Sputtering target, method for producing sputtering target, oxide semiconductor thin film, thin film semiconductor device, and method for producing thin film semiconductor device

By using an oxide film composed of indium, magnesium and tin as a cap layer, the problems of mobility and etching damage in the IGZO thin film transistor are solved, and high mobility and high-fine thin film transistors are achieved, which suppresses the influence of hydrogen and the rise of threshold voltage. .

CN118922579APending Publication Date: 2024-11-08ULVAC INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202380029003.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-25
Filing Date
2023-02-16
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the high mobility applications, the mobility of the existing IGZO thin film transistors is difficult to exceed 10 cm2/Vs, and the etching damage of the active layer and the hydrogen influence suppression effect generated by the CVD process are insufficient, and the threshold voltage rise problem is caused.

Method used

An oxide film composed of indium, magnesium and tin is used as a cap layer with high mobility, and a suitable oxide semiconductor film and film laminate is formed through a specific composition ratio and a manufacturing method, and is used in a thin film semiconductor device.

Benefits of technology

A thin film transistor with a mobility of more than 10 cm2/Vs was realized, which suppressed the influence of etching damage and hydrogen generated by the CVD process, improved the mobility and resistance value of the thin film transistor, and ensured high-fine patterning and good TFT characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922579A_ABST
    Figure CN118922579A_ABST
Patent Text Reader

Abstract

A sputtering target comprising a sintered oxide containing an oxide of the formula InXMgYSnZ consisting of indium, magnesium and tin, in which X is from 0.32 to 0.65 (inclusive), Y is from 0.17 to 0.46 (inclusive), and Z is greater than 0 to 0.22 (inclusive) and is within the range of X + Y + Z = 1.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a sputtering target, a method for manufacturing a sputtering target, an oxide semiconductor thin film, a thin film semiconductor device and a method for manufacturing the same. Background Art

[0002] Thin-film transistors (TFTs) using In-Ga-Zn-O-based oxide semiconductor films (IGZO) as active layers can achieve higher mobility than TFTs using conventional amorphous silicon films as active layers. Therefore, they have been widely used in various displays in recent years (for example, refer to patent documents 1 to 3).

[0003] For example, Patent Document 1 discloses an organic EL display device in which the active layer of a TFT driving an organic EL element is composed of IGZO. Patent Document 2 discloses an organic EL display device in which the channel layer (active layer) is composed of a-IGZO and has a mobility of 5 cm 2 Patent Document 3 discloses a thin film transistor in which an active layer is composed of IGZO and an on / off current ratio is 5 digits or more.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2009-31750

[0007] Patent Document 2: Japanese Patent Application Publication No. 2011-216574

[0008] Patent Document 3: WO2010 / 092810 Summary of the invention

[0009] Problems to be solved by the invention

[0010] In recent years, due to the requirements for higher resolution, lower power consumption, and higher frame rate in various displays, the demand for oxide semiconductors showing higher mobility has been increasing. However, in thin-film transistors using IGZO in the active layer, the mobility is difficult to exceed 10 cm 2 / Vs, it is necessary to develop materials for thin film transistors that show higher mobility.

[0011] Although development of a cap layer that suppresses etching damage to the active layer and the influence of hydrogen generated in the CVD process has been progressed, there is a problem that the suppressive effect is not sufficient.

[0012] In addition, if used for an active layer having high mobility, there occurs a problem that the rise in the threshold voltage for switching the current from being cut off to being on will shift.

[0013] In view of the above actual situation, the purpose of the present invention is to apply a sputtering target and a manufacturing method of an oxide semiconductor thin film capable of forming a cap layer suitable for an active layer with high mobility, an oxide semiconductor thin film and an oxide semiconductor thin film stack, and further a thin film semiconductor device and a manufacturing method thereof.

[0014] Means for solving problems

[0015] As a result of repeated studies to achieve the above object, the inventors found that an oxide thin film containing indium, magnesium, and tin is suitable as a high-mobility cap layer, and completed the present invention.

[0016] The present invention is as follows.

[0017] The first embodiment of the present invention is a sputtering target comprising a material of the formula In consisting of indium, magnesium and tin. X Mg Y Sn Z The oxide sintered body is composed of an oxide of, in which X of the above formula is greater than 0.32 and less than 0.65, Y is greater than 0.17 and less than 0.46, Z is greater than 0 and less than 0.22, and is in the range of X+Y+Z=1.

[0018] A second embodiment of the present invention is the sputtering target of the first embodiment, wherein the oxide sintered body further contains at least one element selected from Si, Ti, W, Zr, Nb, Ni, Ge, Ta, Al and Y, that is, an A group element.

[0019] The third scheme of the present invention is a sputtering target of the second scheme, wherein Si is less than 4at%, Ti is less than 6at%, W is less than 6at%, Zr is less than 7at%, Nb is less than 7at%, Ni is less than 7at%, Ge is less than 7at%, Ta is less than 8at%, Al is less than 8at%, and Y is less than 9at%, and the content of the A group elements is less than 10at%.

[0020] A fourth embodiment of the present invention is a sputtering target according to any one of the first to third embodiments, wherein the oxide sintered body further contains at least one element selected from the group consisting of Mo, Sb, Hf, La, Fe, Ga, Zn, Ca and Sr, i.e., a B group element.

[0021] The fifth scheme of the present invention is a sputtering target of the fourth scheme, wherein Mo is less than 10at%, Sb is less than 13at%, Hf is less than 13at%, La is less than 13at%, Fe is less than 21at%, Ga is less than 27at%, Zn is less than 38at%, Ca is less than 38at%, Sr is less than 38at%, and the total content of elements other than In, Mg and Sn is less than 38at%.

[0022] A sixth aspect of the present invention is the sputtering target according to any one of the first to fifth aspects, wherein the relative density is 90% or more.

[0023] A seventh aspect of the present invention is a method for producing a sputtering target, wherein indium oxide powder, magnesium oxide powder and tin oxide powder are mixed to form a compact, and the compact is sintered at 1100° C. to 1650° C. to produce a sputtering target having an oxide sintered body.

[0024] The eighth embodiment of the present invention is a method for manufacturing a sputtering target, wherein oxides, hydroxides or carbonates of indium, magnesium and tin are mixed, a precursor powder pre-sintered at 1000°C to 1500°C is molded to form a molded body, and the molded body is sintered at a temperature above 1100°C and below 1650°C to manufacture a sputtering target having an oxide sintered body.

[0025] A ninth aspect of the present invention is an oxide semiconductor thin film, which is composed of an oxide semiconductor, wherein the oxide semiconductor is a thin film of a formula In composed of indium, magnesium and tin. X Mg Y Sn Z The oxide is the main component, X in the above formula is greater than 0.32 and less than 0.65, Y is greater than 0.17 and less than 0.46, Z is greater than 0 and less than 0.22, and is in the range of X+Y+Z=1.

