Roughened copper foil, copper foil with carrier, copper-clad laminate, and printed wiring board

By optimizing the surface roughening treatment parameters and chemical treatment of copper foil, the problem of reducing adhesion of copper foil in high-frequency uses is solved, and high adhesion and excellent high-frequency characteristics with thermoplastic resin are achieved, thereby reducing transmission loss .

CN118922588APending Publication Date: 2024-11-08MITSUI MINING & SMELTING CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202380026598.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-02-07
Filing Date
2023-03-16
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the high-frequency use of existing copper foils, the fine refinement of roughened particles leads to a decrease in adhesion with the thermoplastic resin, making it difficult to take into account both high adhesion and excellent high-frequency characteristics.

Method used

By controlling the peak density Sds of the roughened copper foil and the volume of roughened particles per 1 μm2 is 1.57 μm-2 or more and 2.64 μm-2 or less, the skewness Ssk is greater than 0.35, and the sag Sku is greater than 2.70 or more and 4.90 or less, The load area ratio Smr1 of the separation protruding peak and the central part is 11.2% or more, and the surface shape and chemical properties of the copper foil are optimized in combination with the anti-rust treatment layer and/or the silane coupling agent layer.

Benefits of technology

High adhesion and excellent high-frequency characteristics with thermoplastic resin are achieved, transmission loss is reduced, and anchoring effect and moisture resistance of copper foil and resin are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005035661170000161
    Figure BDA0005035661170000161
  • Figure BDA0005035661170000171
    Figure BDA0005035661170000171
  • Figure BDA0005035661170000271
    Figure BDA0005035661170000271
Patent Text Reader

Abstract

Provided is a roughened copper foil capable of achieving both high adhesion to a thermoplastic resin and excellent high-frequency characteristics. The roughened copper foil has a roughened surface on at least one side. The peak top density (Sds) of the roughened surface is from 1.57 [mu] m <-2 > to 2.64 [mu] m <-2 > (inclusive). In addition, the roughened surface has a plurality of roughened particles, and the volume of the roughened particles per 1 [mu] m2 is from 0.11 [mu] m3 to 0.25 [mu] m3 (inclusive). And Sds is a value measured in accordance with EUR15178N under a condition in which cutoff by the S filter and the L filter is not performed. The volume of the roughened particles per 1 [mu] m2 is a value calculated by obtaining an image of the roughened surface using FIB-SEM and three-dimensionally analyzing the image.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a roughened copper foil, a copper foil with a carrier, a copper-clad laminate and a printed circuit board. Background Art

[0002] With the high functionality of portable electronic devices in recent years, in order to process a large amount of information at high speed, the high frequency of signals is constantly developing, requiring printed circuit boards suitable for high-frequency applications such as 5G, millimeter waves, and base station antennas. For such high-frequency printed circuit boards, in order to be able to transmit high-frequency signals without reducing quality, it is desirable to reduce transmission loss. The printed circuit board has a copper foil and an insulating resin substrate processed into a wiring pattern, and the transmission loss is mainly composed of the conductor loss caused by the copper foil and the dielectric loss caused by the insulating resin substrate. Therefore, in order to reduce the dielectric loss caused by the insulating resin substrate, it is convenient as long as a thermoplastic resin with a low dielectric constant can be used. However, thermoplastic resins with a low dielectric constant represented by fluororesins and liquid crystal polymers (LCP) are different from thermosetting resins, and have low chemical activity, so the adhesion with copper foil is low.

[0003] Therefore, a technology for improving the adhesion between copper foil and thermoplastic resin is proposed. For example, Patent Document 1 (International Publication No. 2016 / 174998) discloses a copper foil having a roughened surface, the roughened surface having a ten-point average roughness Rzjis of 0.6 μm or more and 1.7 μm or less, and a half-peak width in the frequency distribution of the height of the roughened particles of 0.9 μm or less. According to the above copper foil, even for an insulating resin substrate such as a liquid crystal polymer film that cannot be expected to be chemically bonded, a high peel strength can be exhibited.

[0004] On the other hand, the conductor loss may increase due to the skin effect of the copper foil, which appears more significantly at higher frequencies. Therefore, in order to suppress the transmission loss in high-frequency applications and reduce the skin effect of the copper foil, the roughening particles are required to be miniaturized. As a copper foil having the above-mentioned fine roughening particles, for example, Patent Document 2 (International Publication No. 2014 / 133164) discloses a surface-treated copper foil having a black roughened surface roughened by attaching copper particles (e.g., roughly spherical copper particles) with a particle size of 10 nm or more and 250 nm or less.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: International Publication No. 2016 / 174998

[0008] Patent Document 2: International Publication No. 2014 / 133164 Summary of the invention

[0009] As mentioned above, copper foil for high-frequency applications requires that the roughened particles be miniaturized, but the adhesion between such copper foil and resin (particularly thermoplastic resin) is easily reduced. In this regard, from the perspective of achieving both high adhesion with thermoplastic resin and excellent high-frequency characteristics, the existing copper foil may not be sufficient, and there is room for improvement.

[0010] The present inventors have obtained the following findings: on the surface of the roughened copper foil, by adjusting the peak density Sds and the peak density per 1 μm 2 The volumes of the roughened particles are controlled within a predetermined range, respectively, so that both high adhesion with the thermoplastic resin and excellent high-frequency characteristics can be achieved.

[0011] Therefore, an object of the present invention is to provide a roughened copper foil capable of achieving both high adhesion to a thermoplastic resin and excellent high-frequency characteristics.

[0012] According to the present invention, the following aspects are provided.

[0013] [Method 1]

[0014] A roughened copper foil having a roughened surface on at least one side.

