Composition for forming coating film, coating film, and article with coating film
By using a coating composition of polyurethane resin and colloidal silica, the problem of difficulty in removing coal and cement waste on the anti-fouling coating film is solved, and efficient sweeping and anti-fouling performance are achieved.
Patent Information
- Application Number
- CN202380029615.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-25
- Filing Date
- 2023-03-23
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
Smart Images

Figure CN118922507A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a coating film-forming composition, a coating film, and an article having a coating film. Background Art
[0002] Conventionally, in order to prevent the adhesion of dirt to structures and scratches, etc., a method of protecting the surfaces of structures and structural members with an antifouling coating film has been used.
[0003] However, when a structural member (adherend) coated with an antifouling coating is handled in a factory, coal, cement, etc. (hereinafter referred to as coal, cement, etc.) may be accidentally attached to the surface of the antifouling coating before the antifouling coating is reapplied. In this case, a cleaning operation is required to remove the coal, cement, etc. attached to the coating surface.
[0004] For example, Patent Document 1 discloses a coating composition having excellent solvent resistance, recoatability, graffiti removability or anti-graffiti properties. The coating composition described in Patent Document 1 contains the following essential components: a liquid organosiloxane compound; an organometallic catalyst; at least one compound selected from an alkoxy-containing organosilane compound having a primary or secondary amino group, an amino-modified silicone oil, and an amino-containing organosiloxane compound; and at least one compound selected from a compound having two or more glycidyl groups in one molecule, a glycidyl-containing silane compound, and a glycidyl-containing organosilicon oligomer.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent No. 4721667 Summary of the invention
[0008] Problems to be solved by the invention
[0009] In the above-mentioned Patent Document 1, although the removability of graffiti such as oil-based pen ink is evaluated, the removability of coal such as coal and cement that easily adheres to construction sites is not evaluated.
[0010] An object of the present invention is to provide a coating film-forming composition capable of obtaining a coating film that can be easily removed even if dirt such as coal and cement adheres thereto, that is, a coating film having excellent cleanability, a coating film formed from the composition, and a coated article having the coating film.
[0011] Means for solving problems
[0012] The inventors of the present application have conducted intensive research to solve the above-mentioned problems and have found that a coating film having excellent cleanability against coal, cement, etc. can be formed by using a coating film-forming composition containing a water-based resin such as a polyurethane resin and colloidal silica and produced by a prescribed method, wherein the elastic modulus of the coating film is greater than a prescribed value, thereby completing the present invention.
[0013] That is, the problems of the present invention can be solved by the following [1] to [8].
[0014] [1]
[0015] A coating film-forming composition comprising an aqueous resin and colloidal silica.
[0016] The elastic modulus of the coating film sample 1 for measurement prepared by the following method is 100 MPa or more.
[0017] Preparation method of coating sample 1 for measurement: the coating film-forming composition is applied on the surface of a PET film having a thickness of 75 μm so as to have a WET thickness of 500 μm, and dried at 22° C. for 24 hours to form a coating film on the PET film. The coating film is cut so as to have an area of 10 mm×100 mm, thereby preparing coating sample 1 for measurement.
[0018] [2]
[0019] The coating film-forming composition as described in the above-mentioned [1], wherein the content of the colloidal silica is 30 parts by mass or less based on 100 parts by mass of the aqueous resin.
[0020] 〔3〕
[0021] The coating film-forming composition according to the above-mentioned [1] or [2], wherein the water-based resin is a polyurethane-based resin.
[0022] [4]
[0023] The coating film-forming composition as described in any one of [1] to [3] above, further comprising a reactive silicone oil.
[0024] 〔5〕
[0025] The coating film-forming composition as described in the above-mentioned [4], wherein the reactive silicone oil is an amino-modified silicone oil.
[0026] [6]
[0027] The coating film-forming composition according to any one of [1] to [5] above, wherein the contact angle of the coating film sample 2 for measurement prepared by the following method is 60° to 100°,
[0028] Preparation method of coating film sample 2 for measurement: the coating film-forming composition was applied to the surface of a 75 μm thick PET film to a WET thickness of 500 μm, and dried at 22° C. for 24 hours to form a coating film on the PET film, thereby preparing coating film sample 2 for measurement.
[0029] 〔7〕
[0030] A coating film formed from the coating film-forming composition according to any one of [1] to [6] above.
[0031] 〔8〕
[0032] A coated article having the coating described in [7] above.
[0033] Effects of the Invention
[0034] The present invention contains a water-based resin and colloidal silica in a composition, and limits the elastic modulus of a coating film produced from the composition to an appropriate range. Therefore, a coating film-forming composition capable of obtaining a coating film having excellent easy-to-clean properties against coal, cement, etc., a coating film formed from the composition, and a coating-film-bearing article having the coating film can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] [ Figure 1 ] Figure 1 It is a cross-sectional view showing a coated article on which a coating film formed from the coating film-forming composition according to the present embodiment is formed.
[0036] [ Figure 2 ] Figure 2 It is a cross-sectional view showing a coating film of coal, cement, etc. adhered to the surface.
[0037] [ Figure 3 ] Figure 3 Schematic diagram showing the method of the coal stain cleanability evaluation test.
[0038] [ Figure 4 ] Figure 4 Schematic diagram showing the method of the cement stain cleanability evaluation test.
[0039] [ Figure 5 ] Figure 5 Schematic diagram showing the method of the paint stain cleanability evaluation test. DETAILED DESCRIPTION
[0040] In the present specification, "A to B" indicating a range means "A or more and B or less." In the present specification, "weight" and "mass", "weight %" and "mass %" are used as synonyms, respectively.
[0041] Hereinafter, the mode for implementing the present invention will be described in detail. It should be noted that the present invention is not limited to the embodiments described below. In addition, in the following drawings, the same reference numerals are sometimes used to mark the parts and parts that play the same role for description, and repeated descriptions are sometimes omitted or simplified. In addition, the embodiments described in the drawings are schematically illustrated in order to clearly illustrate the present invention, and do not necessarily correctly represent the size and scale of the actual product.
[0042] Figure 1 2 is a cross-sectional view showing an article with a coating film formed of a coating film-forming composition according to an embodiment of the present invention. Figure 1 As shown, the coating film 21 is formed by applying the coating film-forming composition according to the embodiment of the present invention onto the surface of the adherend 31 and then drying it.
[0043] in addition, Figure 2 2 is a cross-sectional view showing a coating film with coal, cement, etc. attached to the surface. When the adherend 31 is handled in a factory, coal, cement, etc. 22 may be attached to the surface of the coating film 21. In this application specification, the ease of removing the coal, cement, etc. 22 from the surface of the coating film 21 is referred to as "easy cleaning". It should be noted that Figure 2 In the embodiment, the coal, cement, etc. 22 adheres to the entire surface of the coating film 21 . However, there are cases where the coal, cement, etc. 22 adheres only to a part of the surface of the coating film 21 .
[0044] The coating film-forming composition according to the present embodiment will be described in detail below.