[0026] A tenth aspect of the present invention is the oxide semiconductor thin film according to the ninth aspect, wherein an etching rate when etching is performed with a sulfuric acid, nitric acid-based etchant or an acetic acid-based etchant is 1 nm / sec or more.

[0027] An eleventh aspect of the present invention is the oxide semiconductor thin film of the ninth or tenth aspect, wherein the band gap is 2.5 eV to 3.4 eV, and the resistance value after hydrogen annealing is 1E+2Ω / □ or more.

[0028] The twelfth embodiment of the present invention is the oxide semiconductor film of the ninth to eleventh embodiments, which further contains at least one element selected from Si, Ti, W, Zr, Nb, Ni, Ge, Ta, Al, Y and Mo, i.e., group A elements.

[0029] The thirteenth embodiment of the present invention is the oxide semiconductor film of the twelfth embodiment, wherein Si is less than 4at%, Ti is less than 6at%, W is less than 6at%, Zr is less than 7at%, Nb is less than 7at%, Ni is less than 7at%, Ge is less than 7at%, Ta is less than 8at%, Al is less than 8at%, and Y is less than 9at%, and the content of the A group elements is less than 10at%.

[0030] More preferably, the oxide semiconductor film has high resistance and Eg is in a range where it does not increase (Eg≤3.4).

[0031] The fourteenth embodiment of the present invention is the oxide semiconductor film of the ninth to thirteenth embodiments, which further contains at least one element selected from Mo, Sb, Hf, La, Fe, Ga, Zn, Ca and Sr, that is, a B group element.

[0032] The fifteenth scheme of the present invention is the oxide semiconductor film of the fourteenth scheme, wherein Mo is less than 10at%, Sb is less than 13at%, Hf is less than 13at%, La is less than 13at%, Fe is less than 21at%, Ga is less than 27at%, Zn is less than 38at%, Ca is less than 38at%, Sr is less than 38at%, and the total content of elements other than In, Mg and Sn is less than 38at%.

[0033] More preferably, the oxide semiconductor film has high resistance and Eg is in a range where it does not increase (Eg≤3.4).

[0034] A sixteenth aspect of the present invention is an oxide semiconductor thin film stack including: an active layer composed of a high-mobility oxide semiconductor thin film; and a cap layer composed of the oxide semiconductor thin film of any of the ninth to fifteenth aspects stacked on the active layer.

[0035] A seventeenth aspect of the present invention is the oxide semiconductor thin film stack according to the sixteenth aspect, wherein an etching ratio is appropriate when the cap layer is patterned together with the active layer.

[0036] An eighteenth aspect of the present invention is a thin-film semiconductor device comprising a cap layer composed of the oxide semiconductor thin film according to any of the ninth to fifteenth aspects.

[0037] A nineteenth aspect of the present invention is the thin-film semiconductor device of the eighteenth aspect, wherein the cap layer is provided so as to cover the active layer composed of the high-mobility oxide semiconductor thin film.

[0038] The twentieth embodiment of the present invention is a thin-film semiconductor device of the eighteenth or nineteenth embodiment, comprising: a gate electrode; a gate insulating film arranged on the gate electrode; an active layer arranged on the gate insulating film and composed of a high-mobility oxide semiconductor thin film; a cap layer arranged in a manner covering the active layer; and a source electrode and a drain electrode connected to the active layer and the cap layer.

[0039] The twenty-first embodiment of the present invention is a method for manufacturing a thin-film semiconductor device having a cap layer composed of the oxide semiconductor thin film of the ninth to fifteenth embodiments, wherein a gate insulating film is formed on a gate electrode, an active layer composed of a high-mobility oxide semiconductor thin film is formed on the gate insulating film by a sputtering method, the cap layer is formed on the active layer by a sputtering method, the stacked film of the active layer and the cap layer is patterned to form a metal layer with the patterned active layer and the cap layer as a base film, and the metal layer is patterned by a wet etching method to form a source electrode and a drain electrode.

[0040] Effects of the Invention

[0041] The oxide thin film containing indium, magnesium and tin of the present invention is most suitable as a high-mobility cap layer, which can suppress etching damage and the influence of hydrogen generated in the CVD process. When using this cap layer, a mobility exceeding 10 cm 2 / Vs thin film transistor.

[0042] In addition, the cap layer of the present invention can become a zinc-free oxide semiconductor film, which can be etched with sulfuric acid, nitric acid or acetic acid etchants, and can therefore be well patterned together with a high-mobility active layer. Through high-precision patterning, a high-definition thin-film transistor can be realized. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 This is a graph showing the range of the etching rate of 1 nm / sec for a ternary composite oxide thin film of In, Mg, and Sn.

[0044] Figure 2 This is a graph showing the range of the band gap being 3.4 eV or less for a ternary composite oxide thin film of In, Mg, and Sn.

[0045] Figure 3 This is a graph showing that the resistance value after hydrogen annealing for a ternary composite oxide thin film of In, Mg, and Sn is in the range of 1E+2Ω / □ or more.

[0046] Figure 4 To show that Figures 1 to 3 A diagram of the combined range of the range.

[0047] Figure 5 To show that In in the ternary composite oxide of In, Mg and Sn X Mg Y Sn Z A diagram showing that X, Y, and Z are in the range of Y>X / 2+2Z.

[0048] Figure 6 A diagram showing a schematic structure of an example of a thin film transistor according to the present invention.

[0049] Figure 7 A diagram showing a schematic configuration of an example of a manufacturing process of a thin film transistor according to the present invention.

[0050] Figure 8 A diagram showing a schematic configuration of an example of a manufacturing process of a thin film transistor according to the present invention.

[0051] Fig. 9 The figure shows the results of comparing the S value when the substrate temperature is changed during CVD film formation of the protective layer 16 in the case where the thin film transistor has a cap layer 14 composed of an oxide semiconductor thin film (stacked) and the case where the cap layer 14 is not provided (single layer).

[0052] Fig.10 This is a diagram comparing the Vth of the thin film transistors of Manufacturing Example 1 and Comparative Manufacturing Example 1.

[0053] Fig.11 This is a diagram comparing the Vth of the thin film transistors of Comparative Manufacturing Example 1 and Comparative Manufacturing Example 2. DETAILED DESCRIPTION

[0054] Hereinafter, embodiments of the present invention will be described with reference to the accompanying drawings.

[0055] First, before describing the sputtering target (oxide semiconductor sputtering target) according to the present embodiment, the characteristics of an oxide semiconductor thin film formed using the sputtering target will be described.

[0056] [Oxide semiconductor thin film]

[0057] The oxide semiconductor thin film is used as a cap layer of a high-mobility active layer (inversion layer) in a thin film transistor such as a so-called bottom-gate field effect transistor, for example.

[0058] Here, the high mobility active layer refers to an active layer with a band gap of 3 eV or less. The mobility is 15 cm 2 / V·s or above.