[0015] The peak density Sds of the roughened surface is 1.57 μm. -2 Above and 2.64μm -2 the following,

[0016] The roughened surface has a plurality of roughened particles, each 1 μm 2 The volume of the aforementioned roughened particles is 0.11 μm 3 Above and 0.25μm 3 the following,

[0017] The above Sds is a value measured according to EUR15178N without performing cutoff by S filter and L filter.

[0018] Each 1μm 2 The volume of the roughened grains is a value calculated by obtaining an image of the roughened surface using FIB-SEM and performing three-dimensional analysis on the image.

[0019] [Method 2]

[0020] The roughened copper foil according to Embodiment 1, wherein the skewness Ssk of the roughened surface is greater than 0.35,

[0021] The above-mentioned Ssk is a value measured in accordance with JIS B0681-2:2018 under the conditions that no cutoff by an S filter is performed and the cutoff wavelength by an L filter is 1.0 μm.

[0022] [Method 3]

[0023] The roughened copper foil according to aspect 1 or 2, wherein the kurtosis Sku of the roughened surface is 2.70 or more and 4.90 or less,

[0024] The above-mentioned Sku is a value measured in accordance with JIS B0681-2:2018 under the condition that cutoff by the S filter and the L filter is not performed.

[0025] [Method 4]

[0026] The roughened copper foil according to any one of aspects 1 to 3, wherein a load area ratio Smr1 of the roughened surface separating the protruding peaks and the center is 11.2% or more,

[0027] The above-mentioned Smr1 is a value measured in accordance with JIS B0681-2:2018 under the conditions that no cutoff by an S filter is performed and the cutoff wavelength by an L filter is 1.0 μm.

[0028] [Method 5]

[0029] The roughened copper foil according to any one of aspects 1 to 4, further comprising a rust-proofing layer and / or a silane coupling agent layer on the roughened surface.

[0030] [Method 6]

[0031] A copper foil with a carrier, comprising: a carrier, a release layer provided on the carrier, and the roughened copper foil according to any one of aspects 1 to 5 provided on the release layer with the roughened surface facing the outside.

[0032] [Method 7]

[0033] A copper-clad laminate comprising the roughened copper foil according to any one of aspects 1 to 5.

[0034] [Method 8]

[0035] A printed wiring board comprising the roughened copper foil according to any one of aspects 1 to 5. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1A This is a diagram for explaining the skewness Ssk measured in accordance with JIS B0681-2:2018, and is a diagram showing a surface and its height distribution when Ssk<0.

[0037] Figure 1BThis is a diagram for explaining the skewness Ssk measured in accordance with JIS B0681-2:2018, and is a diagram showing a surface and its height distribution when Ssk>0.

[0038] Figure 2A This is a diagram for explaining the peak density Sds measured according to EUR15178N, and shows that Sds = 5 μm -2 An example of the surface and peak when .

[0039] Figure 2B This is a diagram for explaining the peak top density Sds measured according to EUR15178N, and shows Sds = 1 μm -2 An example of the surface and peak when .

[0040] Figure 3 This is a diagram for explaining the load curve and load area ratio determined in accordance with JIS B0681-2:2018.

[0041] Figure 4 This is a diagram for explaining the load area ratio Smr1 separating the protruding peak portion and the center portion measured in accordance with JIS B0681-2:2018.

[0042] Figure 5 This is the binarized resin replica image obtained in Example 3.

[0043] Figure 6 The diagram shows the x-axis, y-axis, and z-axis, and the slice plane S in FIB-SEM observation and three-dimensional image analysis in relation to the roughened copper foil.

[0044] Figure 7 This is a slice image of the roughened copper foil of Example 9 after forming a mark and a protective film.

[0045] Figure 8 This is an image for explaining the allocation of materials in three-dimensional image analysis.

[0046] Fig. 9 Yes Figure 7 The first inference image generated by machine learning on the image.

[0047] Fig. 10A This is an example of a slice image showing a continuous roughened bottom surface and roughened grains of a roughened copper foil.

[0048] Fig. 10B This is an example of a slice image in which the roughened bottom surface of the roughened copper foil and the roughened grains are discontinuous. DETAILED DESCRIPTION

[0049] definition

[0050] Definitions of terms and parameters used to specify the present invention are shown below.

[0051] In this specification, "skewness Ssk" or "Ssk" refers to a parameter indicating the symmetry of the height distribution measured in accordance with JIS B0681-2:2018. When this value is 0, it means that the height distribution is symmetrical in the upper and lower parts, in other words, it means that protrusions (roughening particles, etc.) of the same size are arranged on the surface. Figure 1A As shown in FIG. 1 , when the value is less than 0, it indicates that the surface has many fine valleys, in other words, it indicates that thick protrusions with rounded corners are arranged on the surface. Figure 1B As shown, when this value is greater than 0, it means that the surface has many fine peaks, in other words, it means that fine and long protrusions are scattered on the surface.

[0052] In this specification, "peak top density Sds" or "Sds" refers to a parameter indicating the number of peak tops per unit area measured in accordance with EUR15178N. Figure 2A and 2B As shown, in the calculation of Sds, the point higher than the 8 neighboring points N is regarded as the peak S. The larger the value, the denser the protrusions are (refer to Figure 2A On the other hand, the smaller the value, the more sparsely the protrusions exist (refer to Figure 2B ).