[0045] [Coating film forming composition]
[0046] The coating film-forming composition of the present embodiment contains an aqueous resin and colloidal silica. The elastic modulus of the coating film sample 1 for measurement prepared by the following method is 100 MPa or more.
[0047] Preparation method of coating sample 1 for measurement: The coating film-forming composition is applied on the surface of a PET film having a thickness of 75 μm so that the WET thickness becomes 500 μm, and the coating film is formed on the PET film by drying at 22° C. for 24 hours. The coating film is cut into pieces having an area of 10 mm×100 mm to prepare coating sample 1 for measurement.
[0048] The coating film forming composition of the present embodiment uses colloidal silica in addition to a water-based resin having a high elastic modulus when forming a coating film, thereby achieving the formation of a coating film with excellent easy cleaning properties for coal, cement, etc. for the first time. The mechanism of action is uncertain, but it is speculated that the surface state of the coating film when the coating film is formed changes by using both a water-based resin having a high elastic modulus when forming a coating film and colloidal silica, thereby improving the removal performance for coal, cement, etc. It should be noted that the present invention is not limited to this mechanism of action.
[0049] Each component contained in the coating film-forming composition will be described in more detail.
[0050] (Water-based resin)
[0051] The coating film forming composition of the present embodiment contains a water-based resin. Here, the water-based resin refers to a resin in a state where the resin is stably dispersed as dispersoid particles in a water-based solvent. In addition, the "water-based solvent" refers to any one of water, a water-soluble organic solvent, or a mixture thereof. Compared with solvent-based resins, water-based resins are excellent in terms of environmental aspects and can also be excellent in operability.
[0052] The coating film-forming composition of the present embodiment can form a coating film having excellent cleaning properties against coal, cement, and the like by using colloidal silica described below in combination with the aqueous resin.
[0053] As water-based resin, various resins can be used, as described below, when forming a film as a film-forming composition, a resin that satisfies a prescribed elastic modulus can be appropriately selected for use. As water-based resin, for example, polyurethane resin, acrylic resin, polystyrene resin, rubber resin, silicone resin, vinyl alkyl ether resin, polyvinyl alcohol resin, polyvinyl pyrrolidone resin, polyacrylamide resin, cellulose resin, polyester resin, fluorine resin, etc. can be cited. Preferably, at least one selected from acrylic resin, polyurethane resin, polystyrene resin, and rubber resin, more preferably acrylic resin and polyurethane resin.
[0054] In addition, from the viewpoint of the elastic modulus when forming a coating film, a water-based resin having an elastic modulus or Young's modulus (23°C) of 300 to 600 MPa is preferred. Here, the elastic modulus refers to the value measured by a tensile test of a film formed by heating the resin at 80°C for 6 hours. In addition, Young's modulus (23°C) refers to the value measured by a tensile test of a film formed of the resin in the same manner as above at 23°C.
[0055] The polyurethane resin is typically a reaction product of a polyol and a polyisocyanate. As the polyol component, preferably used are high molecular weight polyols such as polycarbonate polyol, polyacrylic polyol, polyester polyol, and polyether polyol.
[0056] Representative examples of polycarbonate polyols include: reactants of polyols with phosgene, chloroformate, dialkyl carbonates or diaryl carbonates; ring-opening polymers of cyclic carbonates (alkylene carbonates, etc.); etc. Specifically, among the reactants of polyols with phosgene, polyols such as ethylene glycol, propylene glycol, 1,3-butanediol, 1,4-butanediol, neopentyl glycol, 1,5-pentanediol, 1,6-hexanediol, and 1,9-nonanediol can be used. In addition, among the ring-opening polymers of cyclic carbonates, alkylene carbonates such as ethylene carbonate, propylene carbonate, butylene carbonate, and hexylene carbonate can be used. It should be noted that polycarbonate polyols may be compounds having carbonate bonds in the molecule and having hydroxyl groups at the ends, and may also have both carbonate bonds and ester bonds.
[0057] Polyacrylic acid polyols can be obtained representatively by polymerization of (meth)acrylates and hydroxyl-containing monomers. Examples of (meth)acrylates include methyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and cyclohexyl (meth)acrylate. Examples of hydroxyl-containing monomers include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and 2-hydroxypentyl (meth)acrylate; (meth)acrylate monoesters of polyols such as glycerol and trimethylolpropane; and N-methylol (meth)acrylamide.
[0058] Polyester polyols can be obtained by reacting polyacids with polyols. Examples of polyacids include aromatic dicarboxylic acids such as phthalic acid, isophthalic acid, terephthalic acid, 1,4-naphthalene dicarboxylic acid, 2,5-naphthalene dicarboxylic acid, 2,6-naphthalene dicarboxylic acid, biphenyl dicarboxylic acid, and tetrahydrophthalic acid; aliphatic dicarboxylic acids such as oxalic acid, succinic acid, malonic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, decanedicarboxylic acid, dodecanedicarboxylic acid, octadecane dicarboxylic acid, tartaric acid, alkyl succinic acid, linolenic acid, maleic acid, fumaric acid, mesaconic acid, citraconic acid, and itaconic acid; alicyclic dicarboxylic acids such as hexahydrophthalic acid, tetrahydrophthalic acid, 1,3-cyclohexane dicarboxylic acid, and 1,4-cyclohexane dicarboxylic acid; or reactive derivatives thereof such as anhydrides, alkyl esters, and acyl halides; and the like.
[0059] The polyether polyol can be obtained by ring-opening polymerization of alkylene oxide and then adding it to a polyol. Examples of the polyol include ethylene glycol, diethylene glycol, propylene glycol, dipropylene glycol, glycerol, trimethylolpropane, etc. Examples of the alkylene oxide include ethylene oxide, propylene oxide, butylene oxide, styrene oxide, tetrahydrofuran, etc.
[0060] Examples of the polyisocyanate include aromatic, aliphatic, and alicyclic diisocyanates, and dimers and trimers of these diisocyanates. Examples of aromatic, aliphatic, and alicyclic diisocyanates include toluene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), xylylene diisocyanate (XDI), naphthalene diisocyanate (NDI), phenylene diisocyanate (PPDI), meta-tetramethylxylylene diisocyanate (TMXDI), methylcyclohexane diisocyanate (hydrogenated TDI), dicyclohexylmethane diisocyanate (hydrogenated MDI), cyclohexane diisocyanate (hydrogenated PPDI), di(isocyanatomethyl)cyclohexane (hydrogenated XDI), norbornene diisocyanate (NBDI), isophorone diisocyanate (IPDI), hexamethylene diisocyanate (HDI), butane diisocyanate, 2,4-trimethylhexamethylene diisocyanate, and 2,4,4-trimethylhexamethylene diisocyanate. In addition, dimers, trimers, and polyphenylmethane diisocyanates thereof may be used. Examples of the trimer include isocyanurate type, biuret type, and allophanate type, and any of them can be used appropriately.