[0059] Typical high-mobility oxide semiconductor materials include ITO (In-Sn-O) and IGZO (In-Ga-Zn-O). Since these oxide semiconductor materials are amorphous in crystallinity immediately after film formation, they can be easily patterned using a wet etching method.

[0060] In addition, the high mobility active layers listed in Table 1 below are proposed, revealing the band gap, carrier concentration and mobility. The band gap is less than 3 eV and the mobility is more than 15 cm 2 / V·s.

[0061] [Table 1]

[0062]

[0063] As described above, a high-mobility active layer tends to have a small band gap Eg and a high carrier concentration, and the oxide semiconductor thin film of the present invention is most suitable for use as a cap layer of such a high-mobility active layer.

[0064] The cap layer is generally provided to suppress etching damage to the active layer. However, the oxide semiconductor thin film of the present invention can suppress the influence of hydrogen generated in the CVD process in addition to suppressing etching damage.

[0065] In the oxide semiconductor thin film of the present invention, the composition of the oxide semiconductor thin film of the following formula composed of indium, magnesium and tin is represented by the formula In X Mg Y Sn Z It means that in the above formula, X is 0.32 or more and 0.65 or less, Y is 0.17 or more and 0.46 or less, Z is greater than 0 and 0.22 or less, and X+Y+Z=1.

[0066] Most of the cap layers known so far contain zinc. However, in the present invention, a cap layer composed of an oxide semiconductor thin film having a composition not containing zinc is realized.

[0067] The cap layer of such a composition can be etched using a sulfuric acid, nitric acid or acetic acid etchant, and the etching rate when etching using a sulfuric acid, nitric acid or acetic acid etchant is 1 nm / sec or more.

[0068] This makes it possible to make the etching rate close to that of the high-mobility active layer, and thus to perform etching treatment together, thereby enabling fine patterning of the stacked body of the active layer and the cap layer to be performed satisfactorily.

[0069] In addition, the etching damage of the active layer can be suppressed, and the influence of hydrogen in the CVD process can be suppressed.

[0070] Among them, sulfuric acid and nitric acid based etchants are etchants mainly composed of sulfuric acid and nitric acid, for example, an etchant containing (H2SO4 (7.6-8.4%) + HNO3 (3.8-4.2%). Acetic acid based etchants are etchants mainly composed of acetic acid (HOOC-COOH).

[0071] As a commonly used etchant, in addition to sulfuric acid, nitric acid etchants or acetic acid etchants, there is a mixed solution of phosphoric acid: H3PO4 less than 80%, nitric acid: HNO3 less than 5%, and acetic acid: CH3COOH less than 10%, namely PAN. When using this PAN, it is preferably contained Zn, but the oxide semiconductor film of the present invention can contain Zn as described in detail later and can also cope with etching using PAN.

[0072] Of course, in this case, the etching rate can be set to an etching rate suitable for the active layer, and the etching damage of the active layer can be suppressed, and the effect of suppressing the influence of hydrogen in the CVD process can be achieved.

[0073] By using such a cap layer of the present invention, a mobility exceeding 10 cm 2 / Vs thin film transistor.

[0074] In addition, when the oxide semiconductor thin film of the present invention is stacked as a cap layer with a high-mobility active layer to form a thin film transistor, the shift of the threshold voltage Vth can be suppressed compared to the case where no cap layer is used, and a thin film transistor with good TFT characteristics can be realized. In addition, the threshold voltage (Vth) is the voltage at which the current switches from the off state to the on state.

[0075] In the composition range of the oxide semiconductor thin film of the present invention, the formula In X Mg Y Sn Z It means that X in the above formula is 0.32 or more and 0.65 or less, Y is 0.17 or more and 0.46 or less, Z is more than 0 and 0.22 or less, and X+Y+Z=1, and this range is determined by the following method.

[0076] In the present invention, In is used as a carrier generator, and Mg is used as a carrier killer. Mg has the function of etching control and the function of a hydrogen absorber for removing hydrogen from CVD. In addition, Sn has the function of etching control and the function of mobility control.

[0077] The composition range of each element is determined by the range of etching rate above 1 nm / sec when using sulfuric acid, nitric acid and acetic acid etchants, the range of band gap below 3.4 eV, and the range of resistance value after hydrogen annealing treatment above 1E+2Ω / □.

[0078] In the above formula, X is 0.32 or more and 0.65 or less, Y is 0.17 or more and 0.46 or less, and Z is more than 0 and 0.22 or less, and is in the range of X+Y+Z=1.

[0079] First, for the ternary composite oxide thin film of In, Mg and Sn, the etching rate is determined within the range of 1 nm / sec. The etchant used is an acetic acid etchant (acetic acid (HOOC-COOH)) or a mixed acid etchant of sulfuric acid (7.6-8.4%) and nitric acid (3.8-4.2%). For the determination of the etching rate, an immersion method is used in which a single film cap layer of the oxide semiconductor thin film just after film formation is immersed in an etchant controlled at 40°C.

[0080] exist Figure 1 The results are shown in . The results were in the range of 0<In≤0.65, 0.17≤Mg<1.0, 0<Sn≤0.22, and the etching rate was 1 nm / sec or more.

[0081] Next, the band gap of the ternary composite oxide thin film of In, Mg, and Sn was measured. The band gap was measured as follows.

[0082] 1. Use a spectrometer to measure the transmittance T and reflectance R.

[0083] 2. Calculate the absorption coefficient α from the following formula.

[0084] α=(((-ln(T / (1-R)) / n) / (T / (1-R))

[0085] n: Film thickness [cm] T, R: Measurement data / 100

[0086] 3. Calculate (α×hω)^(1 / 2).

[0087] hω(photon energy)[eV]:1239.8 / wavelength[nm]

[0088] 4. From a coordinate graph with the horizontal axis: hω[eV] and the vertical axis (α×hω)^(1 / 2), the intersection of the tangent line with the maximum slope and the x-axis is set as the band gap.

[0089] exist Figure 2 The results are shown in . As a result, the ranges in which the band gap is 0.34 eV or less are 0.32≤In<1.0, 0<Mg≤0.46, and 0<Sn≤0.67.

[0090] The band gap is preferably 0.34 eV or less because the difference in Eg between the lower layer and the upper layer is important in order to obtain good TFT characteristics. If Eg becomes larger than 0.34 eV and the difference with the active layer is too large, the electrons of the upper layer flow into the active layer side as the lower layer when the semiconductors are bonded to each other, and the Fermi level on the active layer side may move to the vicinity of the conduction band. In this case, the probability of exciting electrons to the conduction band increases, and the threshold voltage of the TFT shifts to the negative direction, resulting in the problem of not being able to obtain good TFT characteristics.

[0091] Furthermore, the resistance value of the ternary composite oxide thin film of In, Mg, and Sn after hydrogen annealing was measured.

