Electrochemical cell

By using a perovskite oxide containing gadolinium, chromium, and manganese, and a gadolinium-doped cerium dioxide hydrogen electrode layer structure in an electrochemical single cell, combined with a metal support and adjustment of the area occupancy of the perovskite oxide, the problem of hydrogen electrode layer cracking was solved, and the structural stability and electrode performance were improved.

CN118922585APending Publication Date: 2024-11-08NGK INSULATORS LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380017707.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2023-02-15
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In existing electrochemical single cells, the hydrogen electrode layer is prone to cracking during repeated operation and shutdown, leading to structural weakening.

Method used

The perovskite oxide containing gadolinium, chromium and manganese and the hydrogen polar layer structure doped with gadolinium dioxide are used to suppress cracks by strengthening the framework structure, combined with a metal support to provide support, and the area occupancy of the perovskite oxide is adjusted in the thickness direction.

Benefits of technology

It effectively suppressed the generation of cracks in the hydrogen electrode layer, maintained the structural stability and electrode performance of the electrochemical single cell, and performed particularly well under high-temperature sintering conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922585A_ABST
    Figure CN118922585A_ABST
Patent Text Reader

Abstract

An electrolytic cell (1) is provided with a hydrogen electrode layer (6), an oxygen electrode layer (9), and an electrolyte layer (7) disposed between the hydrogen electrode layer (6) and the oxygen electrode layer (9). The hydrogen electrode layer (6) is composed of a perovskite-type oxide containing gadolinium, chromium, and manganese, gadolinium-doped cerium dioxide, and nickel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to electrochemical cells. Background Art

[0002] Conventionally, there is known an electrochemical cell (electrolysis cell, fuel cell, etc.) having a hydrogen electrode layer, an oxygen electrode layer, and an electrolyte layer disposed between the hydrogen electrode layer and the oxygen electrode layer (see, for example, Patent Document 1). The hydrogen electrode layer may be composed of gadolinium-doped ceria (GDC) and nickel (Ni).

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Laid-Open No. 2020-155337 Summary of the invention

[0006] When the electrochemical cell is repeatedly operated and stopped, cracks may occur in the porous hydrogen electrode layer. Therefore, it is desirable to suppress the occurrence of cracks in the hydrogen electrode layer by strengthening the skeleton structure of the hydrogen electrode layer.

[0007] An object of the present invention is to provide an electrochemical cell capable of suppressing the occurrence of cracks in a hydrogen electrode layer.

[0008] The electrochemical cell according to the first aspect of the present invention comprises: a hydrogen electrode layer; an oxygen electrode layer; and an electrolyte layer disposed between the hydrogen electrode layer and the oxygen electrode layer. The hydrogen electrode layer is composed of a perovskite oxide containing gadolinium, chromium, and manganese, gadolinium-doped ceria, and nickel.

[0009] The electrochemical cell according to a second aspect of the present invention is the electrochemical cell according to the first aspect, wherein the average area occupancy of the perovskite type oxide in the cross section of the hydrogen electrode layer is 5.00% or less.

[0010] The electrochemical cell involved in the third aspect of the present invention is based on the above-mentioned first or second aspect, and the hydrogen electrode layer has: a first region on the electrolyte layer side based on the center of the thickness direction, and a second region on the opposite side of the electrolyte layer based on the center of the thickness direction, and the first area occupancy of the perovskite oxide in the first region is smaller than the second area occupancy of the perovskite oxide in the second region.

[0011] The electrochemical cell according to a fourth aspect of the present invention is the electrochemical cell according to any one of the first to third aspects, further comprising a plate-shaped metal support that supports the hydrogen electrode layer and has a plurality of supply holes.