[0061] Among these, aliphatic and alicyclic diisocyanates such as methylcyclohexane diisocyanate (hydrogenated TDI), dicyclohexylmethane diisocyanate (hydrogenated MDI), cyclohexane diisocyanate (hydrogenated PPDI), di(isocyanatomethyl)cyclohexane (hydrogenated XDI), norbornene diisocyanate (NBDI), isophorone diisocyanate (IPDI), hexamethylene diisocyanate (HDI), hydrogenated 4,4-diphenylmethane diisocyanate (HMDI), butane diisocyanate, 2,4-trimethylhexamethylene diisocyanate, and 2,4,4-trimethylhexamethylene diisocyanate are particularly preferably used.
[0062] These polyisocyanates can be used alone or in combination. The type and combination of polyisocyanates may be appropriately selected from the viewpoints of the properties of the adherend, solubility, reactivity with hydroxyl groups, and the like.
[0063] As the polyisocyanate, it is preferred to use at least one diisocyanate selected from the group consisting of hexamethylene diisocyanate (HDI), hydrogenated toluene diisocyanate (HTDI), hydrogenated 4,4-diphenylmethane diisocyanate (HMDI), isophorone diisocyanate (IPDI) and hydrogenated xylene diisocyanate (HXDI), and hydrogenated 4,4-diphenylmethane diisocyanate (HMDI) is particularly preferred.
[0064] As the acrylic resin, for example, a resin obtained by emulsion polymerization of a monomer component containing an alkyl (meth)acrylate is preferred.
[0065] As the alkyl (meth)acrylate, for example, methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, isooctyl (meth)acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, tetradecyl (meth)acrylate, etc. can be mentioned. Such alkyl (meth)acrylate can be used alone or in combination of two or more. Among them, as preferred alkyl (meth)acrylate, n-butyl acrylate (BA) and 2-ethylhexyl acrylate (2EHA) can be mentioned.
[0066] In the present specification, "(meth)acrylic acid" refers to acrylic acid and / or methacrylic acid. The acrylic resin includes a resin containing acrylic acid or a derivative thereof as a monomer component and a resin containing methacrylic acid or a derivative thereof as a monomer component.
[0067] The proportion of the (meth) alkyl acrylate in all monomer components used in the synthesis of the acrylic resin is preferably 70% by mass or more, more preferably 85% by mass or more, and further preferably 90% by mass or more. The upper limit of the proportion of the above-mentioned alkyl (meth) acrylate is not particularly limited, and is usually preferably 99.5% by mass or less (for example, 99% by mass or less). Alternatively, the acrylic resin may be a resin obtained by substantially polymerizing only the alkyl (meth) acrylate.
[0068] As polystyrene-based resins, for example, SBS (styrene-butadiene block copolymer), SIS (styrene-isoprene block copolymer), SEBS (styrene-ethylene-butylene-styrene block copolymer), SEPS (styrene-ethylene-propylene-styrene block copolymer), and SEEPS (styrene-ethylene-ethylene-propylene-styrene block copolymer) can be used.
[0069] As the rubber resin, for example, acrylic rubber, diene rubber, butyl rubber, nitrile rubber, hydrogenated nitrile rubber, fluororubber, silicone rubber, ethylene-propylene rubber, chloroprene rubber, urethane rubber, and epichlorohydrin rubber can be used, and acrylic rubber, diene rubber, and urethane rubber are particularly preferred. As the diene rubber, natural rubber, isoprene rubber, butadiene rubber, styrene-butadiene rubber, chloroprene rubber, and acrylonitrile-butadiene rubber can be used, and styrene-butadiene rubber is preferred.
[0070] The water-based resin may contain a compound containing a polar group. Examples of such compounds include the aforementioned resin containing a polar group, a silane coupling agent, a crosslinking agent, silicone oil, etc. Examples of the resin containing a polar group include ionomers, rosin resins, silicone resins, etc.
[0071] The water-based resin in the present embodiment is particularly preferably a polyurethane resin obtained by reacting a polycarbonate diol as a polyol component with a polyisocyanate. As such a polyurethane resin, commercially available resins can also be used, for example, Superflex 420 (made by Daiichi Kogyo Seiyaku Co., Ltd.), ST-008E (made by Ube Industries, Ltd.), etc. It should be noted that Superflex 420 (made by Daiichi Kogyo Seiyaku Co., Ltd.) is a polyurethane resin obtained by reacting a polycarbonate polyol as a polyol component, particularly hexamethylene carbonate, with a diisocyanate of aliphatic and alicyclic systems as polyisocyanate, particularly hydrogenated 4,4-diphenylmethane diisocyanate (HMDI). In addition, ST-008E (made by Ube Industries, Ltd.) is a polyurethane resin obtained by reacting a polycarbonate diol as a polyol component with a polyisocyanate.
[0072] The content of the above-mentioned compound relative to the resin component in the water-based resin is preferably 0.1 to 95 mass %, more preferably 0.5 to 60 mass %, further preferably 0.5 to 40 mass %, particularly preferably 0.5 to 20 mass %, and most preferably 1 to 20 mass % relative to the total mass of the resin component.
[0073] The content of the resin component in the water-based resin is preferably 5 to 95% by mass, more preferably 10 to 90% by mass, further preferably 15 to 80% by mass, particularly preferably 20 to 70% by mass, and most preferably 25 to 60% by mass.
[0074] The water-based resin may be an emulsion or an emulsion-type resin using a polymer emulsion obtained by emulsion polymerization.
[0075] Examples of the emulsion-type resin include emulsions containing the above-mentioned resin components, and a urethane-based emulsion containing urethane rubber is preferred.
[0076] Emulsion polymerization is carried out by emulsifying the monomer components in water by conventional methods. Thus, an aqueous dispersion (polymer emulsion) is prepared. In emulsion polymerization, for example, a surfactant (emulsifier), a free radical polymerization initiator, a chain transfer agent added as needed, etc. are appropriately matched with the monomer components. More specifically, for example, known emulsion polymerization methods such as a one-time feeding method (one-time polymerization method), a monomer dropwise addition method, and a monomer emulsion dropwise addition method can be adopted.
[0077] It should be noted that in the monomer dropwise addition method and the monomer emulsion dropwise addition method, continuous dropwise addition or stepwise dropwise addition can be appropriately selected. These methods can be appropriately combined. Reaction conditions can be appropriately selected, and the polymerization temperature is preferably 40 to 95° C., and the polymerization time is preferably 30 minutes to 24 hours.
[0078] The initiator used in the emulsion polymerization can be appropriately selected from conventionally known polymerization initiators. For example, azo polymerization initiators such as 2,2'-azobisisobutyronitrile can be preferably used. Other examples of polymerization initiators include persulfates such as potassium persulfate; peroxide initiators such as benzoyl peroxide and hydrogen peroxide; substituted ethane initiators such as phenyl substituted ethane; aromatic carbonyl compounds; and the like.
