Active ester resins
By introducing α-methylbenzyl groups into the reactive ester resin, molecular motion is restricted, which solves the problem of insufficient dielectric loss tangent under high temperature conditions and achieves low dielectric loss tangent and excellent insulation performance.
Patent Information
- Application Number
- CN202380029953.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-29
- Filing Date
- 2023-03-23
- Publication Date
- 2024-11-08
AI Technical Summary
Existing reactive ester resins cannot meet the requirements for excellent dielectric loss tangent at high temperatures, resulting in increased transmission loss of electronic components when operating at high temperatures.
An active ester resin containing α-methylbenzyl is used. By introducing α-methylbenzyl into the resin molecule to restrict molecular motion, the dielectric loss tangent under high temperature environment is reduced.
Excellent dielectric loss tangent was achieved in high-temperature environments, reducing transmission losses of electronic components and improving the decontamination resistance of the insulation layer and preventing corona phenomena.
Smart Images

Figure BDA0005057212130000021 
Figure BDA0005057212130000022 
Figure BDA0005057212130000131
Abstract
Description
Technical Field
[0001] The present invention relates to a novel active ester resin and a method for producing the same. In addition, the present invention relates to a resin crosslinking agent, a resin composition, a cured product, a sheet-like laminate, a resin sheet, a printed wiring board, a semiconductor chip package, and a semiconductor device obtained by using the active ester resin. Background Art
[0002] Resin compositions containing crosslinkable resins such as epoxy resins and their crosslinking agents (curing agents) can provide cured products having excellent properties such as insulation, and are therefore widely used as materials for electronic components such as semiconductor chip packages and printed wiring boards.
[0003] On the other hand, in high-speed communications such as the fifth-generation mobile communication system (5G), it is required to reduce the transmission loss when working in a high-frequency environment. In order to reduce this transmission loss, an insulating material with excellent dielectric properties (low dielectric constant, low dielectric loss tangent) is required. As an insulating material that achieves good dielectric properties, for example, a resin composition containing an active ester resin is disclosed in Patent Documents 1 to 4.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent document 1: International Publication No. 2012 / 002119;
[0007] Patent document 2: International Publication No. 2014 / 061450;
[0008] Patent document 3: International Publication No. 2016 / 098488;
[0009] Patent document 4: Japanese Patent Application Publication No. 2012-12534. Summary of the invention
[0010] Problems to be solved by the invention
[0011] The resin compositions containing conventional active ester resins described in Patent Documents 1 to 4 can achieve excellent dielectric loss tangent at room temperature compared to resin compositions containing other crosslinking agents such as phenolic crosslinking agents. However, conventional active ester resins cannot achieve a dielectric loss tangent at a sufficiently satisfactory level in a high temperature environment such as 90°C. Generally, electronic components generate heat and the temperature rises during operation, so from the viewpoint of suppressing transmission loss during operation, it is desired to develop an active ester resin that can achieve a low dielectric loss tangent in a high temperature environment.
[0012] The present invention is proposed in view of the above-mentioned problems, and its purpose is to provide: an active ester resin that can achieve excellent dielectric loss tangent in a high temperature environment and a method for producing the same, a resin crosslinking agent and a resin composition containing the same, and a cured product obtained using the resin composition, a sheet-like laminated material, a resin sheet, a printed wiring board, a semiconductor chip package and a semiconductor device.
[0013] Means for solving problems
[0014] The present inventors have conducted intensive studies to solve the above problems. As a result, the present inventors have found that an active ester resin containing an α-methylbenzyl group can solve the above problems, thereby completing the present invention.
[0015] That is, the present invention includes the following contents.
[0016] [1] An active ester resin containing one or more α-methylbenzyl groups in one molecule.
[0017] [2] The active ester resin described in [1] comprises a partial structure represented by the following formula (I):
[0018] In formula (I),
[0019] Ar B Each independently represents a divalent organic group containing at least one aromatic ring,
[0020] Ar C Each independently represents a divalent organic group containing at least one aromatic ring,
[0021] * indicates a bond.
[0022] [3] The active ester resin described in [1] or [2], which is represented by the following formula (II):
[0023]
[0024] In formula (II),
[0025] Ar A Each independently represents a monovalent organic group containing at least one aromatic ring,
[0026] Ar B Each independently represents a divalent organic group containing at least one aromatic ring,
[0027] Ar C Each independently represents a divalent organic group containing at least one aromatic ring,
[0028] Organic group Ar A 、Organic group ArB and organic group Ar C At least one of the organic groups contains an α-methylbenzyl group,
[0029] n represents a number greater than 0.
[0030] [4] The active ester resin described in [2] or [3], wherein the organic group Ar C It represents a divalent hydrocarbon group containing at least one aromatic ring.
[0031] [5] The active ester resin according to any one of [2] to [4], wherein the organic group Ar C Contains α-methylbenzyl.
[0032] [6] The active ester resin according to any one of [1] to [5], comprising an aromatic ring to which an α-methylbenzyl group is bonded.
[0033] [7] The active ester resin according to [6], wherein an average of 1 to 6 α-methylbenzyl groups are bonded to one aromatic ring to which the α-methylbenzyl group is bonded.
[0034] [8] The active ester resin according to any one of [1] to [7], wherein the content of the α-methylbenzyl group is in the range of 1% by mass to 60% by mass.
[0035] [9] The active ester resin described in any one of [1] to [8], which is a condensation reaction product of (X1) an aromatic polyhydroxy compound comprising (X1-1) a modified aromatic polyhydroxy compound containing an α-methylbenzyl group, (X2) an aromatic carboxylic acid compound or an aromatic acid halide compound, and (X3) an aromatic monohydroxy compound.
[0036]
[10] A method for producing an active ester resin, which is the method for producing an active ester resin according to any one of [1] to [9], comprising the step of reacting the following compounds:
[0037] The present invention comprises (X1) an aromatic polyhydroxy compound containing (X1-1) a modified aromatic polyhydroxy compound having an α-methylbenzyl group, (X2) an aromatic carboxylic acid compound or an aromatic acid halide compound, and (X3) an aromatic monohydroxy compound.
[0038]
[11] A resin crosslinking agent comprising the active ester resin according to any one of [1] to [9].
[0039]
[12] A resin composition comprising the active ester resin according to any one of [1] to [9] and a crosslinkable resin.
[0040]
[13] The resin composition described in
[12] , wherein the crosslinkable resin comprises at least one selected from thermosetting resins and radical polymerizable resins.
[0041]
[14] The resin composition according to
[12] or
[13] , which is used for forming an insulating layer of a printed wiring board.
[0042]
[15] The resin composition according to
[12] or
[13] , which is used for sealing a semiconductor chip.
[0043]
[16] A cured product of the resin composition according to any one of
[12] to
[15] .
[0044]
[17] A sheet-like laminated material comprising the resin composition according to any one of
[12] to
[15] .
[0045]
[18] A resin sheet comprising: a support and a resin composition layer formed on the support,
[0046] The resin composition layer includes the resin composition according to any one of
[12] to
[15] .
[0047]
[19] A printed wiring board comprising an insulating layer comprising a cured product of the resin composition according to any one of
[12] to
[15] .
[0048]
[20] A semiconductor chip package comprising a sealing layer comprising a cured product of the resin composition according to any one of
[12] to
[15] .
[0049] The semiconductor chip package described in
[21]
[20] is a fan-out type package.
[0050]
[22] A semiconductor device comprising the printed wiring board described in
[19] .
[0051]
[23] A semiconductor device comprising the semiconductor chip package described in
[20] or
[21] .
[0052] Effects of the Invention
[0053] According to the present invention, there can be provided: an active ester resin capable of achieving excellent dielectric loss tangent under high temperature environment and a method for producing the same; a resin crosslinking agent and a resin composition containing the same; and a cured product, a sheet-like laminated material, a resin sheet, a printed wiring board, a semiconductor chip package and a semiconductor device obtained by using the resin composition. DETAILED DESCRIPTION
[0054] <Explanation of terms>
[0055] In the present specification, the term "may have a substituent" with respect to a compound or a group refers to both the case where hydrogen atoms of the compound or group are not substituted with a substituent and the case where part or all of the hydrogen atoms of the compound or group are substituted with a substituent.
[0056] In this specification, unless otherwise specified, the term "substituent" refers to a halogen atom, an alkyl, an alkenyl, an alkynyl, an alkapolyenyl, a cycloalkyl, a cycloalkenyl, an alkoxy, a cycloalkyloxy, an aryl, an aryloxy, an arylalkyl, an arylalkoxy, a monovalent heterocyclic group, an alkylidene, an amino, a silyl, an acyl, an acyloxy, a carboxyl, a sulfo, a cyano, a nitro, a hydroxyl, a thiol, and an oxo group. It should be noted that sometimes, groups such as alkyl, alkenyl, alkynyl, alkapolyenyl, cycloalkyl, cycloalkenyl, aryl, arylalkyl, and an alkylidene that only contain carbon and hydrogen are collectively referred to as "hydrocarbon groups". In addition, sometimes, aliphatic hydrocarbon groups having unsaturated bonds such as alkenyl, alkynyl, alkapolyenyl, and cycloalkenyl are collectively referred to as "unsaturated aliphatic hydrocarbon groups".
[0057] The above-mentioned substituent may further have a substituent (hereinafter, sometimes referred to as a "secondary substituent"). As the secondary substituent, the same substituent as the above-mentioned substituent can be used unless otherwise specified.
[0058] In the present specification, unless otherwise specified, examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom.
[0059] In the present specification, unless otherwise specified, the alkyl group may be either linear or branched. The number of carbon atoms in the alkyl group is preferably 1 to 20, more preferably 1 to 14, further preferably 1 to 12, further preferably 1 to 6, and particularly preferably 1 to 3. Examples of the alkyl group include methyl, ethyl, propyl, isopropyl, butyl, sec-butyl, isobutyl, tert-butyl, pentyl, hexyl, heptyl, octyl, nonyl, and decyl.
[0060] In the present specification, unless otherwise specified, the alkenyl group may be either linear or branched. The number of carbon atoms of the alkenyl group is preferably 2 to 20, more preferably 2 to 14, further preferably 2 to 12, further preferably 2 to 6, and particularly preferably 2 or 3. Examples of the alkenyl group include vinyl, allyl, 1-propenyl, butenyl, sec-butenyl, isobutenyl, tert-butenyl, pentenyl, hexenyl, heptenyl, octenyl, nonenyl, and decenyl.
[0061] In the present specification, unless otherwise specified, the alkynyl group may be either linear or branched. The number of carbon atoms in the alkynyl group is preferably 2 to 20, more preferably 2 to 14, further preferably 2 to 12, further preferably 2 to 6, and particularly preferably 2 or 3. Examples of the alkynyl group include ethynyl, propynyl, butynyl, sec-butynyl, isobutynyl, tert-butynyl, pentynyl, hexynyl, heptynyl, octynyl, nonynyl, and decynyl.
[0062] In the present specification, unless otherwise specified, the alkadienyl group may be linear or branched, and the number of double bonds is preferably 2 to 10, more preferably 2 to 6, further preferably 2 to 4, and further preferably 2. The number of carbon atoms in the alkadienyl group is preferably 3 to 20, more preferably 3 to 14, further preferably 3 to 12, and further preferably 3 to 6.
[0063] In the present specification, unless otherwise specified, the number of carbon atoms in a cycloalkyl group is preferably 3 to 20, more preferably 3 to 12, and even more preferably 3 to 6. Examples of the cycloalkyl group include cyclopropyl, cyclobutyl, cyclopentyl, and cyclohexyl.
[0064] In the present specification, unless otherwise specified, the number of carbon atoms in the cycloalkenyl group is preferably 3 to 20, more preferably 3 to 12, and even more preferably 3 to 6. Examples of the cycloalkenyl group include cyclopropenyl, cyclobutenyl, cyclopentenyl, and cyclohexenyl.
[0065] In the present specification, unless otherwise specified, an alkoxy group may be either linear or branched. The number of carbon atoms in the alkoxy group is preferably 1 to 20, more preferably 1 to 12, and further preferably 1 to 6. Examples of the alkoxy group include methoxy, ethoxy, propoxy, isopropoxy, butoxy, sec-butoxy, isobutoxy, tert-butoxy, pentyloxy, hexyloxy, heptyloxy, octyloxy, nonyloxy, and decyloxy.
[0066] In the present specification, unless otherwise specified, the number of carbon atoms in a cycloalkoxy group is preferably 3 to 20, more preferably 3 to 12, and even more preferably 3 to 6. Examples of the cycloalkoxy group include a cyclopropyloxy group, a cyclobutyloxy group, a cyclopentyloxy group, and a cyclohexyloxy group.
[0067] In this specification, unless otherwise specified, an aryl group is a group obtained by removing one hydrogen atom from an aromatic ring of an aromatic hydrocarbon. The number of carbon atoms in the aryl group is preferably 6 to 24, more preferably 6 to 18, further preferably 6 to 14, and further preferably 6 to 10. Examples of the aryl group include phenyl, naphthyl, and anthracenyl.
[0068] In the present specification, unless otherwise specified, the number of carbon atoms in the aryloxy group is preferably 6 to 24, more preferably 6 to 18, further preferably 6 to 14, and further preferably 6 to 10. Examples of the aryloxy group include a phenoxy group, a 1-naphthyloxy group, and a 2-naphthyloxy group.
[0069] In the present specification, unless otherwise specified, the number of carbon atoms in the arylalkyl group is preferably 7 to 25, more preferably 7 to 19, further preferably 7 to 15, and further preferably 7 to 11. Examples of the arylalkyl group include phenyl-C1-C12 Alkyl, naphthyl -C1~C 12 Alkyl and anthracenyl -C1~C 12 alkyl.
[0070] In the present specification, unless otherwise specified, the number of carbon atoms in the arylalkoxy group is preferably 7 to 25, more preferably 7 to 19, further preferably 7 to 15, and further preferably 7 to 11. Examples of the arylalkoxy group include phenyl-C1-C 12 Alkoxy and naphthyl -C1~C 12 Alkoxy.
[0071] In this specification, unless otherwise specified, a monovalent heterocyclic group refers to a group obtained by removing one hydrogen atom from a heterocyclic ring of a heterocyclic compound. The number of carbon atoms in the monovalent heterocyclic group is preferably 3 to 21, more preferably 3 to 15, and even more preferably 3 to 9. The monovalent heterocyclic group also includes a monovalent aromatic heterocyclic group (heteroaryl). Examples of the monovalent heterocyclic group include thienyl, pyrrolyl, furanyl, furyl, pyridyl, pyridazinyl, pyrimidinyl, pyrazinyl, triazinyl, pyrrolidinyl, piperidinyl, quinolyl, and isoquinolyl.
[0072] In the present specification, unless otherwise specified, an alkylidene group refers to a group obtained by removing two hydrogen atoms from the same carbon atom of an alkane. The number of carbon atoms in the alkylidene group is preferably 1 to 20, more preferably 1 to 14, further preferably 1 to 12, further preferably 1 to 6, and particularly preferably 1 to 3. Examples of the alkylidene group include methylidene, ethylidene, propylidene, isopropylidene, butylidene, sec-butylidene, isobutylidene, tert-butylidene, pentylidene, hexylidene, heptylidene, octylidene, nonylidene, and decylidene.
[0073] In this specification, unless otherwise specified, an acyl group refers to a group represented by the formula: -C(=O)-R (wherein R is an alkyl group or an aryl group). The alkyl group represented by R may be either linear or branched. Examples of the aryl group represented by R include phenyl, naphthyl, and anthracenyl. The number of carbon atoms in the acyl group is preferably 2 to 20, more preferably 2 to 13, and further preferably 2 to 7. Examples of the acyl group include acetyl, propionyl, butyryl, isobutyryl, pivaloyl, and benzoyl.
[0074] In this specification, unless otherwise specified, an acyloxy group refers to a group represented by the formula: -OC(=O)-R (wherein R is an alkyl group or an aryl group). The alkyl group represented by R may be either linear or branched. Examples of the aryl group represented by R include phenyl, naphthyl, and anthracenyl. The number of carbon atoms of the acyloxy group is preferably 2 to 20, more preferably 2 to 13, and further preferably 2 to 7. Examples of the acyloxy group include acetoxy, propionyloxy, butyryloxy, isobutyryloxy, pivaloyloxy, and benzoyloxy.
[0075] In this specification, the term "organic group" refers to a group containing at least carbon atoms as backbone atoms, and may be any of linear, branched or cyclic. In this specification, unless otherwise specified, the number of backbone atoms of the organic group is preferably 1 to 3000, more preferably 1 to 1000, further preferably 1 to 100, further preferably 1 to 50, particularly preferably 1 to 30 or 1 to 20. Examples of the organic group include groups consisting of one or more backbone atoms selected from carbon atoms, oxygen atoms, nitrogen atoms and sulfur atoms (including at least carbon atoms).
[0076] In this specification, the term "hydrocarbon group" refers to a group obtained by removing one or more hydrogen atoms from a hydrocarbon compound. Specifically, a monovalent hydrocarbon group refers to a group obtained by removing one hydrogen atom from a hydrocarbon compound, and a divalent hydrocarbon group refers to a group obtained by removing two hydrogen atoms from a hydrocarbon compound. Examples of hydrocarbon groups include: groups containing only carbon atoms and hydrogen atoms among the aliphatic groups and aromatic groups described below. In this specification, aliphatic groups containing only carbon atoms and hydrogen atoms are sometimes referred to as "aliphatic hydrocarbon groups", and aromatic groups containing only carbon atoms and hydrogen atoms are sometimes referred to as "aromatic hydrocarbon groups". Examples of divalent hydrocarbon groups include: alkylene groups, cycloalkylene groups, alkenylene groups, cycloalkenylene groups, alkylene polyenyl groups, and arylene groups.
[0077] In the present specification, the term "aliphatic group" refers to a group obtained by removing one or more hydrogen atoms bonded to an aliphatic carbon of an aliphatic compound. Specifically, a monovalent aliphatic group refers to a group obtained by removing one hydrogen atom bonded to an aliphatic carbon of an aliphatic compound, and a divalent aliphatic group refers to a group obtained by removing two hydrogen atoms bonded to an aliphatic carbon of an aliphatic compound. Examples of the monovalent aliphatic group include: an alkyl group which may have a substituent, a cycloalkyl group which may have a substituent, an alkenyl group which may have a substituent, a cycloalkenyl group which may have a substituent, and an alkadienyl group which may have a substituent (the number of double bonds is preferably 2 to 10, more preferably 2 to 6, further preferably 2 to 4, and further preferably 2). Examples of the divalent aliphatic group include an alkylene group which may have a substituent, a cycloalkylene group which may have a substituent, an alkenylene group which may have a substituent, a cycloalkenylene group which may have a substituent, and an alkylene polyenyl group which may have a substituent (the number of double bonds is preferably 2 to 10, more preferably 2 to 6, further preferably 2 to 4, and further preferably 2). In the present specification, unless otherwise specified, the number of carbon atoms in an aliphatic group is preferably 1 or more, more preferably 2 or more, further preferably 3 or more, 4 or more, 5 or more, or 6 or more, and is preferably 50 or less, more preferably 40 or less, further preferably 30 or less, 20 or less, 18 or less, 16 or less, 14 or less, or 12 or less. The number of carbon atoms does not include the number of carbon atoms of the substituent.
[0078] In this specification, the term "aromatic group" refers to a group after removing one or more hydrogen atoms from the aromatic ring of an aromatic compound. In detail, a monovalent aromatic group refers to a group after removing one hydrogen atom from the aromatic ring of an aromatic compound, and a divalent aromatic group refers to a group after removing two hydrogen atoms from the aromatic ring of an aromatic compound. As a monovalent aromatic group, for example, an aryl group that may have a substituent, a heteroaryl group that may have a substituent, and as a divalent aromatic group, for example, an arylene group that may have a substituent, a heteroarylene group that may have a substituent. In this specification, unless otherwise specified, the number of carbon atoms of the aromatic group is preferably 3 or more, more preferably 4 or more or 5 or more, and more preferably 6 or more, and its upper limit is preferably 24 or less, more preferably 18 or less or 14 or less, and more preferably 10 or less. The number of carbon atoms does not include the number of carbon atoms of the substituent.
