Method for producing water-absorbent resin composition
By surface cross-linking of water-absorbent resin particles and spraying sulfite-based compounds and organic antioxidant aqueous solutions, the problems of gel deterioration and yellow coloring of water-absorbent resin in body fluids are solved, and high gel stability and performance are achieved Improvement.
Patent Information
- Application Number
- CN202380029630.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-30
- Filing Date
- 2023-03-28
- Publication Date
- 2024-11-08
AI Technical Summary
After absorbing body fluids such as human urine, water-absorbing resins are easily affected by body fluid components, resulting in gel deterioration, and the addition of sulfite compounds may cause increased dissolved components and yellow coloring at high temperatures and high humidity.
By spraying the sulfite-based compound aqueous solution and organic antioxidant aqueous solution of the water-absorbent resin particles treated with surface crosslinking, the increase in dissolved components of the water-absorbent resin particles caused by the sulfite-based compound and yellow coloring at high temperature and high humidity is inhibited. , improve gel stability.
It effectively inhibits the increase in dissolved components of water-absorbent resin particles and the yellow coloring under high temperature and high humidity, improves the stability of the gel, and ensures the performance of the water-absorbent resin composition in application.
Smart Images

Figure BDA0005055152780000351 
Figure HDA0005055152790000011 
Figure HDA0005055152790000012
Abstract
Description
Technical Field
[0001] The present invention relates to a method for producing a water-absorbent resin composition, and more particularly to a method for producing a water-absorbent resin composition constituting an absorbent body suitable for use in sanitary materials such as disposable diapers, sanitary napkins, and incontinence pads. Background Art
[0002] In recent years, water-absorbent resins have been widely used in the field of sanitary materials such as diapers, sanitary napkins, and incontinence pads.
[0003] As such a water-absorbing resin, a cross-linked product of a partially neutralized salt polymer of acrylic acid has excellent water absorption performance, and acrylic acid as a raw material thereof is easily available industrially, so it has many advantages such as stable quality, can be produced at low cost, and is unlikely to become corrupted or deteriorated. Therefore, it is considered to be a preferred water-absorbing resin. Prior art literature Patent Literature
[0004] Patent Document 1: Japanese Patent Application Publication No. 2005-29751 Summary of the invention Technical problem to be solved by the invention
[0005] The gel produced by water-absorbent resins absorbing body fluids such as human urine is affected by various components in the body fluids (e.g., vitamin C and iron in urine), and gel degradation is observed. Therefore, various additives (e.g., human urine stabilizers) are added and the production process of water-absorbent resins is improved.
[0006] For example, sulfite compounds as reducing agents can be expected to improve the gel stability of water-absorbent resins by acting as human urine stabilizers. However, the addition of sulfite compounds to water-absorbent resins may cause problems such as an increase in the dissolved components of the water-absorbent resins and yellowing under high temperature and high humidity.
[0007] Under such circumstances, a main object of the present invention is to provide a method for producing a water-absorbent resin composition having high gel stability while suppressing an increase in dissolved components of the water-absorbent resin caused by a sulfite compound and yellowing under high temperature and high humidity. Technical solutions for solving technical problems
[0008] The present inventors have conducted intensive research to solve the above problems. As a result, they have found that by spraying a sulfite compound aqueous solution and an organic antioxidant aqueous solution on water-absorbent resin particles subjected to surface crosslinking treatment, an increase in the dissolved components of the water-absorbent resin particles caused by the sulfite compound and yellowing under high temperature and high humidity can be suppressed, thereby obtaining a water-absorbent resin composition having high gel stability. The present invention was completed by further intensive research based on this finding.
[0009] That is, the present invention provides an invention having the following configuration. Item 1. A method for producing a water-absorbent resin composition, comprising: a step of spraying an aqueous solution of a sulfite compound onto water-absorbent resin particles subjected to a surface crosslinking treatment; and a step of spraying an aqueous solution of an organic antioxidant. Item 2. The method for producing a water-absorbent resin composition according to Item 1, wherein the sulfite compound comprises at least one selected from the group consisting of sodium sulfite, potassium sulfite, calcium sulfite, sodium bisulfite, potassium bisulfite, ammonium bisulfite, sodium pyrosulfite, and potassium pyrosulfite. Item 3. The method for producing a water-absorbent resin composition according to Item 1 or 2, wherein the organic antioxidant comprises at least one selected from ascorbic acids, isoascorbic acids, gallic acids, protocatechuic acids, benzimidazoles, and alkylhydroxyanisole compounds. Item 4. The method for producing a water-absorbent resin composition according to any one of Items 1 to 3, wherein the dissolved content of the water-absorbent resin particles determined by the following measurement method is 19 parts by mass or less. (Dissolved ingredients) 500 g of physiological saline in a 500 mL beaker is stirred with a stirring bar rotating at 600 rpm. The temperature of the physiological saline is set to 25°C. 2.000 g of water-absorbent resin particles are added thereto, and the dispersion containing the water-absorbent resin particles is stirred for 3 hours. The dispersion is filtered with a 75 μm standard sieve and the filtrate is recovered. 80 g of the obtained filtrate is measured into a weighed 100 mL beaker that has been kept constant at 140°C in advance. The filtrate in the beaker is heated in a hot air dryer at 140°C for 15 hours to remove moisture and measure the mass Wa (g) of the remaining solid content. Without placing the water-absorbent resin particles in the physiological saline, a blank test is performed in the same manner as above, and the mass Wb (g) of the solid content remaining in the beaker is measured. The dissolved component is calculated by the following formula. Dissolved component (mass %) = [((Wa-Wb) / 80) × 500 / 2] × 100 Item 5. The method for producing a water-absorbent resin composition according to any one of Items 1 to 4, wherein the spraying amount of the sulfite compound is 0.01 parts by mass or more and 3 parts by mass or less per 100 parts by mass of the water-absorbent resin particles. Item 6. The method for producing a water-absorbent resin composition according to any one of Items 1 to 5, wherein the spray amount of the organic antioxidant is 0.1 parts by mass or more and 20 parts by mass or less relative to 100 parts by mass of the sulfite compound. Item 7. The method for producing a water-absorbent resin composition according to any one of Items 1 to 6, wherein the water-absorbent resin particles have a physiological saline water retention capacity of 25 g / g or more and 60 g / g or less. Item 8. The method for producing a water-absorbent resin composition according to any one of Items 1 to 7, wherein the water-absorbent resin particles have a physiological saline water absorption capacity of 5 ml / g or more and 40 ml / g or less under a load of 4.14 kPa. Effects of the Invention
[0010] According to the present invention, it is possible to provide a method for producing a water-absorbent resin composition having high gel stability, while suppressing an increase in the dissolved components of water-absorbent resin particles caused by a sulfite compound and yellowing under high temperature and high humidity. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] Figure 1 Schematic diagram of the device for measuring the water absorption of physiological saline under a load of 4.14 kPa. Figure 2 This is a schematic diagram of a measuring apparatus used for measuring gel strength. DETAILED DESCRIPTION
[0012] In this specification, the term "comprising" includes "consisting essentially of" and "consisting of". In addition, in this specification, "(meth)acrylic acid" means "acrylic acid or methacrylic acid", and "(meth)acrylate / salt" means "acrylate / salt or methacrylate / salt". It should be noted that "water-soluble" means a solubility of 5% by mass or more in water at 25°C.
[0013] In addition, in this specification, the numerical value connected by "to" means a numerical range including the numerical values before and after "to" as the lower limit and upper limit. When multiple lower limits and multiple upper limits are described separately, any lower limit and upper limit can be selected and connected by "to".
[0014] 1. Method for producing water-absorbent resin composition The method for producing a water-absorbent resin composition of the present invention is characterized by comprising: a step of spraying a sulfite compound aqueous solution on water-absorbent resin particles subjected to surface crosslinking treatment; and a step of spraying an organic antioxidant aqueous solution. The water-absorbent resin composition produced by the method for producing a water-absorbent resin composition of the present invention having such characteristics suppresses the increase of dissolved components of the water-absorbent resin particles caused by the sulfite compound and yellowing under high temperature and high humidity, and has high gel stability. The water-absorbent resin composition of the present invention is described in detail below.
[0015] The method for producing a water-absorbent resin composition of the present invention comprises: a step of spraying a sulfite compound aqueous solution on water-absorbent resin particles subjected to surface crosslinking treatment (hereinafter, sometimes referred to as step (A)); and a step of spraying an organic antioxidant aqueous solution (hereinafter, sometimes referred to as step (B)). The order of step (A) and step (B) is not particularly limited. That is, the steps may be performed in the order of step (A) and step (B), or in the order of step (B) and step (A), or may be performed simultaneously. In the method for producing a water-absorbent resin composition of the present invention, for example, by first performing the step (A) of spraying a sulfite compound aqueous solution on water-absorbent resin particles subjected to surface crosslinking treatment, the sulfite compound aqueous solution permeates into the water-absorbent resin particles. Then, by performing the step (B) of spraying an organic antioxidant aqueous solution, the organic antioxidant aqueous solution further permeates into the water-absorbent resin particles, suppressing the increase of dissolved components of the water-absorbent resin composition caused by the sulfite compound and yellowing under high temperature and high humidity, and exerting high gel stability due to the sulfite compound. The step (A) and the step (B) may be performed only once or a plurality of times.
[0016] In the above-mentioned steps (A) and (B), as methods for spraying the aqueous solution, there are methods using a spray nozzle device, an ultrasonic device based on an ultrasonic vibrator, a method using a rotary atomization centrifugal spray device, etc. In the present invention, the method using a spray nozzle device is preferred. As the spray nozzle device, there is no particular limitation as long as it is a device capable of spraying the aqueous solution, and preferably a one-fluid type or two-fluid type sprayer having a spray pattern such as a flat spray, a hollow cone, or a full cone.
[0017] It should be noted that in the method for producing a water-absorbent resin composition of the present invention, if an aqueous solution containing a sulfite compound and an organic antioxidant is sprayed onto the surface-crosslinked water-absorbent resin particles, the sulfite compound and the organic antioxidant react in the aqueous solution, and the effect of the present invention cannot be achieved.