[0053] In this specification, the "surface load curve" (hereinafter referred to as "load curve") refers to a curve indicating the height of the load area ratio of 0% to 100% determined in accordance with JIS B0681-2:2018. Figure 3 As shown in the figure, the load area ratio is a parameter that indicates the area of ​​a region above a certain height c. The load area ratio at height c is equivalent to Figure 3 Smr(c) in Figure 4 As shown, the secant of the load curve drawn from the load area ratio of 0% along the load curve with the load area ratio difference set to 40% is moved from the load area ratio of 0%, and the position where the inclination of the secant is the most gentle is called the central part of the load curve of the surface. The straight line with the smallest sum of the squares of the deviations in the longitudinal direction relative to the central part is called the equivalent straight line. The part of the height range of the load area ratio of 0% to 100% included in the equivalent straight line is called the central part. The part higher than the central part is called the protruding peak part, and the part lower than the central part is called the protruding valley part.

[0054] In this manual, if Figure 4As shown, "load area ratio Smr1 separating the protruding peak and the center" or "Smr1" refers to a parameter of the load area ratio at the intersection of the height of the upper part of the center and the load curve of the surface (i.e., the load area ratio separating the center and the protruding peak) measured in accordance with JIS B0681-2:2018.

[0055] In this specification, "kurtosis Sku" refers to a parameter indicating the sharpness of the height distribution measured in accordance with JIS B0681-2:2018, also known as kurtosis. Sku=3 means that the height distribution is a normal distribution, in other words, it means that there are protrusions of uniform size arranged on the surface. If Sku>3, it means that there are many sharp peaks and valleys on the surface, in other words, there are many fine protrusions standing on the surface. If Sku<3, it means that the surface is flat, in other words, it means that there are thick protrusions with rounded corners arranged on the surface.

[0056] Ssk, Sds, Smr1 and Sku can be calculated by measuring the surface profile of a specified measurement area (e.g., a two-dimensional area of ​​64.397 μm × 64.463 μm) in the roughened surface using a commercially available laser microscope. In this specification, Ssk and Smr1 are measured without S filter cutoff and with a L filter cutoff wavelength of 1.0 μm. On the other hand, Sds and Sku are measured without S filter and L filter cutoff. In addition, the preferred measurement conditions and analysis conditions for the surface profile using a laser microscope are shown in the embodiments described below.

[0057] In this specification, “per 1 μm 2 The “volume of roughened particles” refers to the value calculated by obtaining an image of the roughened surface using FIB-SEM and performing a three-dimensional analysis of the image. The three-dimensional analysis can be preferably performed using commercially available three-dimensional image processing software (e.g., Dragonfly (version 2022.1.0.1259) manufactured by Object Research System) through the following steps.

[0058] (1) The slice image of the roughened copper foil obtained by FIB-SEM is read and aligned.

[0059] (2) Implement trimming of sliced ​​images.

[0060] (3) Machine learning is performed to extract the Cu portion derived from the roughened copper foil, and a segmentation model is created.

[0061] (4) Apply the segmentation model to the slice image to extract the Cu part.

[0062] (5) Based on the root diameter of the roughened particles, the roughened particles were extracted from the Cu portion.

[0063] (6) Trim the specified analysis area (e.g., 4.5 μm × 4.5 μm) and calculate the 2 The volume of roughened particles.

[0064] Preferred measurement conditions and sample preparation methods of FIB-SEM, details of the analysis method using the above-mentioned three-dimensional image processing software, and a specific calculation method of the root diameter of the roughened particles are described in the examples described later.

[0065] In this specification, the "electrode surface" of the electrolytic copper foil refers to the surface on the side that comes into contact with the cathode during the production of the electrolytic copper foil.

[0066] In this specification, the "deposition surface" of the electrolytic copper foil refers to the surface on the side where the electrolytic copper is deposited during the production of the electrolytic copper foil, that is, the surface on the side not in contact with the cathode.

[0067] Roughened copper foil

[0068] The copper foil of the present invention is a roughened copper foil. The roughened copper foil has a roughened surface on at least one side. The peak density Sds of the roughened surface is 1.57 μm. -2 Above and 2.64μm -2 In addition, the roughened surface has a plurality of roughened particles, each 1 μm 2 The volume of the roughened particles is 0.11 μm 3 Above and 0.25μm 3 In this way, on the surface of the roughened copper foil, the peak density Sds is calculated by comparing the peak density Sds with the peak density Sds per 1 μm. 2 The volumes of the roughened particles are controlled within a predetermined range, respectively, so that both high adhesion with the thermoplastic resin and excellent high-frequency characteristics can be achieved.

[0069] As mentioned above, in order to suppress the transmission loss in high-frequency applications and to reduce the skin effect of copper foil, the roughening particles are required to be miniaturized. However, the anchoring effect of the copper foil with the above-mentioned fine roughening particles and the resin substrate (i.e., the physical adhesion improvement effect utilizing the concavo-convex surface of the copper foil) is reduced, and as a result, the adhesion with the resin is easily deteriorated. In particular, the thermoplastic resin with low dielectric constant represented by fluororesin and liquid crystal polymer (LCP) is different from thermosetting resin, and has low chemical activity, so the adhesion with the copper foil is low. In this way, the low roughness copper foil, which is advantageous in high-frequency characteristics, is originally easy to deteriorate in adhesion with the resin. In contrast, according to the roughening copper foil of the present invention, it is unexpectedly possible to take into account both the high adhesion with the thermoplastic resin and the excellent high-frequency characteristics (such as the reduction of the skin effect).