[0079] As another example of the polymerization initiator, a redox initiator composed of a combination of a peroxide and a reducing agent can be cited. Such polymerization initiators can be used alone or in combination of two or more. The amount of the polymerization initiator used is a usual amount, which can be 0.005 to 1 part by mass, or 0.01 to 1 part by mass, relative to 100 parts by mass of the monomer raw material.
[0080] As the emulsifier, any of anionic, nonionic, and cationic emulsifiers can be used. They can be used alone or in combination of two or more. Anionic or nonionic emulsifiers are usually preferred.
[0081] Examples of the anionic emulsifier include sodium lauryl sulfate, ammonium lauryl sulfate, sodium dodecylbenzenesulfonate, sodium polyoxyethylene alkyl ether sulfate, ammonium polyoxyethylene alkylphenyl ether sulfate, sodium polyoxyethylene alkylphenyl ether sulfate, and the like.
[0082] Examples of the nonionic emulsifier include polyoxyethylene alkyl ether and polyoxyethylene alkylphenyl ether.
[0083] A radical polymerizable emulsifier (reactive emulsifier) having a structure in which a radical polymerizable group such as an propylene group is introduced into the anionic or nonionic emulsifier as described above may also be used. Although not particularly limited, from the viewpoints of polymerization stability during resin synthesis, storage stability of the adhesive composition, etc., it is preferred to use only an emulsifier having no radical polymerizable group.
[0084] In the above polymerization, various chain transfer agents known in the past (also understood as molecular weight regulators or polymerization degree regulators) can be used as needed. The chain transfer agent can be, for example, one or more selected from mercaptans such as n-lauryl mercaptan, tert-lauryl mercaptan, glycidyl mercaptan, and 2-mercaptoethanol. Among them, n-lauryl mercaptan and tert-lauryl mercaptan can be cited as preferred chain transfer agents.
[0085] When a chain transfer agent is used in the polymerization of the monomer raw material, the amount used is not particularly limited, and can be, for example, 0.001 to 0.5 parts by mass, and is usually preferably 0.01 to 0.1 parts by mass, based on 100 parts by mass of the monomer raw material.
[0086] The Mw of the obtained resin is typically 10×10 4 Above, usually 20×10 4 From the viewpoint of properly achieving both adhesive strength and cohesive strength, Mw is preferably 30×10 4 More preferably 40×10 4 More preferably, 50×10 4 The upper limit of Mw is not particularly limited, and may be, for example, 500×10 4 Below, typically 200×10 4 Below, preferably 150×10 4 the following.
[0087] Mw can be adjusted by, for example, the type and amount of polymerization initiator, polymerization temperature, type and amount of emulsifier, presence or absence of chain transfer agent and its type and amount, composition of monomer raw materials, type and degree of crosslinking (gel fraction), etc.
[0088] (Colloidal Silica)
[0089] The coating film forming composition of the present embodiment contains colloidal silica. Colloidal silica imparts hydrophilicity to the coating film forming composition and can improve antifouling properties. In particular, in the coating film forming composition of the present embodiment, in addition to colloidal silica, the above-mentioned water-based resin is also used, thereby forming a coating film with excellent easy cleaning properties against coal, cement, etc.
[0090] Examples of colloidal silica include colloids of fine particles of silicon dioxide (anhydrous silicic acid), as described in, for example, Japanese Patent Application Laid-Open No. 53-112732, Japanese Patent Application Publication No. 57-9051, and Japanese Patent Application Publication No. 57-51653.
[0091] In addition, colloidal silica may contain, for example, alumina, sodium aluminate, etc., as required, and may contain stabilizers such as inorganic bases (eg, sodium hydroxide, potassium hydroxide, lithium hydroxide, ammonia, etc.) and organic bases (eg, tetramethylammonium, etc.) as required.
[0092] Such colloidal silica is not particularly limited and can be produced by a known sol-gel method, specifically, the sol-gel method described in, for example, Werner Stober et al; J. Colloid and Interface Sci., 26, 62-69 (1968), Rickey D. Badley et al; Langmuir 6, 792-801 (1990), Journal of the Color Materials Association, 61[9] 488-493 (1988), etc.
[0093] From the viewpoint of antifouling properties, colloidal silica preferably uses water-dispersed colloidal silica of the type in which spherical silica particles are dispersed in water. In addition, the average particle size of the spherical silica particles dispersed in the colloidal silica is preferably 5 to 100 nm. By making the average particle size 5 nm or more, a hydrophilic effect can be expected. On the other hand, by being 100 nm or less, the transparency of the film can be maintained.
[0094] Here, the average particle size refers to the average particle size based on the number of particles, which can be measured by a particle size distribution measuring device using a dynamic light scattering method as the measuring principle. As such a particle size distribution measuring device, for example, the "Zeta Potential·Particle Size·Molecular Weight Measurement System ELSZ2000ZS" (trade name) manufactured by Otsuka Electronics Co., Ltd. using a homodyne optical system as a frequency analysis method can be cited.
[0095] The content of the colloidal silica (solid content) in the coating film forming composition of the present embodiment is preferably 0.1 parts by mass or more, more preferably 1 parts by mass or more, and further preferably 3 parts by mass or more, based on the content relative to 100 parts by mass of the water-based resin. By making the content of the colloidal silica (solid content) 0.1 parts by mass or more, a coating film with high uniformity can be formed without relying on the coating method, and a hydrophilic effect can be expected.
[0096] In addition, the content of the colloidal silica (solid content) in the coating film forming composition of the present embodiment is preferably 100 parts by mass or less, more preferably 75 parts by mass or less, further preferably 50 parts by mass or less, and particularly preferably 30 parts by mass or less, based on the content relative to 100 parts by mass of the water-based resin. By making the content of the colloidal silica (solid content) below 100 parts by mass, the deterioration of the coating film appearance can be prevented, and a beautiful coating film can be produced without relying on the coating method.
[0097] In addition, the viscosity of colloidal silica is preferably 1 to 25 mPa·s.
[0098] In addition, the pH of the colloidal silica is preferably 7-12, more preferably 8-10.
[0099] In addition, as such colloidal silica, commercially available products can be used, and specific examples include product names "Snowtex (registered trademark)-XL", "Snowtex (registered trademark)-YL", "Snowtex (registered trademark)-ZL", "PST-2", "Snowtex (registered trademark)-20", "Snowtex (registered trademark)-30", "Snowtex (registered trademark)-30L", "Snowtex (registered trademark)-C", "Snowtex (registered trademark)-CM", "Snowtex (registered trademark)-O", "Snowtex (registered trademark)-OS", "Snowtex (registered trademark)-OL", "Snowtex (registered trademark)-50", "Snowtex (registered trademark)-CXS" (all manufactured by Nissan Chemical Industries, Ltd.), and product names "Adelite (registered trademark) AT-30", "Adelite (registered trademark) AT-40", "Adelite (registered trademark) AT-50" (all manufactured by Nippon Aerosil Co., Ltd.).
[0100] (Reactive silicone oil)
[0101] The coating film-forming composition of the present embodiment preferably further contains a reactive silicone oil. The reactive silicone oil refers to a silicone oil having a reactive group at at least one of both ends, one end, and a side chain of a main chain formed by a siloxane bond.