[0092] The hydrogen annealing was performed at 400° C. for 1 h with a mixed gas of Ar+H 2 (H 2 : 6 at %) at a flow rate of 1 L / min.

[0093] In addition, the resistance value was measured by Hall measurement.

[0094] exist Figure 3 The results are shown in . As a result, the ranges of the resistance value of 1E+2 or more are 0<In≤0.65, 0.15≤Mg<1.0, and 0<Sn≤0.85.

[0095] Will Figures 1 to 3 The combined results of the range are shown in Figure 4 As a result, the ranges satisfying all the conditions are 0.32≤In≤0.65, 0.17≤Mg≤0.46, and 0<Sn≤0.22.

[0096] The oxide semiconductor thin film of the present invention can further contain at least one element selected from Si, Ti, W, Zr, Nb, Ni, Ge, Ta, Al and Y, that is, an A group element.

[0097] Among these group A elements, preferably Si is less than 4at%, Ti is less than 6at%, W is less than 6at%, Zr is less than 7at%, Nb is less than 7at%, Ni is less than 7at%, Ge is less than 7at%, Ta is less than 8at%, Al is less than 8at%, and Y is less than 9at%, and the overall content of group A elements is less than 10at%, and the oxide semiconductor film has high resistance, and Eg is in a range without increase (Eg≤3.4).

[0098] Furthermore, the oxide semiconductor thin film of the present invention can further contain at least one element selected from the group consisting of Mo, Sb, Hf, La, Fe, Ga, Zn, Ca and Sr, that is, a B group element.

[0099] Among them, among these group B elements, Mo is preferably less than 10at%, Sb is less than 13at%, Hf is less than 13at%, La is less than 13at%, Fe is less than 21at%, Ga is less than 27at%, Zn is less than 38at%, Ca is less than 38at%, Sr is less than 38at%, and the total content of elements other than In, Mg and Sn is less than 38at%, and the oxide semiconductor film has high resistance, and Eg is in a range without increase (Eg≤3.4).

[0100] Preferred ranges of these Group A elements and Group B elements are determined as described below.

[0101] The band gap Eg (eV) was determined when any one of the A group element and the B group element was added to the three elements of In, Mg, and Sn. The results are shown in Table 2.

[0102] Table 2 shows whether the band gap Eg (eV) can be maintained at 3.4 eV or less. ○ means 3.4 eV or less, and × means more than 3.4 eV.

[0103] The restriction value of the band gap Eg of the cap layer is 3.4 eV, which is defined on the premise that it is a range in which migration of the TFT does not occur. In other words, it means that for InMgSn (Eg: 3.1 eV), how much additional element α is added to maintain Eg below 3.4 eV.

[0104] The addition amount of the A group elements Si, Ti, W, Zr, Nb, Ni, Ge, Ta, Al and Y is less than 10 at %.

[0105] The B group elements Mo, Sb, Hf, La, Fe, Ga, Zn, Ca and Sr are added in an amount exceeding 10 at %.

[0106] [Table 2]

[0107]

[0108] [Sputtering target]

[0109] Next, the sputtering target according to the present embodiment will be described.

[0110] The sputtering target may be a planar target or a cylindrical rotating target. The sputtering target is composed of an oxide semiconductor sintered body containing In, Mg and Sn, and the composition ratio is the same as that of the above-mentioned oxide semiconductor thin film, and the preferred composition ratio is also the same, so repeated description is omitted.

[0111] The composition range of the oxide semiconductor sintered body of the sputtering target of the present invention is given by the formula In X Mg Y Sn Z It means that in the above formula, X is 0.32 or more and 0.65 or less, Y is 0.17 or more and 0.46 or less, Z is greater than 0 and 0.22 or less, and X+Y+Z=1.

[0112] The oxide semiconductor sintered body constituting the sputtering target of the present invention may further contain at least one element selected from Si, Ti, W, Zr, Nb, Ni, Ge, Ta, Al and Y, i.e., group A elements, in addition to In, Mg and Sn.

[0113] Among these A group elements, preferably Si is less than 4at%, Ti is less than 6at%, W is less than 6at%, Zr is less than 7at%, Nb is less than 7at%, Ni is less than 7at%, Ge is less than 7at%, Ta is less than 8at%, Al is less than 8at%, and Y is less than 9at%, and the total content of A group elements is less than 10at%.

[0114] In addition, the oxide semiconductor sintered body constituting the sputtering target of the present invention can further contain at least one element selected from the group consisting of Mo, Sb, Hf, La, Fe, Ga, Zn, Ca and Sr, that is, a B group element.

[0115] Among these B group elements, it is preferred that Mo is less than 10at%, Sb is less than 13at%, Hf is less than 13at%, La is less than 13at%, Fe is less than 21at%, Ga is less than 27at%, Zn is less than 38at%, Ca is less than 38at%, Sr is less than 38at%, and the total content of elements other than In, Mg and Sn is less than 38at%.

[0116] The oxide semiconductor film formed using the sputtering target has the following characteristics: the etching rate when using sulfuric acid, nitric acid and acetic acid etchants is 1 nm / sec or more, the band gap is 2.5 eV or more and 3.4 eV or less, and the resistance value after hydrogen annealing is 1E+2Ω / □ or more, which is most suitable for use as a high-mobility cap layer. In addition, the high-mobility active layer is as described above. It refers to an active layer with a band gap of 3 eV or less. The mobility is 15 cm 2 / V·s or above.

[0117] The cap layer is generally provided to suppress etching damage to the active layer, and the oxide semiconductor thin film formed using the sputtering target of the present invention can suppress the influence of hydrogen generated in the CVD process in addition to suppressing the cap damage.

[0118] The cap layer of such a composition can be etched with a sulfuric acid, nitric acid or acetic acid etchant, and the etching rate when etching with a sulfuric acid, nitric acid or acetic acid etchant is 1 nm / sec or more.

[0119] This makes the etching rates of the high-mobility active layer close to each other, making it suitable to perform etching treatment together, and enables fine patterning of the stacked body of the active layer and the cap layer to be performed well.

[0120] In addition, the etching damage of the active layer can be suppressed, and the influence of hydrogen in the CVD process can be suppressed.

[0121] When PAN is used as an etchant, it is preferably a sputtering target containing Zn. An oxide semiconductor thin film formed using such a sputtering target can also cope with etching using PAN.

[0122] Of course, in this case, the etching rate can be set to an etching rate suitable for the active layer, and the effects of suppressing etching damage to the active layer and suppressing the influence of hydrogen in the CVD process can be achieved.

[0123] When an oxide semiconductor thin film formed using the sputtering target of the present invention is used as a cap layer, a mobility exceeding 10 cm 2 / Vs thin film transistor.

[0124] In addition, when the oxide semiconductor thin film is stacked as a cap layer with a high-mobility active layer to form a thin film transistor, the shift of the threshold voltage Vth can be suppressed compared to the case where no cap layer is used, and a thin film transistor with good TFT characteristics can be realized.

