of the above metals, or a mixed target material composed of powder or sintered body of carbide, nitride or boride of the above metals can be used.

[0099] While using the target material 105 to evaporate the metal source through arc discharge or glow discharge to ionize the metal of the metal source, it is reacted with nitrogen (N2) gas of the nitrogen source, methane (CH4) / acetylene (C2H2) gas of the carbon source or oxygen (O2) gas to deposit a coating layer 20 on the surface of the substrate 10.

[0100] At this time, the sample support table 106 is controlled so that the distance from the position of the target 105 to the position of the substrate 10 is 160 mm or more, preferably 260 mm or more. A plurality of highly straight magnetic lines of force are generated from the center of the surface of the target 105 toward the substrate 10, so that the magnetic flux density near the substrate 10 becomes 0.2 to 0.8 mT (milli-Tesla).

[0101] Sometimes nitrogen is introduced into the AIP apparatus 1000 as a reaction gas, and the atmosphere pressure is set to 2 to 10 Pa. The temperature of the substrate 10 is maintained at 300 to 500° C. A bias voltage of -50 to -200 V is applied to the substrate 10, and an arc discharge of 80 to 200 A is generated between the target 105 (cathode electrode 103) and the anode electrode 104. The metal is vapor-deposited on the substrate 10 while the substrate 10 is rotated and revolved.

[0102] As a method for controlling the magnetic flux density near the substrate 10, the magnetic field can be controlled by, for example, setting an electromagnetic coil or a permanent magnet as a magnetic field generating source around the target material 105, configuring a permanent magnet inside the AIP device 1000, such as in the center, or adjusting the position of adjacent targets 105.

[0103] The magnetic force is calculated by measuring the magnetic flux density at the position of the substrate 10 using a magnetic flux density meter. The magnetic flux density is expressed in mT (milli-Tesla). Here, the distance from the position of the target 105 to the position of the substrate 10 represents the distance measured at the position of the substrate 10 closest to the target 105 and the distance at which the substrate 10 is farthest from the target 105.

[0104] During film formation, Figure 8 When the period in which each position of the substrate 10 as shown becomes the direction in which the substrate 10 is closest to the target 105 is set as the rotation speed of the sample, the period of the difference in the composition of the heavy metal and the light metal in the direction of the thickness of the coating layer 20 can be adjusted by adjusting the rotation speed. Specifically, the rotation speed of the substrate 10 and the sample support table 106 is sometimes adjusted in a manner to become a period of 2 to 20 rpm (revolutions per minute).

[0105] During film formation, the sample support tables 106 on which the substrate 10 is placed may each rotate while the tower 107 rotates, and the table may be rotated in such a manner that the plurality of sample support tables 106 revolve. By adjusting the timing of such revolutions, the thickness of each compound layer constituting the Ta-containing stacked structure 22 and the Mo-containing stacked structure 23 can be controlled.

[0106] By applying a pulsed bias voltage, it is possible to adjust the time or distance for metal ions to fly from the target 105 to the substrate 10. This makes it possible to create a difference in the composition of the heavy metal component and the light metal component during film formation.

[0107] For example, when the substrate 10 is arranged so that the substrate 10 is close to the target 105 and faces the target 105, the heavy metal component from the target 105 flies straight toward the substrate 10, and the heavy metal is deposited on the substrate 10 more than the light metal. On the other hand, when the substrate 10 is arranged so that the substrate 10 is far away from the target 105 and faces the target 105, it is believed that the light metal component is detoured and deposited on the substrate 10, so the amount of heavy metal component deposited is reduced. At this time, it is believed that by maintaining the distance from the position of the target 105 to the position of the substrate 10 long and maintaining a certain degree of magnetic flux density near the substrate 10, the detour of the light metal component is promoted, and the composition difference between the heavy metal component and the light metal component is increased.

[0108] <Cutting tools>

[0109] Next, refer to Fig. 9 The structure of a cutting tool including the above-mentioned coated tool 1 will be described. Fig. 9 This is a front view showing an example of a cutting tool according to an embodiment.

[0110] like Fig. 9 As shown, the cutting tool 100 according to the embodiment includes a coated tool 1 and a tool holder 70 for fixing the coated tool 1 .

[0111] The handle 70 is from the first end ( Fig. 9 ) toward the second end ( Fig. 9 The handle 70 is a rod-shaped member extending from the lower end of the handle. The handle 70 is made of, for example, steel or cast iron. In particular, steel with higher toughness among these materials is sometimes used.