[0102] The coating film formed by the composition containing reactive silicone oil increases the water contact angle due to the reactive silicone oil, and achieves a balance, thereby showing easy cleaning properties not only for coal and cement but also for paint as oily dirt. The mechanism of action is uncertain, but it is speculated that the reactive silicone oil is induced by the functional groups of the oily dirt to transfer to the surface, and the oil is interposed at the interface between the oily dirt and the coating film. It should be noted that the present invention is not limited to this mechanism of action.
[0103] The main chain (main skeleton) formed by the above-mentioned siloxane bond is not limited, and poly (dimethylsiloxane) etc. can be preferably used in particular. In addition, as a reactive group, it is not particularly limited as long as it is a polar atomic group showing reactivity, and examples include polar functional groups containing oxygen atoms, nitrogen atoms, sulfur atoms, etc. that attract each other with hydroxyl groups present on the side of oily dirt. Specifically, for example, hydrogen atoms, hydroxyl groups, amino groups, aminoalkyl groups, methanol groups, epoxy groups, carboxyl groups, mercapto groups, etc. can be mentioned. These reactive groups can have one type alone, or they can have two or more types.
[0104] Among them, from the viewpoint of easy cleaning of coatings as oily stains, as reactive silicone oils, amino-modified silicone oils having an amino group or an aminoalkyl group as a reactive group, epoxy-modified silicone oils having an epoxy group as a reactive group, and mercapto-modified silicone oils having a mercapto group as a reactive group are preferred, and amino-modified silicone oils are particularly preferred.
[0105] Amino-modified silicone oil is a silicone oil having a structure in which a part of the methyl groups of the silicone oil is substituted with amino groups or aminoalkyl groups. It should be noted that the modified site may be any of a side chain, a single end, both ends, or both ends of a side chain. In addition, it may also be an emulsion type.
[0106] As the amino-modified silicone oil, a commercially available amino-modified silicone oil can be used as it is. In particular, an amino-modified silicone oil represented by the following general formula (1) is preferably used. By using the amino-modified silicone oil represented by the formula (1), high reliability can be obtained.
[0107] [Chemical formula 1]
[0108]
[0109] In the above formula (1), R1, R2, and R3 are amino-modified alkyl groups or amino groups, for example, -C3H6-NH2, -C6H4-NH2, -C3H6-NH-C2H4-NH2, -C3H6-NH-CH3, -NH2, etc. Furthermore, R1, R2, and R3 may be the same or different from each other. In addition, R1, R2, and R3 may include any one or more of an alkyl group, an epoxy group, a carboxyl group, a methacryloyl group, a methanol group, a hydroxyl group, a mercapto group, a polyether group, a phenyl group, a fluoroalkyl group, an aralkyl group, and hydrogen.
[0110] In the above formula (1), the repetition number m is a positive number of 0 to 50, and the repetition number n is a positive number of 0 to 50. The range of m=0 to 20 and the range of n=0 to 20 are particularly preferred.
[0111] As the amino-modified silicone oil represented by the above formula (1), in the formula (1), dimethyl polysiloxane modified with aminopropyl groups at both ends, wherein m=0 to 40 and n=0 to 40, is generally particularly preferably used. Among them, dimethyl polysiloxane modified with aminopropyl groups at both ends, wherein m=0 to 20 and n=0 to 20, is preferably used.
[0112] Amino-modified silicone oils such as the amino-modified silicone oil represented by the above general formula (1) can be obtained by a conventionally known production method.
[0113] Examples of the amino-modified silicone oil include KF-868, KF-865, KF-864, KF-859, KF-393, KF-860, KF-877, KF-880, KF-8004, KF-8002, KF-8005, KF-867, X-22-3820W, KF-869, KF-861, X-22-3939A, PAM-E, KF-8010, X-22-161A, X-22-161B, KF-8012, KF-8008, X-22-1660B-3, KF-857, KF-8001, KF-862, X-22-9192, KF-858, Dow BY16-205, FZ-3760, SF8417, BY16-849, BY16-892, FZ-3785, BY16-872, BY16-213, BY16-203, BY16-898, BY16-890, BY16-891, BY16-893, BY16-871, BY16-853U, Chisso; FM-3311, FM-3321, FM-3325, Momentive Performance Materials Co., Ltd. TSF4702, TSF4703, TSF4704, TSF4705, TSF4706, TSF4707, TSF4708, TSF4709, XF42-B1989, XF42-B8922, XF42-C0330, XF49-C1109, SILSOFT A-553, SILSOFT A-843, SILSOFT A-858, XF42-A3335, WACKER L652, WACKER L653, WACKER L655, WACKER L656, WACKER FINISH WR1100, WACKER FINISH WR1200, WACKER FINISH manufactured by Wacker Asahikasei Silicone WR1300, WACKER FINISHWR1600, WACKER FINISH WT1250, WACKER FINISH WT1650, etc.
[0114] Examples of the emulsion type include POLON-MF-14, POLON-MF-14E, POLON-MF-14EC, POLON-MF-29, POLON-MF-39, POLON-MF-44, POLON-MF-52, KM-907, X-52-2265, POLON-MF-51, KM-9771, and POLON-MF-63 manufactured by Shin-Etsu Chemical Co., Ltd.; FZ-4632, FZ-4635, FZ-4640, FZ-4645, FZ-4658, FZ-4671, and FZ-4678 manufactured by Nippon Junker Co., Ltd.; and DOWSIL™ FZ-4634EX, DOWSIL™ FZ-4658, and DOWSIL™ SM manufactured by Dow Corning Toray Co., Ltd. 8709SR emulsion, SM8704C / SM8904, WACKER (registered trademark) FINISH CT 45E manufactured by Wacker Asahikasei Silicone Co., Ltd., and the like.
[0115] Epoxy-modified silicone oil is a silicone oil having a structure in which a portion of the methyl groups of the silicone oil are substituted with epoxy groups. It should be noted that the modified site may be any of a side chain, a single end, both ends, or both ends of a side chain.
[0116] As the epoxy-modified silicone oil, a generally commercially available epoxy-modified silicone oil can be used as it is. Examples of the epoxy-modified silicone oil include X-51-1264, POLON-MF-18T, X-22-343, KF-101, KF-1001, X-22-2000, X-22-2046, KF-102, X-22-163, KF-105, X-22-163A, X-22-163B, X-22-163C, X-22-169AS, X-22-169B, X-22-173BX, X-22-173DX, and X-22-9002 manufactured by Shin-Etsu Chemical Co., Ltd., and DOWSIL™ BY 22-818EX Emulsion, DOWSIL™ BY 22-893, and DOWSIL™ BY 22-9004 manufactured by Dow Corning Toray Co., Ltd. FZ-4602, DOWSILtm SM8716EX emulsion, etc.