[0070] The mechanism for achieving both high adhesion to the resin and excellent high-frequency characteristics is not necessarily certain, but it is considered as follows, for example. That is, if the roughened surface has a thickness of 1 μm 2 The volume of the roughened particles is 0.11 μm 3 Above and 0.25μm 3 The following small values ​​indicate that the surface of the roughened particles has fine particles that are effective in reducing the skin effect. Furthermore, the peak density Sds is 1.57 μm -2 Above and 2.64μm -2 The density of the protrusions on the roughened surface is moderate, and it is possible to achieve a good balance between high adhesion to the thermoplastic resin and excellent high-frequency characteristics. That is, as mentioned above, the peak density Sds is a parameter indicating the number of peaks per unit area, in other words, it can be said to be a parameter related to the size of the roughened particles in the roughened surface. In this regard, by controlling the peak density Sds of the roughened surface to 1.57 μm -2 As a result, the size of the roughened particles becomes fine, which is a surface shape that is effective in reducing the skin effect. On the other hand, by controlling the peak density Sds of the roughened surface to 2.64 μm -2 Then, the size of the roughened particles becomes appropriate, and the surface shape can exert a high anchoring effect with the thermoplastic resin substrate. As a result, it is considered that both high adhesion with the thermoplastic resin and excellent high-frequency characteristics can be achieved.

[0071] Therefore, the Sds of the roughened surface of the roughened copper foil is 1.57 μm. -2 Above and 2.64μm -2 Below, preferably 1.57 μm -2 Above and 2.57μm -2 Below, more preferably 1.62 μm -2 Above and 2.57μm -2 the following.

[0072] In addition, the roughened copper foil has a roughened surface with a thickness of 1 μm. 2 The volume of the roughened particles is 0.11 μm 3 Above and 0.25μm 3 Below, preferably 0.11 μm 3 Above and 0.18μm 3 Below, more preferably 0.11 μm 3 Above and 0.16μm 3 the following.

[0073] The Ssk of the roughened surface of the roughened copper foil is preferably greater than 0.35, more preferably greater than 0.35 and less than 0.79, and further preferably greater than 0.36 and less than 0.57. The larger the numerical value of the Ssk of the roughened surface, the more fine peaks there are, that is, there are elongated roughened particles scattered. Therefore, if the Ssk of the roughened surface is a value greater than 0.35, the roughened particles have a fine longitudinal shape. As a result, compared with the previous roughly spherical roughened particles (Ssk = about 0.2 to 0.3), extremely low and uniform roughened particles (Ssk = about 0 to 0.1), etc., it is possible to exert a high anchoring effect with the thermoplastic resin substrate. In addition, compared with roughened particles with a coarse and large shape (Ssk <0), the skin effect can be reduced. As a result, it is possible to further achieve high adhesion and excellent high-frequency characteristics with thermoplastic resins in a well-balanced manner.

[0074] The Sku of the roughened surface of the roughened copper foil is preferably 2.70 to 4.90, more preferably 3.00 to 4.00, and even more preferably 3.00 to 3.60. If the Sku is within the above range, high adhesion to the thermoplastic resin and excellent high frequency characteristics can be achieved in a well-balanced manner.

[0075] The Smr1 of the roughened surface of the roughened copper foil is preferably 11.2% or more, more preferably 11.2% or more and 13.4% or less, and further preferably 11.3% or more and 12.4% or less. When Smr1 is within the above range, high adhesion to the thermoplastic resin and excellent high-frequency characteristics can be achieved in a well-balanced manner.

[0076] The thickness of the roughened copper foil is not particularly limited, and is preferably 0.1 μm or more and 35 μm or less, more preferably 0.5 μm or more and 5.0 μm or less, and further preferably 1.0 μm or more and 3.0 μm or less. It should be noted that the roughened copper foil is not limited to the roughening of the surface of the ordinary copper foil, and the surface of the copper foil of the copper foil with a carrier can also be roughened. Here, the thickness of the roughened copper foil is the thickness of the height of the roughened particles formed on the surface of the roughened surface (the thickness of the copper foil itself constituting the roughened copper foil).

[0077] The roughened copper foil has a roughened surface on at least one side. That is, the roughened copper foil may have a roughened surface on both sides or only on one side. As described above, the roughened surface preferably has a plurality of roughened particles (preferably longitudinally shaped roughened particles), and these plurality of roughened particles are respectively formed of copper particles. The copper particles may be formed of metallic copper or of a copper alloy.

[0078] The roughening treatment for forming the roughening treatment surface can be preferably performed by forming roughening particles with copper or copper alloy on the copper foil. The roughening treatment is preferably performed according to a plating method that undergoes two stages of plating processes. At this time, in the first stage of the plating process, it is preferred to use a copper sulfate solution with a copper concentration of 5 g / L or more and 9 g / L or less (more preferably 7 g / L or more and 9 g / L or less), a sulfuric acid concentration of 100 g / L or more and 150 g / L or less (more preferably 100 g / L or more and 130 g / L or less), and a tungsten concentration of 5 mg / L or more and 20 mg / L or less (more preferably 10 mg / L or more and 20 mg / L or less) for electrodeposition. The electrodeposition is preferably performed at a liquid temperature of 20°C or more and 50°C or less (more preferably 30°C or more and 50°C or less) and a current density of 10 A / dm 2 Above and 40A / dm 2 Below (more preferably 20A / dm 2 Above and 40A / dm 2 The electroplating is carried out under the plating conditions of 50A·s to 200A·s (more preferably 50A·s to 150A·s). In particular, in the first stage of the plating process, by using a copper sulfate solution having a copper concentration lower than that of the previous method and containing an inorganic additive within the above concentration range, it is easy to form fine longitudinal roughened particles on the treated surface. In the second stage of the plating process, it is preferred to use a copper sulfate solution having a copper concentration of 40g / L to 70g / L (more preferably 50g / L to 70g / L) and a sulfuric acid concentration of 100g / L to 300g / L (more preferably 150g / L to 250g / L) for electroplating. The electroplating is preferably carried out under the conditions of a liquid temperature of 30°C to 60°C (more preferably 40°C to 50°C) and a current density of 10A / dm 2 Above and 40A / dm 2 Below (more preferably 20A / dm 2 Above and 40A / dm 2 The plating process is carried out under the following conditions: the ...