[0018] From the viewpoint of more appropriately exerting the effects of the present invention, preferred sulfite compounds include sodium sulfite, potassium sulfite, calcium sulfite, sodium hydrogen sulfite, potassium hydrogen sulfite, ammonium hydrogen sulfite, sodium pyrosulfite, and potassium pyrosulfite. The sulfite compound contained in the sulfite compound aqueous solution may be only one type or two or more types.
[0019] From the viewpoint of more appropriately exerting the effects of the present invention, in step (A), the spraying amount of the sulfite-based compound is preferably 0.01 parts by mass or more, more preferably 0.1 parts by mass or more, and even more preferably 0.2 parts by mass or more, relative to 100 parts by mass of the water-absorbent resin particles, and is preferably 3 parts by mass or less, more preferably 2 parts by mass or less, and even more preferably 1 part by mass or less, and the preferred range is 0.01 to 3 parts by mass, 0.1 to 2 parts by mass, etc.
[0020] In addition, from the viewpoint of more appropriately exerting the effects of the present invention, the concentration of the sulfite compound contained in the aqueous solution of the sulfite compound is preferably 1% by mass or more, more preferably 5% by mass or more, further preferably 10% by mass or more, and is preferably 25% by mass or less, more preferably 20% by mass or less, and the preferred range is 1 to 25% by mass, 10 to 20% by mass, etc.
[0021] The temperature at which the step (A) is performed is, for example, 10 to 90° C. Alternatively, the step (A) may be performed under atmospheric pressure.
[0022] From the viewpoint of more appropriately exerting the effect of the present invention, as the organic antioxidant, preferably ascorbic acid, isoascorbic acid, gallic acid, protocatechuic acid, benzimidazole and alkylhydroxyanisole can be mentioned. The organic antioxidant contained in the organic antioxidant aqueous solution can be only one kind, or two or more kinds.
[0023] From the viewpoint of more appropriately exerting the effects of the present invention, in step (B), the spraying amount of the organic antioxidant is preferably 0.0001 part by mass or more, more preferably 0.0005 part by mass or more, and even more preferably 0.001 part by mass or more, relative to 100 parts by mass of the water-absorbent resin particles, and is preferably 1 part by mass or less, more preferably 0.1 part by mass or less, and even more preferably 0.01 part by mass or less. The preferred range is 0.0001 to 1 part by mass, 0.001 to 0.01 part by mass, and the like.
[0024] From the viewpoint of more appropriately exerting the effects of the present invention, in step (B), the spray amount of the organic antioxidant is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, and further preferably 1 part by mass or more, relative to 100 parts by mass of the sulfite-based compound. It is preferably 20 parts by mass or less, more preferably 10 parts by mass or less, and further preferably 5 parts by mass or less. The preferred range is 0.1 to 20 parts by mass, 0.5 to 10 parts by mass, etc.
[0025] In addition, from the viewpoint of more appropriately exerting the effects of the present invention, the concentration of the organic antioxidant contained in the organic antioxidant aqueous solution is preferably 0.001 mass % or more, more preferably 0.01 mass % or more, and is preferably 10 mass % or less, more preferably 5 mass % or less, and the preferred range is 0.001 to 10 mass %, 0.01 to 5 mass %, etc.
[0026] The temperature at which the step (B) is performed is, for example, 10 to 90° C. Alternatively, the step (B) may be performed under atmospheric pressure.
[0027] After step (A) and step (B), it is preferred to include a step of drying the water-absorbent resin composition. The drying conditions are not particularly limited as long as they are conditions that can remove at least a portion of the water absorbed by the water-absorbent resin composition in step (A) and step (B), and for example, the composition can be dried by heating at a temperature of 100 to 150° C. for about 30 to 60 minutes. It should be noted that a drying step may or may not be provided between step (A) and step (B).
[0028] Next, the surface-crosslinked water-absorbing resin particles to be subjected to the steps (A) and (B) will be described in detail.
[0029] (Water-absorbent resin particles) The water-absorbent resin particles contained in the water-absorbent resin composition of the present invention are formed by cross-linking a polymer of a water-soluble ethylenically unsaturated monomer, i.e., a cross-linked polymer having a structural unit derived from a water-soluble ethylenically unsaturated monomer. In addition, the water-absorbent resin particles are surface cross-linked. It should be noted that the surface processing method may be, for example, the method described in the <Surface Cross-linking Step> described later.
[0030] From the viewpoint of more appropriately exerting the effects of the present invention, the physiological saline water retention capacity of the water-absorbent resin particles is preferably 25 g / g or more, more preferably 30 g / g or more, and is preferably 60 g / g or less, more preferably 55 g / g or less, and even more preferably 50 g / g or less. Preferred ranges are 25 to 60 g / g, 30 to 50 g / g, and the like.
[0031] In addition, from the viewpoint of more appropriately exerting the effects of the present invention, the water absorption amount of physiological saline under a load of 4.14 kPa of the water-absorbent resin particles is preferably 5 ml / g or more, more preferably 10 ml / g or more, and even more preferably 15 ml / g or more, and is preferably 40 ml / g or less, more preferably 35 ml / g or less, and even more preferably 30 ml / g or less, and the preferred range is 5 to 40 ml / g, 10 to 30 ml / g, etc.
[0032] The physiological saline water retention capacity and the physiological saline water absorption capacity under a load of 4.14 kPa of the water-absorbent resin particles are values measured by the methods described in Examples.
[0033] From the viewpoint of more appropriately exerting the effects of the present invention, the water absorption rate of the water-absorbent resin particles by a vortex method is preferably 60 seconds or less, more preferably 50 seconds or less, and even more preferably 40 seconds or less. It is preferably 1 second or more, more preferably 3 seconds or more, and even more preferably 10 seconds or more. The preferred range is 1 to 60 seconds, 3 to 40 seconds, etc.
[0034] The water absorption rate of the water-absorbent resin particles by a vortex method is a value measured by the method described in Examples.
[0035] The dissolved components of the water-absorbent resin particles are the proportion of compounds eluted from the inside or the surface of the water-absorbent resin particles when the water-absorbent resin particles absorb water in physiological saline, and are expressed as the proportion (%) of the dissolved components per 1 g of the water-absorbent resin particles. The dissolved components of the water-absorbent resin particles are preferably 19% by mass or less, more preferably 17% by mass or less, and further preferably 15% by mass or less, and are preferably 0% by mass or more, more preferably 5% by mass, and the preferred ranges are 0 to 19% by mass, 5 to 15% by mass, and the like.
[0036] The dissolved content of the water-absorbent resin particles is a value measured by the method described in Examples.
[0037] The water-absorbent resin is usually in a granular form. From the viewpoint of avoiding local absorption in the absorbent article and appropriately exerting the effect of the present invention, the median particle size of the water-absorbent resin particles is preferably 150 μm or more, 200 μm or more, 250 μm or more, 280 μm or more, 300 μm or more, or 350 μm or more. In addition, from the viewpoint of making the touch in the absorbent article comfortable and appropriately exerting the effect of the present invention, the median particle size is preferably 850 μm or less, 600 μm or less, 550 μm or less, 500 μm or less, 450 μm or less, or 400 μm or less. That is, the median particle size is preferably 150 to 850 μm, more preferably 200 to 600 μm, further preferably 250 to 500 μm, further preferably 300 to 450 μm, and further preferably 320 to 400 μm. The water-absorbent resin composition of the present invention preferably has a median particle size of 150 to 850 μm, more preferably 200 to 600 μm, further preferably 250 to 500 μm, further preferably 300 to 450 μm, and further preferably 320 to 400 μm.
[0038] It should be noted that the water-absorbent resin particles may be in a form of agglomeration of fine particles (primary particles) in addition to the form of each being composed of a single particle. The shape of the primary particles may be roughly spherical, irregularly shaped, broken, plate-like, etc. In the case of primary particles produced by reversed phase suspension polymerization, roughly spherical single particle shapes with smooth surface shapes such as true spheres, ellipsoids, etc. may be mentioned.
[0039] The median particle size of the water-absorbent resin particles can be measured using a JIS standard sieve, and specifically, is a value measured by the method described in Examples.
[0040] The polymerization method of the water-soluble ethylenically unsaturated monomer can use aqueous solution polymerization, emulsion polymerization, reversed phase suspension polymerization, etc. as representative polymerization methods. In the aqueous solution polymerization method, the water-soluble ethylenically unsaturated monomer aqueous solution is stirred and heated as needed to perform polymerization. In addition, in the reversed phase suspension polymerization method, the water-soluble ethylenically unsaturated monomer is heated in a hydrocarbon dispersion medium under stirring to perform polymerization.
[0041] An example of a method for producing the water-absorbent resin particles will be described below.
[0042] As a specific example of the method for producing water-absorbent resin particles, there can be mentioned a method comprising a step of performing polymerization in the presence of a radical polymerization initiator in a method for producing water-absorbent resin particles by subjecting a water-soluble ethylenically unsaturated monomer to reverse phase suspension polymerization in a hydrocarbon dispersion medium, and a step of surface crosslinking the hydrogel obtained by the polymerization in the presence of a surface crosslinking agent. It should be noted that in the method for producing water-absorbent resin particles of the present invention, an internal crosslinking agent may be added to the water-soluble ethylenically unsaturated monomer as needed to form a hydrogel having an internal crosslinked structure.
[0043] <Polymerization process> [Water-soluble ethylenically unsaturated monomer] Examples of water-soluble ethylenically unsaturated monomers include (meth)acrylic acid (in this specification, "acrylic acid" and "methacrylic acid" are collectively referred to as "(meth)acrylic acid". The same shall apply hereinafter) and its salts; 2-(meth)acrylamide-2-methylpropanesulfonic acid and its salts; nonionic monomers such as (meth)acrylamide, N,N-dimethyl(meth)acrylamide, 2-hydroxyethyl(meth)acrylate, N-hydroxymethyl(meth)acrylamide, and polyethylene glycol mono(meth)acrylate; and amino group-containing unsaturated monomers such as N,N-diethylaminoethyl(meth)acrylate, N,N-diethylaminopropyl(meth)acrylate, and diethylaminopropyl(meth)acrylamide, and their quaternary ammonium compounds. Among these water-soluble ethylenically unsaturated monomers, (meth)acrylic acid or its salts, (meth)acrylamide, and N,N-dimethylacrylamide are preferred from the viewpoint of easy industrial availability, and (meth)acrylic acid and its salts are more preferred. In addition, these water-soluble ethylenically unsaturated monomers may be used alone or in combination of two or more.