[0012] Effects of the Invention

[0013] According to the present invention, it is possible to provide an electrochemical cell capable of suppressing the occurrence of cracks in the hydrogen electrode layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 It is a cross-sectional view showing the structure of an electrolytic cell according to the embodiment. DETAILED DESCRIPTION

[0015] (Electrolytic cell 1)

[0016] Figure 1 It is a cross-sectional view showing the structure of the electrolytic cell 1 according to the embodiment. The electrolytic cell 1 is an example of the “electrochemical cell” according to the present invention.

[0017] The electrolytic cell 1 includes a cell body 10 , a metal support 20 , and a flow path member 30 .

[0018] [Single Cell Main Body 10]

[0019] The cell main body 10 has a hydrogen electrode layer 6 (cathode), an electrolyte layer 7, an anti-reaction layer 8, and an oxygen electrode layer 9 (anode). The hydrogen electrode layer 6, the electrolyte layer 7, the anti-reaction layer 8, and the oxygen electrode layer 9 are stacked in this order starting from the metal support 20 side. The hydrogen electrode layer 6, the electrolyte layer 7, and the oxygen electrode layer 9 are essential components, and the anti-reaction layer 8 is an optional component.

[0020] [Hydrogen pole layer 6]

[0021] The hydrogen electrode layer 6 is disposed between the metal support 20 and the electrolyte layer 7. The hydrogen electrode layer 6 is supported by the metal support 20. Specifically, the hydrogen electrode layer 6 is disposed on the first main surface 20S of the metal support 20. The hydrogen electrode layer 6 covers the region of the first main surface 20S of the metal support 20 where the plurality of supply holes 21 are provided. The hydrogen electrode layer 6 can enter each supply hole 21.

[0022] The raw material gas is supplied to the hydrogen electrode layer 6 through each supply hole 21. The raw material gas contains CO2 and H2O. The hydrogen electrode layer 6 generates H2, CO, and O from the raw material gas according to the electrochemical reaction of co-electrolysis represented by the following formula (1). 2- .

[0023] Hydrogen polar layer 6: CO2+H2O+4e - →CO+H2+2O 2- ···(1)

[0024] The hydrogen electrode layer 6 is composed of a porous material having electronic conductivity. In the present embodiment, the hydrogen electrode layer 6 is composed of a perovskite-type oxide containing gadolinium (Gd), chromium (Cr) and manganese (Mn) (hereinafter referred to as "Gd (Cr, Mn) oxide"), gadolinium-doped ceria (GDC), and nickel (Ni). Gd (Cr, Mn) oxide is a perovskite-type oxide represented by the general formula ABO3. Gd is arranged at the A site, and Cr and Mn are arranged at the B site.

[0025] By including the Gd(Cr, Mn) oxide in the hydrogen electrode layer 6 , the sinterability (neck growth between particles) of the hydrogen electrode layer 6 can be improved, thereby strengthening the skeleton structure of the porous hydrogen electrode layer 6 . This can suppress the occurrence of cracks in the hydrogen electrode layer 6 .

[0026] Here, in the electrolytic cell 1 as a metal-supported cell, the hydrogen electrode layer 6 needs to be formed by low-temperature heat treatment in order to suppress the degradation of the metal support 20, and the skeleton formation of the hydrogen electrode layer 6 is likely to be insufficient. Therefore, in the electrolytic cell 1 as a metal-supported cell, it is particularly effective to suppress cracks by strengthening the skeleton structure of the hydrogen electrode layer 6.

[0027] Gd(Cr, Mn) oxide is represented by the general formula ABO 3. Gd(Cr, Mn) oxide has electrical insulating properties.

[0028] like Figure 1 As shown, the hydrogen electrode layer 6 of this embodiment has: Figure 1 The first region 61 is located on the electrolyte layer 7 side with reference to the dotted line in the figure, and the second region 62 is located on the opposite side of the electrolyte layer 7 with reference to the center in the thickness direction. The thickness direction refers to the direction perpendicular to the first main surface 20S of the metal support 20. The area occupancy of the Gd (Cr, Mn) oxide in the cross section of the hydrogen electrode layer 6 is described below.