[0079] As required, the roughened copper foil may also be subjected to rust-proof treatment to form a rust-proof treatment layer. The rust-proof treatment preferably includes a zinc plating treatment. The zinc plating treatment may be any of a zinc plating treatment and a zinc alloy plating treatment, and the zinc alloy plating treatment is particularly preferably a zinc-nickel alloy treatment. The zinc-nickel alloy treatment may be a plating treatment containing at least Ni and Zn, and may also contain other elements such as Sn, Cr, and Co. The Ni / Zn adhesion ratio in the zinc-nickel alloy plating is preferably 1.2 or more and 10 or less in terms of mass ratio, more preferably 2 or more and 7 or less, and further preferably 2.7 or more and 4 or less. In addition, the rust-proof treatment preferably also includes a chromate treatment, and the chromate treatment is more preferably performed on the surface of the zinc plating after the zinc plating treatment. Thus, the rust resistance can be further improved. A particularly preferred rust-proof treatment is a combination of a zinc-nickel alloy plating treatment and a subsequent chromate treatment.

[0080] As required, the roughened copper foil may be a copper foil having a silane coupling agent treated on the surface and having a silane coupling agent layer formed thereon. Thus, moisture resistance, chemical resistance, and adhesion to adhesives, etc. can be improved. The silane coupling agent layer can be formed by appropriately diluting the silane coupling agent, applying it, and drying it. Examples of silane coupling agents include epoxy-functional silane coupling agents such as 4-glycidylbutyltrimethoxysilane and 3-glycidoxypropyltrimethoxysilane, or 3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-3-(4-(3-aminopropoxy)butoxy)propyl-3-aminopropyltrimethoxysilane, N-phenyl-3-aminopropyl The present invention can be used as the silane coupling agent of claim 1, wherein the silane coupling agent comprises an amino-functional silane coupling agent such as trimethoxy silane, a mercapto-functional silane coupling agent such as 3-mercaptopropyltrimethoxy silane, an olefin-functional silane coupling agent such as vinyltrimethoxy silane and vinylphenyltrimethoxy silane, an acrylic-functional silane coupling agent such as 3-methacryloxypropyltrimethoxy silane, an imidazole-functional silane coupling agent such as imidazole silane, or a triazine-functional silane coupling agent such as triazine silane.

[0081] According to the above reasons, the roughened copper foil preferably also has an antirust treatment layer and / or a silane coupling agent layer on the roughened surface, and more preferably has both an antirust treatment layer and a silane coupling agent layer. In the case where the roughened surface is formed with an antirust treatment layer and / or a silane coupling agent layer, the values ​​of various parameters of the roughened surface in this specification refer to the values ​​obtained by measuring and analyzing the roughened copper foil after the antirust treatment layer and / or the silane coupling agent layer are formed. The antirust treatment layer and the silane coupling agent layer can be formed not only on the roughened surface side of the roughened copper foil, but also on the side where the roughened surface is not formed.

[0082] Copper foil with carrier

[0083] As described above, the roughened copper foil of the present invention can also be provided in the form of a copper foil with a carrier. That is, according to a preferred embodiment of the present invention, a copper foil with a carrier is provided, which comprises a carrier, a peeling layer provided on the carrier, and the roughened copper foil provided on the peeling layer with the roughened surface as the outer side. Of course, in addition to using the roughened copper foil of the present invention, the copper foil with a carrier can adopt a known layer structure.

[0084] The carrier is a support for supporting the roughened copper foil to improve its operability, and a typical carrier includes a metal layer. Examples of such carriers include aluminum foil, copper foil, stainless steel (SUS) foil, resin films with metal coatings on the surface with copper, etc., glass, etc., preferably copper foil. The copper foil can be any one of a rolled copper foil and an electrolytic copper foil, preferably an electrolytic copper foil. The thickness of the carrier is typically less than 250 μm, preferably more than 9 μm and less than 200 μm.

[0085] The peeling layer is a layer that has the function of weakening the peeling strength of the carrier, ensuring the stability of the strength, and further inhibiting the mutual diffusion that may occur between the carrier and the copper foil during press forming at high temperature. The peeling layer is usually formed on one side of the carrier, and can also be formed on both sides. The peeling layer can be any of an organic peeling layer and an inorganic peeling layer. Examples of organic components used in the organic peeling layer include nitrogen-containing organic compounds, sulfur-containing organic compounds, carboxylic acids, etc. Examples of nitrogen-containing organic compounds include triazole compounds, imidazole compounds, etc. Among them, triazole compounds are preferred from the perspective of easy and stable peeling properties. Examples of triazole compounds include 1,2,3-benzotriazole, carboxybenzotriazole, N',N'-bis(benzotriazolylmethyl)urea, 1H-1,2,4-triazole and 3-amino-1H-1,2,4-triazole, etc. Examples of sulfur-containing organic compounds include mercaptobenzothiazole, trithiocyanate, 2-benzimidazolethiol, etc. As examples of carboxylic acids, monocarboxylic acids, dicarboxylic acids, etc. can be cited. On the other hand, as examples of inorganic components used in the inorganic peeling layer, Ni, Mo, Co, Cr, Fe, Ti, W, P, Zn, chromate treatment films, etc. can be cited. It should be noted that the formation of the peeling layer can be carried out by bringing a solution containing peeling layer components into contact with at least one surface of the carrier, fixing the peeling layer components on the surface of the carrier, etc. When the carrier is brought into contact with a solution containing peeling layer components, the contact can be carried out by immersing the carrier in a solution containing peeling layer components, spraying the solution containing peeling layer components, flowing down the solution containing peeling layer components, etc. In addition, a method of forming a film of the peeling layer components by a vapor phase method such as evaporation and sputtering can also be used. In addition, the fixing of the peeling layer components to the surface of the carrier can be carried out by adsorption, drying, and electrodeposition of the peeling layer components in the solution containing the peeling layer components. The thickness of the peeling layer is typically greater than 1 nm and less than 1 μm, preferably greater than 5 nm and less than 500 nm.