[0044] Among them, acrylic acid and its salts are widely used as raw materials for water-absorbent resin particles. These acrylic acid and / or its salts are sometimes copolymerized with the above-mentioned other water-soluble ethylenically unsaturated monomers and used. In this case, acrylic acid and / or its salts are preferably used as the main water-soluble ethylenically unsaturated monomer in an amount of 70 to 100 mol % relative to the total water-soluble ethylenically unsaturated monomers.
[0045] The water-soluble ethylenically unsaturated monomer can be dispersed in a hydrocarbon dispersion medium in the form of an aqueous solution and provided for reverse suspension polymerization. The water-soluble ethylenically unsaturated monomer can improve the dispersion efficiency in the hydrocarbon dispersion medium by forming an aqueous solution. The concentration of the water-soluble ethylenically unsaturated monomer in the aqueous solution is preferably in the range of 20% by mass to below the saturated concentration. In addition, as the concentration of the water-soluble ethylenically unsaturated monomer, it is more preferably 55% by mass or less, further preferably 50% by mass or less, and further preferably 45% by mass or less. On the other hand, as the concentration of the water-soluble ethylenically unsaturated monomer, it is more preferably 25% by mass or more, further preferably 30% by mass or more, and further preferably 35% by mass or more.
[0046] When the water-soluble ethylenically unsaturated monomer has an acid group such as (meth) acrylic acid, 2-(meth) acrylamide-2-methylpropanesulfonic acid, etc., a substance whose acid group is pre-neutralized by an alkaline neutralizer may be used as required. As such an alkaline neutralizer, alkali metal salts such as sodium hydroxide, sodium carbonate, sodium bicarbonate, potassium hydroxide, potassium carbonate, etc.; ammonia, etc. may be cited. In addition, in order to simplify the neutralization operation, these alkaline neutralizers may be used in the form of aqueous solutions. It should be noted that the above-mentioned alkaline neutralizers may be used alone or in combination of two or more.
[0047] The degree of neutralization of the water-soluble ethylenically unsaturated monomer by the alkaline neutralizing agent is preferably 10 to 100 mol %, more preferably 30 to 90 mol %, further preferably 50 to 85 mol %, and further preferably 70 to 80 mol % relative to all acid groups of the water-soluble ethylenically unsaturated monomer.
[0048] [Free Radical Polymerization Initiator] Examples of the radical polymerization initiator added in the polymerization step include persulfates such as potassium persulfate, ammonium persulfate, and sodium persulfate; peroxides such as methyl ethyl ketone peroxide, methyl isobutyl ketone peroxide, di-tert-butyl peroxide, tert-butyl isopropyl peroxide, tert-butyl peracetate, tert-butyl peroxyisobutyrate, tert-butyl peroxypivalate, and hydrogen peroxide; and 2,2'-azobis(2-amidinopropane) dihydrochloride, 2,2'-azobis[2-(N-phenylamidino)propane] Azo compounds such as dihydrochloride, 2,2'-azobis[2-(N-allylamidinyl)propane] dihydrochloride, 2,2'-azobis{2-[1-(2-hydroxyethyl)-2-imidazoline-2-yl]propane} dihydrochloride, 2,2'-azobis{2-methyl-N-[1,1-bis(hydroxymethyl)-2-hydroxyethyl]propionamide}, 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)-propionamide], 4,4'-azobis(4-cyanovaleric acid), etc. Among these free radical polymerization initiators, potassium persulfate, ammonium persulfate, sodium persulfate and 2,2'-azobis(2-amidinopropane) dihydrochloride are preferably used from the viewpoint of easy availability and easy handling. These free radical polymerization initiators can be used alone or in combination of two or more. Furthermore, the above-mentioned radical polymerization initiator may be used in combination with a reducing agent such as sodium sulfite, sodium hydrogen sulfite, ferrous sulfate, and L-ascorbic acid to be used as a redox polymerization initiator.
[0049] The amount of the radical polymerization initiator used is, for example, 0.00005 to 0.01 mol per 1 mol of the water-soluble ethylenically unsaturated monomer. By satisfying this amount, a violent polymerization reaction can be avoided and the polymerization reaction can be completed within a suitable time.
[0050] [Internal crosslinking agent] Examples of internal crosslinking agents include crosslinking agents for polymers of water-soluble ethylenically unsaturated monomers used for crosslinking, such as unsaturated polyesters obtained by reacting diols, triols and other polyols such as (poly)ethylene glycol [the expression "(poly)" indicates both the case with the prefix "poly" and the case without the prefix "poly". The same applies hereinafter], (poly)propylene glycol, 1,4-butanediol, 1,6-hexanediol, trimethylolpropane, (poly)glycerol with unsaturated acids such as (meth)acrylic acid, maleic acid, and fumaric acid; bisacrylamides such as N,N-methylenebisacrylamide; di(meth)acrylates or tri(meth)acrylates obtained by reacting polyepoxides with (meth)acrylic acid; and toluene diisocyanate. Di(meth)acrylic acid carbamoyl esters obtained by reacting polyisocyanates such as esters and hexamethylene diisocyanate with hydroxyethyl (meth)acrylate; compounds having two or more polymerizable unsaturated groups such as allylated starch, allylated cellulose, diallyl phthalate, N,N',N"-triallyl isocyanurate, and divinylbenzene; (poly)ethylene glycol diglycidyl ether, (poly)propylene glycol diglycidyl ether, (poly)glycerol diglycidyl ether Diglycidyl compounds such as triglycidyl compounds, polyglycidyl compounds such as epihalohydrin compounds such as epichlorohydrin, epibromohydrin, and α-methyl epichlorohydrin, compounds having two or more reactive functional groups such as isocyanate compounds such as 2,4-toluene diisocyanate and hexamethylene diisocyanate, 3-methyl-3-hydroxymethyloxetane, 3-ethyl-3-hydroxymethyloxetane, 3-butyl-3-hydroxymethyloxetane, 3-methyl-3-hydroxyethyloxetane, 3-ethyl-3-hydroxyethyloxetane, 3-butyl-3-hydroxyethyloxetane, etc. Oxetane compounds such as oxetane, etc. Among these internal crosslinking agents, polyglycidyl compounds are preferably used, and diglycidyl ether compounds are more preferably used, preferably (poly)ethylene glycol diglycidyl ether, (poly)propylene glycol diglycidyl ether, and (poly)glycerol diglycidyl ether. These internal crosslinking agents can be used alone or in combination of two or more.
[0051] The amount of the internal crosslinking agent used is preferably 0.000001 to 0.02 mol, more preferably 0.00001 to 0.01 mol, further preferably 0.00001 to 0.005 mol, and further preferably 0.00005 to 0.002 mol, based on 1 mol of the water-soluble ethylenically unsaturated monomer.
[0052] [Hydrocarbon dispersion medium] As hydrocarbon dispersion medium, for example, there can be mentioned: aliphatic hydrocarbons having 6 to 8 carbon atoms such as n-hexane, n-heptane, 2-methylhexane, 3-methylhexane, 2,3-dimethylpentane, 3-ethylpentane, and n-octane; alicyclic hydrocarbons such as cyclohexane, methylcyclohexane, cyclopentane, methylcyclopentane, trans-1,2-dimethylcyclopentane, cis-1,3-dimethylcyclopentane, and trans-1,3-dimethylcyclopentane; aromatic hydrocarbons such as benzene, toluene, and xylene. Among these hydrocarbon dispersion mediums, n-hexane, n-heptane, and cyclohexane are particularly preferably used from the viewpoint of being easily available industrially, having stable quality, and being inexpensive. These hydrocarbon dispersion mediums can be used alone or in combination of two or more. It should be noted that as an example of a mixture of hydrocarbon dispersion mediums, suitable results can also be obtained by using commercial products such as Exxsol heptane (manufactured by Exxon Mobil: hydrocarbons containing heptane and its isomers 75 to 85% by mass).
[0053] The amount of the hydrocarbon dispersion medium used is preferably 100 to 1500 parts by mass, more preferably 200 to 1400 parts by mass, relative to 100 parts by mass of the water-soluble ethylenically unsaturated monomer in the first stage, from the viewpoint of uniformly dispersing the water-soluble ethylenically unsaturated monomer and facilitating the control of the polymerization temperature. It should be noted that, as described later, the reversed phase suspension polymerization is carried out in one stage (single stage) or in multiple stages of two or more stages, and the first stage polymerization mentioned above refers to the first stage polymerization reaction in the single stage polymerization or the multistage polymerization (hereinafter the same).
[0054] [Dispersion stabilizer] (Surfactant) In the reverse phase suspension polymerization, a dispersion stabilizer may be used to improve the dispersion stability of the water-soluble ethylenically unsaturated monomer in the hydrocarbon dispersion medium. As the dispersion stabilizer, a surfactant may be used.
[0055] As surfactant, for example, sucrose fatty acid ester, polyglycerol fatty acid ester, sorbitan fatty acid ester, polyoxyethylene sorbitan fatty acid ester, polyoxyethylene glycerol fatty acid ester, sorbitol fatty acid ester, polyoxyethylene sorbitol fatty acid ester, polyoxyethylene alkyl ether, polyoxyethylene alkylphenyl ether, polyoxyethylene castor oil, polyoxyethylene hydrogenated castor oil, alkyl allyl formaldehyde condensation polyoxyethylene ether, polyoxyethylene polyoxypropylene block copolymer, polyoxyethylene polyoxypropylene alkyl ether, polyethylene glycol fatty acid ester, alkyl glucoside, N-alkyl glucamide, polyoxyethylene fatty acid amide, polyoxyethylene alkylamine, phosphate ester of polyoxyethylene alkyl ether, phosphate ester of polyoxyethylene alkyl allyl ether, etc. can be used. Among these surfactants, from the dispersion stability aspect of monomer, sorbitan fatty acid ester, polyglycerol fatty acid ester, sucrose fatty acid ester are particularly preferably used. These surfactants can be used alone or in combination of two or more.
[0056] The amount of the surfactant used is preferably 0.1 to 30 parts by mass, more preferably 0.3 to 20 parts by mass, based on 100 parts by mass of the water-soluble ethylenically unsaturated monomer in the first stage.