[0117] Mercapto-modified silicone oil is a silicone oil having a structure in which a part of the methyl groups of the silicone oil is substituted with mercapto groups. It should be noted that the modified site may be any of a side chain, a single terminal, both terminals, or both terminals of a side chain.
[0118] As the mercapto-modified silicone oil, a commercially available mercapto-modified silicone oil can be used as it is. Examples of the mercapto-modified silicone oil include KM-9769, KF-2001, KF-2004, X-22-167B, and X-22-167C manufactured by Shin-Etsu Chemical Co., Ltd.
[0119] The content of the reactive silicone oil in the composition is preferably 0.1 to 100 parts by mass, more preferably 3 to 50 parts by mass, relative to 100 parts by mass of the water-based resin. Within such a range, the reactive silicone oil increases the water contact angle and achieves a balance, thereby making it easy to clean not only coal and cement but also coatings for oily dirt. The reactive silicone oil may be used alone or in combination of two or more.
[0120] In addition, the content of the amino-modified silicone oil in the above composition is preferably 0.1 to 100 parts by mass, and more preferably 3 to 50 parts by mass, based on the content relative to 100 parts by mass of the water-based resin. If it is within such a range, the amino-modified silicone oil increases the water contact angle and achieves a balance, thereby showing easy cleaning properties not only for coal and cement, but also for coatings as oily dirt. The amino-modified silicone oil can be used alone or in combination of two or more.
[0121] <Elastic modulus of coating sample 1 for measurement: 100 MPa or more>
[0122] The elastic modulus of the coating film sample 1 for measurement produced by the coating film-forming composition of the present embodiment by the method described below is 100 MPa or more.
[0123] Preparation method of coating sample 1 for measurement: the coating film-forming composition is applied on the surface of a PET film having a thickness of 75 μm so as to have a WET thickness of 500 μm, and dried at 22° C. for 24 hours to form a coating film on the PET film. The coating film is cut so as to have an area of 10 mm×100 mm, thereby preparing coating sample 1 for measurement.
[0124] Here, the WET thickness refers to the film thickness immediately after coating.
[0125] The elastic modulus of the coating film sample 1 for measurement can be measured, for example, by peeling the coating film from the PET film of the sample and measuring the coating film using a tensile tester (Autograph AGX-V, manufactured by Shimadzu Corporation).
[0126] When the elastic modulus is 100 MPa or more, the cleaning property of coal, cement, etc. is excellent. The elastic modulus is preferably 150 MPa or more, and more preferably 200 MPa or more.
[0127] <Contact Angle>
[0128] With regard to the coating film forming composition of the present embodiment, from the viewpoint of easy cleaning from coal and cement, the contact angle of the coating film sample 2 for measurement prepared by the following method is preferably 10° to 100°, and from the viewpoint of easy cleaning from coal, cement and paint, it is preferably 60° to 100°.
[0129] Preparation method of coating film sample 2 for measurement: the coating film-forming composition was applied to the surface of a 75 μm thick PET film to a WET thickness of 500 μm, and dried at 22° C. for 24 hours to form a coating film on the PET film, thereby preparing coating film sample 2 for measurement.
[0130] For the coating sample 2 for measurement, the contact angle is measured as follows: 2 μL of water is dropped onto the coating surface, and the water contact angle of the coating surface after 5 minutes is measured by a sessile drop method based on JIS R 3257 using a contact angle meter (e.g., DropMaster, DM-701, manufactured by Kyowa Interface Science Co., Ltd.).
[0131] More specifically, in the embodiment in which the coating film-forming composition of the present embodiment has particularly excellent cleaning properties for coal and cement, the lower the contact angle, the more preferably it is, preferably 100° or less, more preferably 90° or less, further preferably 80° or less, further preferably 70° or less, and particularly preferably 60° or less. By setting the contact angle to the above range, excellent cleaning properties for coal, cement, etc. are achieved.
[0132] In addition, in the embodiment of the coating film forming composition of the present embodiment, in addition to the excellent cleaning property of coal and cement, the above-mentioned contact angle is more preferably 60° or more, and more preferably 65° or more. In addition, it is preferably 100° or less, more preferably 90° or less, and more preferably 85° or less. By making the above-mentioned contact angle into the above-mentioned range, the easy cleaning property of coal, cement and coating is excellent. In the case of this mode, the coating film forming composition particularly preferably contains the above-mentioned reactive silicone oil, especially amino-modified silicone oil.
[0133] (Other ingredients)
[0134] In the scope of not damaging the effect of the present invention, the film-forming composition of the present embodiment can include any appropriate other oils. As such other oils, for example, various non-reactive silicone oils such as dimethyl silicone oil, phenyl-modified silicone oil, long-chain alkyl-modified silicone oil, liquid paraffin, surfactant, liquid hydrocarbon, fluorinated oil, wax, petrolatum, animal fat, fatty acid, etc. can be enumerated. These can be only one kind, or can be more than two kinds.
[0135] When the coating film-forming composition contains such other oil, the easy cleaning property of the coating film may be further improved.
[0136] The coating film forming composition may contain any other appropriate additives within the scope of not impairing the effects of the present invention. Examples of other additives include ultraviolet absorbers, light stabilizers, antioxidants, anti-aging agents, antistatic agents, pigments, colorants, leveling agents, and tackifiers.
[0137] The coating film can be formed by applying the coating film-forming composition of the present embodiment to an adherend and drying it. Even if it is dried at room temperature (25° C.), a highly uniform coating film can be obtained.
[0138] As a coating method, it can be directly applied to any adherend by a known coating method such as spray coating, brush coating, roll coating, curtain coating, roll coating, dip coating, or coater.
[0139] Specific examples of adherends include metal products, wood products, plastic products, glass products, medical parts (e.g., catheters, stents, gloves, tweezers, containers, guides, trays, etc.), painting-related parts (e.g., robot arms, paint booths, hangers, covers, ovens, etc.), buildings (interior and exterior wall surfaces, floor surfaces, and ceiling surfaces), electronic equipment, transportation equipment (e.g., vehicles such as automobiles, two-wheeled vehicles, and railways, and ships, etc.), and various other structures, as well as structural parts constituting them.
[0140] <Coating>
[0141] The coating film of the present embodiment is formed from the above-mentioned coating film-forming composition and is a coating film having excellent surface cleanability.
[0142] The thickness of the coating film can be any appropriate thickness according to the purpose, use environment, etc. The thickness of the coating film is preferably 50 μm to 1000 μm, and more preferably 80 μm to 500 μm. If the thickness of the coating film is 50 μm or more, the effect of protecting the adherend can be fully obtained. In addition, if the thickness of the coating film is 1000 μm or less, the operating efficiency when forming the coating film is excellent.
[0143] The film thickness of the coating film can be measured using, for example, RI-205 manufactured by PEAKOCK.
[0144] <Articles with coating>
[0145] The coated article of this embodiment has the above-mentioned coating. By applying the above-mentioned coating-forming composition to an adherend (article) and drying, a coated article having a coating can be obtained. A highly uniform coating can also be obtained by drying at room temperature (25° C.). The coating method and adherend of the coating-forming composition are as described in the section on the coating-forming composition.