[0086] As required, other functional layers may also be provided between the peeling layer and the carrier and / or the roughened copper foil. As examples of such other functional layers, auxiliary metal layers may be cited. The auxiliary metal layer is preferably formed of nickel and / or cobalt. By forming such an auxiliary metal layer on the surface side of the carrier and / or the surface side of the roughened copper foil, it is possible to suppress the mutual diffusion that may occur between the carrier and the roughened copper foil during hot pressing at high temperatures or for a long time, and ensure the stability of the peel strength of the carrier. The thickness of the auxiliary metal layer is preferably 0.001 μm or more and 3 μm or less.

[0087] Copper Clad Laminated Board

[0088] The roughened copper foil of the present invention is preferably used for the production of copper-clad laminates for printed circuit boards. That is, according to a preferred embodiment of the present invention, a copper-clad laminate having the above-mentioned roughened copper foil is provided. By using the roughened copper foil of the present invention, high adhesion to a thermoplastic resin substrate and excellent high-frequency characteristics can be taken into account in the processing of the copper-clad laminate. The copper-clad laminate comprises the roughened copper foil of the present invention and a resin layer that is closely arranged with the roughened surface of the roughened copper foil. The roughened copper foil can be arranged on one side of the resin layer or on both sides. The resin layer contains a resin, preferably an insulating resin. The resin layer is preferably a prepreg and / or a resin sheet. Prepreg refers to a general term for composite materials impregnated with synthetic resins in substrates such as synthetic resin plates, glass plates, glass woven fabrics, glass nonwoven fabrics, and paper. In addition, from the viewpoint of improving insulation, the resin layer may contain filler particles formed by various inorganic particles such as silica and alumina. The thickness of the resin layer is not particularly limited, but is preferably 1 μm or more and 1000 μm or less, more preferably 2 μm or more and 400 μm or less, and further preferably 3 μm or more and 200 μm or less. The resin layer may be composed of multiple layers. The resin layer such as a prepreg and / or a resin sheet may be provided on the roughened copper foil by a primer resin layer pre-coated on the surface of the copper foil.

[0089] From the viewpoint of providing a copper-clad laminate suitable for high-frequency applications, the resin layer preferably comprises a thermoplastic resin, and more preferably, most (e.g., 50% by weight or more) or most (e.g., 80% by weight or more or 90% by weight or more) of the resin components contained in the resin layer are thermoplastic resins. Preferred examples of thermoplastic resins include polysulfone (PSF), polyethersulfone (PES), amorphous polyarylate (PAR), liquid crystal polymer (LCP), polyetheretherketone (PEEK), thermoplastic polyimide (PI), polyamideimide (PAI), fluororesin, polyamide (PA), nylon, polyacetal (POM), modified polyphenylene ether (m-PPE), polyethylene terephthalate (PET), glass fiber reinforced polyethylene terephthalate (GF-PET), cycloolefin (COP), and any combination thereof. From the viewpoint of the dielectric loss tangent of expectation and excellent heat resistance, as the more preferred example of thermoplastic resin, polysulfone (PSF), polyethersulfone (PES), amorphous polyarylate (PAR), liquid crystal polymer (LCP), polyetheretherketone (PEEK), thermoplastic polyimide (PI), polyamideimide (PAI), fluororesin and their arbitrary combination can be listed. From the viewpoint of low dielectric constant, particularly preferred thermoplastic resin is liquid crystal polymer (LCP) and / or fluororesin. As the preferred example of fluororesin, polytetrafluoroethylene (PTFE), tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), tetrafluoroethylene-ethylene copolymer (ETFE) and their arbitrary combination can be listed. It should be noted that the insulating resin substrate is preferably carried out by pressing while heating to the pasting of the roughening copper foil, so that the thermoplastic resin can be softened and enter the fine concavoconvex of the roughening surface. As a result, the adhesion between the copper foil and the resin can be ensured by the anchor effect produced by the fine irregularities (particularly the longitudinal roughened particles) sinking into the resin.