[0029] Ni preferably exists in the form of metallic Ni in a reducing atmosphere when the electrolytic cell 1 is in operation, but may exist in the form of NiO in an oxidizing atmosphere when the electrolytic cell 1 is stopped.

[0030] The porosity of the hydrogen electrode layer 6 is not particularly limited, and may be, for example, 5% to 70%. The thickness of the hydrogen electrode layer 6 is not particularly limited, and may be, for example, 1 μm to 100 μm.

[0031] The hydrogen electrode layer 6 can be formed by a sintering method.

[0032] [Electrolyte layer 7]

[0033] The electrolyte layer 7 is disposed between the hydrogen electrode layer 6 and the oxygen electrode layer 9. The electrolyte layer 7 covers the entire hydrogen electrode layer 6. In the present embodiment, since the reaction prevention layer 8 is disposed between the electrolyte layer 7 and the oxygen electrode layer 9, the electrolyte layer 7 and the reaction prevention layer 8 are in contact.

[0034] The outer edge of the electrolyte layer 7 is bonded to the first main surface 20S of the metal support 20. This ensures airtightness between the hydrogen electrode layer 6 and the oxygen electrode layer 9, and therefore, there is no need to seal the metal support 20 and the electrolyte layer 7 separately.

[0035] The electrolyte layer 7 allows the O generated in the hydrogen electrode layer 6 to 2- The electrolyte layer 7 is made of a dense material having oxide ion conductivity. The electrolyte layer 7 can be made of, for example, 8YSZ, LSGM (lanthanum gallate), or the like.

[0036] The electrolyte layer 7 is a sintered body made of a dense material having ion conductivity but not electron conductivity. The electrolyte layer 7 can be made of, for example, YSZ (8YSZ), GDC, ScSZ, SDC, LSGM (lanthanum gallate), or the like.

[0037] The porosity of the electrolyte layer 7 is not particularly limited, and may be, for example, 0.1% to 7%. The thickness of the electrolyte layer 7 is not particularly limited, and may be, for example, 1 μm to 100 μm.

[0038] [Anti-reaction layer 8]

[0039] The reaction prevention layer 8 is arranged between the electrolyte layer 7 and the oxygen electrode layer 9. The reaction prevention layer 8 is arranged on the opposite side of the hydrogen electrode layer 6 across the electrolyte layer 7. In the present embodiment, the reaction prevention layer 8 is connected to the electrolyte layer 7. The reaction prevention layer 8 has the function of inhibiting the electrolyte layer 7 and the oxygen electrode layer 9 from reacting to form a reaction layer with a large resistance.

[0040] The reaction prevention layer 8 is made of an ion conductive material. The reaction prevention layer 8 can be made of GDC, SDC or the like.

[0041] The porosity of the reaction-preventing layer 8 is not particularly limited, and may be, for example, 0.1% to 50%. The thickness of the reaction-preventing layer 8 is not particularly limited, and may be, for example, 1 μm to 50 μm.

[0042] [Oxygen electrode layer 9]

[0043] The oxygen electrode layer 9 is arranged on the opposite side of the hydrogen electrode layer 6 with respect to the electrolyte layer 7. In the present embodiment, since the electrolytic cell 1 includes the reaction prevention layer 8, the oxygen electrode layer 9 is arranged on the reaction prevention layer 8. When the electrolytic cell 1 does not include the reaction prevention layer 8, the oxygen electrode layer 9 is arranged on the electrolyte layer 7.

[0044] The oxygen electrode layer 9 is formed by the O transferred from the hydrogen electrode layer 6 through the electrolyte layer 7 according to the chemical reaction of the following formula (2). 2- Generates O2.

[0045] ·Oxygen electrode layer 9:2O 2- →O2+4e - ···(2)

[0046] The oxygen electrode layer 9 is composed of a porous material having oxide ion conductivity and electron conductivity. The oxygen electrode layer 9 can be composed of a composite of one or more of (La, Sr)(Co, Fe)O3, (La, Sr)FeO3, La(Ni, Fe)O3, (La, Sr)CoO3, and (Sm, Sr)CoO3 and an oxide ion conductive material (GDC, etc.).