[0079] In the present specification, the term "aromatic ring" refers to a ring that follows Huckel's rule and has 4p+2 electrons (p is a natural number) contained in the π electron system on the ring, including a monocyclic aromatic ring and a condensed polycyclic aromatic ring formed by the condensation of two or more monocyclic aromatic rings. The aromatic ring can be an aromatic carbocyclic ring having only carbon atoms as ring atoms, or it can be an aromatic heterocyclic ring having heteroatoms such as oxygen atoms, nitrogen atoms, sulfur atoms, etc. as ring atoms in addition to carbon atoms. In the present specification, unless otherwise specified, the number of carbon atoms in the aromatic ring is preferably 3 or more, more preferably 4 or more or 5 or more, and further preferably 6 or more, and the upper limit is preferably 24 or less, more preferably 18 or less or 14 or less, and further preferably 10 or less. The number of carbon atoms does not include the number of carbon atoms of the substituent. As aromatic rings, for example: benzene ring, furan ring, thiophene ring, pyrrole ring, pyrazole ring, Azole ring, iso Monocyclic aromatic rings such as azole ring, thiazole ring, imidazole ring, pyridine ring, pyridazine ring, pyrimidine ring, pyrazine ring, etc.; naphthalene ring, anthracene ring, phenanthrene ring, benzofuran ring, isobenzofuran ring, indole ring, isoindole ring, benzothiophene ring, benzimidazole ring, indazole ring, benzo Azole ring, benzyl isocyanate The present invention relates to a condensed polycyclic aromatic ring formed by condensing two or more monocyclic aromatic rings such as an oxazole ring, a benzothiazole ring, a quinoline ring, an isoquinoline ring, a quinoxaline ring, an acridine ring, a quinazoline ring, a cinnoline ring, a phthalazine ring, etc. Among them, as the aromatic ring, a benzene ring, a naphthalene ring and an anthracene ring are preferred, and a benzene ring and a naphthalene ring are particularly preferred. It should be noted that in this specification, the carbon atoms constituting the aromatic ring are referred to as "aromatic carbon".
[0080] Hereinafter, the present invention will be described in detail based on preferred embodiments of the present invention. However, the present invention is not limited to the following embodiments and examples, and can be implemented with any modifications within the scope of the claims and their equivalents.
[0081] <Active ester resin>
[0082] The active ester resin involved in one embodiment of the present invention contains one or more α-methylbenzyl groups in one molecule. The number of α-methylbenzyl groups contained in one molecule of the active ester resin is usually 1 or more, and can be 2 or more, 4 or more, 6 or more, etc. In addition, the upper limit of the number of α-methylbenzyl groups contained in one molecule of the active ester resin is preferably 20 or less, more preferably 12 or less, and particularly preferably 8 or less. In the case where the active ester resin combination includes molecules with different numbers of α-methylbenzyl groups in one molecule, it is preferred that the average value of the number of α-methylbenzyl groups contained in one molecule of the active ester resin is within the above range.
[0083] Active ester resins generally have an ester bond directly bonded to an aromatic ring. This ester bond can react with a functional group such as an epoxy group to form a bond, so it is sometimes called an "active ester group". This "active ester group" includes not only ester bonds having a structure of aromatic carbon-C(=O)-O-aromatic carbon, but also ester bonds having a structure of aliphatic carbon-C(=O)-O-aromatic carbon, as long as it can react with a functional group to form a bond.
[0084] By curing the resin composition comprising a cross-linking resin such as an active ester resin and an epoxy resin according to the present embodiment, a cured product having a low dielectric loss tangent under a high temperature environment can be obtained. The present inventors speculate that the mechanism for obtaining such an effect is as follows. However, the technical scope of the present invention is not limited to the following mechanism.
[0085] Due to the action of the α-methylbenzyl group, the molecular motion of the active ester resin is restricted. For example, when the α-methylbenzyl group is bonded to an aromatic ring, the rotation of the aromatic ring is restricted. In particular, due to the action of the methyl group contained in the α-methylbenzyl group, the degree of restriction of molecular motion is large. Moreover, by restricting the molecular motion of the active ester resin in this way, the dielectric loss tangent of the cured product under high temperature environment can be effectively reduced.
[0086] According to the research of the present inventors, it is clear that an active ester resin having a benzyl group instead of an α-methylbenzyl group cannot effectively reduce the dielectric loss tangent under a high temperature environment as described above. As in Patent Documents 1 to 4, the effect of an active ester resin containing a benzyl group has been experimentally verified in the past, but the effect of an active ester resin containing an α-methylbenzyl group has not been experimentally verified in the past. In view of this background, the above-mentioned effect based on an active ester resin containing an α-methylbenzyl group is the first to be discovered by the present inventors, and is industrially beneficial.
[0087] In addition, conventional active ester resins have the following problem: poor decontamination when forming vias on the insulating layer, which easily causes peeling (haloing) between the insulating layer and the inner substrate. In contrast, the cured product of the resin composition comprising the active ester resin and the cross-linking resin according to the present embodiment generally has excellent decontamination. Furthermore, the cured product of the resin composition comprising the active ester resin and the cross-linking resin according to the present embodiment generally suppresses haloing.
[0088] The active ester resin involved in one embodiment of the present invention generally contains one or more, preferably two or more aromatic rings in addition to the benzene ring contained in the α-methylbenzyl group. Moreover, the α-methylbenzyl group is preferably bonded to a part or all of the above aromatic rings. Therefore, the active ester resin preferably contains one or more aromatic rings to which the α-methylbenzyl group is bonded. In this case, the α-methylbenzyl group is preferably directly bonded to the aromatic carbon contained in the above aromatic ring.
[0089] The aromatic ring bonded with an α-methylbenzyl group can be selected from the above range, among which an aromatic carbon ring is preferred. In addition, the aromatic ring bonded with an α-methylbenzyl group may be a monocyclic aromatic ring or a condensed polycyclic aromatic ring. The number of carbon atoms of the aromatic ring bonded with an α-methylbenzyl group is preferably 6 or more, preferably 14 or less, and particularly preferably 10 or less. The number of carbon atoms of the above aromatic ring does not include the number of carbon atoms of the α-methylbenzyl group. Preferred aromatic rings bonded with an α-methylbenzyl group include, for example, a benzene ring, a naphthalene ring, and an anthracene ring. The aromatic ring bonded with an α-methylbenzyl group may be one type or two or more types.
[0090] The aromatic ring bonded with the α-methylbenzyl group may be directly bonded to one or more other aromatic rings via a single bond, or may be indirectly bonded via an organic group. Such an organic group may be, for example, an organic group consisting of one or more (e.g., 1 to 3000, 1 to 1000, 1 to 100, 1 to 50) backbone atoms selected from carbon atoms, oxygen atoms, nitrogen atoms, and sulfur atoms. With regard to such an organic group, as a non-backbone atom, in addition to or in place of a hydrogen atom, a halogen atom may also be present. Such an organic group may include a linear structure, a branched structure, and / or a cyclic structure. The organic group may be an organic group that does not contain an aromatic ring, or an organic group that includes an aromatic ring.
[0091] For example, the active ester resin may contain a polyaryleneoxy structure, and an α-methylbenzyl group may be bonded to a part or all of the arylene groups contained in the polyaryleneoxy structure. However, from the viewpoint of significantly exerting the desired effect of the present invention, it is preferred that the α-methylbenzyl group is not bonded to the arylene groups contained in the polyaryleneoxy structure, and it is more preferred that the active ester resin does not contain a polyaryleneoxy structure.
[0092] It is preferred that the α-methylbenzyl group is bonded to one aromatic ring to which the α-methylbenzyl group is bonded in a specific range of numbers on average. Here, the average value of the number of α-methylbenzyl groups bonded to one aromatic ring to which the α-methylbenzyl group is bonded is sometimes referred to as the "average number of bonds". The above average number of bonds is obtained by dividing the number of α-methylbenzyl groups bonded to the aromatic ring by the number of aromatic rings bonded to the α-methylbenzyl group. Specifically, the range of the above average number of bonds is usually 1 or more, preferably 6 or less, more preferably 4 or less, further preferably 3 or less, and particularly preferably 2 or less.
[0093] It is preferred that an active ester group is bonded to the aromatic ring to which the α-methylbenzyl group is bonded. Therefore, it is preferred that a carbonyloxy group or an oxycarbonyl group is bonded to the aromatic ring to which the α-methylbenzyl group is bonded. Among them, it is particularly preferred that an oxygen atom of an active ester group is bonded to the aromatic ring to which the α-methylbenzyl group is bonded.
[0094] The content of α-methylbenzyl groups in the active ester resin is preferably 1% by mass or more, more preferably 5% by mass or more, particularly preferably 10% by mass or more, and preferably 60% by mass or less, more preferably 50% by mass or less, particularly preferably 45% by mass or less. In the production method described below, those skilled in the art can adjust the content of α-methylbenzyl groups to a desired range by adjusting the types of raw materials and the reaction ratio.
[0095] Preferred active ester resins include active ester resins having a partial structure represented by the following formula (I). Therefore, preferred active ester resins include active ester resins having a partial structure represented by the following formula (I) and containing one or more α-methylbenzyl groups in one molecule.
[0096]
[0097] In formula (I),
[0098] Ar B Each independently represents a divalent organic group containing at least one aromatic ring,
[0099] Ar C Each independently represents a divalent organic group containing at least one aromatic ring,
[0100] * indicates a bond.
[0101] -Organic group Ar B Description-
[0102] In formula (I), the group Ar B Each independently represents a divalent organic group containing at least one aromatic ring. B The aromatic ring contained does not include the benzene ring contained in the α-methylbenzyl group. B The aromatic ring contained may be any of a monocyclic aromatic ring and a condensed polycyclic aromatic ring formed by condensing two or more monocyclic aromatic rings. In addition, the aromatic ring may be any of an aromatic carbocyclic ring and an aromatic heterocyclic ring.
[0103] From the viewpoint of significantly obtaining the desired effect of the present invention, the organic group Ar B The aromatic ring contained is preferably an aromatic carbocyclic ring. The number of carbon atoms in the aromatic carbocyclic ring is preferably 6 to 14, more preferably 6 to 10. Therefore, in a suitable embodiment, the organic group Ar B The contained aromatic ring is an aromatic carbocyclic ring having 6 to 14 carbon atoms.
[0104] Organic group Ar BThe contained aromatic ring may have a substituent. The substituent involved is as described above, and from the viewpoint of significantly obtaining the desired effect of the present invention, it is preferably selected from at least one of a halogen atom, a hydrocarbon group and an alkoxy group, and more preferably selected from at least one of a hydrocarbon group and an alkoxy group. Among them, it is more preferably selected from at least one of a hydrocarbon group having 1 to 10 carbon atoms and an alkoxy group having 1 to 10 carbon atoms, more preferably selected from at least one of an alkyl group having 1 to 6 carbon atoms, an aryl group having 6 to 10 carbon atoms, an arylalkyl group having 7 to 10 carbon atoms, an unsaturated aliphatic hydrocarbon group having 2 to 6 carbon atoms, and an alkoxy group having 1 to 6 carbon atoms, and particularly preferably an aryl group having 6 to 10 carbon atoms. In addition, in the organic group Ar B When the contained aromatic ring has an unsaturated aliphatic hydrocarbon group as a substituent, the unsaturated aliphatic hydrocarbon group is preferably an alkenyl group or an alkynyl group, more preferably an alkenyl group, and further preferably an allyl group.
[0105] Organic group Ar B It may contain α-methylbenzyl. B The hydrogen atom of the organic group Ar B Some or all of the hydrogen atoms in the organic group Ar may be replaced by α-methylbenzyl groups. B In the case of containing an α-methylbenzyl group, the α-methylbenzyl group is preferably B Therefore, the organic group Ar B A part or all of the hydrogen atoms in the contained aromatic ring may be substituted with α-methylbenzyl groups.
[0106] Relative to the organic group Ar B The aromatic ring contained may have only one α-methylbenzyl group bonded thereto or may have two or more α-methylbenzyl groups bonded thereto. B The number of α-methylbenzyl groups bonded to the contained aromatic ring is usually 1 or more, preferably 6 or less, more preferably 4 or less, particularly preferably 3 or less.
[0107] Preferably in the organic group Ar B The aromatic ring to which the α-methylbenzyl group is bonded has an active ester group bonded. B The aromatic ring to which the α-methylbenzyl group is bonded and the organic group Ar in formula (I) B The bonded carbonyl is bonded.
[0108] As organic group Ar B Preferred examples of include an arylene group to which an α-methylbenzyl group may be bonded and which may have a substituent. BThe number of carbon atoms of the arylene group in is preferably 6 to 18, more preferably 6 to 14, and still more preferably 6 to 10. The number of carbon atoms does not include the number of carbon atoms of the α-methylbenzyl group and the substituent. B Preferably, it is a phenylene group to which an α-methylbenzyl group may be bonded and which may have a substituent, or a naphthylene group to which an α-methylbenzyl group may be bonded and which may have a substituent. B In particular, a phenylene group which may be bonded to an α-methylbenzyl group and may have a substituent is preferred.
[0109] -Organic group Ar C Description-
[0110] In formula (I), the group Ar C Each independently represents a divalent organic group containing at least one aromatic ring. C The aromatic ring contained does not include the benzene ring contained in the α-methylbenzyl group. C The aromatic ring contained may be any of a monocyclic aromatic ring and a condensed polycyclic aromatic ring formed by condensing two or more monocyclic aromatic rings. In addition, the aromatic ring may be any of an aromatic carbocyclic ring and an aromatic heterocyclic ring.
[0111] From the viewpoint of significantly obtaining the desired effect of the present invention, the organic group Ar C Preferably, the organic group Ar contains two or more monocyclic aromatic rings or at least one condensed polycyclic aromatic ring as the aromatic ring. The monocyclic aromatic ring and the condensed polycyclic aromatic ring are as described above. Therefore, in a suitable embodiment, the organic group Ar C Each independently represents a divalent organic group containing two or more monocyclic aromatic rings, or a divalent organic group containing at least one condensed polycyclic aromatic ring.
[0112] From the viewpoint of significantly obtaining the desired effect of the present invention, the organic group Ar C The aromatic ring contained is preferably an aromatic carbocyclic ring. The number of carbon atoms in the aromatic carbocyclic ring is preferably 6 to 14, more preferably 6 to 10. Therefore, in a suitable embodiment, the organic group Ar C The contained aromatic ring is an aromatic carbocyclic ring having 6 to 14 carbon atoms.
[0113] Among them, from the viewpoint of significantly obtaining the desired effect of the present invention, the organic group Ar CPreferably, it represents a divalent organic group containing two or more monocyclic aromatic carbocyclic rings, or a divalent organic group containing at least one condensed polycyclic aromatic carbocyclic ring. Here, the number of carbon atoms per monocyclic aromatic carbocyclic ring is preferably 6 (i.e., benzene ring). The number of carbon atoms per condensed polycyclic aromatic carbocyclic ring is preferably 10 to 14 (e.g., naphthalene ring, anthracene ring), and more preferably 10.
[0114] Organic group Ar C The aromatic ring contained may have a substituent. The substituent involved is as described above. From the viewpoint of significantly obtaining the desired effect of the present invention, the organic group Ar C The substituents that the aromatic ring may have are preferably selected from the group consisting of B The substituents that the contained aromatic ring may have are within the same range.
[0115] Organic group Ar C There is no particular limitation as long as it contains at least one of the above aromatic rings. As described above, it is a group containing at least carbon atoms as backbone atoms, and is preferably a divalent group consisting of one or more (preferably 1 to 100, 1 to 50, 1 to 30) backbone atoms selected from carbon atoms, oxygen atoms, nitrogen atoms, and sulfur atoms. Among them, from the viewpoint of significantly obtaining the desired effect of the present invention, the organic group Ar C Particularly suitable are those containing only carbon atoms as backbone atoms.
[0116] Therefore, in a particularly suitable embodiment, the organic group Ar C It means: a divalent group containing two or more monocyclic aromatic carbocyclic rings which may have substituents and only carbon atoms as backbone atoms, or a divalent group containing at least one fused polycyclic aromatic carbocyclic ring which may have substituents and only carbon atoms as backbone atoms, wherein the substituent is one or more selected from an alkyl group having 1 to 6 carbon atoms, an aryl group having 6 to 10 carbon atoms, an arylalkyl group having 7 to 10 carbon atoms, an unsaturated aliphatic hydrocarbon group having 2 to 6 carbon atoms, and an alkoxy group having 1 to 6 carbon atoms. The suitable value and range of the number of carbon atoms per monocyclic aromatic carbocyclic ring and fused polycyclic aromatic carbocyclic ring are as described above. In addition, the suitable range of the number of backbone atoms is as described above, and among them, 10 to 50 or 10 to 30 is preferred.
[0117] From the viewpoint of significantly obtaining the desired effect of the present invention, the organic group Ar in formula (I) C The bonded oxygen atom is preferably connected to the organic group Ar C The aromatic carbon (i.e., the carbon atom constituting the above aromatic ring) is bonded.
[0118] Organic group Ar C It may contain α-methylbenzyl. CThe hydrogen atom of the organic group Ar C Some or all of the hydrogen atoms of the organic group Ar may be substituted with α-methylbenzyl groups. C Contains α-methylbenzyl.
[0119] In the organic group Ar C In the case of containing an α-methylbenzyl group, the α-methylbenzyl group is preferably C Therefore, the organic group Ar C A part or all of the hydrogen atoms of the contained aromatic ring are substituted with α-methylbenzyl groups.
[0120] Relative to the organic group Ar C The aromatic ring contained may have only one α-methylbenzyl group bonded thereto or may have two or more α-methylbenzyl groups bonded thereto. C The number of α-methylbenzyl groups bonded to the contained aromatic ring is usually 1 or more, preferably 6 or less, more preferably 4 or less, particularly preferably 3 or less.
[0121] Preferably in the organic group Ar C The aromatic ring to which the α-methylbenzyl group is bonded has an active ester group bonded. C The aromatic ring to which the α-methylbenzyl group is bonded and the organic group Ar in formula (I) C The bonded oxygen atom is bonded.
[0122] As organic group Ar C Preferred examples include groups represented by the following formula (C-1), formula (C-2) or formula (C-3).
[0123]
[0124] In formulas (C-1), (C-2) and (C-3),
[0125] R c1 and R c4 Each independently represents a single bond, or a divalent linking group selected from a divalent hydrocarbon group having 1 to 10 carbon atoms which may have a substituent, an oxygen atom, a sulfonyl group, a carbonyl group, a carbonate group, and a combination thereof,
[0126] R c2 , R c3 and R c5 Each independently represents a substituent,
[0127] mc1, mc2 and mc3 represent numbers from 0 to 4 independently.
[0128] nc1, nc2 and nc3 each independently represent a number from 0 to 4,
[0129] * indicates a bond.
[0130] Among them, mc1+nc1 is greater than or equal to 0 and less than or equal to 4, mc2+nc2 is greater than or equal to 0 and less than or equal to 4, and mc3+nc3 is greater than or equal to 0 and less than or equal to 4.
[0131] In formula (C-1), two benzene rings are shown in addition to those contained in the α-methylbenzyl group. These two benzene rings correspond to the above description of the organic group Ar C The "aromatic ring" mentioned above. That is, the organic group Ar represented by formula (C-1) C is a divalent organic group containing at least two benzene rings. c2 Suitable organic groups as Ar are C As described above with respect to the substituents that the aromatic ring may have, preferably at least one selected from an alkyl group having 1 to 6 carbon atoms, an aryl group having 6 to 10 carbon atoms, an arylalkyl group having 7 to 10 carbon atoms, an unsaturated aliphatic hydrocarbon group having 2 to 6 carbon atoms, and an alkoxy group having 1 to 6 carbon atoms.
[0132] In formula (C-1), mc1 each independently represents a number of 0 to 4, preferably 1 to 3, and more preferably 1 to 2.
[0133] In formula (C-1), nc1 each independently represents a number of 0 to 4, preferably 0 to 3, more preferably 0 to 2, and even more preferably 0 or 1.
[0134] Here, mc1+nc1 is greater than or equal to 0 and less than or equal to 4.
[0135] In formula (C-1), R c1 R represents a single bond, or a divalent linking group selected from a divalent hydrocarbon group having 1 to 10 carbon atoms which may have a substituent, an oxygen atom, a sulfonyl group, a carbonyl group, a carbonate group, and a combination thereof. c1 The divalent linking group represented has preferably 1 to 30 carbon atoms, more preferably 1 to 20 or 1 to 15 carbon atoms.
[0136] As R c1 The divalent hydrocarbon group in includes: a divalent aliphatic hydrocarbon group, a divalent aromatic hydrocarbon group, for example, an alkylene group, a cycloalkylene group, an alkenylene group, a cycloalkenylene group, an alkylene polyalkenyl group (the number of double bonds is preferably 2 to 10, more preferably 2 to 6, further preferably 2 to 4, further preferably 2), an arylene group, etc., preferably an alkylene group, a cycloalkylene group, an alkenylene group, a cycloalkenylene group, an arylene group, and more preferably an alkylene group, a cycloalkylene group, and an arylene group.
[0137] R c1The alkylene group in the group may be straight chain or branched, and the number of carbon atoms is more preferably 1 to 6, and further preferably 1 to 4 or 1 to 3. The number of carbon atoms does not include the number of carbon atoms of the substituent. Examples of the alkylene group include methylene, ethylene, propylene, butylene, pentylene, and hexylene.
[0138] R c1 The number of carbon atoms of the cycloalkylene group is more preferably 3 to 10, 4 to 10, or 6 to 10. The number of carbon atoms does not include the number of carbon atoms of the substituent. Examples of the cycloalkylene group include cyclopropylene, cyclobutylene, cyclopentylene, cyclohexylene, decahydronaphthylene, norbornylene, dicyclopentylene, and adamantylene.