[0125] (Method for producing sputtering target)

[0126] The production of the sputtering target of the present invention is not particularly limited as long as it is a method that can produce an oxide semiconductor sintered body having the above-mentioned composition, and for example, the following two production methods can be exemplified.

[0127] The first method is a method of mixing indium oxide powder, magnesium oxide powder, and tin oxide powder to form a compact, and sintering the compact at 1100° C. to 1650° C. to produce a sputtering target having an oxide sintered body.

[0128] The weight ratio of the raw material powder is determined so as to achieve the target element ratio of the above-mentioned oxide semiconductor sintered body.

[0129] In the method for manufacturing a sputtering target of the present invention, MgO as a raw material reacts with water to generate Mg(OH)2 when the raw materials are mixed, so the viscosity of the slurry increases when the raw materials are mixed, which may hinder uniform mixing. In addition, Mg(OH)2 may generate pores and cracks during sintering.

[0130] Therefore, when magnesium oxide is obtained as a raw material, it is preferably mixed in a dry manner or as a slurry in an organic solvent that does not contain water. Of course, mixing using pure water may be possible by devising measures such as reducing the mixing time.

[0131] In addition, the second method is a method for manufacturing a sputtering target having an oxide sintered body by mixing oxides, hydroxides or carbonates of indium, magnesium and tin, molding a precursor powder pre-sintered at 1000°C to 1500°C to form a molded body, and sintering the molded body at a temperature above 1100°C and below 1650°C.

[0132] The weight ratio of the raw material powder is determined so as to achieve the target element ratio of the above-mentioned oxide semiconductor sintered body.

[0133] The oxide sintered body contained in the sputtering target is prepared by mixing raw material powders such as oxides, hydroxides or carbonates of indium, magnesium and tin to form a compact, pre-sintering the compact at 1000°C to 1500°C to make a compact, and sintering the compact at a temperature above 1100°C and below 1650°C to make a sputtering target having an oxide sintered body.

[0134] In the method for manufacturing a sputtering target of the present invention, the raw material mixed powder is pre-sintered at a temperature of 1000°C to 1500°C, the powder not containing the MgO phase is mixed, and a molded body is formed after drying and granulation. This can prevent the generation of Mg(OH)2 by reaction with the powder and water during mixing after pre-sintering, and there is no need to worry about the increase in slurry viscosity and the obstruction of uniform mixing, and there is no need to worry about the formation of pores and cracks in the hydroxide during sintering.

[0135] Furthermore, the molded body is fired at 1100° C. to 1650° C. to obtain a sintered body.

[0136] When the firing temperature is less than 1100°C, the conductivity and relative density are reduced, and it is not suitable for target use. On the other hand, when the firing temperature exceeds 1650°C, some components evaporate, causing the composition of the fired body to deviate, or the strength of the fired body to decrease due to the coarsening of crystal grains.

[0137] In the sputtering target of the present invention, there is a preferred composition range in order to prevent the above-mentioned generation of Mg(OH) 2 .

[0138] When In:Mg:Sn=a(at%):b(at%):c(at%), in the range of b>a / 2+2c, MgO remains after pre-sintering and sintering, which is not preferred. If MgO remains after sintering, it reacts with moisture in the atmosphere on the surface of the sputtering target to generate Mg(OH)2, which may become a particle source.

[0139] If this range is replaced by In X Mg Y Sn Z X, Y, and Z, then Y>X / 2+2Z.

[0140] The range is shown as Figure 5 .

[0141] like Figure 5 As shown, the range of Y>X / 2+2Z is ​​represented by the shaded area in the figure, which is the range in which the crystalline phase after pre-sintering is composed of In2MgO4 phase, Mg2SnO4 phase, In2O3 phase, SnO2 phase, etc., and does not contain MgO phase. Figure 5 The data of Examples 1-9 and Comparative Examples 1-3 described later are shown in FIG.

[0142] The sputtering target of the present invention preferably has a relative density of 90% or more. If the relative density is less than 90%, cracks or particles may be generated during sputtering, so it is preferably manufactured so that the relative density is 90% or more.

[0143] Hereinafter, the second method will be further exemplified and the production method will be described in detail.

[0144] In this embodiment, the raw material powder is granulated by a spray drying method that can simultaneously dry and granulate. By adding a binder, a pulverizing operation with poor pulverizability is not required, and spherical powder with good fluidity can be used, so that the composition distribution of the sputtering target is easily uniform.

[0145] The raw material powder contains at least oxides, hydroxides or carbonates of indium, magnesium and tin. In addition, powders of one or more oxides selected from elements of group A and elements of group B may be mixed. In addition, a dispersant or the like may be added during the mixing of the raw material powders.

[0146] As a method for pulverizing and mixing the raw material powder, a ball mill can be used, but in addition to the ball mill, other medium stirring mills such as a bead mill and a rod mill can be used. The surface of the balls and beads that become the stirring medium can be coated with a resin, etc. This effectively suppresses the mixing of impurities in the powder.

[0147] The mixed granular powder is pre-sintered at a temperature of 1000°C to 1500°C. If the sintering temperature is less than 1000°C, the pre-sintering is insufficient, the composite oxide is not completely formed, and MgO remains. If the sintering temperature exceeds 1500°C, sintering proceeds during the pre-sintering, and the shape of the primary particles becomes larger, so the sintering density does not increase in the subsequent main sintering.

[0148] The pre-calcined powder is wet-pulverized again with a ball mill or the like together with a dispersant, a binder, etc., and granulated by spray drying.

[0149] The average particle size of the granulated powder is 500 μm or less. If the average particle size of the granulated powder exceeds 500 μm, cracks and splits of the molded body become significant, and granular spots appear on the surface of the sintered body. If such a sintered body is used as a sputtering target, it may cause abnormal discharge or particle generation.

[0150] The more preferred average particle size of the granulated powder is 20 μm or more and 100 μm or less. As a result, the volume change (compression rate) before and after CIP (Cold Isostatic Press) molding is small, cracks in the molded body are suppressed, and a long molded body can be stably produced. In addition, when the average particle size is less than 20 μm, the powder is easy to fly, making it difficult to handle.

[0151] Here, the "average particle size" means a value at which the cumulative % of the particle size distribution measured by a sieving particle size distribution measuring device is 50%. In addition, as the value of the average particle size, a value measured by using "RobotSifter RPS-105M" manufactured by Seishin Enterprise Co., Ltd. is used.

[0152] The granulated powder was heated at 100 MPa / cm 2 The molding pressure is less than 100 MPa, and the molded body is easily broken, difficult to handle, and the relative density of the sintered body is reduced.

[0153] As a molding method, the CIP method is used. The CIP form can be a typical vertical loading type longitudinal method, preferably a horizontal loading type horizontal method. This is because if a longitudinal CIP is used to make a long plate-shaped molded body, the deviation of the powder in the mold will cause fluctuations in thickness, or cracks due to its own weight during processing.