[0090] Printed Circuit Board

[0091] The roughened copper foil of the present invention is preferably used for the production of printed circuit boards. That is, according to a preferred embodiment of the present invention, a printed circuit board having the above-mentioned roughened copper foil is provided. By using the roughened copper foil of the present invention, excellent high-frequency characteristics and high circuit adhesion can be taken into account in the manufacture of printed circuit boards. The printed circuit board of this embodiment comprises a layer structure stacked with a resin layer and a copper layer. The copper layer is a layer derived from the roughened copper foil of the present invention. In addition, regarding the resin layer, as described with respect to the copper-clad laminate. In short, in addition to using the roughened copper foil of the present invention, the printed circuit board can adopt a known layer structure. As a specific example related to the printed circuit board, there can be listed: a single-sided or double-sided printed circuit board in which a circuit is formed after the roughened copper foil of the present invention is bonded to one or both sides of the prepreg, and a single-sided or double-sided printed circuit board in which a circuit is formed after curing and forming a laminate, and a multilayer printed circuit board formed by multilayering them, etc. In addition, as other specific examples, flexible printed circuit boards, COFs, TAB tapes, etc. in which the roughened copper foil of the present invention is formed on a resin film to form a circuit can also be listed. Furthermore, as other specific examples, there can be listed: a build-up circuit board in which a circuit is formed by forming a resin-coated copper foil (RCC) coated with the above-mentioned resin layer on the roughened copper foil of the present invention, laminating the resin layer as an insulating adhesive material layer on the above-mentioned printed circuit board, and then using the roughened copper foil as all or part of the wiring layer by a modified semi-additive process (MSAP), a subtractive process, etc.; a build-up circuit board in which the roughened copper foil is removed and a circuit is formed by a semi-additive process (SAP); a direct build-up wafer in which the lamination of the resin-coated copper foil and the formation of the circuit are repeated alternately on a semiconductor integrated circuit, etc. As more developed specific examples, there can also be listed an antenna element in which the above-mentioned resin-coated copper foil is laminated on a substrate to form a circuit, an electronic material for a panel display in which a pattern is formed by laminating a glass or a resin film with an adhesive layer, an electronic material for window glass, and an electromagnetic wave shielding film formed by coating a conductive adhesive on the roughened copper foil of the present invention, etc. In particular, the printed wiring board having the roughened copper foil of the present invention is suitable as a high-frequency substrate used in applications such as automotive antennas, mobile phone base station antennas, high-performance servers, and collision avoidance radars used in high-frequency bands with signal frequencies of 10 GHz or more.

[0092] Example

[0093] The present invention is further specifically described by the following examples.

[0094] Examples 1 to 11

[0095] The roughened copper foil of the present invention is produced as follows.

[0096] (1) Preparation of electrolytic copper foil

[0097] As the copper electrolyte, a sulfuric acid copper sulfate solution of the composition shown below was used, a titanium electrode with a surface roughness Ra of 0.20 μm was used as the cathode, and a DSA (dimensional stability anode) was used as the anode. The solution temperature was 45° C. and the current density was 55 A / dm 2 Electrolysis was performed to obtain an electrolytic copper foil having a thickness of 18 μm.

[0098] <Composition of sulfuric acid-acid copper sulfate solution>

[0099] -Copper concentration: 80g / L

[0100] - Sulfuric acid concentration: 260g / L

[0101] - Bis(3-sulfopropyl) disulfide concentration: 30mg / L

[0102] -Diallyldimethylammonium chloride polymer concentration: 50mg / L

[0103] -Chlorine concentration: 40mg / L

[0104] (2) Roughening treatment

[0105] The deposited surface of the obtained electrolytic copper foil was subjected to a roughening treatment. The roughening treatment was as shown in Table 1. Examples 1 to 6 and 8 to 11 were subjected to a two-stage roughening treatment (a first roughening treatment and a second roughening treatment), and Example 7 was subjected to a one-stage roughening treatment (a first roughening treatment). At this time, various samples having different characteristics of the roughened surface were prepared by appropriately changing the composition of the acidic copper sulfate solution and the electrodeposition conditions as shown in Table 1.

[0106] Specifically, the conditions of the roughening treatment in each stage are as follows.

[0107] -In the first roughening treatment, electroplating was performed using an acidic copper sulfate solution containing sulfuric acid, copper sulfate and, if necessary, sodium tungstate as an inorganic additive (Examples 1 to 6, 8 and 9) in such a manner that the Cu concentration, sulfuric acid concentration and W concentration are as shown in Table 1, under the electrodeposition conditions (liquid temperature, current density and amount) shown in Table 1.

[0108] In the second roughening treatment, electroplating was performed using an acidic copper sulfate solution containing sulfuric acid and copper sulfate so as to achieve the Cu concentration and sulfuric acid concentration shown in Table 1 under the electrodeposition conditions (liquid temperature, current density, and amount of electricity) shown in Table 1.

[0109] (3) Anti-rust treatment

[0110] The roughened surface of the electrolytic copper foil was subjected to rust-proof treatment including zinc-nickel alloy plating and chromate treatment. First, a solution containing 1 g / L zinc, 2 g / L nickel and 80 g / L potassium pyrophosphate was used at a temperature of 40°C and a current density of 0.5 A / dm 2 Then, an aqueous solution containing 1 g / L of chromic acid was used at pH 12 and a current density of 1 A / dm 2 Under the conditions of , the surface treated with zinc-nickel alloy was chromated.

[0111] (4) Silane coupling agent treatment

[0112] The silane coupling agent treatment was performed by adsorbing an aqueous solution of 6 g / L of 3-aminopropyltrimethoxysilane on the roughened surface of the electrolytic copper foil and evaporating the water with an electric heater. At this time, the surface of the electrolytic copper foil that had not been roughened was not treated with a silane coupling agent.

[0113] [Table 1]

[0114]

[0115] evaluate

[0116] The roughened copper foils prepared in Examples 1 to 11 were subjected to the following various evaluations.

[0117] <Surface properties parameters of roughened surface>

[0118] The roughened surface of the roughened copper foil was measured by surface roughness analysis using a laser microscope in accordance with JIS B0681-2:2018 (Ssk, Sku and Smr1) or EUR15178N (Sds). The specific measurement conditions are shown in Table 2. The surface profile of the obtained roughened surface was analyzed according to the conditions shown in Table 2 to calculate Ssk, Sku and Smr1. For each example, the above parameters were calculated in 10 different fields of view, and the average value in all fields of view was used as the surface property parameter of the roughened surface in the sample. The results are shown in Table 3.