[0057] (Polymer dispersant) Furthermore, as a dispersion stabilizer used in the reverse phase suspension polymerization, a polymeric dispersant may be used together with the above-mentioned surfactant.
[0058] Examples of the polymer dispersant include maleic anhydride-modified polyethylene, maleic anhydride-modified polypropylene, maleic anhydride-modified ethylene-propylene copolymer, maleic anhydride-modified EPDM (ethylene-propylene-diene terpolymer), maleic anhydride-modified polybutadiene, maleic anhydride-ethylene copolymer, maleic anhydride-propylene copolymer, maleic anhydride-ethylene-propylene copolymer, maleic anhydride-butadiene copolymer, polyethylene, polypropylene, ethylene-propylene copolymer, oxidized polyethylene, oxidized polypropylene, oxidized ethylene-propylene copolymer, ethylene-acrylic acid copolymer, ethyl cellulose, ethyl hydroxyethyl cellulose, etc. Among these polymer dispersants, maleic anhydride-modified polyethylene, maleic anhydride-modified polypropylene, maleic anhydride-modified ethylene-propylene copolymer, maleic anhydride-ethylene copolymer, maleic anhydride-propylene copolymer, maleic anhydride-ethylene-propylene copolymer, polyethylene, polypropylene, ethylene-propylene copolymer, oxidized polyethylene, oxidized polypropylene, oxidized ethylene-propylene copolymer, etc. are particularly preferably used from the perspective of monomer dispersion stability. These polymer-based dispersants may be used alone or in combination of two or more.
[0059] The amount of the polymer dispersant used is preferably 0.1 to 30 parts by mass, more preferably 0.3 to 20 parts by mass, based on 100 parts by mass of the water-soluble ethylenically unsaturated monomer in the first stage.
[0060] [Other ingredients] In the method for producing water-absorbent resin particles, other components may be added to the aqueous solution containing the water-soluble ethylenically unsaturated monomer as necessary to carry out reverse phase suspension polymerization. As other components, various additives such as a thickener and a chain transfer agent may be added.
[0061] As an example, a thickener may be added to an aqueous solution containing a water-soluble ethylenically unsaturated monomer to perform reversed phase suspension polymerization. By adding a thickener and adjusting the viscosity of the aqueous solution, the median particle size obtained in the reversed phase suspension polymerization can be controlled.
[0062] As thickeners, for example, hydroxyethyl cellulose, hydroxypropyl cellulose, methyl cellulose, carboxymethyl cellulose, polyacrylic acid, polyacrylic acid (partially) neutralized product, polyethylene glycol, polyacrylamide, polyethylene imine, dextrin, sodium alginate, polyvinyl alcohol, polyvinyl pyrrolidone, polyethylene oxide, etc. It should be noted that if the stirring speed during polymerization is the same, there is a tendency that the higher the viscosity of the aqueous solution of the water-soluble ethylenically unsaturated monomer, the larger the primary particles and / or secondary particles of the obtained particles.
[0063] [Inverse suspension polymerization] When reverse phase suspension polymerization is performed, for example, a monomer aqueous solution containing a water-soluble ethylenically unsaturated monomer is dispersed in a hydrocarbon dispersion medium in the presence of a dispersion stabilizer. At this time, the dispersion stabilizer (surfactant, polymer dispersant) may be added before or after the monomer aqueous solution is added, provided that the dispersion stabilizer is added before the polymerization reaction is started.
[0064] Among them, it is preferred to disperse the monomer aqueous solution and then disperse the surfactant in the hydrocarbon dispersion medium in which the polymer dispersant is dispersed, and then perform polymerization, from the viewpoint of easily reducing the amount of the hydrocarbon dispersion medium remaining in the obtained water-absorbing resin particles.
[0065] Such reversed phase suspension polymerization may be carried out in one stage or in multiple stages of two or more stages. In addition, from the viewpoint of improving productivity, it is preferably carried out in two to three stages.
[0066] When carrying out reversed-phase suspension polymerization with multistages above two stages, after carrying out the reversed-phase suspension polymerization of the first stage, in the reaction mixture obtained by the first stage polyreaction, add water-soluble ethylenically unsaturated monomers and mix, carry out the reversed-phase suspension polymerization of the second stage later with the method identical with the first stage.In the reversed-phase suspension polymerization of each stage after the second stage, preferably except water-soluble ethylenically unsaturated monomers, the amount of the water-soluble ethylenically unsaturated monomers that free radical polymerization initiator adds during the reversed-phase suspension polymerization of each stage after the second stage is used as a benchmark, in the scope of the mol ratio of each above-mentioned composition relative to water-soluble ethylenically unsaturated monomers, add, carry out reversed-phase suspension polymerization.It should be noted that, in the polymerization after the second stage, as required, also internal crosslinking agent can be added in the water-soluble ethylenically unsaturated monomers.
[0067] The reaction temperature of the polymerization reaction is preferably 20 to 110° C., more preferably 40 to 90° C., from the viewpoint of rapidly advancing the polymerization and shortening the polymerization time to improve economic efficiency, and easily removing the polymerization heat to smoothly advance the reaction.
[0068] <Surface cross-linking process> Next, the water-absorbent resin particles of the present invention are obtained by adding a surface crosslinking agent to a hydrogel having an internal crosslinking structure obtained by polymerizing a water-soluble ethylenically unsaturated monomer and performing crosslinking (surface crosslinking reaction). The surface crosslinking reaction is preferably performed in the presence of a surface crosslinking agent after the water-soluble ethylenically unsaturated monomer is polymerized. In this way, by performing a surface crosslinking reaction on the hydrogel having an internal crosslinking structure after polymerization, the crosslinking density near the surface of the water-absorbent resin particles can be increased, thereby obtaining water-absorbent resin particles having improved various properties such as water absorption capacity under load.
[0069] As the surface crosslinking agent, there can be mentioned compounds having two or more reactive functional groups. For example, there can be mentioned: polyols such as ethylene glycol, propylene glycol, 1,4-butanediol, diethylene glycol, triethylene glycol, trimethylolpropane, glycerol, polyethylene glycol, polypropylene glycol, and polyglycerol; polyglycidyl compounds such as (poly)ethylene glycol diglycidyl ether, (poly)glycerol diglycidyl ether, (poly)glycerol triglycidyl ether, trimethylolpropane triglycidyl ether, (poly)propylene glycol polyglycidyl ether, and (poly)glycerol polyglycidyl ether; halogenated epoxy compounds such as epichlorohydrin, epibromohydrin, and α-methylepichlorohydrin; isocyanate compounds such as 2,4-toluene diisocyanate and hexamethylene diisocyanate; 3-methyl-3-hydroxymethyloxetane, 3-ethyl-3-hydroxymethyloxetane, 3-butyl-3-hydroxymethyloxetane, 3-methyl-3-hydroxyethyl Oxetane compounds such as oxetane, 3-ethyl-3-hydroxyethyloxetane, and 3-butyl-3-hydroxyethyloxetane; oxazoline compounds such as 1,2-ethylenebisoxazoline; carbonate compounds (such as alkylene carbonate) such as ethylene carbonate, propylene carbonate, 4,5-dimethyl-1,3-dioxolane-2-one, 4,4-dimethyl-1,3-dioxolane-2-one, 4-ethyl-1,3-dioxolane-2-one, 4-hydroxymethyl-1,3-dioxolane-2-one, 1,3-dioxane-2-one, 4-methyl-1,3-dioxane-2-one, 4,6-dimethyl-1,3-dioxane-2-one, and 1,3-dioxolane-2-one; hydroxyalkylamide compounds such as bis[N,N-di(β-hydroxyethyl)]adipamide. Among these surface crosslinking agents, preferred are polyglycidyl compounds such as (poly)ethylene glycol diglycidyl ether, (poly)glycerol diglycidyl ether, (poly)glycerol triglycidyl ether, trimethylolpropane triglycidyl ether, (poly)propylene glycol polyglycidyl ether, and (poly)glycerol polyglycidyl ether; and carbonate compounds (e.g., alkylene carbonates) such as ethylene carbonate, propylene carbonate, 4,5-dimethyl-1,3-dioxolane-2-one, 4,4-dimethyl-1,3-dioxolane-2-one, 4-ethyl-1,3-dioxolane-2-one, 4-hydroxymethyl-1,3-dioxolane-2-one, 1,3-dioxane-2-one, 4-methyl-1,3-dioxane-2-one, 4,6-dimethyl-1,3-dioxane-2-one, and 1,3-dioxolane-2-one. These surface cross-linking agents may be used alone or in combination of two or more.
[0070] The amount of the surface crosslinking agent used is preferably 0.00001 to 0.01 mol, more preferably 0.00005 to 0.005 mol, and even more preferably 0.0001 to 0.002 mol, based on 1 mol of the total amount of the water-soluble ethylenically unsaturated monomers used in the polymerization.
[0071] As a method for adding the surface crosslinking agent, the surface crosslinking agent can be added as it is or as an aqueous solution, or can be added as a solution using a hydrophilic organic solvent as a solvent as needed. Examples of the hydrophilic organic solvent include: lower alcohols such as methanol, ethanol, n-propanol, and isopropanol; ketones such as acetone and methyl ethyl ketone; ethers such as diethyl ether, dioxane, and tetrahydrofuran; amides such as N,N-dimethylformamide; sulfoxides such as dimethyl sulfoxide, etc. These hydrophilic organic solvents can be used alone, in combination of two or more, or as a mixed solvent with water.
[0072] As the time for adding the surface crosslinking agent, as long as the polymerization reaction of the water-soluble ethylenically unsaturated monomer is almost completely completed, it is preferably added in the presence of 1 to 400 parts by mass of water relative to 100 parts by mass of the water-soluble ethylenically unsaturated monomer, more preferably in the presence of 5 to 200 parts by mass of water, further preferably in the presence of 10 to 100 parts by mass of water, and further preferably in the presence of 20 to 60 parts by mass of water. It should be noted that the amount of water refers to the total amount of water contained in the reaction system and the water used as needed when adding the surface crosslinking agent.
[0073] The reaction temperature in the surface crosslinking reaction is preferably 50 to 250° C., more preferably 60 to 180° C., further preferably 60 to 140° C., and further preferably 70 to 120° C. The reaction time in the surface crosslinking reaction is preferably 1 to 300 minutes, and more preferably 5 to 200 minutes.