[0139] R c1 The alkenylene group in the formula (a) may be straight-chain or branched, and the number of carbon atoms is more preferably 2 to 6, and further preferably 2 to 4. The number of carbon atoms does not include the number of carbon atoms of the substituent. Examples of the alkenylene group include ethenylene, propenylene, butenylene, pentenylene, and hexenylene.
[0140] R c1 The number of carbon atoms of the cycloalkenylene group in is more preferably 3 to 10, 4 to 10, or 6 to 10. The number of carbon atoms does not include the number of carbon atoms of the substituent. Examples of the cycloalkenylene group include cyclopropenylene, cyclobutenylene, cyclopentenylene, cyclohexenylene, and norbornenylene.
[0141] R c1 The carbon number of the arylene group in is more preferably 6 to 10. The carbon number of the substituent is not included in the carbon number. Examples of the arylene group include a phenylene group, a naphthylene group, and an indandiyl group.
[0142] From the viewpoint of significantly obtaining the desired effect of the present invention, R c1The divalent linking group represented is preferably a divalent hydrocarbon group having 1 to 10 carbon atoms which may have a substituent, or a divalent group consisting of a combination thereof. Among them, an alkylene group having 1 to 6 carbon atoms which may have a substituent, a cycloalkylene group having 6 to 10 carbon atoms which may have a substituent, an alkenylene group having 2 to 6 carbon atoms which may have a substituent, a cycloalkenylene group having 6 to 10 carbon atoms which may have a substituent, an arylene group having 6 to 10 carbon atoms which may have a substituent, or a divalent group consisting of a combination thereof is more preferred. An alkylene group having 1 to 6 carbon atoms which may have a substituent, a cycloalkylene group having 6 to 10 carbon atoms which may have a substituent, an arylene group having 6 to 10 carbon atoms which may have a substituent, or a divalent group consisting of a combination thereof is further preferred. An alkylene group having 1 to 6 carbon atoms which may have a substituent, an arylene group having 6 to 10 carbon atoms which may have a substituent, or a divalent group consisting of a combination thereof is particularly preferred. Preferred examples of the divalent group composed of a combination of hydrocarbon groups include: C1-C6 alkylene-C6-C 10 Arylene-C1~C6 alkylene, C1~C6 alkylene-C6~C 10 Arylene-C6~C 10 Arylene-C1 to C6 alkylene, etc. In the divalent group composed of a combination of these, the suitable range of the carbon number of the alkylene group and the arylene group, and the optional substituents are as described above.
[0143] R c1 The substituents that the divalent hydrocarbon group in may have are as described above. Among them, the substituent is preferably at least one selected from alkyl groups and aryl groups, and more preferably at least one selected from alkyl groups having 1 to 6 carbon atoms and aryl groups having 6 to 10 carbon atoms.
[0144] From the viewpoint of significantly obtaining the desired effect of the present invention, the organic group Ar represented by the formula (C-1) is particularly suitable. C An example is shown below.
[0145] In a suitable embodiment, in formula (C-1),
[0146] R c1 represents a single bond, an alkylene group having 1 to 6 carbon atoms which may have a substituent, a cycloalkylene group having 6 to 10 carbon atoms which may have a substituent, an arylene group having 6 to 10 carbon atoms which may have a substituent, or a divalent group consisting of a combination thereof,
[0147] R c2 Each independently represents an alkyl group having 1 to 6 carbon atoms, an aryl group having 6 to 10 carbon atoms, an arylalkyl group having 7 to 10 carbon atoms, an unsaturated aliphatic hydrocarbon group having 2 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms,
[0148] mc1 is independently 1 or 2,
[0149] nc1 is independently 0 or 1.
[0150] In a more suitable embodiment, in formula (C-1),
[0151] R c1 represents a single bond, an alkylene group having 1 to 3 carbon atoms which may have a substituent, a cycloalkylene group having 6 to 10 carbon atoms which may have a substituent, a (C1 to C3 alkylene-C6 to C 10 Arylene-C1-C3 alkylene) or (C1-C3 alkylene-C6-C 10 Arylene-C6~C 10 Arylene-C1~C3 alkylene),
[0152] R c2 each independently represents an alkyl group having 1 to 3 carbon atoms, an aryl group having 6 to 10 carbon atoms, an arylalkyl group having 7 to 10 carbon atoms, an allyl group, or an alkoxy group having 1 to 3 carbon atoms,
[0153] mc1 is independently 1 or 2,
[0154] nc1 is independently 0 or 1.
[0155] In a particularly suitable embodiment, in formula (C-1),
[0156] R c1 represents a single bond, an alkylene group having 1 to 3 carbon atoms which may have a substituent, a (C1 to C3 alkylene-C6 to C 10 Arylene-C1-C3 alkylene) or (C1-C3 alkylene-C6-C 10 Arylene-C6~C 10 Arylene-C1~C3 alkylene),
[0157] R c2 each independently represents an alkyl group having 1 to 3 carbon atoms, an aryl group having 6 to 10 carbon atoms, an arylalkyl group having 7 to 10 carbon atoms, an allyl group, or an alkoxy group having 1 to 3 carbon atoms,
[0158] mc1 is independently 1 or 2,
[0159] nc1 is independently 0 or 1.
[0160] In formula (C-2), one naphthalene ring is shown. This naphthalene ring corresponds to the above-mentioned organic group Ar C The "aromatic ring" mentioned above. That is, the organic group Ar represented by formula (C-2) Cis a divalent organic group containing at least one naphthalene ring. c3 Suitable organic groups as Ar are C As described above with respect to the substituents that the aromatic ring may have, preferably at least one selected from an alkyl group having 1 to 6 carbon atoms, an aryl group having 6 to 10 carbon atoms, an arylalkyl group having 7 to 10 carbon atoms, an unsaturated aliphatic hydrocarbon group having 2 to 6 carbon atoms, and an alkoxy group having 1 to 6 carbon atoms.
[0161] In formula (C-2), mc2 each independently represents a number of 0 to 4, preferably 1 to 3, and more preferably 1 to 2.
[0162] In the formula (C-2), nc2 each independently represents a number of 0 to 4, preferably 0 to 3, more preferably 0 to 2, and even more preferably 0 or 1.
[0163] Here, mc2+nc2 is greater than or equal to 0 and less than or equal to 4.
[0164] From the viewpoint of significantly obtaining the desired effect of the present invention, the organic group Ar represented by the formula (C-2) is particularly suitable. C An example is shown below.
[0165] In a suitable embodiment, in formula (C-2),
[0166] R c3 Each independently represents an alkyl group having 1 to 6 carbon atoms, an aryl group having 6 to 10 carbon atoms, an arylalkyl group having 7 to 10 carbon atoms, an unsaturated aliphatic hydrocarbon group having 2 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms,
[0167] mc2 is independently 1 or 2,
[0168] nc2 is independently 0 or 1.
[0169] In a more suitable embodiment, in formula (C-2),
[0170] R c3 each independently represents an alkyl group having 1 to 3 carbon atoms, an aryl group having 6 to 10 carbon atoms, an arylalkyl group having 7 to 10 carbon atoms, an allyl group, or an alkoxy group having 1 to 3 carbon atoms,
[0171] mc2 is independently 1 or 2,
[0172] nc2 is independently 0 or 1.
[0173] In formula (C-3), two naphthalene rings are shown. These two naphthalene rings correspond to the above-mentioned organic group Ar C The "aromatic ring" mentioned above. That is, the organic group Ar represented by formula (C-3)C is a divalent organic group containing at least two naphthalene rings. c5 Suitable organic groups as Ar are C As described above with respect to the substituents that the aromatic ring may have, preferably at least one selected from an alkyl group having 1 to 6 carbon atoms, an aryl group having 6 to 10 carbon atoms, an arylalkyl group having 7 to 10 carbon atoms, an unsaturated aliphatic hydrocarbon group having 2 to 6 carbon atoms, and an alkoxy group having 1 to 6 carbon atoms.
[0174] In formula (C-3), mc3 each independently represents a number of 0 to 4, preferably 1 to 3, and more preferably 1 to 2.
[0175] In the formula (C-3), nc3 each independently represents a number of 0 to 4, preferably 0 to 3, more preferably 0 to 2, and even more preferably 0 or 1.
[0176] Here, mc3+nc3 is greater than or equal to 0 and less than or equal to 4.
[0177] In formula (C-3), R c4 R represents a single bond, or a divalent linking group selected from a divalent hydrocarbon group having 1 to 10 carbon atoms which may have a substituent, an oxygen atom, a sulfonyl group, a carbonyl group, a carbonate group, and a combination thereof. c4 The number of carbon atoms of the divalent linking group represented is preferably 1 to 20, more preferably 1 to 10 or 1 to 6.
[0178] R c4 The divalent hydrocarbon group in R includes suitable examples thereof, c1 The same is true for the divalent hydrocarbon group in R. Among them, an alkylene group having 1 to 6 carbon atoms which may have a substituent or a cycloalkylene group having 6 to 10 carbon atoms which may have a substituent is preferred. Suitable examples of the substituent are also the same as those of R. C1 The same applies to the divalent hydrocarbon groups in .
[0179] From the viewpoint of significantly obtaining the desired effect of the present invention, the organic group Ar represented by the formula (C-3) is particularly suitable. C An example is shown below.
[0180] In a suitable embodiment, in formula (C-3),
[0181] R c4 represents a single bond, an alkylene group having 1 to 6 carbon atoms which may have a substituent, or a cycloalkylene group having 6 to 10 carbon atoms which may have a substituent,
[0182] R c5 Each independently represents an alkyl group having 1 to 6 carbon atoms, an aryl group having 6 to 10 carbon atoms, an arylalkyl group having 7 to 10 carbon atoms, an unsaturated aliphatic hydrocarbon group having 2 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms,
[0183] mc3 is 1 or 2 independently,
[0184] nc3 is independently 0 or 1.
[0185] In a more suitable embodiment, in formula (C-3),
[0186] R c4 represents a single bond or an alkylene group having 1 to 3 carbon atoms which may have a substituent,
[0187] R c5 each independently represents an alkyl group having 1 to 3 carbon atoms, an aryl group having 6 to 10 carbon atoms, an arylalkyl group having 7 to 10 carbon atoms, an allyl group, or an alkoxy group having 1 to 3 carbon atoms,
[0188] mc3 is 1 or 2 independently,
[0189] nc3 is independently 0 or 1.
[0190] Among the above, from the viewpoint of significantly obtaining the desired effect of the present invention, the organic group Ar C It is preferably a divalent hydrocarbon group containing at least one aromatic ring.
[0191] As organic group Ar C Preferred specific examples include: divalent groups represented by the following formulae (c-1) to (c-11). The divalent groups represented by formulae (c-1) to (c-8) are equivalent to the organic groups represented by the above formula (C-1), the divalent groups represented by formula (c-9) are equivalent to the organic groups represented by the above formula (C-2), and the divalent groups represented by formulae (c-10) and (c-11) are equivalent to the organic groups represented by the above formula (C-3).
[0192]
[0193]
[0194] In formulae (c-1) to (c-11), mc represents 0, 1 or 2, and preferably represents 1 or 2. * represents a bond.
[0195] As a more preferable active ester resin, the resin represented by the following formula (II) is mentioned.
[0196]
[0197] In formula (II),
[0198] Ar A Each independently represents a monovalent organic group containing at least one aromatic ring,
[0199] Ar B Each independently represents a divalent organic group containing at least one aromatic ring,
[0200] Ar C Each independently represents a divalent organic group containing at least one aromatic ring,
[0201] Organic group Ar A 、Organic group Ar B and organic group Ar C At least one of the organic groups contains an α-methylbenzyl group,
[0202] n represents a number greater than 0.
[0203] In formula (II), the group Ar B are independently the group Ar in formula (I) B In formula (II), the group Ar C are independently the group Ar in formula (I) C same.
[0204] -Organic group Ar A Description-
[0205] In formula (II), the group Ar A Each independently represents a monovalent organic group containing at least one aromatic ring. A The aromatic ring contained does not include the benzene ring contained in the α-methylbenzyl group. A The aromatic ring contained may be any of a monocyclic aromatic ring and a condensed polycyclic aromatic ring obtained by condensing two or more monocyclic aromatic rings. In addition, the aromatic ring may be any of an aromatic carbocyclic ring and an aromatic heterocyclic ring.
[0206] As an aromatic ring, the organic group Ar A It may contain one or more monocyclic aromatic rings, or may contain at least one condensed polycyclic aromatic ring. The monocyclic aromatic ring and the condensed polycyclic aromatic ring are as described above. Therefore, in one embodiment, the organic group Ar A Each independently represents a monovalent organic group containing one or two or more monocyclic aromatic rings, or a monovalent organic group containing at least one condensed polycyclic aromatic ring.
[0207] From the viewpoint of significantly obtaining the desired effect of the present invention, the organic group Ar A The aromatic ring contained is preferably an aromatic carbocyclic ring. The number of carbon atoms in the aromatic carbocyclic ring is preferably 6 to 14, more preferably 6 to 10. Therefore, in a suitable embodiment, the organic group ArA The contained aromatic ring is an aromatic carbocyclic ring having 6 to 14 carbon atoms.
[0208] Therefore, from the viewpoint of significantly obtaining the desired effect of the present invention, the organic group Ar A represents a monovalent organic group containing a monocyclic aromatic carbocyclic ring or a monovalent organic group containing a condensed polycyclic aromatic carbocyclic ring. Here, the number of carbon atoms per monocyclic aromatic carbocyclic ring is preferably 6 (i.e., benzene ring). The number of carbon atoms per condensed polycyclic aromatic carbocyclic ring is preferably 10 to 14 (e.g., naphthalene ring, anthracene ring), and more preferably 10.
[0209] Organic group Ar A The aromatic ring contained may have a substituent. The substituent involved is as described above. From the viewpoint of significantly obtaining the desired effect of the present invention, the organic group Ar A The substituents that the aromatic ring may have are preferably selected from the group consisting of B The substituents that the contained aromatic ring may have are within the same range.
[0210] Organic group Ar A There is no particular limitation as long as it contains at least one of the above aromatic rings. As described above, it is a group containing at least carbon atoms as backbone atoms, and is preferably a monovalent group consisting of one or more (preferably 1 to 100, 1 to 50, 1 to 30) backbone atoms selected from carbon atoms, oxygen atoms, nitrogen atoms, and sulfur atoms. Among them, from the viewpoint of significantly obtaining the desired effect of the present invention, the organic group Ar A , particularly suitably contain only carbon atoms as backbone atoms.
[0211] Therefore, in a particularly suitable embodiment, the organic group Ar A It represents a monovalent group containing a monocyclic aromatic carbocyclic ring which may have a substituent and only carbon atoms as backbone atoms, or a monovalent group containing a fused polycyclic aromatic carbocyclic ring which may have a substituent and only carbon atoms as backbone atoms, wherein the substituent is one or more selected from an alkyl group having 1 to 6 carbon atoms, an aryl group having 6 to 10 carbon atoms, an arylalkyl group having 7 to 10 carbon atoms, an unsaturated aliphatic hydrocarbon group having 2 to 6 carbon atoms, and an alkoxy group having 1 to 6 carbon atoms. The suitable value and range of the number of carbon atoms per monocyclic aromatic carbocyclic ring and fused polycyclic aromatic carbocyclic ring are as described above. In addition, the suitable range of the number of backbone atoms is as described above, and among them, 10 to 50 or 10 to 30 is preferred.
[0212] From the viewpoint of significantly obtaining the desired effect of the present invention, the organic group Ar in formula (II) A The bonded oxygen atom is preferably connected to the organic group Ar AThe aromatic carbon (i.e., the carbon atom constituting the above aromatic ring) is bonded.
[0213] In formula (II), the organic group Ar A 、Organic group Ar B and organic group Ar C At least one of the organic groups in contains an α-methylbenzyl group. A It may contain α-methylbenzyl. A The hydrogen atom of the organic group Ar A Some or all of the hydrogen atoms in the organic group Ar may be replaced by α-methylbenzyl groups. A In the case of containing an α-methylbenzyl group, the α-methylbenzyl group is preferably A Therefore, the organic group Ar A A part or all of the hydrogen atoms of the contained aromatic ring are substituted with α-methylbenzyl groups.
[0214] Relative to the organic group Ar A The aromatic ring contained may have only one α-methylbenzyl group bonded thereto or may have two or more α-methylbenzyl groups bonded thereto. A The number of α-methylbenzyl groups bonded to the contained aromatic ring is usually 1 or more, preferably 6 or less, more preferably 4 or less, particularly preferably 3 or less.
[0215] Preferably in the organic group Ar A The aromatic ring to which the α-methylbenzyl group is bonded has an active ester group bonded. A The aromatic ring to which the α-methylbenzyl group is bonded and the organic group Ar in formula (II) A The bonded oxygen atom is bonded.
[0216] As organic group Ar A Preferred examples include an aryl group which may be bonded to an α-methylbenzyl group and may have a substituent, among which a phenyl group which may be bonded to an α-methylbenzyl group and may have a substituent, and a naphthyl group which may be bonded to an α-methylbenzyl group and may have a substituent are preferred.
[0217] As organic group Ar A Particularly preferred specific examples include organic groups represented by the following formulae (A-1) to (A-6).
[0218]
[0219] In formulae (A-1) to (A-6), ma each independently represents 1 or 2, and * represents a bond.
[0220] Description of -n-
[0221] In formula (II), n represents a number greater than 0. n generally represents the average value of the number of repetitions in formula (II). The specific range of n is generally greater than 0, preferably greater than 0.2, more preferably greater than 0.3, greater than 0.5 or greater than 0.7, and further preferably greater than 0.8, greater than 0.9, or greater than 1.0. The upper limit of n is preferably less than 10, more preferably less than 8, less than 6, less than 5, less than 4, or less than 3. In a suitable embodiment, n in formula (II) is a number satisfying 0<n≤3. n can be an integer, for example, it can also be 1, 2 or 3.
[0222] The number average molecular weight (Mn) of the active ester resin is preferably 10,000 or less, more preferably 5,000 or less, further preferably 3,000 or less, and particularly preferably 2,000 or less. The lower limit is not particularly limited as long as it is an active ester resin containing an α-methylbenzyl group, and can be, for example, 400 or more, 500 or more, etc. The number average molecular weight of the resin can be measured as a polystyrene conversion value by gel permeation chromatography (GPC).
[0223] The active ester equivalent of the active ester resin is preferably 150 g / eq. or more, more preferably 180 g / eq. or more, particularly preferably 200 g / eq. or more, and preferably 5000 g / eq. or less, more preferably 2000 g / eq. or less, further preferably 1000 g / eq. or less, particularly preferably 500 g / eq. or less. The active ester equivalent represents the mass of a resin containing 1 equivalent of an active ester group.
[0224] <Method for producing active ester resin>
[0225] An example of a method for producing an active ester resin according to an embodiment of the present invention is shown below.
[0226] As a first example of a method for producing an active ester resin according to an embodiment of the present invention, a method for producing an active ester resin comprising the following esterification step can be cited: reacting (X1) an aromatic polyhydroxy compound with (X2) an aromatic carboxylic acid compound or an aromatic acyl halide compound. In the production method according to this example, as required, (X3) an aromatic monohydroxy compound can be further reacted. The reaction of (X1) an aromatic polyhydroxy compound, (X2) an aromatic carboxylic acid compound or an aromatic acyl halide compound, and (X3) an aromatic monohydroxy compound can be carried out in the form of a condensation reaction. In the production method according to the first example, an active ester resin according to an embodiment of the present invention can be produced by using a compound containing an α-methylbenzyl group as any one or more of (X1) an aromatic polyhydroxy compound, (X2) an aromatic carboxylic acid compound or an aromatic acyl halide compound, and (X3) an aromatic monohydroxy compound.
[0227] (X1) Aromatic polyhydroxy compounds refer to compounds containing an aromatic ring and two or more hydroxyl groups. The hydroxyl group is preferably directly bonded to the aromatic ring. Examples of (X1) aromatic polyhydroxy compounds include: bisphenols such as biphenol, bisphenol A, bisphenol F, bisphenol S, bisphenol AF, allylated bisphenol A, fluorene bisphenol, terpene diphenol, tetrabromobisphenol A, 4,4'-biphenol, 2,2'-biphenol, 3,3',5,5'-tetramethyl-1,1'-biphenyl-4,4'-diol, phenol aralkyl type bisphenol, dicyclopentadiene type bisphenol; triphenols such as tris-(4-hydroxyphenyl)methane; tetraphenols such as 1,1,2,2-tetrakis(4-hydroxyphenyl)ethane; hydroquinone, resorcinol, catechol, 1,4-naphthalene diol, 1,6-naphthalene diol, 2,3-naphthalene diol, etc. Phenol polymers such as condensation products or addition products of phenols (alkyl-substituted or unsubstituted phenol, alkyl-substituted or unsubstituted naphthol, alkyl-substituted or unsubstituted hydroquinone, alkyl-substituted or unsubstituted resorcinol, alkyl-substituted or unsubstituted naphthalene diol, etc.) and formaldehyde, acetaldehyde, benzaldehyde, p-hydroxybenzaldehyde, o-hydroxybenzaldehyde, furfural, p-hydroxyacetophenone, o-hydroxyacetophenone, dicyclopentadiene, 4,4'-bis(chloromethyl)-1,1'-biphenyl, 4,4'-bis(methoxymethyl)-1,1'-biphenyl, 1,4-bis(chloromethyl)benzene, 1,4-bis(methoxymethyl)benzene, etc.