[0047] The porosity of the oxygen electrode layer 9 is not particularly limited, and may be, for example, 20% to 60%. The thickness of the oxygen electrode layer 9 is not particularly limited, and may be, for example, 1 μm to 100 μm.

[0048] The method for forming the oxygen electrode layer 9 is not particularly limited, and a sintering method, a spraying method, a PVD method, a CVD method, or the like can be used.

[0049] [Metal support 20]

[0050] The metal support 20 supports the cell body 10. The metal support 20 is formed in a plate shape. The metal support 20 may be in a flat plate shape or in a curved plate shape. The metal support 20 may be capable of maintaining the strength of the electrolytic cell 1, and its thickness is not particularly limited, and may be, for example, 0.1 mm to 2.0 mm.

[0051] The metal support body 20 has a plurality of supply holes 21 , a first main surface 20S, and a second main surface 20T.

[0052] Each supply hole 21 penetrates the metal support 20 from the first main surface 20S to the second main surface 20T. Each supply hole 21 is open on the first main surface 20S and the second main surface 20T. Each supply hole 21 is formed in the area of ​​the first main surface 20S that is bonded to the hydrogen electrode layer 6. Each supply hole 21 is connected to the flow path 30a formed between the metal support 20 and the flow path component 30.

[0053] Each supply hole 21 can be formed by mechanical processing (such as punching), laser processing, or chemical processing (such as etching). Alternatively, when the metal support 20 is composed of a porous metal, each supply hole 21 can be a pore in the porous metal. Therefore, each supply hole 21 may not be formed perpendicular to the first main surface 20S and the second main surface 20T.

[0054] The cell body 10 is joined to the first main surface 20S. The flow path member 30 is joined to the second main surface 20T. The first main surface 20S is provided on the opposite side to the second main surface 20T.

[0055] The metal support 20 is made of a metal material. For example, the metal support 20 is made of an alloy material containing Cr (chromium). Examples of such metal materials include Fe-Cr-Mn alloy steel, Ni-Cr-Mn alloy steel, etc. The Cr content in the metal support 20 is not particularly limited and may be between 4% by mass and 30% by mass. The Mn content in the metal support 20 is not particularly limited and may be between 0% by mass and 1% by mass.

[0056] The metal support 20 may contain Ti (titanium) or Zr (zirconium). The content of Ti in the metal support 20 is not particularly limited, and may be 0.01 mol% to 1.0 mol%. The content of Zr in the metal support 20 is not particularly limited, and may be 0.01 mol% to 0.4 mol%. The metal support 20 may contain Ti in the form of TiO2 (titanium dioxide), and may contain Zr in the form of ZrO2 (zirconium dioxide).

[0057] The metal support 20 may have an oxide film formed on the surface by oxidation of the constituent elements of the metal support 20. As the oxide film, for example, a representative example is a chromium oxide film. The oxide film partially or entirely covers the surface of the metal support 20. In addition, the oxide film may partially or entirely cover the inner wall surface of each supply hole 21.

[0058] [Flow path member 30]

[0059] The flow path member 30 is bonded to the second main surface 20T of the metal support 20. The flow path member 30 forms a flow path 30a with the metal support 20. The raw material gas is supplied to the flow path 30a. The raw material gas supplied to the flow path 30a is supplied to the hydrogen electrode layer 6 of the cell body 10 through each supply hole 21 of the metal support 20.

[0060] The flow path member 30 may be made of, for example, an alloy material. The flow path member 30 may be formed of the same material as the metal support 20. In this case, the flow path member 30 may be substantially integrated with the metal support 20.