[0074] <Drying process> After the above-mentioned reversed phase suspension polymerization, a drying step may be included in which water, hydrocarbon dispersion medium, etc. are removed by distillation by applying energy such as heat from the outside. In the case of dehydrating the hydrogel after the reversed phase suspension polymerization, the system in which the hydrogel is dispersed in the hydrocarbon dispersion medium is heated, thereby temporarily distilling water and the hydrocarbon dispersion medium out of the system by azeotropic distillation. At this time, if only the hydrocarbon dispersion medium removed by distillation is returned to the system, continuous azeotropic distillation can be performed. In this case, the temperature in the system during drying is maintained below the temperature of azeotropy with the hydrocarbon dispersion medium, so it is preferred from the viewpoint of not easily causing the resin to deteriorate. Next, water and hydrocarbon dispersion medium are removed by distillation to obtain water-absorbent resin particles. By controlling the treatment conditions of the drying step after the polymerization and adjusting the dehydration amount, the various properties of the obtained water-absorbent resin particles can be controlled.
[0075] In the drying process, the drying treatment by distillation may be carried out under normal pressure or under reduced pressure. In addition, from the viewpoint of improving the drying efficiency, it may be carried out under a stream of nitrogen or the like. When the drying treatment is carried out under normal pressure, the drying temperature is preferably 70°C to 250°C, more preferably 80°C to 180°C, further preferably 80°C to 140°C, and further preferably 90°C to 130°C. In addition, when the drying treatment is carried out under reduced pressure, the drying temperature is preferably 40°C to 160°C, and more preferably 50°C to 110°C.
[0076] The water content of the water-absorbing resin particles obtained by the production method of the present invention is preferably 20 mass % or less, more preferably 15 mass % or less, further preferably 10 mass % or less, and preferably in the range of 1 to 10 mass %.
[0077] It should be noted that, when a surface crosslinking step using a surface crosslinking agent is performed after polymerization of the monomers by reverse phase suspension polymerization, the drying step using distillation is performed after the surface crosslinking step is completed. Alternatively, the surface crosslinking step and the drying step may be performed simultaneously.
[0078] The water-absorbent resin composition of the present invention may contain additives according to the purpose. Examples of such additives include inorganic powders, surfactants, oxidants, reducing agents, free radical chain inhibitors, antioxidants, antibacterial agents, and the like. For example, by adding 0.05 to 5 parts by mass of amorphous silica as an inorganic powder relative to 100 parts by mass of the water-absorbent resin particles, the fluidity of the water-absorbent resin composition can be further improved. It should be noted that the above-mentioned additives are preferably hydrophilic or water-soluble.
[0079] In the water-absorbent resin composition of the present invention, the content of the water-absorbent resin particles (excluding additives) is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more.
[0080] The physiological saline water retention capacity of the water-absorbent resin composition obtained by the production method of the present invention is preferably 25 g / g or more, more preferably 30 g / g or more, and is preferably 60 g / g or less, more preferably 55 g / g or less, and even more preferably 50 g / g or less. The preferred range is 25 to 60 g / g, 30 to 50 g / g, etc.
[0081] The water-absorbent resin composition obtained by the production method of the present invention preferably has a physiological saline water absorption capacity of 5 ml / g or more under a load of 4.14 kPa, more preferably 10 ml / g or more, and even more preferably 15 ml / g or more, and is preferably 40 ml / g or less, more preferably 35 ml / g or less, and even more preferably 30 ml / g or less, and the preferred range is 5 to 40 ml / g, 10 to 30 ml / g, etc.
[0082] The physiological saline water retention capacity and the physiological saline water absorption capacity under a load of 4.14 kPa of the water-absorbent resin composition are values measured by the methods described in Examples, respectively.
[0083] From the viewpoint of more appropriately exerting the effects of the present invention, the water absorption rate of the water-absorbent resin composition by a vortex method is preferably 60 seconds or less, more preferably 50 seconds or less, and even more preferably 40 seconds or less. It is preferably 1 second or more, more preferably 3 seconds or more, and even more preferably 10 seconds or more. Preferred ranges are 1 to 60 seconds, 3 to 40 seconds, and the like.
[0084] The water absorption rate of the water-absorbent resin composition by a vortex method is a value measured by the method described in Examples.
[0085] The dissolved content of the water-absorbent resin composition obtained by the production method of the present invention is preferably 19% by mass or less, more preferably 17% by mass or less, and even more preferably 15% by mass or less. It is preferably 0% by mass or more, more preferably 5% by mass or more, and the preferred range is 0 to 19% by mass, 5 to 15% by mass, etc.
[0086] The dissolved content of the water-absorbent resin composition is a value measured by the method described in Examples.
[0087] The "yellowness" of the water-absorbent resin composition of the present invention evaluated by the method described in Examples is preferably 39 or less, more preferably 36 or less, and even more preferably 33 or less. The lower limit of the yellowness is 5, for example.
[0088] The "initial value of gel strength" of the water-absorbent resin composition of the present invention evaluated by the method described in the Examples is preferably 5000 N / m 2 More than 6000 N / m 2 More than, more preferably 6500N / m 2 It should be noted that the upper limit of the initial value of the gel strength is, for example, 20000 N / m 2 .
[0089] The water-absorbent resin composition of the present invention preferably has a "gel strength after standing at 37° C. for 28 hours" evaluated by the method described in the Examples of 5000 N / m 2 More than 6000 N / m 2 It should be noted that the upper limit of the gel strength is, for example, 20000 N / m 2 .
[0090] 2. Absorbents and absorbent articles The water-absorbent resin composition of the present invention constitutes an absorbent body used in sanitary materials such as sanitary products and disposable diapers, and is suitable for use in absorbent articles including the absorbent body.
[0091] Here, the absorbent using the water-absorbent resin composition of the present invention includes the water-absorbent resin composition of the present invention. The absorbent may further include hydrophilic fibers. As the composition of the absorbent, there can be cited a sheet structure in which the water-absorbent resin composition is fixed on a non-woven fabric or between a plurality of non-woven fabrics, a mixed dispersion obtained by mixing the water-absorbent resin composition and the hydrophilic fibers in a uniform composition, a sandwich structure in which the water-absorbent resin composition is sandwiched between layered hydrophilic fibers, and a structure in which the water-absorbent resin composition and the hydrophilic fibers are wrapped with a paper towel. It should be noted that other components may be added to the absorbent, such as adhesive adhesives such as heat-fusible synthetic fibers, hot-melt adhesives, and adhesive emulsions for improving the shape retention performance of the absorbent.
[0092] The content of the water-absorbent resin composition in the absorbent body is preferably 5 to 100% by mass, more preferably 10 to 95% by mass, further preferably 20 to 90% by mass, and further preferably 30 to 80% by mass.
[0093] Examples of hydrophilic fibers include cellulose fibers such as cotton pulp, mechanical pulp, chemical pulp, and semi-chemical pulp obtained from wood, artificial cellulose fibers such as rayon and cellulose acetate, and fibers made of synthetic resins such as polyamide, polyester, and polyolefin obtained by hydrophilization treatment. The average fiber length of the hydrophilic fibers is usually 0.1 to 10 mm, or 0.5 to 5 mm.
[0094] The absorbent article of the present invention can be prepared by holding an absorbent body using the water-absorbent resin composition of the present invention between a liquid-permeable sheet (top sheet) through which liquid can pass and a liquid-impermeable sheet (back sheet) through which liquid cannot pass. The liquid-permeable sheet is arranged on the side in contact with the body, and the liquid-impermeable sheet is arranged on the side opposite to the side in contact with the body.
[0095] Examples of liquid-permeable sheets include air-through, spunbond, chemically bonded, needle-punched nonwoven fabrics and porous synthetic resin sheets made of fibers such as polyethylene, polypropylene, and polyester. Examples of liquid-impermeable sheets include synthetic resin films made of resins such as polyethylene, polypropylene, and polyvinyl chloride. Example
[0096] The present invention will be described in detail below with reference to Examples and Comparative Examples, but the present invention is not limited to the Examples.
[0097] The water-absorbent resin particles obtained in the following preparation examples and the water-absorbent resin compositions obtained in the examples and comparative examples were evaluated by the following various tests. Unless otherwise specified, the measurements were performed under an environment of a temperature of 25±2° C. and a humidity of 50±10%.
[0098] [Manufacturing of water-absorbent resin particles] <Production Example 1> A round-bottomed cylindrical separable flask with an inner diameter of 11 cm and a volume of 2 L and equipped with stirring blades having four inclined blades with a blade diameter of 5 cm in two stages was prepared as a reflux cooler, a dropping funnel, a nitrogen inlet pipe, and a stirrer. In this flask, 293 g of n-heptane as a hydrocarbon dispersion medium was taken, 0.736 g of maleic anhydride-modified ethylene-propylene copolymer (Mitsui Chemicals, Inc., HI-WAX1105A) as a polymer dispersant was added, and the temperature was raised to 80° C. while stirring to dissolve the dispersant, and then cooled to 50° C. On the other hand, 92.0 g (1.03 mol) of an 80.5 mass % aqueous solution of acrylic acid as a water-soluble ethylenically unsaturated monomer was taken in a beaker having an internal volume of 300 mL, and 147.7 g of a 20.9 mass % aqueous solution of sodium hydroxide was added dropwise while cooling with ice water. After 75 mol % neutralization, 0.092 g of hydroxyethyl cellulose (Sumitomo Seika Co., Ltd., HEC AW-15F) as a thickener, 0.0736 g (0.272 mmol) of potassium persulfate as a water-soluble free radical polymerization agent, and 0.010 g (0.057 mmol) of ethylene glycol diglycidyl ether as an internal crosslinking agent were added and dissolved to prepare an aqueous liquid of the first stage. Then, the aqueous liquid prepared as above was added to a separable flask and stirred for 10 minutes. Then, a surfactant solution of 0.736 g of HLB3 sucrose stearate (Mitsubishi Chemical Foods Co., Ltd., Ryoto Sugar Ester S-370) dissolved in 6.62 g of n-heptane as a surfactant was further added to a 20 mL-tube bottle. The system was fully substituted with nitrogen while the stirrer speed was set to 550 rpm for stirring. The flask was immersed in a 70°C water bath for heating and polymerization was carried out for 60 minutes to obtain a first-stage polymerization slurry.