[0228] When a compound containing an α-methylbenzyl group is used as the (X1) aromatic polyhydroxy compound, the method for producing the active ester resin may include a modification step of introducing an α-methylbenzyl group into the (X1) aromatic polyhydroxy compound. In the following description, the (X1) aromatic polyhydroxy compound not containing an α-methylbenzyl group may be referred to as "(X1-2) unmodified aromatic polyhydroxy compound", and the (X1) aromatic polyhydroxy compound containing an α-methylbenzyl group may be referred to as "(X1-1) modified aromatic polyhydroxy compound".
[0229] For example, by reacting the unmodified aromatic polyhydroxy compound (X1-2) with styrene in the presence of an acid catalyst, the α-methylbenzyl group can be bonded to the aromatic ring of the unmodified aromatic polyhydroxy compound (X1-2) to obtain the modified aromatic polyhydroxy compound (X1-1). Examples of the acid catalyst include: inorganic acids such as phosphoric acid, sulfuric acid, and hydrochloric acid; organic acids such as oxalic acid, benzenesulfonic acid, toluenesulfonic acid, methanesulfonic acid, and fluoromethanesulfonic acid; and Friedel-Crafts catalysts such as aluminum chloride, zinc chloride, tin chloride, ferric chloride, and diethyl sulfate.
[0230] The amount of the acid catalyst used can be appropriately selected according to the target α-methylbenzyl group introduction amount. For example, in the case of an inorganic acid and an organic acid, the amount of the acid catalyst can be 0.001 to 10.0 parts by mass, preferably 0.01 to 7.0 parts by mass, relative to 100 parts by mass of the total amount of the (X1-2) unmodified aromatic polyhydroxy compound and styrene. In addition, in the case of a Friedel-Crafts catalyst, the amount of the acid catalyst can be 0.2 to 3.0 moles, preferably 0.5 to 2.0 moles, relative to 1 mole of the (X1-2) unmodified aromatic polyhydroxy compound.
[0231] The reaction of the unmodified aromatic polyhydroxy compound (X1-2) with styrene may be carried out in the absence of a solvent or in the presence of a solvent. As the solvent, for example, the same solvent as used in the condensation reaction described below may be used. The reaction temperature is preferably 60° C. to 180° C., more preferably 80° C. to 160° C. The reaction time is not particularly limited, but is preferably 1 hour to 100 hours.
[0232] After the reaction is completed, the acid catalyst can be removed by neutralization, water washing or decomposition, and the modified aromatic polyhydroxy compound (X1-1) can be separated by general operations such as extraction and distillation. The neutralization and water washing can be carried out according to conventional methods, for example, alkaline substances such as sodium hydroxide, potassium hydroxide, sodium carbonate, ammonia, triethylenetetramine, aniline, etc. can be used as neutralizers.
[0233] When producing a preferred active ester resin containing a partial structure represented by formula (I) or a preferred active ester resin represented by formula (II), the polyvalent aromatic hydroxy compound (X1) is preferably a compound represented by the following formula (X1-C). C With the organic group Ar in formula (I) C same.
[0234]
[0235] In the (X2) component, the (X2-1) aromatic carboxylic acid compound represents a compound containing an aromatic ring and a carboxyl group. The (X2-1) aromatic carboxylic acid compound may contain one carboxyl group in one molecule, but preferably contains two or more carboxyl groups in one molecule, and particularly preferably contains two carboxyl groups in one molecule. In addition, it is preferred that the carboxyl group is directly bonded to the aromatic ring. Examples of (X2-1) aromatic carboxylic acid compounds include: isophthalic acid which may have a substituent, terephthalic acid which may have a substituent, 2,6-naphthalene dicarboxylic acid which may have a substituent, 1,6-naphthalene dicarboxylic acid which may have a substituent, 2,7-naphthalene dicarboxylic acid which may have a substituent, and the like. In addition, the (X2-2) aromatic acyl halide compound represents an acyl halide compound of the above-mentioned (X2-1) aromatic carboxylic acid compound. Examples of (X2-2) aromatic acyl halide compounds include: isophthaloyl chloride which may have a substituent, terephthaloyl chloride which may have a substituent, and the like.
[0236] In the case of manufacturing a preferred active ester resin containing a partial structure represented by formula (I) or a preferred active ester resin represented by formula (II), as the aromatic carboxylic acid compound (X2-1), a compound represented by the following formula (X2-B1) is preferred. In addition, as the aromatic acyl halide compound (X2-2), a compound represented by the following formula (X2-B2) is preferred. In formula (X2-B1) and formula (X2-B2), the group Ar B With the organic group Ar in formula (I) B In the formula (X2-B2), X represents a halogen atom.
[0237]
[0238] (X3) Aromatic monohydroxy compound refers to a compound containing an aromatic ring and one hydroxyl group. Preferably, the hydroxyl group is directly bonded to the aromatic ring. Examples of (X3) aromatic monohydroxy compound include phenol, cresol, p-tert-butylphenol, 1-naphthol, 2-naphthol, o-phenylphenol, p-phenylphenol, and the like.
[0239] When a compound containing an α-methylbenzyl group is used as the (X3) aromatic monohydroxy compound, the method for producing the active ester resin may include a modification step of introducing an α-methylbenzyl group into the (X3) aromatic monohydroxy compound. The introduction of the α-methylbenzyl group into the (X3) aromatic monohydroxy compound may be carried out, for example, by a method comprising reacting the (X3) aromatic monohydroxy compound with styrene in the presence of an acid catalyst. The reaction may be carried out in the same manner as the reaction of the (X1-2) unmodified aromatic polyhydroxy compound with styrene.
[0240] When producing a preferred active ester resin represented by formula (II), the aromatic monohydroxy compound (X3) is preferably a compound represented by the following formula (X3-A).A With the organic group Ar in formula (II) A same.
[0241]
[0242] In the condensation reaction of component (X1), component (X2) and component (X3), condensation (esterification) occurs between component (X2) and component (X1) and between component (X2) and component (X3). In the reaction, by changing the conditions such as the quantitative ratio of each component, the degree of condensation between component (X2) and component (X1) can be adjusted, and the structure of the resulting active ester resin (for example, the number of repetitions n in formula (II)) can be adjusted.
[0243] The condensation reaction can be carried out in a solvent-free system without using a solvent, or can be carried out in an organic solvent system using an organic solvent. Examples of organic solvents used in the condensation reaction include: ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; acetate solvents such as ethyl acetate, butyl acetate, cellosolve acetate, propylene glycol monomethyl ether acetate, and carbitol acetate; carbitol solvents such as cellosolve and butyl carbitol; aromatic hydrocarbon solvents such as toluene and xylene; amide solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone. One organic solvent may be used alone, or two or more may be used in combination.
[0244] A base may be used in the condensation reaction. Examples of the base include alkali metal hydroxides such as sodium hydroxide (caustic soda) and potassium hydroxide; tertiary amines such as triethylamine, pyridine, and N,N-dimethyl-4-aminopyridine (DMAP). The base may be used alone or in combination of two or more.
[0245] A condensation agent and a phase transfer catalyst may also be used in the condensation reaction. These substances may be conventionally known optional substances that can be used in esterification reactions.
[0246] The reaction temperature in the condensation reaction is not particularly limited as long as the condensation reaction proceeds, and can be, for example, in the range of 0° C. to 80° C. The reaction time in the condensation reaction is not particularly limited as long as the target active ester resin structure is achieved, and can be, for example, in the range of 30 minutes to 8 hours.
[0247] The active ester resin can be purified after the condensation reaction. For example, after the condensation reaction, in order to remove the by-product salt and the excess starting raw materials from the system, purification treatments such as water washing and precision filtration can be applied. In detail, after the condensation reaction, the necessary amount of water required for the by-product salt is mixed and dissolved, and the liquid is allowed to stand and the water layer is discarded. Then, the mixed acid is neutralized as needed, and the water is repeatedly washed. After that, after a dehydration process based on a pharmaceutical or azeotropic agent, impurities are removed by precision filtration and purification, the organic solvent is removed by distillation as needed to obtain an active ester resin. It is also possible to directly use the solvent for the resin composition without completely removing the organic solvent.
[0248] As a second example of a method for producing an active ester resin according to one embodiment of the present invention, there can be cited a method comprising the following steps: an esterification step of reacting (X1) an aromatic polyhydroxy compound, (X2) an aromatic carboxylic acid compound or an aromatic acyl halide compound, and, if necessary, further reacting (X3) an aromatic monohydroxy compound to obtain a polyester resin as a condensation product; and a modification step of introducing an α-methylbenzyl group into the above-mentioned polyester resin. The esterification step can be carried out in the same manner as the production method according to the first example. In addition, the modification step can be carried out in the same manner as the modification step of introducing an α-methylbenzyl group into the (X1) aromatic polyhydroxy compound in the production method according to the first example. If a specific example is cited, an active ester resin can be obtained by reacting a polyester resin with styrene in the presence of an acid catalyst to bond the α-methylbenzyl group to the aromatic ring of the polyester resin.
[0249] Among the above-mentioned production methods, from the viewpoint of achieving a high yield, the production method involved in the first example is preferred, and the production method using the (X1) aromatic polyhydroxy compound containing an α-methylbenzyl group is further preferred. In addition, from the viewpoint of obtaining an active ester resin that can effectively improve the dielectric loss tangent under a high temperature environment, the production method using the (X3) aromatic monohydroxy compound is particularly preferred. Therefore, in a preferred embodiment, the production method of the active ester resin is preferably produced by a production method comprising the following steps: reacting the (X1) aromatic polyhydroxy compound containing the (X1-1) modified aromatic polyhydroxy compound containing an α-methylbenzyl group, the (X2) aromatic carboxylic acid compound or aromatic acyl halide compound, and the (X3) aromatic monohydroxy compound. In the case of adopting such a preferred production method, the active ester resin can be produced as a condensation reaction product of (X1) an aromatic polyhydroxy compound containing (X1-1) a modified aromatic polyhydroxy compound containing an α-methylbenzyl group, (X2) an aromatic carboxylic acid compound or an aromatic acid halide compound, and (X3) an aromatic monohydroxy compound.
[0250] The active ester resin involved in this embodiment, when combined with a cross-linking resin, can provide a cured product that exhibits excellent dielectric properties under high temperature environments, and can achieve the low transmission loss required for 5G applications. In addition, the cured product of the resin composition in which the combination of the active ester resin and the cross-linking resin involved in this embodiment generally has excellent detergency. Moreover, the cured product of the resin composition in which the combination of the active ester resin and the cross-linking resin involved in this embodiment generally suppresses halos. Therefore, in a suitable embodiment, the above-mentioned active ester resin can be suitably used as a resin cross-linking agent. The active ester resin can be provided, for example, alone as a resin cross-linking agent, or as a solution-state resin cross-linking agent mixed with an appropriate solvent.
[0251] <Resin composition>
[0252] The resin composition can be produced using the above-mentioned active ester resin. The resin composition according to one embodiment of the present invention contains the above-mentioned active ester resin and a crosslinkable resin.
[0253] In the resin composition of the present embodiment, the crosslinkable resin is not particularly limited in type as long as it can be crosslinked in combination with the active ester resin. From the viewpoint of being able to bring particularly excellent effects in combination with the active ester resin, the crosslinkable resin is preferably one or more selected from thermosetting resins and free radical polymerizable resins.
[0254] As the thermosetting resin and the radical polymerizable resin, known resins used in forming an insulating layer of a printed wiring board or a semiconductor chip package can be used. Hereinafter, the thermosetting resin and the radical polymerizable resin that can be used as the crosslinking resin will be described.
[0255] Examples of the thermosetting resin include epoxy resins, benzocyclobutene resins, epoxy acrylate resins, urethane acrylate resins, urethane resins, cyanate resins, polyimide resins, benzocyclobutene resins, epoxy acrylate resins, urethane acrylate resins, urethane resins, cyanate resins, polyimide resins, The thermosetting resin may be used alone or in combination of two or more. Among them, in combination with an active ester resin, the crosslinking resin preferably includes an epoxy resin from the viewpoint of significantly obtaining the effect of the present invention.
[0256] The type of the epoxy resin is not particularly limited as long as it has one or more (preferably two or more) epoxy groups in one molecule. Examples of the epoxy resin include bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol S epoxy resin, bisphenol AF epoxy resin, novolac epoxy resin, tert-butylcatechol epoxy resin, naphthol epoxy resin, naphthalene epoxy resin, naphthylene ether epoxy resin, glycidylamine epoxy resin, glycidylester epoxy resin, cresol novolac epoxy resin, biphenyl epoxy resin, phenol aralkyl epoxy resin, biphenyl aralkyl epoxy resin, fluorene skeleton epoxy resin, dicyclopentadiene epoxy resin, anthracene epoxy resin, linear aliphatic epoxy resin, epoxy resin having a butadiene structure, alicyclic epoxy resin, heterocyclic epoxy resin, spiro ring-containing epoxy resin, cyclohexanedimethanol epoxy resin, trimethylol epoxy resin, halogenated epoxy resin, and the like. According to the resin composition containing the active ester resin, a cured product exhibiting excellent dielectric properties in a high temperature environment can be obtained regardless of the type of the epoxy resin.
[0257] Epoxy resins can be divided into epoxy resins that are liquid at a temperature of 20°C (hereinafter sometimes referred to as "liquid epoxy resins") and epoxy resins that are solid at a temperature of 20°C (hereinafter sometimes referred to as "solid epoxy resins"). For the resin composition involved in the present embodiment, as an epoxy resin, only a liquid epoxy resin may be included, only a solid epoxy resin may be included, and a liquid epoxy resin and a solid epoxy resin may be included in combination. When a liquid epoxy resin and a solid epoxy resin are included in combination, the blending ratio (liquid: solid) can be set to a range of 20:1 to 1:20 (preferably 10:1 to 1:10, more preferably 3:1 to 1:3) in terms of mass ratio.
[0258] The epoxy equivalent of the epoxy resin is preferably 50 to 2000 g / eq., more preferably 60 to 1000 g / eq., and further preferably 80 to 500 g / eq. The epoxy equivalent is the mass of the epoxy resin containing 1 equivalent of epoxy groups, and can be measured according to JIS K7236.
[0259] The weight average molecular weight (Mw) of a thermosetting resin such as an epoxy resin is preferably 100 to 5,000, more preferably 250 to 3,000, and even more preferably 400 to 1,500. The weight average molecular weight Mw of the resin can be measured as a polystyrene-equivalent value by a GPC method.
[0260] As a free radical polymerizable resin, as long as it has one or more (preferably two or more) free radical polymerizable unsaturated groups in one molecule, its type is not particularly limited. As a free radical polymerizable resin, for example, there can be mentioned: a resin having one or more selected from maleimide group, vinyl group, allyl group, styryl group, vinylphenyl group, acryloyl group, methacryloyl group, fumaryl group and maleoyl group as a free radical polymerizable unsaturated group. Among them, from the viewpoint of significantly obtaining the effect of the present invention, the cross-linking resin preferably contains one or more selected from maleimide resin, (meth) acrylic resin and styrene resin.
[0261] The maleimide resin is not particularly limited in its type as long as it has one or more (preferably two or more) maleimide groups (2,5-dihydro-2,5-dioxo-1H-pyrrol-1-yl) in one molecule. As maleimide resins, for example, there can be mentioned: "BMI-3000J", "BMI-5000", "BMI-1400", "BMI-1500", "BMI-1700", "BMI-689" (all manufactured by Designer Molecules), etc., maleimide resins containing an aliphatic skeleton with 36 carbon atoms derived from dimer diamine; maleimide resins containing an indane skeleton recorded in Japan Invention Association Publication Technical Bulletin No. 2020-500211; maleimide resins containing an aromatic ring skeleton directly bonded to the nitrogen atom of the maleimide group, such as "MIR-3000-70MT" (manufactured by Nippon Kayaku Co., Ltd.), "BMI-4000" (manufactured by Yamato Chemical Co., Ltd.), and "BMI-80" (manufactured by KI Chemical Co., Ltd.).
[0262] As a (meth)acrylic resin, as long as it has one or more (preferably two or more) (meth)acryloyl groups in one molecule, its type is not particularly limited, and it may be a monomer or an oligomer. Here, the term "(meth)acryloyl group" is a general term for acryloyl groups and methacryloyl groups. Examples of methacrylic resins include: "A-DOG" (manufactured by Shin-Nakamura Chemical Industry Co., Ltd.), "DCP-A" (manufactured by Kyoeisha Chemical Co., Ltd.), "NPDGA", "FM-400", "R-687", "THE-330", "PET-30", "DPHA" (all manufactured by Nippon Kayaku Co., Ltd.) and other (meth)acrylic resins.
[0263] The styrene resin is not particularly limited in type as long as it has one or more (preferably two or more) styrene groups or vinylphenyl groups in one molecule, and may be a monomer or an oligomer. Examples of the styrene resin include: "OPE-2St", "OPE-2St1200", "OPE-2St 2200" (all manufactured by Mitsubishi Gas Chemical Co., Ltd.) and the like.
[0264] The resin composition according to the present embodiment may contain only a thermosetting resin, only a radical polymerizable resin, or a combination of a thermosetting resin and a radical polymerizable resin as the crosslinkable resin.
[0265] In the resin composition according to the present embodiment, the mass ratio of the active ester resin to the cross-linking resin (active ester resin / cross-linking resin) may be 1 or more, preferably 1.05 or more, and more preferably 1.10 or more. The upper limit of the mass ratio (active ester resin / cross-linking resin) may be, for example, 2 or less, 1.9 or less, or 1.8 or less.
[0266] The resin composition according to the present embodiment may further include a crosslinking accelerator. By including a crosslinking accelerator, the crosslinking time and the crosslinking temperature can be effectively adjusted.
[0267] Examples of the crosslinking accelerator include organic phosphine compounds such as “TPP”, “TPP-K”, “TPP-S”, and “TPTP-S” (manufactured by Hokko Chemical Industry Co., Ltd.); imidazole compounds such as “CUREZOL 2MZ”, “2E4MZ”, “Cl1Z”, “Cl1Z-CN”, “Cl1Z-CNS”, “Cl1Z-A”, “2MZ-OK”, “2MA-OK”, and “2PHZ” (manufactured by Shikoku Chemical Industry Co., Ltd.); amine adduct compounds such as NOVACURE (manufactured by Asahi Kasei Industries Co., Ltd.) and Fujicure (manufactured by Fuji Chemical Industries Co., Ltd.); amine compounds such as 1,8-diazabicyclo[5.4.0]undecene-7,4-dimethylaminopyridine, benzyldimethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, and 4-dimethylaminopyridine; and organic metal complexes or organic metal salts such as cobalt, copper, zinc, iron, nickel, manganese, and tin.
[0268] When the resin composition according to the present embodiment includes a crosslinking accelerator, the content of the crosslinking accelerator in the resin composition can be determined according to the properties required of the resin composition. When the non-volatile component in the resin composition is set to 100% by mass, the content of the crosslinking accelerator is preferably 0.001% by mass or more, more preferably 0.01% by mass or more, particularly preferably 0.04% by mass or more, preferably 10% by mass or less, more preferably 5% by mass or less, and further preferably 1% by mass or less.
[0269] The resin composition according to the present embodiment may further contain an inorganic filler. By containing an inorganic filler, the linear thermal expansion coefficient can be reduced or the dielectric loss tangent can be further reduced.
[0270] As the inorganic filler, for example, silica, aluminum oxide, barium sulfate, talc, clay, mica powder, aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, magnesium oxide, boron nitride, aluminum borate, barium titanate, strontium titanate, calcium titanate, magnesium titanate, bismuth titanate, titanium oxide, barium zirconate, calcium zirconate, etc. can be mentioned. Among them, silica is suitable. As silica, for example, amorphous silica, fused silica, crystalline silica, synthetic silica, hollow silica, etc. can be mentioned. In addition, as silica, spherical silica is preferred. One inorganic filler can be used alone, or two or more can be used in combination. Commercially available products of inorganic fillers include, for example, "UFP-30" (manufactured by Denka); "YC100C", "YA050C", "YA050C-MJE", "YA010C", "SC2500SQ", "SO-C4", "SO-C2", "SO-C1", "SC-C2" (all manufactured by ADMATECHS); "SILFIL NSS-3N", "SILFIL NSS-4N", "SILFIL NSS-5N" (manufactured by Tokuyama), etc.