[0112] The tool holder 70 has a tool groove 73 at the end of the first end side. The tool groove 73 is a portion for assembling the coated tool 1, and has a seating surface intersecting the rotation direction of the cutter and a restraining side surface inclined relative to the seating surface. A threaded hole is provided on the seating surface for screwing a screw 75 described later.

[0113] The coated tool 1 is located in the knife groove 73 of the tool holder 70 and is assembled to the tool holder 70 by means of a screw 75. That is, the screw 75 is inserted into the through hole 5 of the coated tool 1, and the front end of the screw 75 is inserted into the threaded hole formed on the seating surface of the knife groove 73 so that the screw parts are screwed together. Thus, the coated tool 1 is assembled to the tool holder 70 in a manner that the cutting edge part 3 protrudes outward from the tool holder 70.

[0114] In the embodiment, a cutting tool used in so-called turning processing is illustrated. As turning processing, for example, inner diameter processing, outer diameter processing and slotting processing can be cited. As a cutting tool, it is not limited to a cutting tool used in turning processing. For example, the coated tool 1 can also be used for a cutting tool used in milling processing. As a cutting tool used in milling processing, for example, milling cutters such as flat milling cutters, front milling cutters, side milling cutters and slotting milling cutters, and end mills such as single-edge end mills, multi-edge end mills, tapered edge end mills and ball-end end mills can be cited.

[0115] Example

[0116] Below, refer to Figure 10 to Figure 13 The present invention will be described in detail with reference to the following examples.

[0117] Fig.10 This is a table showing the production conditions of the coating layer formed on the substrate. Fig.11 : is a table showing the structure of the coating layer formed on the substrate.

[0118] exist Figure 8 In the AIP device shown in FIG. Fig.10 The manufacturing conditions shown in the figure were used to form a coating layer on a substrate composed of WC-based cemented carbide, thereby producing coated cutting tools of samples No. 1 to No. 4. Fig.10 Under the conditions of arc current (mA), target composition, distance between target and substrate (mm), magnetic flux density near substrate (mT), and rotation speed of sample support table (rpm), a coating layer is formed on the surface of substrate. The distance between target and substrate (mm) varies with the rotation of sample support table. Fig.10 Correspondingly, the magnetic flux density (mT) near the substrate also varies within the range of values ​​shown. Fig.10 The values ​​vary within the range shown.

[0119] Regarding the coated tools of samples No. 1 and No. 2, a plurality of Ta-containing stacked structures and a plurality of Mo-containing stacked structures are formed on the surface of the substrate. Here, a plurality of Ta-containing stacked structures and a plurality of Mo-containing stacked structures are stacked alternately. Regarding the coated tool of sample No. 3, only a plurality of Mo-containing stacked structures are formed on the surface of the substrate. Regarding the coated tool of sample No. 4, only a plurality of Ta-containing stacked structures are formed on the surface of the substrate.

[0120] Here, on the surface of the substrate, Fig.10The stacking times (times) shown in FIG. 1 and FIG. 2 form a group of Ta-containing stacked structures and Mo-containing stacked structures, only Ta-containing stacked structures, and only Mo-containing stacked structures. That is, the number of Ta-containing stacked structures and the number of Mo-containing stacked structures are respectively the same as Fig.10 The number of stacking times is the same as shown. Fig.10 During the stacking time (minutes) shown, a Ta-containing stacked structure and a Mo-containing stacked structure are each formed on the surface of the substrate.

[0121] like Fig.11 As shown, for the coated tools of samples No. 1 and No. 2, the Ta-containing stacked structure is composed of the first compound layer and the second compound layer, and the Mo-containing stacked structure is composed of the third compound layer and the fourth compound layer. For the coated tool of sample No. 3, the Mo-containing stacked structure is composed of the third compound layer and the fourth compound layer. For the coated tool of sample No. 4, the Ta-containing stacked structure is composed of the first compound layer and the second compound layer.

[0122] The first compound layer and the second compound layer each include (Al a Ti b Ta c )N-represented Ta-containing compound. Here, a, b and c are Fig.11 The values ​​shown. Fig.11 The values ​​of a, b, and c shown are average values ​​for the Ta-containing compounds contained in the plurality of first compound layers or the plurality of second compound layers contained in the Ta-containing stacked structure. The average composition of the Ta-containing stacked structure composed of the first compound layer and the second compound layer is Fig.10 The compositions of the targets used to produce the Ta-containing stacked structures shown are consistent.