[0099] On the other hand, in another beaker having an internal volume of 500 mL, 128.8 g (1.43 mol) of an 80.5 mass % aqueous solution of acrylic acid as a water-soluble ethylenically unsaturated monomer was taken, and while cooling with ice water, 159.0 g of a 27 mass % aqueous solution of sodium hydroxide was added dropwise, and after 75 mol % neutralization, 0.103 g (0.381 mmol) of potassium persulfate as a water-soluble free radical polymerization initiator and 0.0116 g (0.067 mmol) of ethylene glycol diglycidyl ether as an internal crosslinking agent were added and dissolved to prepare an aqueous liquid of the second stage.
[0100] While stirring with the stirrer set at 1000 rpm, the interior of the separable flask system was cooled to 27°C, and then the entire amount of the aqueous liquid of the second stage was added to the polymerization slurry liquid of the first stage. After the interior of the system was replaced with nitrogen for 30 minutes, the flask was immersed in a water bath at 70°C again to raise the temperature, and a polymerization reaction was carried out for 60 minutes to obtain a hydrogel polymer.
[0101] Then, the flask was immersed in an oil bath set at 125° C., and 253.9 g of water was discharged to the outside of the system by azeotropic distillation of n-heptane and water while refluxing n-heptane. Then, 4.42 g (0.507 mmol) of a 2% by mass aqueous solution of ethylene glycol diglycidyl ether as a surface crosslinking agent was added to the flask, and the mixture was kept at 83° C. for 2 hours.
[0102] Then, n-heptane was evaporated and dried at 125°C, and the mixture was passed through a sieve with an aperture of 850 μm to obtain 217.2 g of water-absorbent resin particles (1). The water-absorbent resin particles (1) had a saline water retention capacity of 42 g / g and a saline water absorption capacity of 15 mL / g under a load of 4.14 kPa.
[0103] <Production Example 2> 221.9 g of water-absorbent resin particles (2) were obtained by the same operation as in Production Example 1 except that the amount of water discharged to the outside of the system by azeotropic distillation of n-heptane and water was changed from 253.9 g to 265.9 g. The water-absorbent resin particles (2) had a water retention capacity of 51 g / g in physiological saline and a water absorption capacity of 13 mL / g in physiological saline under a load of 4.14 kPa.
[0104] <Production Example 3> 222.1 g of water-absorbent resin particles (3) were obtained by the same operation as in Production Example 1 except that the amount of water discharged to the outside of the system by azeotropic distillation of n-heptane and water was changed from 253.9 g to 240.7 g in Production Example 1. The water retention capacity of the water-absorbent resin particles (3) was 32 g / g in physiological saline, and the water absorption capacity of the physiological saline under a load of 4.14 kPa was 30 mL / g.
[0105] [Production of water-absorbent resin composition] <Example 1> 20 g of the water-absorbent resin particles (1) obtained in Production Example 1 were weighed into a round-bottomed cylindrical separable flask having an inner diameter of 11 cm and equipped with an anchor-type stirring blade made of fluororesin. Next, 0.2 g of a 20% by mass sodium sulfite aqueous solution was taken with a 3 mL syringe while stirring at 300 rpm, and a fine atomizer (Fine Atomizer Oral) (Yoshikawa Chemicals Co., Ltd.) was set at the tip of the syringe, and sprayed in the separable flask for 1 second. Next, 0.2 g of a 1% by mass L(+)-ascorbic acid aqueous solution was sprayed in the same manner as above, and stirred for 10 minutes to obtain a mixture. After heating the mixture at 100° C. for 30 minutes, 0.5 parts by mass of amorphous silica (Tokusil NP-S, Oriental Silicas Corporation) was further mixed with 100 parts by mass of the water-absorbent resin particles (1) to obtain a water-absorbent resin composition (1).
[0106] <Example 2> In Example 1, the same operation as in Example 1 was carried out, except that the order of spraying and adding the aqueous solutions was changed from 0.2 g of a 20 mass % sodium sulfite aqueous solution and then 0.2 g of a 1 mass % L(+)-ascorbic acid aqueous solution to 0.2 g of a 1 mass % L(+)-ascorbic acid aqueous solution and then 0.2 g of a 20 mass % sodium sulfite aqueous solution, to obtain a water-absorbent resin composition (2).
[0107] <Example 3> In Example 1, the same operation as in Example 1 was carried out except that 0.2 g of the 1 mass % L(+)-ascorbic acid aqueous solution was changed to 0.2 g of the 0.2 mass % L(+)-ascorbic acid aqueous solution to obtain a water-absorbent resin composition (3).
[0108] <Example 4> In Example 1, the same operation as in Example 1 was carried out except that 0.2 g of the 1 mass % L(+)-ascorbic acid aqueous solution was changed to 0.5 g of the 0.02 mass % L(+)-ascorbic acid aqueous solution to obtain a water-absorbent resin composition (4).
[0109] <Example 5> In Example 1, the same operation as in Example 1 was carried out except that the amount of the 20 mass % sodium sulfite aqueous solution added was changed from 0.2 g to 2 g, and the 1 mass % L(+)-ascorbic acid aqueous solution was changed from 0.2 g to 0.2 g of the 2 mass % L(+)-ascorbic acid aqueous solution. A water-absorbent resin composition (5) was obtained.
[0110] <Example 6> 20 g of the water-absorbent resin particles (1) obtained in Production Example 1 were weighed into a round-bottomed cylindrical separable flask having an inner diameter of 11 cm and equipped with an anchor-type stirring blade made of fluororesin. Next, 2 g of a 20% by mass sodium sulfite aqueous solution was taken with a 3 mL syringe while stirring at 300 rpm, and a mouth fine atomizer (Yoshikawa Chemicals Co., Ltd.) was set at the tip of the syringe, and sprayed into the separable flask in 1 second. Next, 0.2 g of a 2% by mass L(+)-ascorbic acid aqueous solution was sprayed in the same manner as above, and stirred for 10 minutes to obtain a mixture. The mixture was heated at 100° C. for 30 minutes to obtain a heated mixture. 0.7 parts by mass of diethylenetriaminepentaacetic acid (DTPA) was added as a powder to 100 parts by mass of the heated mixture, and mixed for 30 minutes using a cross-rotation mixer manufactured by Meiwa Industry Co., Ltd. (conditions: revolution speed 50 rpm, rotation speed 50 rpm), and further 0.5 parts by mass of amorphous silica (Tokusil NP-S manufactured by Rikantō Chemical Co., Ltd.) was mixed with 100 parts by mass of the water-absorbent resin particles (1), thereby obtaining a water-absorbent resin composition (6).
[0111] <Comparative Example 1> 0.2 parts by mass of sodium sulfite and 0.01 parts by mass of L(+)-ascorbic acid were added as powders to 100 parts by mass of the water-absorbent resin particles (1) obtained in Production Example 1, and mixed for 30 minutes using a cross-rotation mixer manufactured by Meiwa Industry Co., Ltd. (conditions: revolution speed 50 rpm, rotation speed 50 rpm). Furthermore, 0.5 parts by mass of amorphous silica (Tokusil NP-S manufactured by Rikantō Chemical Co., Ltd.) was mixed to 100 parts by mass of the water-absorbent resin particles (1), thereby obtaining a water-absorbent resin composition (7).
[0112] <Comparative Example 2> In Comparative Example 1, a water-absorbent resin composition (8) was obtained by the same operation as in Comparative Example 2 except that the amount of sodium sulfite added was changed from 0.2 parts by mass to 0.1 parts by mass and the amount of L(+)-ascorbic acid added was changed from 0.01 parts by mass to 0.02 parts by mass.
[0113] <Comparative Example 3> To 100 parts by mass of the water-absorbent resin particles (1) obtained in Production Example 1, 2 parts by mass of sodium sulfite, 0.02 parts by mass of L(+)-ascorbic acid and 0.7 parts by mass of diethylenetriaminepentaacetic acid (DTPA) were added as powders, and mixed for 30 minutes using a cross-rotation mixer manufactured by Meiwa Industry Co., Ltd. (conditions: revolution speed 50 rpm, rotation speed 50 rpm). Furthermore, 0.5 parts by mass of amorphous silica (Tokusil NP-S manufactured by Rikantsu Chemical Co., Ltd.) was mixed with 100 parts by mass of the water-absorbent resin particles (1), thereby obtaining a water-absorbent resin composition (9).
[0114] <Comparative Example 4> A water-absorbent resin composition (10) was obtained by the same operation as in Example 1 except that 0.2 g of a 1 mass % L(+)-ascorbic acid aqueous solution was not used.
[0115] <Comparative Example 5> In Example 1, except not using 0.2 g of the 20 mass % sodium sulfite aqueous solution, the same operation as in Example 1 was carried out to obtain a water-absorbent resin composition (11).
[0116] <Comparative Example 6> 20 g of the water-absorbent resin particles (1) obtained in Production Example 1 were weighed into a round-bottomed cylindrical separable flask having an inner diameter of 11 cm and equipped with an anchor-type stirring blade made of fluororesin. Then, while stirring at 300 rpm, 0.2 g of a 20% by mass sodium sulfite aqueous solution was taken with a 3 mL syringe, and a nozzle fine atomizer (Yoshikawa Chemicals Co., Ltd.) was set at the tip of the syringe, and the mixture was sprayed in the separable flask every 1 second, and stirred for 10 minutes to obtain a mixture. The mixture was heated at 100° C. for 30 minutes to obtain a heated mixture. 0.01 parts by mass of L(+)-ascorbic acid was added directly in the form of powder to 100 parts by mass of the heated mixture, and the mixture was mixed for 30 minutes using a cross-rotation mixer manufactured by Meiwa Industry Co., Ltd. (conditions: revolution speed 50 rpm, rotation speed 50 rpm). Furthermore, 0.5 parts by mass of amorphous silica (Tokusil NP-S manufactured by Rikantō Chemical Co., Ltd.) was mixed with 100 parts by mass of the water-absorbent resin particles (1), thereby obtaining a water-absorbent resin composition (12).