[0061] The flow path component 30 has a frame 31 and an interconnector 32. The frame 31 is an annular component that surrounds the side of the flow path 30a. The frame 31 is bonded to the second main surface 20T of the metal support 20. The interconnector 32 is a plate-shaped component that electrically connects the electrolytic cell 1 to an external power source or other electrolytic cells in series. The interconnector 32 is bonded to the frame 31.

[0062] As described above, in the flow path member 30 of the present embodiment, the frame body 31 and the interconnector 32 are separate components, but the frame body 31 and the interconnector 32 may be integrated.

[0063] [Area Occupancy of Gd(Cr, Mn) Oxide in Hydrogen Electrode Layer 6]

[0064] As described above, the hydrogen electrode layer 6 is composed of GDC, Gd(Cr, Mn) oxide, and Ni.

[0065] The average area occupancy of the Gd(Cr, Mn) oxide in the hydrogen electrode layer 6 is preferably 5.00% or less. This can prevent the excessive presence of the electrically insulating Gd(Cr, Mn) oxide, thereby ensuring the electrical conductivity required for the hydrogen electrode layer 6.

[0066] The lower limit of the average area occupancy of Gd(Cr, Mn) oxide in the hydrogen electrode layer 6 is not particularly limited and may be 0.50% or more. When the average area occupancy is less than 0.50%, it is difficult to accurately detect the average area occupancy in the calculation method described below.

[0067] The average area occupancy of the Gd(Cr, Mn) oxide can be calculated as follows.

[0068] First, the hydrogen electrode layer 6 is cut along the thickness direction.

[0069] Next, the cross section of the hydrogen electrode layer 6 was subjected to precision mechanical grinding and then to ion milling processing using IM4000 manufactured by Hitachi High-Technologies Corporation.

[0070] Next, a SEM image of an arbitrary position in the first region 61 of the hydrogen electrode layer 6 magnified 10,000 times was obtained using a FE-SEM (Field Emission Scanning Electron Microscope) using an inner lens secondary electron detector.

[0071] Next, the brightness of the SEM image was classified into 256 levels, and the brightness difference of the main phase, Ni phase, and gas phase was converted into three values. The main phase contains GDC and Gd (Cr, Mn) oxides. The Ni phase contains Ni. The main phase and Ni phase are solid phases.

[0072] Next, EDX (Energy Dispersive X-ray Spectroscopy) was used to obtain the EDX spectrum at the main phase position. Then, the EDX spectrum was semi-quantitatively analyzed to identify the elements present at the main phase position. Thus, on the SEM image, the main phase was divided into a region where GDC existed and a region where Gd (Cr, Mn) oxide existed.

[0073] Next, the SEM image was analyzed using image analysis software HALCON manufactured by MVTec (Germany), thereby obtaining an analysis image in which the Gd(Cr, Mn) oxide was highlighted.

[0074] Next, the total area of ​​the Gd (Cr, Mn) oxides in the analysis image is divided by the total area of ​​the solid phase (ie, the region excluding the gas phase), thereby determining the first area occupancy of the Gd (Cr, Mn) oxides in the first region 61 .

[0075] In addition, the second area occupancy of the Gd (Cr, Mn) oxide in the second region 62 is obtained by the same method as the first area occupancy of the Gd (Cr, Mn) oxide in the first region 61 .

[0076] Then, the arithmetic mean of the first and second area occupancies is calculated as the average area occupancy of the Gd (Cr, Mn) oxide in the hydrogen electrode layer 6 .

[0077] Here, the first area occupancy of the Gd (Cr, Mn) oxide in the first region 61 is preferably smaller than the second area occupancy of the Gd (Cr, Mn) oxide in the second region 62. Thus, the three-phase interface (reaction field) in the first region 61 where the electrode reaction is active can be ensured, and the skeleton structure of the second region 62 that is prone to thermal stress due to the difference in thermal expansion coefficient with the metal support 20 can be strengthened. Accordingly, it is possible to simultaneously maintain electrode performance and suppress cracks.