[0123] like Fig.11 As shown, for the coated tools of samples No. 1 and No. 2, a of the first compound layer, b of the first compound layer, c of the first compound layer, a of the second compound layer, b of the second compound layer, and c of the second compound layer have the relationship that a of the first compound layer is less than a of the second compound layer, b of the first compound layer is less than b of the second compound layer, and c of the first compound layer is greater than c of the second compound layer.

[0124] The third compound layer and the fourth compound layer each include (Al d Cr e Si f Mo g ) is a Mo-containing compound represented by Fig.11 The values ​​shown. Fig.11The values of d, e, f, and g shown are the average values for the Mo-containing compounds contained in the multiple third compound layers or the multiple fourth compound layers included in the Mo-containing laminate. The average composition of the Mo-containing laminate composed of the third compound layer and the fourth compound is consistent with Fig.10 the composition of the target used to manufacture the Mo-containing laminate shown.

[0125] As Fig.11 shown, the d of the third compound layer, the e of the third compound layer, the g of the third compound layer, the d of the fourth compound layer, the e of the fourth compound layer, and the g of the fourth compound layer have the relationships of d of the third compound layer < d of the fourth compound layer, e of the third compound layer > e of the fourth compound layer, and g of the third compound layer > g of the fourth compound layer.

[0126] Regarding the coated cutting tools of Sample No. 1 and No. 2, the thicknesses of the Ta-containing laminate and the Mo-containing laminate are Fig.11 the value of 400 nm as the thickness (nm) of each laminate shown. Regarding the coated cutting tool of Sample No. 3, the thickness of the Mo-containing laminate is Fig.11 4000 nm as shown. Regarding the coated cutting tool of Sample No. 4, the thickness of the Ta-containing laminate is Fig.11 4000 nm as shown.

[0127] Regarding the coated cutting tools of Sample No. 1 and No. 2, the average thicknesses of the first compound layer, the second compound layer, the third compound layer, and the fourth compound layer are Fig.11 the value of 8 nm as the average thickness (nm) of the compound layer shown. Regarding the coated cutting tool of Sample No. 3, the average thicknesses of the third compound layer and the fourth compound layer are Fig.11 8 nm as shown. Regarding the coated cutting tool of Sample No. 4, the average thicknesses of the first compound layer and the second compound layer are Fig.11 8 nm as shown.

[0128] <X-ray diffraction spectrum>

[0129] The coated cutting tools of Sample No. 1 to No. 4 were heat-treated by maintaining the coating layer at 1200 °C for 0.5 hours in a nitrogen atmosphere. After that, using an X-ray diffractometer "MiniFlex600" (manufactured by Rigaku Corporation), the X-ray diffraction spectrum of the heat-treated coating layer was measured. The optical system of the above X-ray diffractometer is a focusing method optical system. The X-ray tube of the above X-ray diffractometer is Cu, and its output is 40 kV / 15 mA.

[0130] The measurement conditions of the X-ray diffraction spectrum are as follows.

[0131] Measurement method: 2θ scanning

[0132] Measuring range: 30 degrees to 46 degrees

[0133] Step: 0.01 degree

[0134] Scanning speed: 2 degrees / minute

[0135] Fig. 12A This is a diagram showing an X-ray diffraction spectrum measured for the coating layer of the coated tool of Sample No. 1 after heat treatment. Fig. 12B This is a diagram showing an X-ray diffraction spectrum measured for the coating layer of the coated tool of Sample No. 2 after heat treatment. Fig. 12C This is a diagram showing an X-ray diffraction spectrum measured for the coating layer of the coated tool of Sample No. 3 after heat treatment. Fig.12D This is a diagram showing an X-ray diffraction spectrum measured for the coating layer of the coated tool of Sample No. 4 after heat treatment.

[0136] exist Fig. 12A , Fig. 12B , Fig. 12C as well as Fig.12D In the graph, the horizontal axis represents the diffraction angle 20 (degrees) of the X-ray, and the vertical axis represents the intensity of the X-ray (arbitrary unit). θ is the Bragg angle of the X-ray (degrees).

[0137] exist Fig. 12A , Fig. 12B , Fig. 12C as well as Fig.12D The diffraction peak in the range of 33 to 34 degrees corresponds to the (100) plane of the hexagonal crystal of the metal nitride contained in the coating layer after heat treatment. The diffraction peak in the range of 36.3 to 36.5 degrees corresponds to the (002) plane of the hexagonal crystal.

[0138] about Fig. 12A , Fig. 12B , Fig. 12C as well as Fig.12D The X-ray diffraction spectrum shown in FIG. 1 shows the intensity of the diffraction peak corresponding to the (100) plane of the hexagonal crystal and the intensity of the diffraction peak corresponding to the (002) plane of the hexagonal crystal. The ratio Ih(100) / Ih(002) was calculated from the obtained Ih(100) and the obtained Ih(002).