[0154] Furthermore, the molded body is fired at 1100° C. to 1650° C. to obtain a sintered body.

[0155] When the firing temperature is less than 1100°C, the conductivity and relative density are reduced, and the target is not suitable. On the other hand, when the firing temperature exceeds 1650°C, some components evaporate, causing the composition of the fired body to deviate, or the strength of the fired body to decrease due to the coarsening of the crystal grains.

[0156] The molded body is fired in air or in an oxidizing atmosphere, thereby stably producing a target oxide sintered body.

[0157] In the preparation of the granulated powder, a powder having an average primary particle size of 0.3 μm or more and 1.5 μm or less is used. This can shorten the mixing and pulverizing time and improve the dispersibility of the raw material powder in the granulated powder.

[0158] The angle of repose of the granulated powder is preferably 32° or less. This improves the fluidity of the granulated powder, and improves the moldability and sinterability.

[0159] (Processing steps)

[0160] The sintered body produced as described above is machined into a plate shape having a desired shape, size, and thickness, thereby producing a sputtering target composed of an In-Mg-Sn-O-based sintered body. The sputtering target is welded to a backing plate.

[0161] According to this embodiment, a long sputtering target with a length of more than 1000 mm in the longitudinal direction can be manufactured. Thus, a large sputtering target without a segmented structure can be manufactured, thereby preventing the degradation of film properties that may occur due to sputtering of the bonding material (solder) invading the gap (joint) of the segmented portion, and stable film formation becomes possible. In addition, it is difficult to generate particles caused by the reattachment (redeposition) of sputtered particles accumulated in the above-mentioned gap.

[0162] [Evaluation of sputtering target]

[0163] (Resistivity value distribution)

[0164] The resistivity value was measured by a direct current four-probe method using Model Sigma-5+ manufactured by NPS.

[0165] The resistivity value was defined as the average resistivity value of five points on the sputtered surface side after the sintered body was processed.

[0166] (Relative density)

[0167] The density of the sintered body is determined by the mercury Archimedean method or by direct calculation from the dimensions and weight.

[0168] (Crystal Structure)

[0169] The generation of the composite oxide was confirmed by XRD of the calcined powder.

[0170] An example of the apparatus and measurement conditions used in X-ray diffraction is as follows.

[0171] X-ray diffraction apparatus: RINT manufactured by Rigaku Corporation

[0172] Scanning method: 2θ / θ method

[0173] Target: Cu

[0174] Tube voltage: 40kV

[0175] Tube current: 20mA

[0176] Scanning speed: 2.000° / min

[0177] Sampling width: 0.050°

[0178] Divergence slit: 1°

[0179] Scattering slit: 1°

[0180] Light receiving slit: 0.3mm

[0181] [Thin Film Transistor]

[0182] exist Figure 6Schematic diagram of an example of a thin film transistor according to the present invention is shown in FIG.

[0183] The thin film transistor 100 of this embodiment includes a gate electrode 11 , a gate insulating film 12 , an active layer 13 , a cap layer 14 , a source electrode 15S, a drain electrode 15D, and a protective film 16 on a substrate 10 .

[0184] The gate electrode 11 is composed of a conductive film formed on the surface of the substrate 10. The substrate 10 is typically a transparent glass substrate. The gate electrode 11 is typically composed of a metal single layer film or a metal multilayer film such as molybdenum (Mo), titanium (Ti), aluminum (Al), copper (Cu), etc., and is formed by, for example, a sputtering method. In this embodiment, the gate electrode 11 is composed of molybdenum. There is no particular limitation on the thickness of the gate electrode 11, and it is, for example, 200 nm. The gate electrode 11 is formed by, for example, a sputtering method, a vacuum evaporation method, or the like.

[0185] The active layer 13 functions as a channel layer of the thin film transistor 100. The thickness of the active layer 13 is, for example, 10 nm to 200 nm. The active layer 13 is a high-mobility active layer and is composed of an IGZO (In-Ga-Zn-O) oxide semiconductor thin film. The active layer 13 is formed by, for example, sputtering.

[0186] The gate insulating film 12 is formed between the gate electrode 11 and the active layer 13. The gate insulating film 12 is composed of, for example, a silicon oxide film (SiOx), a silicon nitride film (SiNx), or a laminated film thereof. The film forming method is not particularly limited, and may be a CVD method, a sputtering method, an evaporation method, etc. The film thickness of the gate insulating film 12 is not particularly limited, and is, for example, 200 nm to 400 nm.

[0187] The cap layer 14 is composed of the above-mentioned oxide semiconductor thin film of the present invention, and the detailed composition is as described above.

[0188] The cap layer 14 is patterned together with the active layer 13. As the etchant, the above-mentioned etchant can be used.

[0189] The source electrode 15S and the drain electrode 15D are formed separately from each other on the active layer 13 and the cap layer 14. The source electrode 15S and the drain electrode 15D can be composed of, for example, a metal single layer film of aluminum, molybdenum, copper, titanium, or a multilayer film of these metals. As described later, the source electrode 15S and the drain electrode 15D can be formed simultaneously by patterning a metal film. The thickness of the metal film is, for example, 100 nm to 200 nm. The source electrode 15S and the drain electrode 15D are formed by, for example, sputtering, vacuum evaporation, or the like.

[0190] The source electrode 15S and the drain electrode 15D are covered with a protective film 16. The protective film 16 is made of an electrically insulating material such as a silicon oxide film, a silicon nitride film, or a laminated film thereof. The protective film 16 is used to shield the element portion including the active layer 13 and the cap layer 14 from the outside air. The film thickness of the protective film 16 is not particularly limited, and is, for example, 100 nm to 300 nm. The protective film 16 is formed by, for example, a CVD method.

[0191] After the protective film 16 is formed, an annealing treatment is performed. Thus, the active layer 13 is activated. The annealing conditions are not particularly limited, but in this embodiment, the annealing is performed at about 30° C. in the air for 1 hour. At this time, it is believed that the cap layer 14 has the function of inhibiting the diffusion of hydrogen from the protective layer 16 to the active layer 13 due to heat.

[0192] Interlayer connection holes 16S and 16D for connecting the source / drain electrodes 15S and 15D to a wiring layer (not shown) are provided at appropriate positions in the protective film 16. The wiring layer is used to connect the thin film transistor 100 to a peripheral circuit (not shown) and is made of a transparent conductive film such as ITO.

[0193] (Method for manufacturing thin film transistor)

[0194] Reference Figure 7 and Figure 8 , an example of a method for manufacturing a thin film transistor of the present invention is described.