[0078] The first area occupancy of the Gd (Cr, Mn) oxide in the first region 61 is not particularly limited, and may be, for example, 0.50% to 10.0%. The second area occupancy of the Gd (Cr, Mn) oxide in the second region 62 is not particularly limited, and may be, for example, 0.50% to 10.0%.

[0079] (Variation of the embodiment)

[0080] As mentioned above, although embodiment of this invention is described, this invention is not limited to these embodiment, Various changes can be made as long as they do not deviate from the summary of this invention.

[0081] [Modification 1]

[0082] In the above embodiment, the hydrogen electrode layer 6 functions as a cathode and the oxygen electrode layer 9 functions as an anode. However, the hydrogen electrode layer 6 may function as an anode and the oxygen electrode layer 9 may function as a cathode. In this case, the constituent materials of the hydrogen electrode layer 6 and the oxygen electrode layer 9 are exchanged, and the raw material gas is flowed to the outer surface of the hydrogen electrode layer 6.

[0083] [Modification 2]

[0084] In the above embodiment, the electrolytic cell 1 is described as an example of an electrochemical cell, but the electrochemical cell is not limited to the electrolytic cell. An electrochemical cell is a general term for an element that is configured with a pair of electrodes in order to convert electrical energy into chemical energy in such a way that an electromotive force is generated by an overall redox reaction, and an element that converts chemical energy into electrical energy. Therefore, the electrochemical cell includes, for example, a fuel cell that uses oxide ions or protons as carriers.

[0085] [Variation 3]

[0086] In the above embodiment, the electrolytic cell 1 includes the reaction prevention layer 8 , and therefore the reaction prevention layer 8 is connected to the electrolyte layer 7 . However, when the electrolytic cell 1 does not include the reaction prevention layer 8 , the oxygen electrode layer 9 is connected to the electrolyte layer 7 .

[0087] Example

[0088] Hereinafter, examples of the electrochemical cell according to the present invention will be described; however, the present invention is not limited to the examples described below.

[0089] (Examples 1 to 10)

[0090] The electrolytic cells of Examples 1 to 10 were produced as follows.

[0091] First, a metal support body made of Fe—Cr—Mn alloy steel and having a plurality of supply holes formed therein is prepared.

[0092] Next, GDC powder, Gd (Cr, Mn) oxide powder, NiO powder, butyral resin, polymethyl methacrylate beads as a pore-forming material, plasticizer, dispersant, and solvent are mixed to prepare a slurry for the hydrogen electrode layer. At this time, the amount of Gd (Cr, Mn) oxide powder added is adjusted to change the average area occupancy of Gd (Cr, Mn) oxide in the hydrogen electrode layer as shown in Table 1. Then, the slurry for the hydrogen electrode layer is printed on the first main surface of the metal support by a scraper method to form a molded body of the hydrogen electrode layer.

[0093] Next, YSZ powder, butyral resin, plasticizer, dispersant, and solvent are mixed to prepare electrolyte layer slurry, and then the electrolyte slurry is printed by doctor blade method so as to cover the molded body of hydrogen electrode layer, thereby forming a molded body of electrolyte layer.

[0094] Next, GDC powder, polyvinyl alcohol, and a solvent are mixed to prepare a reaction-preventing layer slurry, and then the reaction-preventing layer slurry is printed on the molded body of the electrolyte layer by a doctor blade method to form a molded body of the reaction-preventing layer.

[0095] Next, the respective molded bodies of the hydrogen electrode layer, electrolyte layer, and reaction prevention layer sequentially arranged on the metal support were fired in the air (1050° C., 1 hour) to form the hydrogen electrode layer, electrolyte layer, and reaction prevention layer.

[0096] Next, (La, Sr)(Co, Fe)O3 powder, polyvinyl alcohol, and a solvent are mixed to prepare an oxygen electrode layer slurry. The oxygen electrode layer slurry is then printed on the reaction-proof layer using a doctor blade method to form a molded body of the oxygen electrode layer.