[0139] <Cutting test>

[0140] Cutting tests were conducted on coated cutting tools of samples No. 1 to No. 4. The test conditions of the cutting tests were as follows: A hard material type for milling (model: PNMU1205ANER-GM) was used as a substrate, and the cutting tests were conducted under the following conditions.

[0141] (1) Cutting method: Milling of square materials with a size of 80 mm × 125 mm × 300 mm

[0142] (2) Cutting workpiece: FCD450

[0143] (3) Cutting speed Vc: 150 m / min and 200 m / min

[0144] (4) Feed rate of each blade fz: 0.12mm / t

[0145] (5) Axial penetration depth ap: 2 mm

[0146] (6) Processing method: dry and wet

[0147] (7) Evaluation method: Under the above conditions, a 80 mm × 300 mm surface of a workpiece was milled, and the time point when the Vb wear width of the tool flank reached 0.1 mm was determined as the life of the coated tool.

[0148] Fig.13 This is a table showing the results of X-ray diffraction spectrum measurement and cutting test on coated cutting tools of Samples No. 1 to No. 4.

[0149] like Fig.13 As shown, for the coated tool of sample No. 1, Ih(100) / Ih(002) is 0.29. For the coated tool of sample No. 2, Ih(100) / Ih(002) is 0.9. For the coated tool of sample No. 3, Ih(100) / Ih(002) is 1.57. For the coated tool of sample No. 4, Ih(100) / Ih(002) is 1.75.

[0150] Regarding the coated tools of samples No. 1 and No. 2, the X-ray diffraction spectra measured for the coating layer after heat treatment satisfy the relationship of Ih (100) / Ih (002) ≤ 0.9. On the other hand, regarding the coated tools of samples No. 3 and No. 4, the X-ray diffraction spectra measured for the coating layer after heat treatment do not satisfy the relationship of Ih (100) / Ih (002) ≤ 0.9. The coated tools of samples No. 1 and No. 2 are equivalent to the embodiments of the present invention. The coated tools of samples No. 3 and No. 4 are equivalent to the comparative examples of the present invention.

[0151] In this way, it can be confirmed that by forming a coating layer in the following manner, that is, the coating layer includes a plurality of Ta-containing stacked structures and a plurality of Mo-containing stacked structures, the plurality of Ta-containing stacked structures each include a first compound layer containing Ta in a first composition ratio and a second compound layer containing Ta in a second composition ratio different from the first composition ratio, and the plurality of Mo-containing stacked structures each include a third compound layer containing Mo in a third composition ratio and a fourth compound layer containing Mo in a fourth composition ratio different from the third composition ratio, so that a coating layer can be obtained in which the X-ray diffraction spectrum measured after the coating layer is maintained at a temperature of 1200°C for 0.5 hours in a non-oxidizing atmosphere satisfies the relationship Ih(100) / Ih(002)≤0.9.

[0152] like Fig.13 As shown, the life of the coated tools of samples No. 1 and No. 2 is the same as or longer than the life of the coated tools of samples No. 3 and No. 4 for either dry machining or wet machining, and for either low-speed machining or high-speed machining. Therefore, it can be confirmed that the life of the coated tool can be extended when the X-ray diffraction spectrum measured for the coating layer after being kept at a temperature of 1200° C. for 0.5 hours in a non-oxidizing atmosphere satisfies the relationship of Ih(100) / Ih(002)≤0.9.

[0153] Of the coated tools of samples No. 1 and No. 2, the coated tool of sample No. 1 has an X-ray diffraction spectrum measured for the coating layer after heat treatment that satisfies the relationship of Ih(100) / Ih(002)≤0.3. On the other hand, the coated tool of sample No. 2 has an X-ray diffraction spectrum measured for the coating layer after heat treatment that does not satisfy the relationship of Ih(100) / Ih(002)≤0.3.

[0154] like Fig.13 As shown, the life of the coated tool of sample No. 1 is longer than that of the coated tool of sample No. 2 in both dry machining and wet machining, and in both low-speed machining and high-speed machining. Therefore, it can be confirmed that the life of the coated tool can be further extended when the X-ray diffraction spectrum measured after the coating layer is kept at a temperature of 1200° C. for 0.5 hours in a non-oxidizing atmosphere satisfies the relationship of Ih(100) / Ih(002)≤0.3.