[0195] like Figure 7 As shown in (a), first, a gate electrode material layer 11a is formed on a substrate 10 by sputtering at room temperature. Figure 7 As shown in (b), the gate electrode 11 is formed by wet patterning. Figure 7 As shown in (c), the gate insulating film 12 is formed by CVD. Here, SiO X / SiN X Then, as Figure 7 As shown in (d), the active layer material layer 13a and the cap layer material layer 14a are sequentially formed by sputtering at a temperature of 100°C on the substrate 10. Then, as shown in FIG. Figure 8 As shown in (a), the active layer material layer 13a and the cap layer material layer 14a are patterned by etching to form the active layer 13 and the cap layer 14. As an etchant, for example, sulfuric acid or nitric acid-based etchant is used for etching, and then, for example, annealing is performed at 400°C for 1 hour in the atmosphere. Figure 8 As shown in (b), a source and drain metal material layer 15a is formed by sputtering at room temperature. Figure 8 As shown in (c), the source electrode 15S and the drain electrode 15D are formed by patterning. Figure 8As shown in (d), a protective film material layer 16a is formed by CVD. The protective film material layer 16a is, for example, SiOx with a film thickness of 300 nm. The protective film material layer 16a is annealed at 300°C in the atmosphere and then dried and patterned to form interlayer connection holes 16S and 16D of the source electrode 15S and the drain electrode 15D (see Figure 6 ).

[0196] The thin film transistor according to the present invention described above has the following effect: for the material of the high-mobility active layer 13 which tends to have a small band gap Eg, the Vth of the TFT does not shift when stacked with the cap layer 14, thereby suppressing external factors during TFT production.

[0197] Specifically, the cap layer 14 of the present invention has a function of suppressing damage to the active layer 13 during a hydrogen process in manufacturing a TFT and during patterning of the source electrode 15S and the drain electrode 15D.

[0198] By the way, in the case of no suppression by the cap layer 14, in the case of a hydrogen process, the resistance is reduced due to the diffusion of hydrogen into the active layer 13, and a problem of not being able to obtain good TFT characteristics occurs. In addition, if the suppression of etching damage to the active layer 13 by the cap layer 14 does not work, the weak bond of the oxide semiconductor film of the active layer 13 is cut by the etching solution, resulting in defects in the film, deteriorating the S value of TFT characteristics, and not being able to obtain good transistor characteristics.

[0199] Fig. 9 In thin film transistors, Figure 6 The figure shows the change of substrate temperature during the CVD film formation of the protective layer 16 and the comparison of S values ​​in the case of having a cap layer 14 composed of the oxide semiconductor thin film of the present invention (stacked) and the case of not having the cap layer 14 (single layer) (not shown). In-Sn-Ge-O+α was used as the active layer 13, and the cap layer 14 was set to In-Mg-Sn-O of the present invention, and the values ​​were 15 nm respectively.

[0200] As a result, it can be seen that if the cover layer 14 is not set as a single-layer structure, etching damage will occur in the active layer 13, and the S value of the TFT characteristics will increase and deteriorate. If the cover layer 14 of the present invention is set to form a stacked structure, the etching damage is suppressed and the S value is suppressed from increasing.

[0201] Example

[0202] (Examples 1-9)

[0203] Indium oxide, magnesium hydroxide, and tin oxide were weighed and mixed using a ball mill so as to have the composition shown in the following Table 3. The mixed granular powder was pre-calcined and sintered in an oxygen atmosphere to obtain a sintered body.

[0204] Table 3 shows the results of measuring the relative density and resistivity of the sintered body.

[0205] In Example 1-9, indium oxide, magnesium hydroxide, and tin oxide were used as raw materials, and the pre-sintering temperature was set at 1000°C to 1500°C, and sintering was performed in an oxygen atmosphere to obtain a sintered body having a relative density of 90% or more. In addition, the calcination temperature was set at 1000°C to 1200°C, and sintering was performed at 1500°C or more in an oxygen atmosphere to obtain a sintered body having a relative density of 97% or more and a resistivity of 10 mΩ·cm or less.

[0206] Furthermore, in any of Examples 1 to 9, no MgO remained after calcination.

[0207] (Comparative Examples 1-5)

[0208] In Comparative Example 1, the same method as in Example 1 was used except that the calcination temperature was 950°C which is lower than 1000°C. However, MgO remained after the calcination.

[0209] In Comparative Example 2, the same procedures as in Example 3 were followed except that the sintering was carried out in the air atmosphere, but the relative density was less than 90%.

[0210] In Comparative Example 3, the same method as in Example 3 was used except that the sintering temperature was set at 1650° C. However, the crystal grains were coarsened, which was not preferable as a sputtering target.

[0211] In Comparative Example 4, the same procedures as in Example 3 were performed except that MgO was used as the Mg raw material, but the relative density was less than 90%.

[0212] In Comparative Example 5, the same procedures as in Example 3 were followed except that MgCO 3 was used as the Mg raw material, but the relative density was less than 90%.

[0213] [Table 3]

[0214]

[0215] [Table 4]

[0216]

[0217] Note: * Grain coarsening

[0218] (Thin Film Transistor Manufacturing Example 1)

[0219] like Figure 6 A thin film transistor having a cap layer 14 composed of the oxide semiconductor thin film of the present invention is manufactured as in the structure of FIG.

[0220] As the active layer 13, In-Sn-Ge-O+α shown in Table 1 is used, with a film thickness of 50 nm, and the cap layer 14 is In-Mg-Sn-O (composition: In: 54Mg: 31Sn: 15) of the present invention, with a film thickness of 50 nm.

[0221] (Thin Film Transistor Comparative Manufacturing Example 1)

[0222] In addition to not setting Figure 6 Except for the cap layer 14, a thin film transistor is manufactured in the same manner.

[0223] (Thin Film Transistor Comparative Manufacturing Example 2)

[0224] exist Figure 6 A thin film transistor is manufactured in the same manner except that a different composition of IGZO is used as a cap layer than that of conventional IGZO.

[0225] Fig.10 Vth was compared between a case where the cap layer 14 composed of the oxide semiconductor thin film of the present invention was provided (laminated) as in the thin film transistor (laminated) structure of Manufacturing Example 1 and a case where the cap layer 14 was not provided (single layer: Comparative Manufacturing Example 1).

[0226] As a result, the threshold voltage Vth was substantially the same in the case of the stacked structure with the cap layer 14 of the present invention (Manufacturing Example 1) and the case without the cap layer 14 (single layer; Comparative Manufacturing Example 1), and there was no shift in Vth due to the provision of the cap layer 14.

[0227] The band gap Eg of the single-layer structure of Comparative Example 1 is 2.7 eV, while the band gap Eg of the stacked structure with the cap layer 14 of Example 1 is 3.1 eV. The difference in Eg is 0.4 eV, and the increase in Eg is small.

[0228] exist Fig.11 In addition to using different compositions of IGZO as the capping layer of the stacked structure, Figure 6 The threshold voltage Vth was compared between the case where a conventional IGZO cap layer of different composition was provided in the thin film transistor of the same comparative manufacturing example 2 (laminated layer; comparative manufacturing example 2) and the case where no cap layer was provided (single layer; comparative manufacturing example 1).