[0097] Next, the molded body of the oxygen electrode layer was fired in the air (1000° C., 1 hour) to form an oxygen electrode.

[0098] Finally, a flow path member made of Fe—Cr—Mn alloy steel was connected to the second main surface of the metal support using crystallized glass. Through the above operations, the electrolytic cells of Examples 1 to 10 were completed.

[0099] (Comparative Example 1)

[0100] The electrolytic cell of Comparative Example 1 was produced by the same steps as in Examples 1 to 10, except that the slurry for the hydrogen electrode layer was prepared without using the Gd(Cr, Mn) oxide powder.

[0101] (Area Occupancy of Gd(Cr, Mn) Oxide in Hydrogen Electrode Layer)

[0102] The area occupancy of the Gd(Cr, Mn) oxide in the hydrogen electrode layer was calculated using the method described in the above embodiment. The calculation results are shown in Table 1.

[0103] (Thermal cycle test)

[0104] While supplying a mixed gas of Ar and hydrogen (4% hydrogen relative to Ar) to the hydrogen electrode layer from the flow path in the flow path component to maintain a reducing atmosphere, the process of raising the temperature from room temperature to 750°C in 2 hours and then cooling it to room temperature in 4 hours was set as one cycle and repeated 10 times.

[0105] Then, the cross section of the hydrogen electrode was observed by FE-SEM to check whether cracks with a length of 1 μm or more were generated in the hydrogen electrode. In Table 1, the case where no cracks were generated in the hydrogen electrode was evaluated as "0", and the case where cracks were generated in the hydrogen electrode was evaluated as "×".

[0106] (Initial Performance Evaluation)

[0107] While the temperature of the electrolytic cell was raised to 750°C, a mixed gas of water vapor and hydrogen (mixing ratio 50:50) was supplied to the hydrogen electrode layer from the flow path in the flow path component, and air was supplied to the oxygen electrode layer. The flow path was scanned at 0.5 A / cm 2 The current value is used to obtain the electrolysis voltage at that time. Then, the electrolysis voltage increase rate is calculated using the following formula (3) with the electrolysis voltage of Comparative Example 1 as the reference.

[0108] Electrolysis voltage increase rate of each example (%) = 100 × ((electrolysis voltage of each example) - (electrolysis voltage of Comparative Example 1)) / (electrolysis voltage of Comparative Example 1) ... (3)

[0109] In Table 1, the case where the electrolysis voltage increase rate was less than 1% was evaluated as "0", and the case where the electrolysis voltage increase rate was 1% or more was evaluated as "△".

[0110] [Table 1]

[0111]

[0112] As shown in Table 1, in Examples 1 to 10 in which the hydrogen electrode layer contains Gd (Cr, Mn) oxide, cracks in the hydrogen electrode layer can be suppressed. This result is obtained because the skeleton structure of the porous hydrogen electrode layer can be strengthened by improving the sinterability (neck growth between particles) of the hydrogen electrode layer. This effect is effective in metal-supported single cells that are difficult to sinter at high temperatures.

[0113] In Examples 1 to 8, in which the average area occupancy of Gd(Cr, Mn) oxide was set to 5.00% or less, sufficient initial performance was maintained. This result was obtained because the excessive presence of Gd(Cr, Mn) oxide having electrical insulation properties was suppressed.

[0114] (Examples 11 to 14)

[0115] Except that the hydrogen electrode layer had a two-layer structure, the electrolytic cells of Examples 11 to 14 were produced by the same steps as in Examples 1 to 10. Here, only the method of forming the two-layer structure hydrogen electrode layer will be described.

[0116] First, GDC powder, Gd (Cr, Mn) oxide powder, NiO powder, butyral resin, polymethyl methacrylate beads as a pore-forming material, plasticizer, dispersant, and solvent are mixed to prepare a first region slurry and a second region slurry, respectively. Then, the second region slurry is printed on the first main surface of the metal support to form a second region molded body, and then the first region slurry is printed on the second region molded body to form a first region molded body.