[0155] As described above, the coated tool of the embodiment (as an example, the coated tool 1) comprises a substrate (as an example, the substrate 10) and a coating layer (as an example, the coating layer 20) located on the substrate and composed of cubic crystals. The X-ray diffraction spectrum measured for the coating layer after being kept at a temperature of 1200° C. for 0.5 hours in a non-oxidizing atmosphere satisfies the relationship of Ih(100) / Ih(002)≤0.9. Ih(100) is the intensity of the diffraction peak corresponding to the (100) plane of the hexagonal crystal formed in the coating layer. Ih(002) is the intensity of the diffraction peak corresponding to the (002) plane of the hexagonal crystal.

[0156] Therefore, according to the coated tool of the embodiment, the life of the tool can be extended.

[0157] Figure 1 The shape of the coated tool 1 shown is only an example and is not limited to the shape of the coated tool based on the present invention. The coated tool based on the present invention may also have, for example: a rod-shaped body having a rotation axis and extending from a first end to a second end; a cutting edge located at the first end of the body; and a groove extending spirally from the cutting edge toward the second end of the body.

[0158] Note (1): A coated tool, wherein the coated tool comprises: a substrate; and a coating layer, which is located on the substrate and is composed of cubic crystals, and an X-ray diffraction spectrum of the coating layer measured after being maintained at a temperature of 1200°C for 0.5 hours in a non-oxidizing atmosphere satisfies the relationship Ih(100) / Ih(002)≤0.9, where Ih(100) is the intensity of a diffraction peak corresponding to a 9 (100) plane of a hexagonal crystal formed in the coating layer, and Ih(002) is the intensity of a diffraction peak corresponding to a (002) plane of the hexagonal crystal.

[0159] Note (2): The coated tool according to Note (1), wherein the X-ray diffraction spectrum satisfies the relationship Ih(100) / Ih(002)≤0.3.

[0160] Note (3): A cutting tool, wherein the cutting tool comprises: a rod-shaped shank having a tool groove at an end thereof; and the coated tool described in Note (1) or (2), which is located in the tool groove.

[0161] Further effects and / or variations can be easily derived by those skilled in the art. Therefore, the broader scheme of the present invention is not limited to the specific detailed and representative embodiments shown and described above. Therefore, various changes can be made without departing from the spirit or scope of the concept of the general invention defined by the attached technical solutions and their equivalents.

[0162] Description of Reference Numerals

[0163] 1 Coated tool

[0164] 2 Blade body

[0165] 3 Cutting edge

[0166] 5Through holes

[0167] 10 Matrix

[0168] 20 coating layers

[0169] 21 Middle Layer

[0170] 22Ta-containing stacked structure

[0171] 22a First compound layer

[0172] 22b Second compound layer

[0173] 23 Mo-containing laminated structure

[0174] 23a The third compound layer

[0175] 23b Fourth compound layer

[0176] 70 handle

[0177] 73 knife slots

[0178] 75 screws

[0179] 100 cutting tools

[0180] 101 Vacuum Chamber

[0181] 102 Gas inlet

[0182] 103 cathode electrode

[0183] 104 Anode electrode

[0184] 105 Target

[0185] 106 Sample support table

[0186] 107 Tower

[0187] 108 Heater

[0188] 109 Gas outlet

[0189] 110 Bias power supply

[0190] 1000AIP device.

Claims

1. A coated tool, wherein: The coated tool has: a substrate; and a coating layer, which is located on the substrate and is composed of cubic crystals, The X-ray diffraction spectrum of the coating layer measured after being kept at a temperature of 1200° C. for 0.5 hour in a non-oxidizing atmosphere satisfies the relationship of Ih(100) / Ih(002)≤0.9, Ih(100) is the intensity of the diffraction peak corresponding to the (100) plane of the hexagonal crystal formed in the coating layer, Ih(002) is the intensity of the diffraction peak corresponding to the (002) plane of the hexagonal crystal.

2. The coated tool according to claim 1, wherein: The X-ray diffraction spectrum satisfies the relationship of Ih(100) / Ih(002)≤0.

3.

3. A cutting tool, wherein: The cutting tool has: A rod-shaped handle having a knife groove at the end; and The coated cutting tool according to claim 1 or 2, which is located in the cutting groove.

Citation Information

Patent Citations

  • Surface coated cutting tool

    CN108349015A

  • Surface coat cutting tool excellent in chipping resistance and wear resistance

    JP2016064470A

  • Coated cutting tool

    JP2019181586A

  • Hard coating, hard-coated tool, and their production methods

    US20190177839A1

  • Surface-coated cutting tool

    US20220001457A1