[0271] From the viewpoint that the surface of the insulating layer formed by the cured product has low roughness and is easy to form fine wiring, the average particle size of the inorganic filler is preferably less than 5 μm, more preferably less than 2 μm, and further preferably less than 1 μm. There is no particular limitation on the lower limit of the average particle size, for example, it can be more than 0.01 μm, more than 0.02 μm, more than 0.03 μm, etc. The average particle size of the inorganic filler can be measured by a laser diffraction / scattering method based on Mie scattering theory. Specifically, a particle size distribution of an inorganic filler can be prepared on a volume basis by a laser diffraction scattering particle size distribution measuring device, and the median particle size is measured as the average particle size. The sample can be measured using a sample obtained by weighing 100 mg of an inorganic filler and 10 g of methyl ethyl ketone into a vial and dispersing it by ultrasonic waves for 10 minutes. For the measurement sample, a laser diffraction particle size distribution measuring device is used, and the wavelength of the light source is set to blue and red, and the volume-based particle size distribution of the inorganic filler is measured in a flow cell (flow cell) mode, and the average particle size as the median particle size can be calculated based on the obtained particle size distribution. As a laser diffraction particle size distribution measuring device, for example, "LA-960" manufactured by Horiba Manufacturing Co., Ltd. can be cited.
[0272] The inorganic filler material is preferably surface treated with a surface treatment agent to improve its moisture resistance and dispersibility. The surface treatment agent is: aminosilane coupling agent, urea silane coupling agent, epoxy silane coupling agent, mercapto silane coupling agent, vinyl silane coupling agent, styrene silane coupling agent, acrylate silane coupling agent, isocyanate silane coupling agent, sulfide silane coupling agent, organic silazane compound, titanate coupling agent, etc.
[0273] In the case where the resin combination involved in the present embodiment includes an inorganic filler, the content of the inorganic filler in the resin combination can be determined according to the characteristics required by the resin combination. When the non-volatile component in the resin combination is set to 100 mass %, the content of the inorganic filler in the resin combination can be, for example, more than 5 mass %, more than 10 mass %, preferably more than 30 mass %, more preferably more than 40 mass %, more preferably more than 50 mass %. The upper limit of the content of the inorganic filler is not particularly limited, for example, it can be less than 90 mass %, less than 85 mass %, etc.
[0274] The resin composition according to the present embodiment may further contain a thermoplastic resin. When the resin composition contains a thermoplastic resin, the mechanical strength of the cured product can be increased, and the film-forming ability when used in the form of a resin sheet can be further improved.
[0275] Examples of the thermoplastic resin include phenoxy resin, polyvinyl acetal resin, polyimide resin, polyamide-imide resin, polyetherimide resin, polysulfone resin, polyethersulfone resin, polyphenylene ether resin, polycarbonate resin, polyetheretherketone resin, and polyester resin, and phenoxy resin and polyvinyl acetal resin are particularly preferred. These thermoplastic resins may be used alone or in combination of two or more. The weight average molecular weight of the thermoplastic resin is preferably in the range of 8,000 to 200,000, and more preferably in the range of 12,000 to 100,000.
[0276] The content of the thermoplastic resin is not particularly limited, but is preferably 0.001% by mass or more, more preferably 0.01% by mass or more, further preferably 0.1% by mass or more, particularly preferably 0.5% by mass or more, and is preferably 10% by mass or less, more preferably 5% by mass or less, when the non-volatile component in the resin composition is set to 100% by mass.
[0277] The resin composition of the present embodiment may further include optional additives. Examples of such additives include: organic fillers such as rubber particles; free radical polymerization initiators such as peroxide-based free radical polymerization initiators and azo-based free radical polymerization initiators; phenol-based crosslinking agents, benzophenone-based crosslinking agents, and the like. any resin crosslinking agent other than active ester resin such as oxazine crosslinking agent, acid anhydride crosslinking agent, cyanate crosslinking agent; organic metal compounds such as organic copper compounds, organic zinc compounds, organic cobalt compounds; colorants such as phthalocyanine blue, phthalocyanine green, iodine green, diazo yellow, crystal violet, titanium oxide, carbon black; polymerization inhibitors such as hydroquinone, catechol, pyrogallol, phenothiazine; leveling agents such as silicone leveling agent and acrylic polymer leveling agent; thickeners such as Benton and montmorillonite; defoaming agents such as silicone defoaming agent, acrylic defoaming agent, fluorine defoaming agent, vinyl resin defoaming agent; ultraviolet absorbers such as benzotriazole ultraviolet absorbers; adhesion enhancers such as urea silane; triazole adhesion imparting agent, tetrazole adhesion imparting agent, triazine adhesion imparting agent Adhesion imparting agents such as adhesives; antioxidants such as hindered phenol antioxidants; fluorescent whitening agents such as stilbene derivatives; surfactants such as fluorine-based surfactants and silicone-based surfactants; flame retardants such as phosphorus-based flame retardants (such as phosphate compounds, phosphazene compounds, phosphinic acid compounds, red phosphorus), nitrogen-based flame retardants (such as melamine sulfate), halogen-based flame retardants, inorganic flame retardants (such as antimony trioxide); dispersants such as phosphate-based dispersants, polyoxyalkylene-based dispersants, acetylene-based dispersants, silicone-based dispersants, anionic dispersants, cationic dispersants; stabilizers such as borate-based stabilizers, titanate-based stabilizers, aluminate-based stabilizers, zirconate-based stabilizers, isocyanate-based stabilizers, carboxylic acid-based stabilizers, and carboxylic anhydride-based stabilizers, etc. The content of the additives involved can be determined according to the characteristics required by the resin composition.
[0278] The resin composition of the present embodiment may further contain an organic solvent as a volatile component. Examples of the organic solvent include ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; ester solvents such as methyl acetate, ethyl acetate, butyl acetate, isobutyl acetate, isoamyl acetate, methyl propionate, ethyl propionate, and γ-butyrolactone; tetrahydropyran, tetrahydrofuran, 1,4-dihydropyran, and 1,4-dihydrofuran. ether solvents such as alkane, diethyl ether, diisopropyl ether, dibutyl ether, diphenyl ether; alcohol solvents such as methanol, ethanol, propanol, butanol, ethylene glycol; 2-ethoxyethyl acetate, propylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, carbitol acetate (ethyl diglycol Ether ester solvents such as acetate, γ-butyrolactone, and methyl methoxypropionate; ester alcohol solvents such as methyl lactate, ethyl lactate, and methyl 2-hydroxyisobutyrate; ether alcohol solvents such as 2-methoxypropanol, 2-methoxyethanol, 2-ethoxyethanol, propylene glycol monomethyl ether, and diethylene glycol monobutyl ether (butyl carbitol); amide solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone; sulfoxide solvents such as dimethyl sulfoxide; nitrile solvents such as acetonitrile and propionitrile; aliphatic hydrocarbon solvents such as hexane, cyclopentane, cyclohexane, and methylcyclohexane; aromatic hydrocarbon solvents such as benzene, toluene, xylene, ethylbenzene, and trimethylbenzene. The organic solvent may be used alone or in combination of two or more.
[0279] When the resin composition involved in this embodiment contains an organic solvent, the content of the organic solvent in the resin composition can be determined according to the properties required of the resin composition. When all the components in the resin composition are set to 100 mass%, for example, it can be set to less than 60 mass%, less than 40 mass%, less than 30 mass%, less than 20 mass%, less than 15 mass%, less than 10 mass%, etc.
[0280] The resin composition according to the present embodiment can be produced by appropriately mixing the essential components among the above-mentioned components, and kneading or mixing them using a kneading device such as a three-roll mill, a ball mill, a bead mill, a sand mill, or a stirring device such as a super mixer or a planetary mixer as needed.
[0281] By curing the resin composition involved in the present embodiment, a cured product can be obtained. Generally, volatile components such as organic solvents contained in the resin composition can be volatilized by the heat given during curing, but non-volatile components such as active ester resins, cross-linking resins, cross-linking accelerators, inorganic fillers, thermoplastic resins and optional additives will not volatilize due to the heat during thermal curing. Therefore, the cured product may include non-volatile components of the resin composition or their reaction products.
[0282] The resin composition according to the present embodiment, which contains an active ester resin and a crosslinking resin in combination, can provide a cured product having low dielectric properties under high temperature environments. Therefore, when the cured product is applied to an insulating layer of a printed wiring board or a semiconductor chip package, the transmission loss under high temperature environments can be reduced.
[0283] In one embodiment, the cured product of the resin composition according to the present embodiment may exhibit a low dielectric loss tangent (Df) under a high temperature environment of 90° C. For example, as described in the column of <Determination of Dielectric Properties (High Temperature)> in the examples described later, when measured at a measurement frequency of 10 GHz and 90° C., the dielectric loss tangent (Df) of the cured product of the resin composition according to the present embodiment may preferably be 0.01 or less, 0.008 or less, 0.007 or less, 0.006 or less, 0.005 or less, 0.004 or less, or 0.003 or less.
[0284] The cured product of the resin composition according to the present embodiment can usually exhibit a low dielectric loss tangent (Df) at room temperature. For example, as described in the <Determination of Dielectric Properties (Room Temperature)> column of the embodiment described later, when measured at a measurement frequency of 5.8 GHz and 23° C., the dielectric loss tangent (Df) of the cured product of the resin composition according to the present embodiment can be preferably 0.01 or less, 0.008 or less, 0.006 or less, 0.005 or less, 0.004 or less, or 0.003 or less.
[0285] The cured product of the resin composition according to the present embodiment can generally exhibit a low relative dielectric constant (Dk) under a high temperature environment of 90° C. For example, as described in the column <Measurement of Dielectric Properties (High Temperature)> of the Examples described later, when measured at a measurement frequency of 10 GHz and 90° C., the relative dielectric constant (Dk) of the cured product of the resin composition according to the present embodiment can preferably be 3.3 or less, 3.2 or less, 3.1 or less, 3.0 or less, or 2.8 or less.
[0286] The cured product of the resin composition according to the present embodiment can generally exhibit a low relative dielectric constant (Dk) at room temperature. For example, as described in the column <Determination of Dielectric Properties (Room Temperature)> of the embodiments described later, when measured at a measurement frequency of 5.8 GHz and 23° C., the relative dielectric constant (Dk) of the cured product of the resin composition according to the present embodiment can preferably be 3.3 or less, 3.2 or less, 3.1 or less, 3.0 or less, or 2.8 or less.
[0287] The cured product of the resin composition involved in the present embodiment can usually exhibit excellent detergency. Generally, when an insulating layer is formed by a cured product of a resin composition, holes such as vias and through holes are sometimes formed on the insulating layer. When such holes are formed on the insulating layer, stains as resin residues can be formed in the holes. The property of being able to easily remove such stains is called "decontamination". For example, when the decontamination is evaluated by the method described in the "Evaluation of Decontamination" column of the embodiments described later, the cured product of the resin composition involved in the present embodiment can make the maximum length of the stain extending from the wall surface at the bottom of the via hole (maximum stain length) less than 5μm. Generally, the shorter the maximum stain length, the better the decontamination property.
[0288] The cured product of the resin composition involved in the present embodiment can usually have the property that it is difficult to cause a halo defect after the via is formed. Usually, an insulating layer is sometimes formed on the inner substrate by the cured product of the resin composition. If a via is formed on the insulating layer and a roughening treatment is performed, peeling sometimes occurs around the via and between the insulating layer and the inner substrate to form a gap. "Halo" means the peeling between the above-mentioned insulating layer and the inner substrate. The cured product of the resin composition involved in the present embodiment can usually suppress the degree of the above-mentioned halo. For example, the halo ratio measured by the method described in the column "Evaluation of Halos" in the later-described embodiments can preferably be 50% or less. For the halo ratio, the size of the gap formed by the halo is represented by taking the bottom size of the inner substrate side of the via as the reference, and the smaller the halo ratio Hb is, the more effectively the halo can be suppressed.
[0289] The resin composition involved in the present embodiment can be suitably used as the resin composition (resin composition for forming the insulating layer of printed wiring board) for forming the insulating layer of printed wiring board, and can be more suitably used as the resin composition (resin composition for forming the interlayer insulating layer of printed wiring board) for forming the interlayer insulating layer of printed wiring board. The resin composition involved in the present embodiment can also be suitable for use in the case where the printed wiring board is a component built-in circuit board. The resin composition involved in the present embodiment can also be suitably used as the resin composition (resin composition for sealing semiconductor chip) for sealing semiconductor chip, and then, can be suitably used as the resin composition for forming the rewiring layer as the insulating layer for forming the rewiring layer (resin composition for forming the rewiring layer). In addition, the resin composition involved in the present embodiment can be widely used in the purposes of resin composition required for sheet-like laminated materials such as resin sheets, prepregs, solder resists, bottom filling materials, chip bonding materials, filling resins, component embedding resins, etc.
[0290] <Sheet-shaped laminated materials (resin sheets, prepregs)>
[0291] The resin composition according to the present embodiment may be used as it is, or may be used in the form of a sheet-like laminated material containing the resin composition.
[0292] As the sheet-like laminated material, the following resin sheets and prepregs are preferred.
[0293] In one embodiment, the resin sheet includes a support and a layer of a resin composition formed on the support (hereinafter, sometimes simply referred to as a “resin composition layer”). The resin composition layer contains the above-mentioned resin composition, and preferably contains only the above-mentioned resin composition.
[0294] The thickness of the resin composition layer is suitable for different values according to the purpose, and can be appropriately determined according to the purpose. For example, from the viewpoint of the thinning of printed wiring boards and semiconductor chip packages, the thickness of the resin composition layer is preferably 200 μm or less, more preferably 150 μm or less, 120 μm or less, 100 μm or less, 80 μm or less, 60 μm or less or 50 μm or less. The lower limit of the thickness of the resin composition layer is not particularly limited, and can usually be 1 μm or more, 5 μm or more, etc.
[0295] Examples of the support include thermoplastic resin films, metal foils, and release papers, and thermoplastic resin films and metal foils are preferred. Therefore, in a preferred embodiment, the support is a thermoplastic resin film or a metal foil.
[0296] When a thermoplastic resin film is used as a support, examples of the thermoplastic resin include polyesters such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN), acrylics such as polycarbonate (PC) and polymethyl methacrylate (PMMA), cyclic polyolefins, triacetyl cellulose (TAC), polyether sulfide (PES), polyether ketone, polyimide, etc. Among them, polyethylene terephthalate and polyethylene naphthalate are preferred, and inexpensive polyethylene terephthalate is particularly preferred.
[0297] When a metal foil is used as a support, examples of the metal foil include copper foil and aluminum foil, preferably copper foil. The copper foil may be a foil made of copper alone or an alloy of copper and other metals (e.g., tin, chromium, silver, magnesium, nickel, zirconium, silicon, titanium, etc.).
[0298] For the support, the surface bonded to the resin composition layer may also be subjected to surface treatments such as matte treatment, corona treatment, and antistatic treatment. In addition, as the support, a support with a release layer having a release layer on the surface bonded to the resin composition layer may be used. As a release agent used in the release layer of the support with a release layer, for example, there can be mentioned: one or more release agents selected from alkyd resins, polyolefin resins, urethane resins, and silicone resins. The support with a release layer can use commercial products, for example, there can be mentioned: "SK-1", "AL-5", "AL-7" manufactured by LINTEC, which is a PET film having a release layer with an alkyd resin-based release agent as the main component; "Lumirror T60" manufactured by Toray; "Purex" manufactured by Teijin; "Unipeel" manufactured by UNITIKA, etc.
[0299] The thickness of the support is not particularly limited, but is preferably in the range of 5 μm to 75 μm, more preferably in the range of 10 μm to 60 μm. When a support with a release layer is used, the thickness of the entire support with a release layer is preferably in the above range.
[0300] When a metal foil is used as a support, a metal foil with a support substrate in which a peelable support substrate is attached to a thin metal foil can be used. In one embodiment, the metal foil with a support substrate comprises: a support substrate, a peeling layer provided on the support substrate, and a metal foil provided on the peeling layer. When a metal foil with a support substrate is used as a support, the resin composition layer is provided on the metal foil.
[0301] In the metal foil with a supporting substrate, the material of the supporting substrate is not particularly limited, and examples thereof include: copper foil, aluminum foil, stainless steel foil, titanium foil, copper alloy foil, etc. When copper foil is used as the supporting substrate, it may be electrolytic copper foil or rolled copper foil. In addition, the peeling layer is not particularly limited as long as the metal foil can be peeled off from the supporting substrate, and examples thereof include: an alloy layer of an element selected from Cr, Ni, Co, Fe, Mo, Ti, W, and P; an organic film, etc.
[0302] In the metal foil with a supporting substrate, as a material of the metal foil, for example, copper foil and copper alloy foil are preferable.
[0303] In the metal foil with a supporting substrate, the thickness of the supporting substrate is not particularly limited, but is preferably in the range of 10 μm to 150 μm, more preferably in the range of 10 μm to 100 μm. The thickness of the metal foil can be, for example, in the range of 0.1 μm to 10 μm.
[0304] In one embodiment, the resin sheet may further include an optional layer as required. As the optional layer involved, for example, a protective film is provided on the surface of the resin composition layer that is not bonded to the support (i.e., the surface on the opposite side of the support). The thickness of the protective film is not particularly limited, for example, 1 μm to 40 μm. By laminating the protective film, dust can be prevented from adhering to the surface of the resin composition layer or causing damage to the surface of the resin composition layer.
[0305] The resin sheet can be produced, for example, by directly applying a liquid resin composition on a support using a die coater or the like, or by preparing a resin varnish obtained by dissolving the resin composition in an organic solvent and applying the varnish on a support, followed by drying to form a resin composition layer.
[0306] Examples of the organic solvent include the same organic solvents as those described as the components of the resin composition. The organic solvent may be used alone or in combination of two or more.
[0307] Drying can be carried out by a drying method such as heating or hot air blowing. The drying conditions are not particularly limited, and the drying is performed in a manner such that the content of the organic solvent in the resin composition layer is usually 10% by mass or less, preferably 5% by mass or less. Although it varies depending on the boiling point of the organic solvent in the resin composition or resin varnish, for example, in the case of using a resin composition or resin varnish containing 30% by mass to 60% by mass of an organic solvent, a resin composition layer can be formed by drying at 50° C. to 150° C. for 3 minutes to 10 minutes.
[0308] The resin sheet can be stored by winding it into a roll. When the resin sheet has a protective film, it can be used by peeling off the protective film.
[0309] In one embodiment, the prepreg is formed by impregnating a sheet-like fiber base material with a resin composition.
[0310] The sheet-like fiber substrate used for the prepreg is not particularly limited, and a sheet-like fiber substrate commonly used as a prepreg substrate such as glass cloth, aramid nonwoven fabric, liquid crystal polymer nonwoven fabric, etc. can be used. From the viewpoint of thinning a printed wiring board or a semiconductor chip package, the thickness of the sheet-like fiber substrate is preferably 50 μm or less, more preferably 40 μm or less, further preferably 30 μm or less, and particularly preferably 20 μm or less. There is no particular lower limit on the thickness of the sheet-like fiber substrate. It is usually 10 μm or more.
[0311] The prepreg can be produced by a known method such as a hot melt method or a solvent method.
[0312] The thickness of the prepreg may be in the same range as that of the resin composition layer in the above-mentioned resin sheet.
[0313] The sheet-like laminated material can be suitably used for forming an insulating layer of a printed wiring board (insulating layer for a printed wiring board), and can be more suitably used for forming an interlayer insulating layer of a printed wiring board (interlayer insulating layer for a printed wiring board). The sheet-like laminated material can also be suitably used for sealing a semiconductor chip (for sealing a semiconductor chip), and can be suitably used for a rewiring forming layer as an insulating layer for forming a rewiring layer.
[0314] <Printed wiring board>
[0315] A printed wiring board according to one embodiment of the present invention comprises an insulating layer formed of a cured product of the resin composition. The insulating layer comprises the cured product of the resin composition, and preferably comprises only the cured product of the resin composition.
[0316] The printed wiring board can be produced, for example, by a method including the following steps:
[0317] (i) forming a resin composition layer on the inner substrate;
[0318] (ii) A step of curing (for example, thermally curing) the resin composition layer to form an insulating layer.
[0319] In step (i), the resin composition may be applied onto the inner substrate to form the resin composition layer, but it is preferably formed by laminating a resin sheet on the inner substrate such that the resin composition layer of the resin sheet is bonded to the inner substrate.
[0320] The "inner layer substrate" used in step (i) refers to a member that becomes a substrate of a printed wiring board, and examples thereof include: a glass epoxy substrate, a metal substrate, a polyester substrate, a polyimide substrate, a BT resin substrate, a thermosetting polyphenylene ether substrate, and the like. In addition, the substrate may have a conductor layer on one or both sides thereof, and the conductor layer may also be patterned. An inner layer substrate having a conductor layer (circuit) formed on one or both sides of a substrate is sometimes referred to as an "inner layer circuit substrate". In addition, when manufacturing a printed wiring board, an intermediate product on which an insulating layer and / or a conductor layer is to be further formed is also included in the "inner layer substrate" described in the present invention. In the case where the printed wiring board is a circuit board with built-in components, an inner layer substrate with built-in components can be used.