[0117] Here, in Examples 11 to 14, the amount of Gd (Cr, Mn) oxide powder added in the first region slurry is adjusted to be less than the amount of Gd (Cr, Mn) oxide powder added in the second region slurry. Thus, as shown in Table 2, the average area occupancy of Gd (Cr, Mn) oxide in the first region of the hydrogen electrode layer is made smaller than the average area occupancy of Gd (Cr, Mn) oxide in the second region of the hydrogen electrode layer.

[0118] For Examples 11 to 14, the measurement of the area occupancy of the Gd (Cr, Mn) oxide, the heat cycle test, and the initial performance evaluation were carried out in the same manner as in Examples 1 to 10.

[0119] The measurement results are shown in Table 2. In Table 2, regarding the thermal cycle test, the case where no cracks were generated in the hydrogen electrode was evaluated as "0". In addition, in Table 2, regarding the initial performance evaluation, the case where the electrolysis voltage increase rate was less than 0.5% was evaluated as "A", the case where the electrolysis voltage increase rate was 0.5% or more and less than 1% was evaluated as "B", the case where the electrolysis voltage increase rate was 1.0% or more and less than 3.0% was evaluated as "C", and the case where the electrolysis voltage increase rate was 3.0% or more and less than 10% was evaluated as "D".

[0120] [Table 2]

[0121]

[0122] As shown in Table 2, in Example 11, in which the average area occupancy of Gd (Cr, Mn) oxide in the first region of the hydrogen electrode layer is smaller than the average area occupancy of Gd (Cr, Mn) oxide in the second region of the hydrogen electrode layer, the initial performance can be further improved compared with Example 12. This is because: by reducing the area occupancy of Gd (Cr, Mn) oxide in the first region where the electrode reaction is active, the three-phase interface in the first region can be ensured.

[0123] Similarly, in Example 13, in which the average area occupancy of Gd (Cr, Mn) oxide in the first region of the hydrogen electrode layer is smaller than the average area occupancy of Gd (Cr, Mn) oxide in the second region of the hydrogen electrode layer, the initial performance can be further improved compared to Example 14.

[0124] In Examples 11 and 12 in which the average area occupancy of the Gd(Cr, Mn) oxide was set to 5.00% or less, the initial performance was further improved compared to Examples 13 and 14.

[0125] Explanation of symbols

[0126] 1 single battery

[0127] 6 Hydrogen polar layer

[0128] 61 First Area

[0129] 62 Second Area

[0130] 7 Electrolyte layer

[0131] 8 Anti-reaction layer

[0132] 9 Oxygen electrode layer

[0133] 10Single battery main body

[0134] 20Metal support

[0135] 21 Supply hole

[0136] 30 Flow path components

[0137] 30a flow path

Claims

1. An electrochemical cell, wherein: have: Hydrogen polar layer; an oxygen electrode layer; and an electrolyte layer, the electrolyte layer being arranged between the hydrogen electrode layer and the oxygen electrode layer, The hydrogen electrode layer is composed of a perovskite-type oxide containing gadolinium, chromium, and manganese, gadolinium-doped cerium dioxide, and nickel.

2. The electrochemical cell according to claim 1, wherein: The average area occupancy of the perovskite type oxide in the cross section of the hydrogen electrode layer is 5.00% or less.

3. The electrochemical cell according to claim 1 or 2, wherein: The hydrogen electrode layer has a first region located on the electrolyte layer side with respect to the center in the thickness direction, and a second region located on the opposite side to the electrolyte layer with respect to the center in the thickness direction. A first area occupancy of the perovskite type oxide in the first region is smaller than a second area occupancy of the perovskite type oxide in the second region.

4. The electrochemical cell according to claim 1, wherein: The electrochemical cell further includes a plate-shaped metal support that supports the hydrogen electrode layer and has a plurality of supply holes.