[0146] Example
[0147] Hereinafter, the present invention will be specifically described by way of examples, but the present invention is not limited to these examples. It should be noted that the following "parts" means "parts by mass".
[0148] <Elastic modulus>
[0149] Using an applicator (YBA type Baker applicator, manufactured by Yoshimitsu Seiki), the coating film forming composition of each embodiment and comparative example was applied to the surface of a PET film (Lumirror S10#75, manufactured by Toray Co., Ltd.) having a thickness of 75 μm in a manner such that the WET thickness was 500 μm, and dried at 22° C. for 24 hours to form a coating film, which was cut out in a manner such that the area of the coating film became 10 mm×100 mm to obtain a coating film sample 1 for measurement. The coating film was peeled off from the PET film of the coating film sample 1 for measurement, and the elastic modulus of the coating film was evaluated using a tensile tester (Autograph AGX-V, manufactured by Shimadzu Corporation). The results are shown in Tables 1 to 3.
[0150] <Contact Angle>
[0151] Using an applicator (YBA type Baker applicator, manufactured by Yoshimitsu Seiki), the coating film-forming composition of each embodiment and comparative example was applied to the surface of a PET film (Lumirror S10#75, manufactured by Toray Co., Ltd.) having a thickness of 75 μm in a manner such that the WET thickness was 500 μm, and dried at 22° C. for 24 hours to form a coating film, thereby preparing a coating film sample 2 for measurement. For the coating film sample 2 for measurement, 2 μL of water was dropped onto the coating film surface, and the water contact angle of the coating film surface after 5 minutes was measured using a contact angle meter (DropMaster, DM-701, manufactured by Kyowa Interface Science Co., Ltd.) by a sessile drop method based on JIS R 3257. The results are shown in Tables 1 to 3.
[0152] <Evaluation test of coal dirt cleanability>
[0153] The coal dirt cleanability evaluation test is based on JSTM J 7602:2003: Pollution promotion test method for building exterior wall materials. Figure 3Specifically, first, 10 mg of carbon black (Orion Engineered Carbons, FW200), 45 mg of Kanto loam (8 kinds of JIS test powder 1 made by APPIE), 135 mg of yellow ochre (PG230 made by Holbein Works), and 10 mg of silica (3 kinds of JIS test powder 1 made by APPIE) were added to 200 mL of water, and the mixture was stirred at 1000 rpm for 3 minutes using a Homo Disper to obtain a contaminated liquid.
[0154] Then, the color difference of the above-mentioned coating sample 2 for measurement was measured using a colorimeter (manufactured by Konica Minolta, CR-20) and used as the "initial hue" (L1, a1, b1). Then, 0.5 mL of the contaminated liquid was dripped onto the surface of the above-mentioned coating sample 2 for measurement using a Pipetman (automatic pipette), dried overnight, and the contaminated part was wiped with a cloth moistened with water, and the hue of the same part was measured and used as the "hue after cleaning" (L2, a2, b2). The "initial hue" and the "hue after cleaning" were compared, and the color difference ΔE was calculated using the following formula.
[0155] ΔE={(ΔL * ) 2 +(Δa * ) 2 +(Δb * ) 2} 1 / 2
[0156] ΔL=L1-L2
[0157] Δa=a1-a2
[0158] Δb=b1-b2
[0159] It should be noted that L1, a1, and b1 refer to “initial hue”, and L2, a2, and b2 refer to “hue after cleaning”.
[0160] [Evaluation of the cleanability of coal waste]
[0161] The cleanability of coal dust was evaluated according to the following three levels.
[0162] ◎: ΔE≤2.2
[0163] 0: 2.2<ΔE<11
[0164] ×:11≤ΔE
[0165] The results are shown in Tables 1 to 3.
[0166] <Evaluation test of cement dirt cleanability>
[0167] Passed the cement dirt cleanability evaluation test Figure 4 The method shown is carried out. Specifically, first, the above-mentioned coating sample 2 for measurement is adhered to an acrylic resin substrate (transparent, thickness 2mm, 150mm×100mm) with a transparent tape to obtain a test piece. Add 100g of water and 30g of cement (ordinary Portland cement made by household chemicals) to a disposable measuring cup 300mL, stir with a spatula for 2 minutes to obtain cement slurry. On the surface of the test piece, place 3cm of the end of a pure cotton water line (No.10 made by Takumi, line thickness 1.1mm, length 23cm) into a vinyl chloride ring frame (inner diameter 25mm, outer diameter 32mm, height 1cm), and pour 10g of cement slurry from the top, fill the ring frame with cement slurry, and form a cement attachment. Make 5 cement attachments for 1 sample. A loop was made at the end of the pure cotton waterline exposed from the cement attachment, and the loop of the pure cotton waterline was hung on a tensile testing machine (MX2-500N manufactured by IMADA, dynamometer: ZTS-500N manufactured by IMADA), and the cement attachment was stretched to obtain the peeling force on the sample as the cement adhesion.
[0168] [Evaluation of the cleanability of cement dirt]
[0169] The cleanability of cement stains was evaluated according to the following two levels.
[0170] 0: Cement adhesion <5 (N)
[0171] ×: 5(N)≤cement adhesion
[0172] The results are shown in Tables 1 to 3.
[0173] <Evaluation test for easy cleaning of paint stains>
[0174] The paint dirt cleanability evaluation test is based on JIS K 5600 5-6 (1999): cross-cut test method. Figure 5 The method shown is carried out. Specifically, first, a coating film-forming composition of each embodiment and comparative example with a liquid film thickness of 100 μm is applied to an electrogalvanized steel plate (bonded steel plate; 100×150×2 mm) with a brush, and the test piece is dried for 1 day. An oil-based paint with a liquid film thickness of 100 μm is applied to the test piece with a brush, and after drying at room temperature for 1 day, a grid is made with a width of 4 mm, and a tape (manufactured by Nitto Denko, No. 31B) is firmly attached, and the test piece is peeled upward. Confirm the residue of the paint stain and evaluate it with a score of 0-10. If there is no residue, it is 0 points, and if all residues remain, it is 10 points.
[0175] The paint stain cleanability was evaluated according to the following two levels.
[0176] 0: 0-2 points
[0177] ×: 3-10 points
[0178] The results are shown in Tables 1 to 3.
[0179] <Easy to clean evaluation>
[0180] The above-mentioned cleanability tests (coal stain cleanability evaluation test, cement stain cleanability evaluation test, and paint stain cleanability evaluation test) were evaluated as follows. The results are shown in Tables 1 to 3.
[0181] [Evaluation (coal + cement)]
[0182] ◎: The cleanability of coal dirt is ◎, and the cleanability of cement dirt is 0.
[0183] 0: The cleanability of coal dirt is 0, and the cleanability of cement dirt is 0.
[0184] ×: At least one of the coal stain cleanability and the cement stain cleanability is ×.