[0321] The lamination of the inner substrate and the resin sheet can be performed, for example, by heat-pressing the resin sheet onto the inner substrate from the support body side. As a member for heat-pressing the resin sheet onto the inner substrate (hereinafter, sometimes referred to as a "heat-pressing member"), for example, a heated metal plate (SUS end plate, etc.) or a metal roller (SUS roller, etc.) can be cited. It should be noted that it is preferred that the heat-pressing member is not directly pressed onto the resin sheet, but is pressed through an elastic material such as heat-resistant rubber so that the resin sheet fully follows the surface unevenness of the inner substrate.
[0322] The lamination of the inner substrate and the resin sheet can be implemented by vacuum lamination. In the vacuum lamination method, the heating and pressing temperature is preferably 60°C to 160°C, more preferably 80°C to 140°C, the heating and pressing pressure is preferably 0.098MPa to 1.77MPa, more preferably 0.29MPa to 1.47MPa, and the heating and pressing time is preferably 20 seconds to 400 seconds, more preferably 30 seconds to 300 seconds. Lamination can be preferably implemented under reduced pressure conditions of 26.7hPa or less.
[0323] Lamination can be performed using a commercially available vacuum laminator. Examples of commercially available vacuum laminators include a vacuum pressurizing laminator manufactured by Meiki Mfg. Co., Ltd., a vacuum applicator manufactured by Nikko-Materials Co., Ltd., and a batch vacuum pressurizing laminator.
[0324] After lamination, the laminated resin sheet can be smoothed by pressing the heating and pressing member at normal pressure (atmospheric pressure), for example, from the support side. The pressing conditions for the smoothing treatment can be set to the same conditions as the heating and pressing conditions for the above-mentioned lamination. The smoothing treatment can be performed using a commercially available laminator. It should be noted that the lamination and smoothing treatment can be performed continuously using the above-mentioned commercially available vacuum laminator.
[0325] The support may be removed between step (i) and step (ii), or after step (ii). It should be noted that, when a metal foil is used as the support, the support may not be peeled off, and the metal foil may be used to form the conductor layer. In addition, when a metal foil with a supporting substrate is used as the support, the supporting substrate (and the peeling layer) may also be peeled off. Furthermore, the metal foil may be used to form the conductor layer.
[0326] In step (ii), the resin composition layer is cured (eg, thermally cured) to form an insulating layer composed of a cured product of the resin composition. The curing conditions of the resin composition layer are not particularly limited, and conditions commonly used when forming an insulating layer of a printed wiring board can be used.
[0327] For example, the heat curing conditions of the resin composition layer vary depending on the type of the resin composition, and in one embodiment, the curing temperature is preferably 120° C. to 250° C., more preferably 150° C. to 240° C., and further preferably 180° C. to 230° C. The curing time may be preferably 5 minutes to 240 minutes, more preferably 10 minutes to 150 minutes, and further preferably 15 minutes to 120 minutes.
[0328] Before the resin composition layer is thermally cured, the resin composition layer may be preheated at a temperature lower than the curing temperature. For example, before the resin composition layer is thermally cured, the resin composition layer may be preheated at a temperature of usually 50° C. to 120° C., preferably 60° C. to 115° C., more preferably 70° C. to 110° C., for usually 5 minutes or more, preferably 5 minutes to 150 minutes, more preferably 15 minutes to 120 minutes, and further preferably 15 minutes to 100 minutes.
[0329] When manufacturing a printed wiring board, the following steps may be further implemented: (iii) a step of opening a hole in the insulating layer; (iv) a step of roughening the insulating layer; (v) a step of forming a conductor layer. These steps (iii) to (v) may be implemented according to various methods known to those skilled in the art for manufacturing printed wiring boards. It should be noted that, in the case where the support is removed after step (ii), the removal of the support may be implemented between step (ii) and step (iii), between step (iii) and step (iv), or between step (iv) and step (v). In addition, as needed, the formation of the insulating layer and the conductor layer of steps (i) to (v) may be repeatedly implemented to form a multilayer wiring board.
[0330] In another embodiment, a printed wiring board can be produced using the above-mentioned prepreg. The production method is basically the same as that in the case of using a resin sheet.
[0331] Step (iii) is a step of drilling holes in the insulating layer, thereby forming holes such as via holes and through holes in the insulating layer. Step (iii) can be carried out using, for example, a drill, laser, plasma, etc., depending on the composition of the resin composition used to form the insulating layer. The size and shape of the hole can be appropriately determined according to the design of the printed wiring board.
[0332] Step (iv) is a step of roughening the insulating layer. Usually, in step (iv), contamination removal (decontamination) is also performed. There are no particular restrictions on the steps and conditions of the roughening treatment, and the known steps and conditions commonly used when forming the insulating layer of the printed wiring board can be adopted. For example, swelling treatment based on swelling liquid, roughening treatment based on oxidant, and neutralization treatment based on neutralizing liquid can be sequentially implemented to roughen the insulating layer.
[0333] There is no particular limitation on the swelling liquid used for the roughening treatment, and examples thereof include alkaline solutions, surfactant solutions, etc., preferably alkaline solutions. As the alkaline solution, sodium hydroxide solutions and potassium hydroxide solutions are more preferred. As commercially available swelling liquids, for example, there are "Swelling Dip Securiganth P" and "Swelling Dip Securiganth SBU" manufactured by Atotech Japan. There is no particular limitation on the swelling treatment based on the swelling liquid, and for example, it can be carried out by immersing the insulating layer in a swelling liquid at 30°C to 90°C for 1 minute to 20 minutes. From the viewpoint of suppressing the swelling of the resin of the insulating layer to an appropriate level, it is preferred to immerse the insulating layer in a swelling liquid at 40°C to 80°C for 5 minutes to 15 minutes.
[0334] As the oxidant used for the roughening treatment, there is no particular limitation, and examples thereof include: an alkaline permanganate solution obtained by dissolving potassium permanganate or sodium permanganate in an aqueous solution of sodium hydroxide. The roughening treatment based on an oxidant such as an alkaline permanganate solution is preferably performed by immersing the insulating layer in an oxidant solution heated to 60°C to 100°C for 10 minutes to 30 minutes. In addition, the concentration of permanganate in the alkaline permanganate solution is preferably 5% to 10% by mass. As commercially available oxidants, examples thereof include: alkaline permanganate solutions such as "Concentrate Compact CP" and "Dosing Solution Securiganth P" manufactured by Atotech Japan.
[0335] In addition, as the neutralizing solution used for the roughening treatment, an acidic aqueous solution is preferred, and commercially available products include, for example, "Reduction solution Securiganth P" manufactured by Atotech Japan. The treatment with the neutralizing solution can be performed by immersing the treated surface subjected to the roughening treatment with the oxidant in the neutralizing solution at 30°C to 80°C for 5 to 30 minutes. In view of operability, etc., it is preferred to immerse the object subjected to the roughening treatment with the oxidant in the neutralizing solution at 40°C to 70°C for 5 to 20 minutes.
[0336] Step (v) is a step of forming a conductor layer, and a conductor layer is formed on the insulating layer. There is no particular limitation on the conductor material used for the conductor layer. In a suitable embodiment, the conductor layer comprises one or more metals selected from gold, platinum, palladium, silver, copper, aluminum, cobalt, chromium, zinc, nickel, titanium, tungsten, iron, tin and indium. The conductor layer may be a single metal layer or an alloy layer. As the alloy layer, for example, a layer formed by an alloy of two or more metals selected from the above (for example, nickel-chromium alloy, copper-nickel alloy and copper-titanium alloy) can be cited. Among them, from the viewpoints of versatility, cost, ease of patterning, etc. of the formation of the conductor layer, a single metal layer of chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver or copper, or an alloy layer of nickel-chromium alloy, copper-nickel alloy, or copper-titanium alloy is preferred, a single metal layer of chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver or copper, or an alloy layer of nickel-chromium alloy is more preferred, and a single metal layer of copper is further preferred.
[0337] The conductor layer may be a single-layer structure, or a multi-layer structure in which two or more single metal layers or alloy layers composed of different types of metals or alloys are stacked. In the case where the conductor layer is a multi-layer structure, the layer in contact with the insulating layer is preferably a single metal layer of chromium, zinc or titanium, or an alloy layer of a nickel-chromium alloy.
[0338] The thickness of the conductor layer depends on the desired design of the printed wiring board, but is usually 3 μm to 35 μm, preferably 5 μm to 30 μm.
[0339] In one embodiment, the conductor layer can be formed by electroplating. For example, the surface of the insulating layer can be electroplated using a conventionally known technique such as a semi-additive method or a full-additive method to form a conductor layer having a desired wiring pattern. From the perspective of ease of manufacture, it is preferably formed by a semi-additive method. An example of forming a conductor layer by a semi-additive method is shown below.
[0340] First, a plating seed layer is formed on the surface of the insulating layer by electroless plating. Next, a mask pattern is formed on the formed plating seed layer to expose a portion of the plating seed layer corresponding to a desired wiring pattern. After a metal layer is formed on the exposed plating seed layer by electrolytic plating, the mask pattern is removed. Thereafter, the unnecessary plating seed layer is removed by etching or the like, and a conductor layer having a desired wiring pattern can be formed.
[0341] In other embodiments, the conductor layer can be formed using a metal foil. In the case of using a metal foil to form a conductor layer, step (v) is suitable for implementation between step (i) and step (ii). For example, after step (i), the support is removed and a metal foil is laminated on the surface of the exposed resin composition layer. The lamination of the resin composition layer and the metal foil can be implemented by a vacuum lamination method. The lamination conditions can be the same as those described for step (i). Then, step (ii) is implemented to form an insulating layer. Afterwards, using the metal foil on the insulating layer, a conductor layer with a desired wiring pattern can be formed by previously known techniques such as a subtractive method and a modified semi-additive method.
[0342] Metal foil can be produced by known methods such as electrolysis and rolling. Commercially available metal foils include HLP foil and JXUT-III foil manufactured by JX Nippon Mining & Metals Co., Ltd., and 3EC-III foil and TP-III foil manufactured by Mitsui Mining & Co., Ltd.
[0343] Alternatively, when a metal foil or a metal foil with a supporting substrate is used as a support of the resin sheet, the conductor layer can be formed using the metal foil as described above.
[0344] <Semiconductor chip packages>
[0345] The semiconductor chip package may be provided with a sealing layer formed by a cured product of the above-mentioned resin composition. The sealing layer comprises a cured product of the above-mentioned resin composition, preferably only comprises a cured product of the above-mentioned resin composition. In addition, the semiconductor chip package may be provided with an insulating layer (rewiring forming layer) composed of a cured product of the above-mentioned resin composition for forming a rewiring layer.
[0346] The semiconductor chip package can be manufactured, for example, using the above-mentioned resin composition or resin sheet by a method including the following steps (1) to (6). In order to form the sealing layer of step (3) or the rewiring forming layer of step (5), the above-mentioned resin composition and resin sheet can be used. Below, an example of using a resin composition and a resin sheet to form a sealing layer and a rewiring forming layer is shown, but the technology for forming the sealing layer and the rewiring forming layer of a semiconductor chip package is well known, and those skilled in the art can use the resin composition and the resin sheet according to the known technology to manufacture a semiconductor package.
[0347] (1) A step of laminating a temporary fixing film on a substrate;
[0348] (2) A step of temporarily fixing the semiconductor chip on a temporary fixing film;
[0349] (3) a step of forming a sealing layer on a semiconductor chip;
[0350] (4) a step of peeling the substrate and the temporary fixing film from the semiconductor chip;
[0351] (5) forming a rewiring formation layer as an insulating layer on the surface of the semiconductor chip from which the substrate and the temporary fixing film have been peeled off; and
[0352] (6) A step of forming a rewiring layer as a conductor layer on the rewiring formation layer.
[0353] -Process (1)-
[0354] The material used for the substrate is not particularly limited. Examples of the substrate include: silicon wafers; glass wafers; glass substrates; metal substrates such as copper, titanium, stainless steel, and cold-rolled steel sheets (SPCC); substrates (such as FR-4 substrates) in which epoxy resins are impregnated on glass fibers and heat-cured; and substrates composed of bismaleimide triazine resins (BT resins).
[0355] The temporary fixing film can be peeled off from the semiconductor chip in step (4), and the material is not particularly limited as long as it can temporarily fix the semiconductor chip. A commercially available product can be used as the temporary fixing film. Examples of commercially available products include REVALPHA manufactured by Nitto Denko Corporation.
[0356] -Process (2)-
[0357] The temporary fixation of semiconductor chips can be performed using a known device such as a flip chip bonder or a die bonder. The layout and number of semiconductor chips can be appropriately set according to the shape and size of the temporary fixation film, the number of target semiconductor packages to be produced, etc. For example, they can be arranged in a matrix of multiple rows and columns for temporary fixation.
[0358] -Process (3)-
[0359] A resin composition layer is formed on the semiconductor chip and cured (e.g., thermally cured) to form a sealing layer. The resin composition layer can be formed, for example, by laminating a resin composition layer of a resin sheet on the semiconductor chip or by coating the resin composition on the semiconductor chip.
[0360] For example, the stacking of semiconductor chip and resin sheet can be carried out by heating and pressing the resin sheet on the semiconductor chip from the support body side after removing the protective film of the resin sheet. As the heating and pressing component for heating and pressing the resin sheet on the semiconductor chip, for example, a heated metal plate (SUS end plate, etc.) or a metal roller (SUS roller, etc.) can be cited. It should be noted that it is preferred that the heating and pressing component is not directly pressed on the resin sheet, but is pressed through an elastic material such as heat-resistant rubber so that the resin sheet fully follows the surface unevenness of the semiconductor chip. The stacking of semiconductor chip and resin sheet can be implemented by vacuum lamination, and the stacking conditions can be the same as the stacking conditions described for the manufacturing method of the printed wiring board, and the preferred range can also be the same.
[0361] After lamination, the resin composition is thermally cured to form a sealing layer. The thermal curing conditions are the same as those described in the method for producing a printed wiring board.
[0362] The support of the resin sheet may be peeled off after the resin sheet is laminated on the semiconductor chip and thermally cured, or the support may be peeled off before the resin sheet is laminated on the semiconductor chip.
[0363] When the sealing layer is formed by applying the resin composition, the coating conditions may be the same as those for forming the resin composition layer described with respect to the resin sheet, and the preferred ranges may also be the same.
[0364] -Process (4)-
[0365] The method of peeling off the substrate and the temporary fixing film can be appropriately changed according to the material of the temporary fixing film, for example, there can be mentioned: a method of peeling off by heating the temporary fixing film to make it foam (or expand); and a method of peeling off by irradiating ultraviolet rays from the substrate side to reduce the adhesive force of the temporary fixing film, etc.
[0366] In the method of peeling off by heating the temporary fixing film to make it foam (or expand), the heating conditions are usually 100 to 250°C for 1 to 90 seconds or 5 to 15 minutes. In the method of peeling off by irradiating ultraviolet rays from the substrate side to reduce the adhesive force of the temporary fixing film, the irradiation amount of ultraviolet rays is usually 10 mJ / cm 2 ~1000mJ / cm 2 .
[0367] -Process (5)-
[0368] The material for forming the rewiring forming layer (insulating layer) is not particularly limited as long as the rewiring forming layer (insulating layer) has insulating properties. From the viewpoint of easily manufacturing a semiconductor chip package, ultraviolet curable resins and thermosetting resins are preferred. The above-mentioned resin composition or resin sheet can be used to form the rewiring forming layer.
[0369] After the rewiring formation layer is formed, via holes may be formed in the rewiring formation layer to provide interlayer connection between the semiconductor chip and the conductor layer described later. The via holes may be formed by a known method depending on the material of the rewiring formation layer.
[0370] -Process (6)-
[0371] The formation of the conductor layer on the rewiring formation layer can be carried out in the same manner as step (v) described in relation to the method for producing a printed wiring board. It should be noted that steps (5) and (6) may be repeated to alternately stack (build-up) the conductor layer (rewiring layer) and the rewiring formation layer (insulating layer).
[0372] When manufacturing a semiconductor chip package, the following steps may be further performed: (7) a step of forming a solder resist layer on a conductor layer (rewiring layer); (8) a step of forming bumps; (9) a step of cutting a plurality of semiconductor chip packages into individual semiconductor chip packages and singulating them. These steps may be performed according to various methods known to those skilled in the art and used in the manufacture of semiconductor chip packages.
[0373] When the above-mentioned resin composition or resin sheet is used to form a sealing layer or a rewiring formation layer, whether the semiconductor package is a fan-in (Fan-In) type package or a fan-out (Fan-Out) type package, a semiconductor chip package with very little transmission loss can be achieved. In addition, the semiconductor chip package can achieve low transmission loss in a high temperature environment. In one embodiment, the semiconductor chip package is a fan-out (Fan-Out) type package. The resin composition and resin sheet involved in the above-mentioned embodiment can be applied to both fan-out panel-level package (FO-PLP) and fan-out wafer-level package (FO-WLP). In one embodiment, the semiconductor package is a fan-out panel-level package (FOPLP). In another embodiment, the semiconductor package is a fan-out wafer-level package (FOWLP).
[0374] <Semiconductor devices>
[0375] A semiconductor device according to one embodiment of the present invention comprises a layer of a cured product of the resin composition according to the above-mentioned embodiment. The semiconductor device generally comprises the above-mentioned printed wiring board or semiconductor chip package. As semiconductor devices, various semiconductor devices for electrical products (e.g., computers, mobile phones, digital cameras, and televisions) and vehicles (e.g., motorcycles, cars, trams, ships, and airplanes) can be cited.
[0376] Example
[0377] The present invention is specifically described below by way of examples. The present invention is not limited to these examples. It should be noted that, below, "parts" and "%" indicating quantities refer to "parts by mass" and "% by mass" respectively, unless otherwise expressly stated. The temperature condition when the temperature is not particularly specified is room temperature (23°C). The pressure condition when the air pressure is not particularly specified is atmospheric pressure (1 atm).
[0378] <Mass spectrometry conditions>
[0379] In the examples and comparative examples described below, the samples were diluted to 1 mg / mL with tetrahydrofuran (THF) and measured by liquid chromatography-mass spectrometry (LC / MS) under the following conditions.
[0380] HPLC: ACQUITY UPLC (manufactured by Waters, Japan)
[0381] MS: SQ Detector2 (manufactured by Waters, Japan)
[0382] Column: ACQUITY UPLC BEH C8 1.7 μm, 2.1 mm × 50 mm (manufactured by Waters, Japan)
[0383] Mobile phase A: 2mmol ammonium acetate aqueous solution
[0384] Mobile phase B: 2-propanol / THF (80:20)
[0385] Mixing time and mixing ratio of mobile phase (A%): 0 min (50%) → 5 min (5%) → 12 min (5%) → 12.1 min (50%) → 14 min (50%)
[0386] Flow rate: 0.25mL / min
[0387] Analysis time: 14 minutes
[0388] Column temperature: 40°C
[0389] Ion mode: ESI (electrospray ionization) positive or negative
[0390] Ion polarity: positive detection mode or negative detection mode
[0391] Desolventizing gas flow rate: 700L / hour, 250℃
[0392] Cone gas: 70L / hour
[0393] Ion source heater: 150°C
[0394] <Method for measuring hydroxyl equivalent>
[0395] In the examples and comparative examples described below, the hydroxyl group equivalent was quantitatively determined by acetylation of the hydroxyl groups in the sample with acetic anhydride-pyridine in accordance with JIS-K0070, followed by hydrolysis and back titration of the remaining acetic acid.
[0396] <Example 1: Synthesis of α-methylbenzyl group-containing polyester resin (1a)>
[0397] (1-1) Synthesis of an α-methylbenzyl-containing aromatic dihydroxy compound (1x)
[0398]
[0399] In a four-mouth round-bottomed beaker equipped with a stirring device, a thermometer and a condenser, 224.0 g (1.4 moles) of 2,7-dihydroxynaphthalene (reagent), 291.2 g (2.8 moles) of styrene monomer (reagent), 5.2 g of p-toluenesulfonic acid monohydrate (reagent) as an acid catalyst and 1300 g of toluene as a reaction solvent were placed in a composition ratio of 2.0 in the theoretical structure shown in the above formula (1x), and the temperature was raised to 100°C while paying attention to heat generation. Then, it was reacted at 100°C for 6 hours. After that, the temperature was lowered to 60°C, 300 g of distilled water and an appropriate amount of 48% sodium hydroxide aqueous solution for neutralization were added, and the liquid was separated by standing, and the lower layer of by-product salt water layer was discarded. Furthermore, the same amount of distilled water was added, and after washing and purification twice, it was heated and azeotropic dehydration was performed. After the obtained solution was finely filtered to remove impurities, toluene was distilled under reduced pressure at a maximum temperature of 120°C to obtain 490 g of solid matter.
[0400] The hydroxyl equivalent of the solid material was measured according to the above-mentioned measurement method, and a value of 187 g / eq. (theoretical value: 184 g / eq.) was obtained.