[0117] <Comparative Example 7> 20 g of the water-absorbent resin particles (1) obtained in Production Example 1 were weighed into a round-bottomed cylindrical separable flask having an inner diameter of 11 cm and equipped with an anchor-type stirring blade made of fluororesin. Then, while stirring at 300 rpm, 0.2 g of a 1% by mass aqueous solution of L(+)-ascorbic acid was taken with a 3 mL syringe, and a nozzle fine atomizer (Yoshikawa Chemicals Co., Ltd.) was set at the tip of the syringe, and the mixture was sprayed into the separable flask every 1 second, and stirred for 10 minutes to obtain a mixture. The mixture was heated at 100° C. for 30 minutes to obtain a heated mixture. 0.2 parts by mass of sodium sulfite was added as a powder to 100 parts by mass of the heated mixture, and the mixture was mixed for 30 minutes using a cross-rotation mixer manufactured by Meiwa Industry Co., Ltd. (conditions: revolution speed 50 rpm, rotation speed 50 rpm). Furthermore, 0.5 parts by mass of amorphous silica (Tokusil NP-S manufactured by Rikantō Chemical Co., Ltd.) was mixed with 100 parts by mass of the water-absorbent resin particles (1), thereby obtaining a water-absorbent resin composition (13).
[0118] <Example 7> In Example 1, except that 20 g of the water-absorbent resin particles (2) obtained in Preparation Example 2 was used instead of 20 g of the water-absorbent resin particles (1) obtained in Preparation Example 1, the same operation as in Example 1 was carried out to obtain a water-absorbent resin composition (14).
[0119] <Example 8> In Example 3, a water-absorbent resin composition (15) was obtained by performing the same operation as in Example 3 except that 20 g of the water-absorbent resin particles (2) obtained in Preparation Example 2 was used instead of 20 g of the water-absorbent resin particles (1) obtained in Preparation Example 1.
[0120] <Example 9> In Example 1, the same operation as in Example 1 was carried out except that 20 g of the water-absorbent resin particles (2) obtained in Production Example 2 was used instead of 20 g of the water-absorbent resin particles (1) obtained in Production Example 1 and the amount of the 20 mass % sodium sulfite aqueous solution added was changed from 0.2 g to 0.1 g, thereby obtaining a water-absorbent resin composition (16).
[0121] <Example 10> In Example 1, except that 20 g of the water-absorbent resin particles (3) obtained in Preparation Example 3 was used instead of 20 g of the water-absorbent resin particles (1) obtained in Preparation Example 1, the same operation as in Example 1 was carried out to obtain a water-absorbent resin composition (17).
[0122] [Evaluation of water-absorbent resin particles] <Water retention of saline solution> A cotton bag (cotton broad No. 60, 100 mm wide x 200 mm long) weighing 2.0 g of water-absorbent resin particles was placed in a 500 mL beaker. 500 g of a 0.9 mass % sodium chloride aqueous solution (physiological saline) was injected into the cotton bag containing the water-absorbent resin particles at once so as not to form lumps, and the upper part of the cotton bag was tied with a rubber band and left to stand for 30 minutes, thereby swelling the water-absorbent resin particles. After 30 minutes, the cotton bag was dehydrated for 1 minute using a dehydrator (manufactured by Kokusan Co., Ltd., product number: H-122) with a centrifugal force set to 167 G, and the mass Wd (g) of the cotton bag including the swollen gel after dehydration was measured. The same operation was performed without adding water-absorbent resin particles, and the empty mass We (g) of the cotton bag when wet was measured, and the water retention of the physiological saline was calculated according to the following formula. Water retention of saline solution (g / g) = [Wd-We] / 2.0
[0123] <Water absorption of physiological saline solution under 4.14kPa load> 4.14kPa water absorption of saline solution under load (water absorption under load) Figure 1 The measurement is performed using a measuring device schematically shown in the figure. Two measurements are performed on a type of water-absorbent resin particles, and an average value is obtained. The measuring device comprises a burette portion 1, a fixture 3, a catheter 5, a stand 11, a measuring table 13, and a measuring portion 4 placed on the measuring table 13. The burette portion 1 comprises: a burette 21 having a scale, a rubber stopper 23 that tightly covers the opening at the upper portion of the burette 21, a stopcock 22 connected to the front end of the lower portion of the burette 21, and an air introduction tube 25 and a stopcock 24 connected to the lower portion of the burette 21. The burette portion 1 is fixed by the fixture 3. The flat measuring table 13 has a through hole 13a with a diameter of 2 mm formed in the center thereof, and is supported by a stand 11 with a variable height. The through hole 13a of the measuring table 13 and the stopcock 22 of the burette portion 1 are connected via a catheter 5. The inner diameter of the catheter 5 is 6 mm.
[0124] The measuring section 4 includes a cylinder 31 made of Plexiglas, a polyamide net 32 bonded to one opening of the cylinder 31, and a weight 33 movable in the cylinder 31 in the vertical direction. The cylinder 31 is placed on the measuring table 13 via the polyamide net 32. The inner diameter of the cylinder 31 is 20 mm. The mesh of the polyamide net 32 is 75 μm (200 mesh). The weight 33 has a diameter of 19 mm and a mass of 119.6 g. As described later, it can apply a load of 4.14 kPa (0.6 psi) to the water-absorbent resin particles 10a uniformly arranged on the polyamide net 32.
[0125] First, close the stopcock 22 and the stopcock 24 of the burette part 1, and inject 0.9 mass % physiological saline adjusted to 25°C into the burette 21 from the upper opening of the burette 21. Next, after sealing the upper opening of the burette 21 with the rubber stopper 23, open the stopcock 22 and the stopcock 24. Fill the interior of the catheter 5 with 0.9 mass % saline 50 in a manner that does not allow air bubbles to enter. The height of the measuring table 13 is adjusted so that the height of the water surface of the 0.9 mass % saline solution reaching the through hole 13a is the same as the height of the upper surface of the measuring table 13. After adjustment, read the height of the water surface of the 0.9 mass % saline 50 in the burette 21 using the scale of the burette 21, and use its position as the zero point (the reading value at 0 seconds).
[0126] In the measuring section 4, 0.10 g of the water-absorbent resin particles 10a were evenly arranged on the polyamide mesh 32 in the cylinder 31, and a weight 33 was arranged on the water-absorbent resin particles 10a, and the cylinder 31 was set so that the center thereof coincided with the catheter opening in the center of the measuring table 13. The amount of physiological saline reduced in the burette 21 (i.e., the amount of physiological saline absorbed by the water-absorbent resin particles 10a) Wc (mL) after 60 minutes from the time when the water-absorbent resin particles 10a began to absorb the physiological saline from the catheter 5 was read, and the physiological saline absorption capacity of the water-absorbent resin particles 10a under a load of 4.14 kPa was calculated by the following formula. 4.14 kPa water absorption capacity of physiological saline under load (mL / g) = Wc (mL) / mass of water-absorbent resin particles (g)
[0127] <Measurement of water absorption rate by vortex method> 50±0.1 g of physiological saline adjusted to 25±0.2°C was weighed in a 100 mL beaker in a constant temperature water bath, stirred with a magnetic stirring bar (8 mmφ×30 mm without ring), and a vortex was generated at a rotation speed of 600 rpm. 2.0±0.002 g of water-absorbent resin particles were added to the above-mentioned physiological saline at once, and the time (seconds) from the addition of the water-absorbent resin particles to the moment when the vortex on the liquid surface converged was measured, and the time was taken as the water absorption rate of the water-absorbent resin particles. This water absorption rate is also expressed as the vortex method or vortex time.
[0128] <Dissolved ingredients> 500 g of physiological saline in a 500 mL beaker is stirred by a stirring bar (cylindrical, ringless, 8 mm in diameter x 30 mm in length) rotating at 600 rpm. The temperature of the physiological saline is 25°C. 2.000 g of water-absorbing particles are added thereto, and the dispersion containing the water-absorbing particles is stirred for 3 hours. The dispersion is filtered with a 75 μm standard sieve, and the filtrate is recovered. 80 g of the obtained filtrate is measured into a weighed 100 mL beaker that has been kept constant at 140°C in advance. The filtrate in the beaker is heated in a hot air dryer (manufactured by ADVANTEC, FV-320) at 140°C for 15 hours to remove moisture, and the mass Wa (g) of the remaining solid content is measured. Without placing the water-absorbing particles in the physiological saline, a blank test is performed in the same manner as above, and the mass Wb (g) of the solid content remaining in the beaker is measured. The dissolved component is calculated by the following formula. Dissolved component (mass %) = [((Wa-Wb) / 80) × 500 / 2] × 100
[0129] <Median particle size (particle size distribution)> 10 g of water-absorbent resin particles were sieved using a sonic vibration sieve measuring device (Robot Shifter RPS-01, manufactured by Seishin Enterprise Co., Ltd.), sieves with mesh sizes of 850 μm, 600 μm, 500 μm, 425 μm, 300 μm, 250 μm and 180 μm and a receiving plate according to the JIS standard. The mass percentage of the particles remaining on each sieve relative to the total mass percentage was calculated. The mass percentage of the particles remaining on each sieve was accumulated in order from the particles with the largest particle size, and the relationship between the mesh size of the sieve and the cumulative value of the mass percentage of the particles remaining on the sieve was plotted on a logarithmic probability paper. By connecting the plots on the probability paper with a straight line, the particle size corresponding to the cumulative mass percentage of 50% was obtained, and it was taken as the median particle size.
[0130] <Water content> 2.0 g of water-absorbent resin particles were placed in an aluminum foil box (No. 8) that was previously made to a constant weight (W1 (g)), and the mouth of the aluminum foil box was gently closed. The total mass W2 (g) of the aluminum foil box containing the sample was accurately weighed. The aluminum foil box containing the sample was dried for 2 hours using a hot air dryer (manufactured by ADVANTEC, model: FV-320) with an internal temperature set at 105°C. The dried aluminum foil box containing the sample was cooled to room temperature in a desiccator. The total mass W3 (g) of the aluminum foil box containing the sample after cooling was measured. The moisture content of the sample was calculated according to the following formula. Water content [mass %] = [{(W2-W1)-(W3-W1)} / (W2-W1)] × 100
[0131] [Evaluation of water-absorbent resin composition] <Water retention of saline solution> The physiological saline water retention capacity of the water absorbent resin composition was measured in the same manner as the physiological saline water retention capacity measured for the above-mentioned water absorbent resin particles.