[0185] [Evaluation (coal + cement + paint)]
[0186] ◎: The cleanability of coal dirt is ◎, the cleanability of cement dirt is 0, and the cleanability of paint dirt is 0.
[0187] 0: The cleanability of coal dirt is 0, the cleanability of cement dirt is 0, and the cleanability of paint dirt is 0.
[0188] △: The cleanability of coal dirt is ◎ or 0, the cleanability of cement dirt is 0, and the cleanability of paint dirt is ×.
[0189] ×: The cleanability of coal stains is 0 or ×, the cleanability of cement stains is ×, and the cleanability of paint stains is ×.
[0190] <Preparation of coating film forming composition>
[0191] (Example 1)
[0192] Using Homo Disper (Laborution, manufactured by PRIMIX), Superflex 420 (100 parts (hereinafter, the resin solid content weight is converted to 100 parts)) and POLON-MF-14EC (5 parts) were stirred at 2000 rpm for 1 minute, and Snowtex C (12.5 parts) was slowly added while stirring at 2000 rpm. After all the addition, the mixture was stirred at 3000 rpm for 3 minutes to obtain the coating film-forming composition of Example 1.
[0193] (Examples 2 to 28, Comparative Examples 1 to 4)
[0194] Coating film-forming compositions of Examples 2 to 28 and Comparative Examples 1 to 4 were obtained in the same manner as in Example 1 except that the types and contents of the components were changed as described in Tables 1 to 3. In addition, "-" in Tables 1 to 3 means that the component is not contained.
[0195] In addition, the details of each component in Table 1 to Table 3 are as follows.
[0196] <Polyurethane resin>
[0197] Superflex 420: Made by Daiichi Industrial Pharmaceutical Co., Ltd.
[0198] ·ST-008E: Made by Ube Industries
[0199] ·UW-1005E: Made by Ube Industries
[0200] SF460: Made by Ube Industries
[0201] <Colloidal Silica>
[0202] Snowtex 30: Made by Nissan Chemical Co., Ltd.
[0203] Snowtex C: Made by Nissan Chemical Co., Ltd.
[0204] Snowtex CM: Made by Nissan Chemical Co., Ltd.
[0205] <Reactive Silicone Oil>
[0206] (Amino modified silicone oil)
[0207] ·POLON-MF-14EC: Made by Shin-Etsu Chemical Co., Ltd.
[0208] ·POLON-MF-14E: Made by Shin-Etsu Chemical Co., Ltd.
[0209] ·POLON-MF-14: Made by Shin-Etsu Chemical Co., Ltd.
[0210] ·KM-9771: Made by Shin-Etsu Chemical Co., Ltd.
[0211] (Epoxy modified silicone oil)
[0212] ·X-51-1264: Made by Shin-Etsu Chemical Co., Ltd.
[0213] (Mercapto modified silicone oil)
[0214] ·KM-9769: Shin-Etsu Chemical Co., Ltd. <Non-reactive silicone oil>
[0215] (Phenyl modified silicone oil)
[0216] KM-9739: Made by Shin-Etsu Chemical Co., Ltd. (long-chain alkyl-modified silicone oil)
[0217] ·X-52-8046: Made by Shin-Etsu Chemical Co., Ltd. (dimethyl silicone oil)
[0218] ·KM-862T: Made by Shin-Etsu Chemical Co., Ltd. [Table 1]
[0219]
[0220] [Table 2]
[0221]
[0222] [Table 3]
[0223]
[0224] As shown in Tables 1 to 3, the coating film-forming compositions of Examples 1 to 28 contain aqueous resins and colloidal silica, and the coating films produced using the compositions have an elastic modulus of 100 MPa or more, indicating that they are excellent in terms of cleanability against coal stains and cement stains.
[0225] In addition, in the coating film-forming compositions of the examples, as the contact angle was low, the tendency was observed that the cleaning properties of soot stains and cement stains were more excellent.
[0226] Furthermore, in the coating film-forming compositions of the Examples, when the contact angle was in the range of 60° to 100°, a tendency was observed to show excellent cleaning properties against not only coal stains and cement stains but also paint stains.
[0227] Furthermore, it was found that among the coating film-forming compositions of the Examples, the coating film-forming composition containing the reactive silicone oil was excellent in the ease of cleaning of paint stains.
[0228] On the other hand, the coating film-forming compositions of Comparative Examples 1 to 3 had a coating film having an elastic modulus as low as less than 100 MPa, and thus had poor cleaning properties against cement stains.
[0229] In addition, the coating film forming composition of Comparative Example 4 does not contain colloidal silica, so the result is that the cleaning property of cement dirt is poor. Therefore, even if the elastic modulus of the coating film formed by the coating film forming composition is 100 MPa or more, when the composition does not contain colloidal silica, the effect of using it in combination with the water-based resin cannot be obtained, indicating that the effect of improving the cleaning property of cement dirt is not obtained.
[0230] In the above, various embodiments are described with reference to the accompanying drawings, but the present invention is certainly not limited to the relevant examples. It should be understood that those skilled in the art can think of various variations or modifications within the scope of the claims, which also belong to the technical scope of the present invention. In addition, the various constituent elements in the above embodiments may also be combined arbitrarily without departing from the scope of the gist of the invention.
[0231] It should be noted that the present application is based on the Japanese patent application (Japanese Patent Application No. 2022-050819) filed on March 25, 2022, the contents of which are incorporated herein by reference.
[0232] Description of Reference Numerals
[0233] 21 coating
[0234] 22Coal, cement, etc.
[0235] 31 Adhesive
Claims
1. A coating film-forming composition comprising an aqueous resin and colloidal silica, in, The elastic modulus of the coating film sample 1 for measurement prepared by the following method is 100 MPa or more. Preparation method of coating sample 1 for measurement: the coating film-forming composition is applied on the surface of a PET film having a thickness of 75 μm so as to have a WET thickness of 500 μm, and dried at 22° C. for 24 hours to form a coating film on the PET film, and the coating film is cut so as to have an area of 10 mm×100 mm, thereby preparing coating sample 1 for measurement.
2. The coating film-forming composition according to claim 1, wherein The content of the colloidal silica is 30 parts by mass or less relative to 100 parts by mass of the aqueous resin.
3. The coating film-forming composition according to claim 1, wherein The water-based resin is a polyurethane-based resin. The coating film-forming composition according to claim 1 , further comprising a reactive silicone oil.
5. The coating film-forming composition according to claim 4, wherein The reactive silicone oil is amino-modified silicone oil.
6. The coating film-forming composition according to claim 1, wherein The contact angle of the coating sample 2 for measurement prepared by the following method is 60° to 100°. Preparation method of coating film sample 2 for measurement: the coating film-forming composition was applied to the surface of a 75 μm thick PET film to a WET thickness of 500 μm, and dried at 22° C. for 24 hours to form a coating film on the PET film, thereby preparing coating film sample 2 for measurement. 7 . A coating film formed from the coating film-forming composition according to claim 1 .
8. A coated article comprising the coating according to claim 7.