[0401] In addition, the mass spectrum (negative ion mode) of the solid substance was measured according to the above-mentioned measurement method. In the mass spectrum, spectral peaks of m / z=263 corresponding to m=1, m / z=367 corresponding to m=2, and m / z=471 corresponding to m=3 were detected. In addition, the peak of the polynaphthalene ether structure obtained by etherifying dihydroxy compounds with each other was not detected.
[0402] From these analysis data, it was confirmed that the obtained solid material had the target molecular structure, that is, the structure of the α-methylbenzyl-modified aromatic dihydroxy compound (1x) involved in the theoretical structure represented by the above formula (1x).
[0403] (1-2) Esterification reaction: Synthesis of polyester resin (1a) containing α-methylbenzyl group
[0404]
[0405] In a four-mouth round bottom beaker equipped with a stirring device, a thermometer, a dropping funnel and a nitrogen blowing port, 441.6 g (2.4 mol of hydroxyl groups) of the α-methylbenzyl-modified aromatic dihydroxy compound (1x) obtained in the above step (1-1) were placed in a composition ratio such that the n value in the theoretical structure represented by the above formula (1a) was 1.0 and the active ester group equivalent was 229 g / eq., 345.6 g (2.4 mol) of 1-naphthol (reagent), 487.2 g (2.4 mol) of isophthaloyl chloride (reagent), 1.3 g of tetra-n-butylammonium bromide (reagent) and 1100 g of toluene were stirred while blowing nitrogen to completely dissolve. 771.7 g (4.8 mol) of a 25% aqueous solution of caustic soda was added dropwise over 2 hours at 30°C so as to finally raise the temperature to 60°C while paying attention to heat generation. After that, stirring was continued for 2 hours at 60°C, 300 g of distilled water was added, and the solution was allowed to stand for separation, and the lower by-product salt water layer was discarded. Furthermore, the same amount of distilled water was added, and the solution was washed and purified twice, and then heated for azeotropic dehydration. After the obtained solution was finely filtered to remove impurities, toluene was distilled under reduced pressure at a maximum temperature of 200°C to obtain 950 g of solid matter.
[0406] The mass spectrum (positive ion mode) of the obtained solid material was measured according to the above-mentioned measurement method. In the mass spectrum, spectral peaks of m / z=917 corresponding to m=2 / n=1 and m / z=1415 corresponding to m=2 / n=2 were detected. Based on these analytical data, it was confirmed that the obtained solid material had the target molecular structure, that is, the structure of the α-methylbenzyl-containing polyester resin (1a) involved in the theoretical structure shown in the above formula (1a).
[0407] <Example 2: Synthesis of α-methylbenzyl group-containing polyester resin (2a)>
[0408] (2-1) Synthesis of an α-methylbenzyl-containing aromatic dihydroxy compound (2x)
[0409]
[0410] 485 g of a solid substance was obtained in the same manner as in step (1-1) of Example 1 except that 2,7-dihydroxynaphthalene (reagent) was changed to 224.0 g (1.4 mol) of 1,6-dihydroxynaphthalene (reagent).
[0411] The hydroxyl equivalent of the solid material was measured according to the above-mentioned measurement method, and a value of 186 g / eq. (theoretical value: 184 g / eq.) was obtained.
[0412] In addition, the mass spectrum of the solid substance was measured according to the above-mentioned measurement method (negative ion mode). In the mass spectrum, spectral peaks of m / z=263 corresponding to m=1, m / z=367 corresponding to m=2, and m / z=471 corresponding to m=3 were detected.
[0413] From these analysis data, it was confirmed that the obtained solid substance had the target molecular structure, that is, the structure of the α-methylbenzyl-modified aromatic dihydroxy compound (2x) involved in the theoretical structure represented by the above formula (2x).
[0414] (2-2) Esterification reaction: Synthesis of polyester resin (2a) containing α-methylbenzyl group
[0415]
[0416] 930 g of a solid material was obtained in the same manner as in step (1-2) of Example 1 except that the α-methylbenzyl-modified aromatic dihydroxy compound (1x) was changed to 441.6 g (2.4 mol of hydroxyl groups) of the α-methylbenzyl-modified aromatic dihydroxy compound (2x).
[0417] The mass spectrum (positive ion mode) of the obtained solid material was measured according to the above-mentioned measurement method. In the mass spectrum, the spectral peaks of m / z=917 corresponding to m=2 / n=1 and m / z=1415 corresponding to m=2 / n=2 were detected. In addition, the peak of the polynaphthalene ether structure obtained by etherification of dihydroxy compounds was not detected. Based on these analytical data, it was confirmed that the obtained solid material had the target molecular structure, that is, the structure of the α-methylbenzyl-containing polyester resin (2a) involved in the theoretical structure shown in the above formula (2a).
[0418] <Example 3: Synthesis of α-methylbenzyl group-containing polyester resin (3a)>
[0419] (3-1) Synthesis of an α-methylbenzyl-containing aromatic dihydroxy compound (3x)
[0420]
[0421] 480 g of a solid substance was obtained in the same manner as in step (1-1) of Example 1 except that 2,7-dihydroxynaphthalene (reagent) was changed to 224.0 g (1.4 mol) of 1,5-dihydroxynaphthalene (reagent).
[0422] The hydroxyl equivalent of the solid material was measured according to the above-mentioned measurement method, and a value of 182 g / eq. (theoretical value: 184 g / eq.) was obtained.
[0423] In addition, the mass spectrum of the solid substance was measured according to the above-mentioned measurement method (negative ion mode). In the mass spectrum, spectral peaks of m / z=263 corresponding to m=1, m / z=367 corresponding to m=2, and m / z=471 corresponding to m=3 were detected.
[0424] From these analysis data, it was confirmed that the obtained solid material had the target molecular structure, that is, the structure of the α-methylbenzyl-modified aromatic dihydroxy compound (3x) involved in the theoretical structure represented by the above formula (3x).
[0425] (3-2) Esterification reaction: Synthesis of polyester resin (3a) containing α-methylbenzyl group
[0426]
[0427] 930 g of a solid material was obtained in the same manner as in step (1-2) of Example 1 except that the α-methylbenzyl-modified aromatic dihydroxy compound (1x) was changed to 441.6 g (2.4 mol of hydroxyl groups) of the α-methylbenzyl-modified aromatic dihydroxy compound (3x).
[0428] The mass spectrum (positive ion mode) of the obtained solid material was measured according to the above-mentioned measurement method. In the mass spectrum, the spectral peaks of m / z=917 corresponding to m=2 / n=1 and m / z=1415 corresponding to m=2 / n=2 were detected. In addition, the peak of the polynaphthalene ether structure obtained by etherification of dihydroxy compounds was not detected. Based on these analytical data, it was confirmed that the obtained solid material had the target molecular structure, that is, the structure of the polyester resin (3a) containing α-methylbenzyl group involved in the theoretical structure shown in the above formula (3a).
[0429] <Example 4: Synthesis of α-methylbenzyl group-containing polyester resin (4a)>
[0430]
[0431] In a four-mouth round-bottomed beaker equipped with a stirring device, a thermometer, a dropping funnel and a nitrogen blowing port, 441.6 g (2.4 mol of hydroxyl groups) of an α-methylbenzyl-modified aromatic dihydroxy compound (1x) obtained in the same manner as step (1-1) of Example 1 were placed in a composition ratio of 3.0 in the theoretical structure represented by the above formula (4a) and 246 g / eq., 136.0 g (0.8 mol) of 2-phenylphenol (reagent), 324.8 g (1.6 mol) of isophthaloyl chloride, 0.9 g of tetra-n-butylammonium bromide and 1000 g of toluene, and the mixture was stirred while blowing nitrogen to completely dissolve. 512.0 g (3.2 mol) of a 25% aqueous solution of caustic soda was added dropwise over 2 hours at 30°C while finally raising the temperature to 60°C with caution for heat generation. After that, stirring was continued for 2 hours at 60°C, 300 g of distilled water was added, and the solution was allowed to stand for separation, and the lower by-product salt water layer was discarded. Furthermore, the same amount of distilled water was added, and the solution was washed and purified twice, and then heated for azeotropic dehydration. After the obtained solution was finely filtered to remove impurities, toluene was distilled under reduced pressure at a maximum temperature of 200°C to obtain 708 g of solid matter.
[0432] The mass spectrum (positive ion mode) of the obtained solid material was measured according to the above-mentioned measurement method. In the mass spectrum, spectral peaks of m / z=969 corresponding to m=2 / n=1, m / z=1468 corresponding to m=2 / n=2, and m / z=1966 corresponding to m=2 / n=3 were detected. Based on these analytical data, it was confirmed that the obtained solid material had the target molecular structure, that is, the structure of the α-methylbenzyl-containing polyester resin (4a) involved in the theoretical structure shown in the above formula (4a).
[0433] <Example 5: Synthesis of α-methylbenzyl group-containing polyester resin (5a)>
[0434] (5-1) Synthesis of an α-methylbenzyl-containing aromatic dihydroxy compound (5x)
[0435]
[0436] In a four-mouth round-bottomed beaker equipped with a stirring device, a thermometer and a condenser, 300.0 g (1.5 mol) of bisphenol F (manufactured by Honshu Chemical Co., Ltd.), 312.0 g (3.0 mol) of styrene monomer (reagent), 6.1 g of p-toluenesulfonic acid monohydrate (reagent) as an acid catalyst and 1300 g of toluene as a reaction solvent were placed in a composition ratio such that the total value of m in the theoretical structure represented by the above formula (5x) was 2.0, and the temperature was raised to 100°C while paying attention to heat generation. Then, the reaction was allowed to proceed at 100°C for 6 hours. After that, the temperature was lowered to 60°C, 300 g of distilled water and an appropriate amount of 48% sodium hydroxide aqueous solution for neutralization were added, and the solution was allowed to stand for separation, and the lower layer of by-product salt water was discarded. Furthermore, the same amount of distilled water was added, and the solution was washed and purified twice, and then heated for azeotropic dehydration. After the obtained solution was finely filtered to remove impurities, toluene was distilled under reduced pressure at a maximum temperature of 120°C to obtain 550 g of a solid substance.
[0437] The hydroxyl equivalent of the solid substance was measured according to the above-mentioned measurement method, and a value of 207 g / eq. (theoretical value: 204 g / eq.) was obtained.
[0438] In addition, the mass spectrum (negative ion mode) of the solid component was measured according to the above-mentioned measurement method. In the mass spectrum, the spectral peaks of m / z=304 corresponding to the total value of m=1, m / z=409 corresponding to the total value of m=2, and m / z=513 corresponding to the total value of m=3 were detected. In addition, the peak of the polyether structure obtained by etherifying dihydroxy compounds with each other was not detected.
[0439] From these analysis data, it was confirmed that the obtained solid substance had the target molecular structure, that is, the structure of the α-methylbenzyl-modified aromatic dihydroxy compound (5x) involved in the theoretical structure represented by the above formula (5x).
[0440] (5-2) Esterification reaction: Synthesis of polyester resin (5a) containing α-methylbenzyl group
[0441]
[0442] In a four-mouth round bottom beaker equipped with a stirring device, a thermometer, a dropping funnel and a nitrogen blowing port, 489.6 g (2.4 mol of hydroxyl groups) of the α-methylbenzyl-modified aromatic dihydroxy compound (5x) obtained in the above step (5-1) were placed in a composition ratio of 1.0 in the theoretical structure represented by the following formula (5a) and 252 g / eq., 408.0 g (2.4 mol) of 2-phenylphenol (reagent), 487.2 g (2.4 mol) of isophthaloyl chloride (reagent), 1.4 g of tetra-n-butylammonium bromide (reagent) and 1250 g of toluene, and the mixture was stirred while blowing nitrogen to completely dissolve. 768.0 g (4.8 mol) of a 25% aqueous solution of caustic soda was added dropwise over 2 hours at 30°C while finally raising the temperature to 60°C with caution for heat generation. After that, stirring was continued at 60°C for 2 hours, 300 g of distilled water was added, and the solution was allowed to stand for separation, and the lower by-product salt water layer was discarded. Furthermore, the same amount of distilled water was added, and the solution was washed and purified twice, and then heated for azeotropic dehydration. After the obtained solution was finely filtered to remove impurities, toluene was distilled under reduced pressure at a maximum temperature of 200°C to obtain 785 g of solid matter.
[0443] The mass spectrum (positive ion mode) of the obtained solid material was measured according to the above-mentioned measurement method. In the mass spectrum, the spectral peaks of m / z=1009 corresponding to the total value of m=2 / n=1 and m / z=1548 corresponding to the total value of m=2 / n=2 were detected. Based on these analytical data, it was confirmed that the obtained solid material had the target molecular structure, that is, the structure of the α-methylbenzyl-containing polyester resin (5a) involved in the theoretical structure shown in the above formula (5a).
[0444] <Example 6: Synthesis of α-methylbenzyl group-containing polyester resin (6a)>
[0445]
[0446] In a four-mouth round-bottomed beaker equipped with a stirring device, a thermometer, a dropping funnel and a nitrogen blowing port, 441.6 g (2.4 mol of hydroxyl groups) of an α-methylbenzyl-modified aromatic dihydroxy compound (1x) obtained in the same manner as in step (1-1) of Example 1 were placed in a composition ratio such that n value in the theoretical structure represented by the above formula (6a) was 1.0 and the active ester group equivalent was 256 g / eq., 521.9 g (2.4 mol) of styrenated phenol (manufactured by Sanko Co., Ltd., 258 mgKOH / g), 487.2 g (2.4 mol) of isophthaloyl chloride (reagent), 1.3 g of tetra-n-butylammonium bromide (reagent) and 1100 g of toluene were stirred while blowing nitrogen and dissolved completely. 512.0 g (3.2 mol) of a 25% aqueous solution of caustic soda was added dropwise over 2 hours at 30°C while finally raising the temperature to 60°C with caution for heat generation. After that, stirring was continued for 2 hours at 60°C, 300 g of distilled water was added, and the solution was allowed to stand for separation, and the lower by-product salt water layer was discarded. Furthermore, the same amount of distilled water was added, and the solution was washed and purified twice, and then heated for azeotropic dehydration. After the obtained solution was finely filtered to remove impurities, toluene was distilled under reduced pressure at a maximum temperature of 200°C to obtain 708 g of solid matter.
[0447] The mass spectrum (positive ion mode) of the obtained solid material was measured according to the above-mentioned measurement method. In the mass spectrum, spectral peaks of m / z=1041 corresponding to m=2 / n=1 and m / z=1556 corresponding to m=2 / n=2 were detected. Based on these analytical data, it was confirmed that the obtained solid material had the target molecular structure, that is, the structure of the α-methylbenzyl-containing polyester resin (6a) involved in the theoretical structure shown in the above formula (6a).
[0448] <Example 7: Synthesis of α-methylbenzyl group-containing polyester resin (7a)>
[0449] (7-1) Synthesis of an α-methylbenzyl-containing aromatic dihydroxy compound (7x)
[0450]
[0451] In a four-mouth round bottom beaker equipped with a stirring device, a thermometer and a condenser, 495.0 g (1.5 mol) of dicyclopentadiene diphenol ("J-DPP-85", manufactured by JFE Chemical Co., Ltd., hydroxyl equivalent 165) was placed in a composition ratio in which the total value of m in the theoretical structure represented by the above formula (7x) was 1.0, 156.0 g (1.5 mol) of styrene monomer (reagent), 6.5 g of p-toluenesulfonic acid monohydrate (reagent) as an acid catalyst and 1200 g of toluene as a reaction solvent were placed, and the temperature was raised to 100° C. while paying attention to heat generation. Then, the reaction was allowed to proceed at 100° C. for 6 hours. After that, the temperature was lowered to 60° C., 300 g of distilled water and an appropriate amount of 48% sodium hydroxide aqueous solution for neutralization were added, and the liquid was separated by standing, and the lower by-product salt water layer was discarded. Furthermore, the same amount of distilled water was added, and after washing and purification were performed twice, it was heated and azeotropic dehydration was performed. After the obtained solution was subjected to precision filtration to remove impurities, toluene was distilled under reduced pressure at a maximum temperature of 120° C. to obtain 605 g of a solid substance.
[0452] The hydroxyl equivalent of the solid material was measured according to the above-mentioned measurement method, and a value of 214 g / eq. (theoretical value: 212 g / eq.) was obtained.
[0453] In addition, the mass spectrum (negative ion mode) of the solid substance was measured according to the above-mentioned measurement method. In the mass spectrum, the peaks of m / z=425 corresponding to the total value of m=1, m / z=529 corresponding to the total value of m=2, and m / z=633 corresponding to the total value of m=3 were detected. In addition, the peak of the polyether structure obtained by etherifying dihydroxy compounds with each other was not detected.
[0454] From these analysis data, it was confirmed that the obtained solid substance had the target molecular structure, that is, the structure of the α-methylbenzyl-modified aromatic dihydroxy compound (7x) involved in the theoretical structure represented by the above formula (7x).
[0455] (7-2) Esterification reaction: Synthesis of polyester resin (7a) containing α-methylbenzyl group
[0456]
[0457] In a four-mouth round-bottomed beaker equipped with a stirring device, a thermometer, a dropping funnel and a nitrogen blowing port, 645.6 g (2.4 mol of hydroxyl groups) of the α-methylbenzyl-modified aromatic dihydroxy compound (7x) obtained in the above step (7-1) were placed in a composition ratio such that the n value in the theoretical structure represented by the above formula (7a) was 1.0 and the active ester group equivalent was 269 g / eq., 225.9 g (2.4 mol) of phenol (reagent), 487.2 g (2.4 mol) of isophthaloyl chloride (reagent), 1.4 g of tetra-n-butylammonium bromide (reagent) and 1200 g of toluene were stirred while blowing nitrogen to completely dissolve. 768.0 g (4.8 mol) of a 25% aqueous solution of caustic soda was added dropwise over 2 hours at 30°C so as to finally raise the temperature to 60°C while paying attention to heat generation. After that, stirring was continued for 2 hours at 60°C, 300 g of distilled water was added, and the solution was allowed to stand for separation, and the lower by-product salt water layer was discarded. Furthermore, the same amount of distilled water was added, and the solution was washed and purified twice, and then heated for azeotropic dehydration. After the obtained solution was finely filtered to remove impurities, toluene was distilled under reduced pressure at a maximum temperature of 200°C to obtain 860 g of solid matter.
[0458] The mass spectrum (positive ion mode) of the obtained solid material was measured according to the above-mentioned measurement method. In the mass spectrum, spectral peaks of m / z=873 corresponding to the total value of m=1 / n=1 and m / z=1428 corresponding to the total value of m=1 / n=2 were detected. Based on these analytical data, it was confirmed that the obtained solid material had the target molecular structure, that is, the structure of the α-methylbenzyl-containing polyester resin (7a) involved in the theoretical structure shown in the above formula (7a).
[0459] <Example 8: Synthesis of α-methylbenzyl group-containing polyester resin (8a)>
[0460] (8-1) Synthesis of an α-methylbenzyl-containing aromatic dihydroxy compound (8x)
[0461]
[0462] In a four-mouth round-bottomed beaker equipped with a stirring device, a thermometer and a condenser, 279.3 g (1.5 mol) of 4,4'-biphenyl (reagent), 468.0 g (4.5 mol) of styrene monomer (reagent), 7.5 g of p-toluenesulfonic acid monohydrate (reagent) as an acid catalyst, and 750 g of dimethyl sulfoxide as a reaction solvent were placed in a composition ratio in which the total value of m in the theoretical structure shown in the above formula (8x) was 3.0, and the temperature was raised to 130°C while paying attention to heat generation. Then, it was reacted at 130°C for 48 hours. After that, the temperature was lowered to 60°C, 300 g of distilled water and an appropriate amount of 48% sodium hydroxide aqueous solution for neutralization were added, and the liquid was separated by standing, and the lower by-product salt water layer was discarded. Furthermore, the same amount of distilled water was added, and after washing and purification twice, it was heated and azeotropic dehydration was performed. After the obtained solution was subjected to microfiltration to remove impurities, toluene and dimethyl sulfoxide were distilled under reduced pressure at a maximum temperature of 120° C. to obtain 760 g of a solid substance.
[0463] The hydroxyl equivalent of the solid substance was measured according to the above-mentioned measurement method, and a value of 253 g / eq. (theoretical value: 249 g / eq.) was obtained.
[0464] In addition, the mass spectrum (negative ion mode) of the solid component was measured according to the above-mentioned measurement method. In the mass spectrum, the spectral peaks of m / z=290 corresponding to the total value of m=1, m / z=395 corresponding to the total value of m=2, and m / z=499 corresponding to the total value of m=3 were detected. In addition, the peak of the polyether structure obtained by etherifying dihydroxy compounds with each other was not detected.
[0465] From these analysis data, it was confirmed that the obtained solid substance had the target molecular structure, that is, the structure of the α-methylbenzyl-modified aromatic dihydroxy compound (8x) involved in the theoretical structure represented by the above formula (8x).