[0229] As a result, it was found that the thin film transistor (laminated layer) of Comparative Manufacturing Example 2 had a significantly shifted Vth compared to the single layer of Comparative Manufacturing Example 1.

[0230] In addition, the band gap Eg in the case of the single-layer structure of comparative manufacturing example 1 is 2.7 eV, while the Eg in the case of the stacked structure with a cap layer of comparative manufacturing example 2 is 3.4 eV. Compared with the case where the oxide semiconductor thin film of the present invention is used as the cap layer 14, the increase in the band gap Eg is greater.

Claims

1. A sputtering target comprising a formula In consisting of indium, magnesium and tin X Mg Y Sn Z The oxide sintered body is composed of an oxide of, in which X of the above formula is greater than 0.32 and less than 0.65, Y is greater than 0.17 and less than 0.46, Z is greater than 0 and less than 0.22, and is in the range of X+Y+Z=1.

2. The sputtering target according to claim 1, wherein The oxide sintered body further contains at least one element selected from Si, Ti, W, Zr, Nb, Ni, Ge, Ta, Al and Y, that is, an A group element.

3. The sputtering target according to claim 2, wherein: Si is less than 4 at%, Ti is less than 6 at%, W is less than 6 at%, Zr is less than 7 at%, Nb is less than 7 at%, Ni is less than 7 at%, Ge is less than 7 at%, Ta is less than 8 at%, Al is less than 8 at%, Y is less than 9 at%, and the content of the A group elements is less than 10 at%.

4. The sputtering target according to any one of claims 1 to 3, wherein The oxide sintered body further contains at least one element selected from the group consisting of Mo, Sb, Hf, La, Fe, Ga, Zn, Ca and Sr, that is, a B group element.

5. The sputtering target according to claim 4, wherein: Mo is less than 10at%, Sb is less than 13at%, Hf is less than 13at%, La is less than 13at%, Fe is less than 21at%, Ga is less than 27at%, Zn is less than 38at%, Ca is less than 38at%, Sr is less than 38at%, and the total content of elements other than In, Mg and Sn is less than 38at%.

6. The sputtering target according to any one of claims 1 to 5, wherein The relative density is above 90%.

7. A method for producing a sputtering target, wherein: Indium oxide powder, magnesium oxide powder, and tin oxide powder are mixed to form a compact, and the compact is sintered at 1100° C. to 1650° C. to produce a sputtering target having an oxide sintered body according to any one of claims 1 to 6.

8. A method for producing a sputtering target, wherein: Oxides, hydroxides or carbonates of indium, magnesium and tin are mixed, a precursor powder pre-sintered at 1000°C to 1500°C is molded to form a molded body, and the molded body is sintered at a temperature of 1100°C to 1650°C to produce a sputtering target having an oxide sintered body according to any one of claims 1 to 6.

9. An oxide semiconductor thin film, which is composed of an oxide semiconductor, wherein the oxide semiconductor is a thin film of a formula In composed of indium, magnesium and tin. X Mg Y Sn Z The oxide is the main component, X in the above formula is greater than 0.32 and less than 0.65, Y is greater than 0.17 and less than 0.46, Z is greater than 0 and less than 0.22, and is in the range of X+Y+Z=1.

10. The oxide semiconductor thin film according to claim 9, wherein The etching rate when etching is performed using a sulfuric acid, nitric acid or acetic acid etchant is 1 nm / sec or more.

11. The oxide semiconductor thin film according to claim 9 or 10, wherein The band gap is 2.5 eV or more and 3.4 eV or less, and the resistance value after hydrogen annealing is 1E+2Ω / □ or more.

12. The oxide semiconductor thin film according to any one of claims 9 to 11, further comprising at least one element selected from Si, Ti, W, Zr, Nb, Ni, Ge, Ta, Al, Y and Mo, i.e., a group A element.

13. The oxide semiconductor thin film according to claim 12, wherein Si is less than 4at%, Ti is less than 6at%, W is less than 6at%, Zr is less than 7at%, Nb is less than 7at%, Ni is less than 7at%, Ge is less than 7at%, Ta is less than 8at%, Al is less than 8at%, and Y is less than 9at%, and the content of the A group elements is less than 10at%.

14. The oxide semiconductor thin film according to any one of claims 9 to 13, further comprising at least one element selected from the group B of Mo, Sb, Hf, La, Fe, Ga, Zn, Ca and Sr.

15. The oxide semiconductor thin film according to claim 14, wherein Mo is less than 10 at %, Sb is less than 13 at %, Hf is less than 13 at %, La is less than 13 at %, Fe is less than 21 at %, Ga is less than 27 at %, Zn is less than 38 at %, Ca is less than 38 at %, Sr is less than 38 at %, and the total content of elements other than In, Mg and Sn is less than 38 at %.

16. An oxide semiconductor thin film stack comprising: an active layer composed of a high-mobility oxide semiconductor thin film; and a cap layer composed of the oxide semiconductor thin film according to any one of claims 9 to 15 stacked on the active layer.

17. The oxide semiconductor thin film stack according to claim 16, wherein: The etching ratio when the cap layer is patterned together with the active layer is appropriate.

18. A thin-film semiconductor device comprising a cap layer comprising the oxide semiconductor thin film according to any one of claims 9 to 15.

19. The thin film semiconductor device according to claim 18, wherein: The cap layer is provided so as to cover the active layer composed of the high-mobility oxide semiconductor thin film.

20. A thin-film semiconductor device according to claim 18 or 19, comprising: a gate electrode; a gate insulating film arranged on the gate electrode; an active layer arranged on the gate insulating film and composed of a high-mobility oxide semiconductor thin film; a cap layer arranged in a manner covering the active layer; and a source electrode and a drain electrode connected to the active layer and the cap layer.

21. A method for manufacturing a thin-film semiconductor device, comprising: a method for manufacturing a thin-film semiconductor device having a cap layer composed of an oxide semiconductor thin film according to any one of claims 9 to 15, wherein: A gate insulating film is formed on the gate electrode, an active layer composed of a high-mobility oxide semiconductor film is formed on the gate insulating film by a sputtering method, the cap layer is formed on the active layer by a sputtering method, the stacked film of the active layer and the cap layer is patterned to form a metal layer with the patterned active layer and the cap layer as a base film, and the metal layer is patterned by a wet etching method to form a source electrode and a drain electrode.

Citation Information

Patent Citations

  • Organic el display device and manufacturing method thereof

    JP2009031750A

  • Thin film transistor and method for manufacturing the same

    JP2011216574A

  • Method for manufacturing transistor, transistor, and sputtering target

    WO2010092810A1

  • Thin-film field-effect transistor and method for manufacturing the same

    TW201140850A

  • Oxide sintered body and oxide semiconductor thin film

    WO2012029408A1