[0132] <Water absorption of physiological saline solution under 4.14kPa load> The physiological saline water absorption under a load of 4.14 kPa of the water absorbent resin composition was measured in the same manner as the physiological saline water absorption under a load of 4.14 kPa measured for the water absorbent resin particles.
[0133] <Measurement of water absorption rate by vortex method> The water absorption rate of the water absorbent resin composition is measured in the same manner as the water absorption rate by the eddy current method measured for the water absorbent resin particles.
[0134] <Dissolved ingredients> The dissolved content of the water-absorbent resin composition was measured in the same manner as the dissolved content of the water-absorbent resin particles.
[0135] <Median particle size (particle size distribution)> The median particle size (particle size distribution) of the water-absorbent resin composition is measured in the same manner as the median particle size (particle size distribution) measured for the above-mentioned water-absorbent resin particles.
[0136] <Water content> The water content of the water absorbent resin composition was measured in the same manner as the water content of the water absorbent resin particles.
[0137] <Yellow coloration test under high temperature and high humidity (measurement of yellowness)> 2.0 g of the water-absorbent resin composition was placed in a glass measuring container having an inner diameter of 3 cm, and the yellowness of the water-absorbent resin composition was measured using a colorimeter (ColorMeter ZE6000, manufactured by Nippon Denshoku Industries Co., Ltd.) in which X, Y, and Z, which are tristimulus values of the colorimetric colorimeter, were calibrated using a standard white plate. The yellowness was calculated as an initial value using the following formula based on X, Y, and Z (tristimulus values) of the obtained water-absorbent resin composition.
[0138] Yellowness = 100 (1.28X-1.06Z) / Y
[0139] In addition, the test of the coloration of the water-absorbent resin composition over time was conducted as follows. That is, 2.0 g of the water-absorbent resin composition was uniformly placed in a glass dish with an inner diameter of 3 cm and a depth of 1 cm, and the container was stored in a constant temperature and humidity chamber (LHU-113 manufactured by ESPEC Co., Ltd.) set at a temperature of 70±2°C and a relative humidity of 90±2% for 7 days. Then, the container was taken out from the constant temperature and humidity chamber, left for a period of time, and cooled to room temperature. The total amount of the water-absorbent resin composition in the container was placed in a glass measuring container with an inner diameter of 3 cm, and the yellowness of the water-absorbent resin composition was measured using a colorimeter (ColorMeter ZE6000, manufactured by Nippon Denshoku Industries Co., Ltd.). The yellowness was calculated by the following formula based on the X, Y, and Z (tristimulus values) of the obtained water-absorbent resin composition.
[0140] Yellowness = 100 (1.28X-1.06Z) / Y
[0141] <Test of gel absorbing artificial urine> Using artificial urine, a test of a gel (swollen gel) formed by water absorption by the water-absorbent resin composition was conducted.
[0142] (Preparation of artificial urine) Artificial urine of the following composition was prepared. Urea: 20.0g Sodium chloride: 8.0g Calcium chloride dihydrate: 0.3g Magnesium sulfate heptahydrate: 0.8 g L(+)-ascorbic acid: 0.2 g Ion exchange water: 970.9g
[0143] (Preparation of swollen gel) 39.0 g of the artificial urine was weighed in a beaker with an internal volume of 100 mL, and a magnetic stirring bar (8 mm φ × 30 mm) was placed in the beaker, which was placed on a magnetic stirrer (HS-30D manufactured by Iuchi Co., Ltd.), and the magnetic stirring bar was rotated at 600 rpm. Next, 1.00 g of the water-absorbent resin composition was placed in the stirring beaker, and the mixture was stirred until the vortex disappeared and the liquid surface became horizontal, thereby preparing a swollen gel to be a measurement sample. After the swollen gel was prepared, the beaker containing the swollen gel was immediately covered with a plastic wrap (DIAWRAP manufactured by Mitsubishi Chemical Corporation).
[0144] (Determination of gel strength) The gel strength after standing for a specified time under various temperature conditions was measured using Figure 2 The measurement principle is shown in the apparatus for carrying out the measurement. Figure 2The device shown is composed of a support portion 50a, a movable platen 60, a driving portion 70 for driving the movable platen 60, and a measuring portion 80. In the support portion 50a, a stand 53 is fixed to the upper part of a pillar 52 erected on the support platform 51. The movable platen 60 is mounted on the pillar 52 in a manner that it can move up and down. The movable platen 60 can carry a measurement sample (gel) 61. A pulse motor 71 is mounted on the stand 53, and the movable platen 60 is moved up and down via a wire 73 by rotating a pulley 72. In the measuring portion 80, a reel pressure-sensitive shaft 84 is mounted on a force sensor 81 for measuring strain caused by deformation via a precision spring 82 and a connecting shaft 83. The reel pressure-sensitive shaft 84 has a disk at the front end. The diameter of the disk can be changed according to the measurement conditions. A counterweight 90 can be mounted on the upper part of the reel pressure-sensitive shaft 84. The working principle of the device for measuring the gel strength is as follows. The precision spring 82 is fixed to the load cell 81 (stress detector) at the top, and the pressure-sensitive shaft 84 with a reel is connected at the bottom, and a predetermined counterweight 90 is placed on the plate to be suspended vertically. The movable platen 60 on which the test sample 61 is placed rises at a constant speed by the rotation of the pulse motor 71. A constant speed load is applied to the test sample 61 via the precision spring 82, and the strain caused by the deformation is measured by the load cell 81 to measure the hardness. Gel strength value (N / m 2 ) was measured using Curdmeter-MAX (manufactured by Feiniao Equipment, model: ME-500) with a disk 16 mmφ with a disk pressure-sensitive shaft 84, a load of 400 g, a speed of 7 sec / inch, and a viscosity mode setting under the following temperature and standing time conditions: (initial value of gel strength) and (gel strength after standing at 37°C for 28 hours).
[0145] (Initial value of gel strength) After the swollen gel was allowed to stand for 60 minutes at a temperature of 25±2° C. and a relative humidity of 50±10%, the gel strength (initial value of the gel strength) was measured by the above method.
[0146] (Gel strength after standing at 37°C for 28 hours) After the preparation, the swollen gel was allowed to stand for 28 hours in a constant temperature and humidity chamber (LHU-113 manufactured by ESPEC Co., Ltd.) set at a temperature of 37±2°C and a relative humidity of 60±10%, and then the gel strength was measured by the above method. The gel strength value at this time was taken as the gel strength after standing at 37°C for 28 hours.
[0147] [Table 1] Description of Reference Numerals
[0148] 1 Burette section 3. Fixture 4 Measurement unit 5 Catheter 10a Water-absorbent resin particles 11 racks 13. Measuring table 13a Through hole 15 Nylon mesh 21 Burette 22 Plug 23 Rubber stopper 24 Plug 25 Air inlet pipe 31 Cylinder 32 Polyamide mesh 33 Counterweight 50a Supporting part 51 Support platform 52 Pillar 53 stand 60 Movable platen 61 Measurement sample 70 Drive unit 71 Pulse motor 72 Pulley 73 Wire 80 Measurement Unit 81 Force sensor 82 Precision Spring 83 Connecting shaft 84 Reel-like finale 90 counterweight.
Claims
1. A method for producing a water-absorbent resin composition, characterized in that: have: a step of spraying an aqueous solution of a sulfite compound onto the water-absorbing resin particles subjected to the surface cross-linking treatment; and The process of spraying an aqueous solution of an organic antioxidant.
2. The method for producing a water-absorbent resin composition according to claim 1, wherein The sulfite compound includes at least one selected from the group consisting of sodium sulfite, potassium sulfite, calcium sulfite, sodium bisulfite, potassium bisulfite, ammonium bisulfite, sodium pyrosulfite and potassium pyrosulfite.
3. The method for producing a water-absorbent resin composition according to claim 1 or 2, wherein: The organic antioxidant comprises at least one selected from ascorbic acid, isoascorbic acid, gallic acid, protocatechuic acid, benzimidazole and alkylhydroxyanisole.
4. The method for producing a water-absorbent resin composition according to claim 1 or 2, wherein: The dissolved content of the water-absorbent resin particles determined by the following measurement method is 19 parts by mass or less: Regarding dissolved ingredients, 500 g of physiological saline in a 500 mL beaker was stirred with a stirring bar rotating at 600 rpm, the temperature of the physiological saline was set to 25° C., 2.000 g of water-absorbent resin particles were added thereto, and the dispersion containing the water-absorbent resin particles was stirred for 3 hours; the dispersion was filtered with a 75 μm standard sieve, the filtrate was recovered, and 80 g of the obtained filtrate was measured and put into a weighed 100 mL beaker that had been weighed and reached a constant weight at 140° C. in advance; the filtrate in the beaker was heated in a hot air dryer at 140° C. for 15 hours to remove moisture, and the mass Wa of the residual solid content was measured in grams. A blank test was performed in the same manner as above without placing the water-absorbent resin particles in the physiological saline solution, and the mass Wb of the solid content remaining in the beaker was measured in grams. The dissolved components were calculated by the following formula: Dissolved content (mass %)=[((Wa-Wb) / 80)×500 / 2]×100.
5. The method for producing a water-absorbent resin composition according to claim 1 or 2, wherein: The spraying amount of the sulfite compound is 0.01 parts by mass or more and 3 parts by mass or less relative to 100 parts by mass of the water-absorbing resin particles.
6. The method for producing a water-absorbent resin composition according to claim 1 or 2, wherein: The spraying amount of the organic antioxidant is 0.1 parts by mass or more and 20 parts by mass or less relative to 100 parts by mass of the sulfite-based compound.
7. The method for producing a water-absorbent resin composition according to claim 1 or 2, wherein: The water-absorbent resin particles have a physiological saline water retention capacity of 25 g / g or more and 60 g / g or less.
8. The method for producing a water-absorbent resin composition according to claim 1 or 2, wherein: The water-absorbent resin particles have a physiological saline water absorption capacity of 5 ml / g or more and 40 ml / g or less under a load of 4.14 kPa.
Citation Information
Patent Citations
Water-absorbing resin composition
JP2005029751A