[0466] (8-2) Esterification reaction: Synthesis of polyester resin (8a) containing α-methylbenzyl group
[0467]
[0468] In a four-mouth round-bottomed beaker equipped with a stirring device, a thermometer, a dropping funnel and a nitrogen blowing port, 645.6 g (2.4 mol of hydroxyl groups) of the α-methylbenzyl-modified aromatic dihydroxy compound (8x) obtained in the above step (8-1) were placed in a composition ratio such that the n value in the theoretical structure represented by the above formula (8a) was 2.0 and the active ester group equivalent was 279 g / eq., 345.6 g (2.4 mol) of 1-naphthol (reagent), 487.2 g (2.4 mol) of isophthaloyl chloride (reagent), 1.5 g of tetra-n-butylammonium bromide (reagent) and 1300 g of toluene were placed, and the mixture was stirred while blowing nitrogen to completely dissolve. Then, 768.0 g (4.8 mol) of a 25% aqueous solution of caustic soda was added dropwise over 2 hours at 30°C so as to finally raise the temperature to 60°C while paying attention to heat generation. After that, stirring was continued for 2 hours at 60°C, 300 g of distilled water was added, and the solution was allowed to stand for separation, and the lower by-product salt water layer was discarded. Furthermore, the same amount of distilled water was added, and the solution was washed and purified twice, and then heated for azeotropic dehydration. After the obtained solution was finely filtered to remove impurities, toluene was distilled under reduced pressure at a maximum temperature of 200°C to obtain 810 g of solid matter.
[0469] The mass spectrum (positive ion mode) of the obtained solid material was measured according to the above-mentioned measurement method. In the mass spectrum, the peaks of m / z=943 corresponding to the total value of m=2 / n=1, m / z=1468 corresponding to the total value of m=2 / n=2, m / z=1047 corresponding to the total value of m=3 / n=1, and m / z=1676 corresponding to the total value of m=3 / n=2 were detected. Based on these analytical data, it was confirmed that the obtained solid material had the target molecular structure, that is, the structure of the polyester resin (8a) containing an α-methylbenzyl group involved in the theoretical structure shown in the above formula (8a).
[0470] <Comparative Example 1: Synthesis of benzyl group-containing polyester resin (9)>
[0471] (C1-1) Synthesis of aromatic dihydroxy compounds containing benzyl groups (9x)
[0472]
[0473] In a four-mouth round-bottomed beaker equipped with a stirring device, a thermometer and a condenser, 224.0g (1.4 mol) of 2,7-dihydroxynaphthalene, 302.4g (2.8 mol) of benzyl alcohol, and 5.2g of p-toluenesulfonic acid monohydrate (reagent) as an acid catalyst were placed, and the temperature was raised to 150°C while paying attention to the heat generation, and the generated water was distilled out of the system while stirring for 4 hours. After that, the temperature was lowered to 60°C, 300g of distilled water and an appropriate amount of 48% sodium hydroxide aqueous solution for neutralization were added, and the liquid was separated by standing, and the lower layer of by-product salt water layer was discarded. Furthermore, the same amount of distilled water was added, and after washing and purification twice, it was heated and azeotropic dehydration was performed. After the obtained solution was finely filtered to remove impurities, toluene was distilled under reduced pressure at a maximum temperature of 120°C to obtain 450g of solid matter.
[0474] The hydroxyl equivalent of the solid substance was measured according to the above-mentioned measurement method, and a value of 200 g / eq. was obtained.
[0475] In addition, the mass spectrum (negative ion mode) of the solid component was measured according to the above-mentioned measurement method. In the mass spectrum, spectral peaks of m / z=250 corresponding to the structure obtained by adding one benzyl group to 2,7-dihydroxynaphthalene, m / z=340 corresponding to the structure obtained by adding two benzyl groups, and m / z=430 corresponding to the structure obtained by adding three benzyl groups were confirmed. In addition, spectral peaks of m / z=392 corresponding to the structure obtained by adding one benzyl group to the dimer of 2,7-dihydroxynaphthalene generated by dehydration between two molecules of 2,7-dihydroxynaphthalene, m / z=483 corresponding to the structure obtained by adding two benzyl groups, m / z=573 corresponding to the structure obtained by adding three benzyl groups, and m / z=663 corresponding to the structure obtained by adding four benzyl groups were confirmed. Furthermore, spectral peaks of m / z=535 corresponding to a structure in which one benzyl group was added to a trimer of 2,7-dihydroxynaphthalene generated by dehydration between three molecules of 2,7-dihydroxynaphthalene, m / z=625 corresponding to a structure in which two benzyl groups were added, m / z=715 corresponding to a structure in which three benzyl groups were added, and m / z=805 corresponding to a structure in which four benzyl groups were added were confirmed.
[0476] From these analysis data, it was confirmed that the obtained solid material had a benzyl-modified dihydroxynaphthalene and a benzyl-modified dihydroxypolynaphthalene ether structure as represented by formula (9x).
[0477] (C1-2) Esterification reaction: Synthesis of polyester resin (9a) containing benzyl group
[0478]
[0479] In a four-mouth round-bottomed beaker equipped with a stirring device, a thermometer, a dropping funnel and a nitrogen blowing port, 480 g (2.4 mol of hydroxyl groups) of the benzyl-modified aromatic dihydroxy compound (9x) obtained in the above step (C1-1) were placed in a composition ratio such that the n value in the theoretical structure represented by the above formula (9a) was 2.0 and the active ester group equivalent was 247 g / eq., 345.6 g (2.4 mol) of 1-naphthol (reagent), 487.2 g (2.4 mol) of isophthaloyl chloride (reagent), 1.5 g of tetra-n-butylammonium bromide (reagent) and 1300 g of toluene were placed, and the mixture was stirred while blowing nitrogen to completely dissolve. Then, 768.0 g (4.8 mol) of a 25% aqueous solution of caustic soda was added dropwise over 2 hours at 30°C while finally raising the temperature to 60°C with caution for heat generation. After that, stirring was continued for 2 hours at 60°C, 300 g of distilled water was added, and the solution was allowed to stand for separation, and the lower by-product salt water layer was discarded. Furthermore, the same amount of distilled water was added, and the solution was washed and purified twice, and then heated for azeotropic dehydration. After the obtained solution was finely filtered to remove impurities, toluene was distilled under reduced pressure at a maximum temperature of 200°C to obtain 770 g of solid matter.
[0480] The mass spectrum (positive ion mode) of the obtained solid material was measured according to the above-mentioned measurement method. In the mass spectrum, spectral peaks of m / z=889 corresponding to p=0 / m=2 / n=1, m / z=1211 corresponding to p=1 / m=2 / n=1, and m / z=1360 corresponding to p=0 / m=2 / n=2 were detected. Based on these analytical data, it was confirmed that the obtained solid material had the target molecular structure, that is, the structure of the polyester resin (9a) of the benzyl-modified polynaphthalene ether structure involved in the theoretical structure shown in the above formula (9a).
[0481] <Examples 9 to 16 and Comparative Example 2>
[0482] (1) Preparation of resin composition
[0483] The synthesized polyester resins (1a) to (9a), bisphenol A type liquid epoxy resin ("850S" manufactured by DIC Corporation, epoxy equivalent 183 g / eq.), and biphenyl aralkyl type epoxy resin ("NC3000" manufactured by Nippon Kayaku Co., Ltd., epoxy equivalent 275 g / eq.) were melt-mixed at 150° C. in the composition shown in Table 1. Next, 4-dimethylaminopyridine ("DMAP" manufactured by Koroei Chemical Industry Co., Ltd.) was mixed to prepare a resin composition.
[0484] (2) Production of solidified products
[0485] The prepared resin composition was filled into a mold (100 mm×100 mm×0.5 mm) coated with a release agent, and heat-cured at 150° C. for 10 minutes to obtain a cured product. The cured product was taken out of the mold and further heat-cured at 200° C. for 3 hours to produce a sheet-shaped cured product.
[0486] (3) Evaluation of cured products
[0487] The evaluation test was carried out on the sheet-shaped cured product according to the following procedure.
[0488] <Measurement of dielectric properties (room temperature)>
[0489] The sheet-like cured product was cut into test pieces of a predetermined size, and the relative dielectric constant and dielectric loss tangent were measured at a measurement frequency of 5.8 GHz and 23° C. using a split cylinder resonator (“CR-710” manufactured by EM Labs) and a PNA microwave network analyzer (“N5227B” manufactured by Keysight). For each cured product, five test pieces were measured (n=5), and the average value was calculated.
[0490] <Measurement of dielectric properties (high temperature)>
[0491] The sheet-like cured product was cut into test pieces of a predetermined size, and the relative dielectric constant and dielectric loss tangent were measured at a measurement frequency of 10 GHz and 90° C. using a split cylinder resonator (“CR-710” manufactured by EM Labs) and a PNA microwave network analyzer (“N5227B” manufactured by Keysight). For each cured product, five test pieces were measured (n=5), and the average value was calculated.
[0492] (3) Results of Examples 9 to 16 and Comparative Example 2
[0493] The measurement results in Examples 9 to 16 and Comparative Example 2 are shown in Table 1. In Table 1, the unit of the amount of each component represents parts by mass. In Table 1, the meanings of the abbreviations are as follows.
[0494] Dk: relative dielectric constant.
[0495] Df: dielectric loss tangent.
[0496] [Table 1]
[0497] [Table 1. Results of Examples 9 to 16 and Comparative Example 2]
[0498]
[0499] <Examples 17 to 24 and Comparative Example 3>
[0500] (1) Preparation of resin composition varnish
[0501] The synthesized polyester resins (1a) to (9a), bisphenol A type liquid epoxy resin ("850S" manufactured by DIC Corporation, epoxy equivalent 183 g / eq.), biphenyl aralkyl type epoxy resin ("NC3000H" manufactured by Nippon Kayaku Co., Ltd., epoxy equivalent 291 g / eq.), 4-dimethylaminopyridine ("DMAP" manufactured by Korei Chemical Industry Co., Ltd.), phenoxy resin ("YL6954BH30" manufactured by Mitsubishi Chemical Corporation), spherical silica ("SO-C2" manufactured by ADMATECHS, average particle size 0.50 μm), methyl ethyl ketone (MEK) and cyclohexanone were mixed with the composition shown in Table 2 to prepare a resin composition varnish.
[0502] (2) Preparation of resin sheets
[0503] The prepared resin composition varnish was applied onto a polyethylene terephthalate film (38 μm thick, hereinafter referred to as “PET film”) using a die coater so that the thickness of the dried resin composition layer was 40 μm, and dried at 80° C. to 120° C. (100° C. on average) for 6 minutes to produce a resin sheet.
[0504] (3) Production of solidified products
[0505] The produced resin sheet was heated at 190° C. for 120 minutes to thermally cure the resin composition layer. Then, the PET film was peeled off to obtain a sheet-like cured product.
[0506] (4) Evaluation of cured product
[0507] The evaluation test was carried out on the sheet-shaped cured product according to the following procedure.
[0508] <Measurement of dielectric properties (high temperature)>
[0509] The sheet-shaped cured products produced in Examples 17 to 24 and Comparative Example 3 were subjected to a dielectric property evaluation test in the same manner as in Examples 9 to 16 and Comparative Example 2.
[0510] <Evaluation of stain removal performance>
[0511] (Base treatment of inner substrate)
[0512] As the inner substrate, a glass cloth-based epoxy resin double-sided copper-clad laminate with copper foil on the surface was prepared (copper foil thickness 18 μm, substrate thickness 0.8 mm, "R1515A" manufactured by Panasonic). The copper foil on the surface of the inner substrate was etched with a copper etching amount of 1 μm using a microetchant ("CZ8101" manufactured by MEC) to perform a roughening treatment. Afterwards, it was dried at 190° C. for 30 minutes.
[0513] (Lamination and curing of resin sheets)
[0514] The resin sheets obtained in the above-mentioned examples and comparative examples were laminated on both sides of the inner substrate using an intermittent vacuum pressure laminator (a two-stage laminator "CVP700" manufactured by Nikko-Materials) in such a manner that the resin composition layer was bonded to the inner substrate. The lamination was performed by reducing the pressure for 30 seconds to a pressure of 13 hPa or less, and then pressing at a temperature of 100° C. and a pressure of 0.74 MPa for 30 seconds.
[0515] Next, the laminated resin sheet was smoothed by hot pressing for 60 seconds at atmospheric pressure, 100°C, and a pressure of 0.5 MPa. It was then placed in an oven at 130°C and heated for 30 minutes, and then transferred to an oven at 170°C and heated for 30 minutes. The resin composition layer was cured by the above heating to obtain an insulating layer containing a cured product of the resin composition. Therefore, by the above operation, an intermediate substrate having a layer structure of PET film / insulating layer / inner substrate / insulating layer / PET film was obtained.
[0516] (Via Formation)
[0517] The insulating layer was processed using a CO2 laser processing machine (LK-2K212 / 2C) manufactured by Via Machinery, and a via hole was formed on the insulating layer. The above processing was performed under the conditions of a frequency of 2000 Hz, a pulse width of 3 μs, an output power of 0.95 W, and a number of shots of 3. In addition, the via hole formed had a top diameter (diameter) of 50 μm on the surface of the insulating layer and a diameter of 40 μm on the bottom surface of the insulating layer. The top diameter represents the diameter of the opening of the via hole. Furthermore, the PET film was peeled off afterwards.
[0518] (Roughening treatment)
[0519] The intermediate substrate was immersed in Swelling DipSecuriganth P manufactured by Atotech Japan as a swelling solution at 60°C for 10 minutes. Next, the intermediate substrate was immersed in Concentrate Compact P (KMnO4: 60 g / L, NaOH: 40 g / L aqueous solution) manufactured by Atotech Japan as a roughening solution at 80°C for 20 minutes. Thereafter, the intermediate substrate was immersed in Reduction solutionSecuriganth P manufactured by Atotech Japan as a neutralizing solution at 40°C for 5 minutes. The obtained intermediate substrate is referred to as evaluation substrate A.
[0520] (Evaluation of stain removal properties)
[0521] The bottom of the via of the evaluation substrate A was observed using a scanning electron microscope (SEM). Based on the image obtained by the observation, the maximum contamination length from the wall surface of the via bottom was measured and evaluated according to the following criteria. The maximum contamination length indicates the longest contamination length among the contaminations formed at the bottom of the via.
[0522] “○” The maximum contamination length is less than 5μm;
[0523] “×” means the maximum contamination length is more than 5 μm.
[0524] <Evaluation of Halo>
[0525] For evaluation substrate A, cross-sectional observation was performed using a FIB-SEM composite device ("SMI3050SE" manufactured by SII Nanotech). In detail, using FIB (focused ion beam), the insulating layer was cut into a cross section parallel to the thickness direction of the insulating layer and passing through the center of the bottom of the via hole. The cross section was observed by SEM. Based on the observed image, the bottom diameter and top diameter of the via hole were measured. The bottom diameter represents the diameter of the bottom of the via hole, and the top diameter represents the diameter of the via hole opening.
[0526] In addition, in the image observed by SEM, a gap portion formed by continuously peeling off the insulating layer from the copper foil of the inner substrate from the edge of the hole bottom was observed. Therefore, based on the observed image, the distance r1 from the center of the hole bottom to the edge of the hole bottom (equivalent to the inner radius of the gap portion) and the distance r2 from the center of the hole bottom to the end of the far side of the above-mentioned gap portion (equivalent to the outer radius of the gap portion) were measured, and the difference r2-r1 between these distances r1 and r2 was calculated as the halo distance from the edge of the hole bottom at the measurement location.
[0527] The above measurements were performed at 5 randomly selected vias. Then, the average value of the top diameters of the 5 vias was used as the top diameter Lt of the sample after the roughening treatment. In addition, the average value of the bottom diameters of the 5 vias was used as the bottom diameter Lb of the sample after the roughening treatment. Moreover, the average value of the halo distances of the 5 vias was used as the halo distance Wb from the bottom edge of the sample.
[0528] Based on the above measurement results, the halo ratio Hb (the ratio of the halo distance Wb from the bottom edge of the roughened hole to the bottom radius (Lb / 2) of the via hole after the roughening treatment, "Wb / (Lb / 2)") is calculated. If the halo ratio Hb is less than 50%, it is judged as "○", and if the halo ratio Ht is greater than 50%, it is judged as "×".
[0529] (5) Results of Examples 17 to 24 and Comparative Example 3
[0530] The measurement results in Examples 17 to 24 and Comparative Example 3 are shown in Table 2. In Table 2, the units of the amounts of the components represent parts by mass. In Table 2, the meanings of the abbreviations are as follows.
[0531] Dk: relative dielectric constant.
[0532] Df: dielectric loss tangent.
[0533] [Table 2]
[0534] [Table 2. Results of Examples 17 to 24 and Comparative Example 3]
[0535]
[0536] [discuss]
[0537] As shown in Tables 1 and 2, it was confirmed that when the resin composition contains the active ester resin of the present invention, a cured product having excellent dielectric properties at high temperatures can be obtained. In addition, it was confirmed that even when the active ester resin of the present invention is used as a resin crosslinking agent, a cured product having good dielectric properties at high temperatures can be obtained. Furthermore, according to the resin composition containing the active ester resin of the present invention, it was confirmed that a cured product having good detergency and small halo can usually be obtained.
Claims
1. An active ester resin containing one or more α-methylbenzyl groups in one molecule.
2. The active ester resin according to claim 1, comprising a partial structure represented by the following formula (I): In formula (I), Ar B Each independently represents a divalent organic group containing at least one aromatic ring, Ar C Each independently represents a divalent organic group containing at least one aromatic ring, * indicates a bond.
3. The active ester resin according to claim 1, which is represented by the following formula (II): In formula (II), Ar A Each independently represents a monovalent organic group containing at least one aromatic ring, Ar B Each independently represents a divalent organic group containing at least one aromatic ring, Ar C Each independently represents a divalent organic group containing at least one aromatic ring, Organic group Ar A 、Organic group Ar B and organic group Ar C At least one of the organic groups contains an α-methylbenzyl group, n represents a number greater than 0.
4. The active ester resin according to claim 2, wherein Organic group Ar C It represents a divalent hydrocarbon group containing at least one aromatic ring.
5. The active ester resin according to claim 2, wherein Organic group Ar C Contains α-methylbenzyl. The active ester resin according to claim 1 , comprising an aromatic ring to which an α-methylbenzyl group is bonded.
7. The active ester resin according to claim 6, wherein On average, 1 to 6 α-methylbenzyl groups are bonded to one aromatic ring to which an α-methylbenzyl group is bonded.
8. The active ester resin according to claim 1, wherein The content of the α-methylbenzyl group is in the range of 1% by mass to 60% by mass.
9. The active ester resin according to claim 1, which is a condensation reaction product of (X1) an aromatic polyhydroxy compound comprising (X1-1) a modified aromatic polyhydroxy compound containing an α-methylbenzyl group, (X2) an aromatic carboxylic acid compound or an aromatic acid halide compound, and (X3) an aromatic monohydroxy compound.
10. A method for producing an active ester resin, the method comprising reacting the following compounds: The present invention comprises (X1) an aromatic polyhydroxy compound containing (X1-1) a modified aromatic polyhydroxy compound having an α-methylbenzyl group, (X2) an aromatic carboxylic acid compound or an aromatic acid halide compound, and (X3) an aromatic monohydroxy compound.
11. A resin crosslinking agent comprising the active ester resin according to any one of claims 1 to 9. 12 . A resin composition comprising the active ester resin according to claim 1 and a crosslinkable resin.
13. The resin composition according to claim 12, wherein The crosslinkable resin includes one or more selected from thermosetting resins and radical polymerizable resins.
14. The resin composition according to claim 12, which is used for forming an insulating layer of a printed wiring board.
15. The resin composition according to claim 12, which is used for sealing a semiconductor chip.
16. A cured product of the resin composition according to claim 12.
17. A sheet-like laminated material comprising the resin composition according to claim 12.
18. A resin sheet comprising: a support and a resin composition layer formed on the support, in, The resin composition layer comprises the resin composition according to claim 12 .
19. A printed wiring board comprising an insulating layer comprising a cured product of the resin composition according to claim 12. 20 . A semiconductor chip package comprising a sealing layer comprising a cured product of the resin composition according to claim 12 . 21 . The semiconductor chip package of claim 20 , which is a fan-out package.
22. A semiconductor device comprising the printed wiring board according to claim 19.
23. A semiconductor device comprising the semiconductor chip package according to claim 20.
Citation Information
Patent Citations
Thermosetting resin composition, cured product of the same, active ester resin, semiconductor sealing material, prepreg, circuit board and build-up film
JP2012012534A
Nitrogen-containing heterocyclic compounds as FXR modulators
JP2020500211A
Thermosetting resin composition, cured product thereof, active ester resin, semiconductor sealing material, prepreg, printed circuit board, and build-up film
WO2012002119A1
Active ester resin, epoxy resin composition, cured product thereof, prepreg, circuit board, and build-up film
WO2014061450A1
Thermosetting resin composition, cured object obtained therefrom, and active ester resin for use in same
WO2016098488A1