[0119] [Table 2]

[0120] Table 2

[0121]

[0122] On the other hand, the calculation of Sds is performed as follows. First, the measurement data obtained using the above-mentioned laser microscope is read in using analysis software (manufactured by Olympus Corporation, "OLS5100 LEXT (version 2.1.2.215)"), and the unprocessed data is directly converted into a LEXT file format for output. The LEXT file is read in using another analysis software (manufactured by Digital Surf, "MountainsMap (version 9.0.9878)") and analyzed (analysis area: 64.397μm×64.463μm). Specifically, from the analysis object label, select "Parameter table" and "Default settings" in order to display the parameter analysis screen. In the parameter analysis screen, "EUR15178N" is selected as the standard, "First order surface" is selected as the wavelength processing, "Least squares surface" is selected as the F calculation (F operation) for shape removal, and "Sds" and "Sa" are selected as parameters. On the other hand, in this screen, the S filter and the L filter are not selected (that is, there is no cutoff based on the S filter and the L filter). Then, select "Export Analysis Results" and save the analysis results, and read the peak density Sds and the arithmetic mean height Sa from the analysis results. For each example, the calculation of the above parameters is implemented in 10 different fields of view. In order to remove noise, the total of 2 fields of view, 1 field of view with the maximum value of the arithmetic mean height Sa and 1 field of view with the minimum value of the arithmetic mean height Sa in the 10 fields of view, are excluded, and the average value of the Sds in the remaining 8 fields of view is used as the Sds of the roughened surface in the sample. The results are shown in Table 3.

[0123] <Root diameter of roughened particles>

[0124] The root diameter of the roughened particles used in the three-dimensional analysis of the slice image described later is calculated as follows. First, as a resin film, a prepreg (R-5670NF, 45 μm thick × 2 sheets, manufactured by Panasonic Corporation) is prepared. The roughened copper foil obtained is laminated in a manner that its roughened surface is in contact with the resin film, and a vacuum press is used to press under the conditions of a pressing pressure of 3.0 MPa, a temperature of 190 ° C, and a pressing time of 90 minutes to make a copper-clad laminate. For the copper-clad laminate, the roughened copper foil is removed using a cupric chloride etching solution. In this way, a resin film (hereinafter referred to as a "resin replica") having a surface having a surface shape of a roughened surface transferred thereto is obtained. Then, using a Schottky field emission scanning electron microscope (FE-SEM, manufactured by JEOL Ltd., JSM-7900F), observation was performed from a direction perpendicular to the transfer surface of the above-mentioned resin replica (Tilt: 0°) under the conditions of an acceleration voltage of 5.0 kV and an observation magnification of 30,000 times to obtain a resin replica image (image size: 1280 pixels × 1024 pixels).

[0125] The obtained resin replica image was analyzed as follows using image analysis software (NIRECO CORPORATION, "LUZEX (Version 1.60.8.2)"). In this image analysis, a region of 1260 pixels x 940 pixels (=10.25 μm) from which the photographing information region was removed was removed from the obtained resin replica image. 2 ) is taken as the analysis object. First, the resin replica image is binarized under the condition of a threshold value of 125. For reference, the binarized resin replica image obtained in Example 3 is shown in Figure 5 .like Figure 5 As shown, in the binarized resin replica image, the area indicated by black is regarded as the root portion R of the transferred roughened particles. Next, the binarized resin replica image is subjected to the filtering processes (1) to (5) described below in order.

[0126] (1) Snowball filter DILATE intensity 2

[0127] (2) Logical filter SHRINK strength 1

[0128] (3) Logic filter FILLHOLES

[0129] (4) Logical filter THIN strength 1

[0130] (5) Logical filter CIRCLE strength 3

[0131] In the filtered resin replica image, the portion of the root portion R of the roughened particles with an equivalent circle diameter less than 0.05 μm is removed as noise. The above operation is performed with three different fields of view to produce a box plot of the equivalent circle diameters of the root portion R of all roughened particles observed after removing the above noise. In the box plot, the maximum value (end of the line) after removing the outliers is taken as the root diameter of the roughened particles. It should be noted that when the first quartile is set to Q1, the third quartile is set to Q3, and the interquartile range (=Q3-Q1) is set to IQR, the outliers in the box plot are defined as values ​​greater than Q3+1.5×IQR or less than Q1-1.5×IQR.

[0132] <Obtaining Slice Images>

[0133] Using a FIB-SEM device (Carl Zeiss, Crossbeam 540, SEM and FIB simultaneous control: Atlas Engine v5.5.3), slice images were obtained under the following measurement conditions. The slice images were obtained as follows: Figure 6As shown, the x-axis and z-axis are set as the in-plane directions of the roughened copper foil 10, and the y-axis is set as the thickness direction of the roughened copper foil 10. On this basis, a cross-sectional image of the roughened copper foil 10 of a slice plane S parallel to the xy plane is obtained, and the slice plane is moved parallel to the z-axis direction by 10 nm each time, and a cross-sectional image is obtained at the same time, thereby obtaining the slice image. The observation area is set to x:y:z=19.5μm:19.5μm:9.5μm.

[0134] (FIB processing conditions)

[0135] -Accelerating voltage: 30kV

[0136] - Slice thickness: 10nm (interval between slice planes S)

[0137] (SEM observation conditions)

[0138] -Accelerating voltage: 1.0kV

[0139] -Working distance:5mm

[0140] -Tilt: 54° (with Tilt correction of SEM image)

[0141] -Pixel size: 5nm×5nm

[0142] -Detector: INLENSE detector

[0143] In addition, in the three-dimensional image analysis described later, from the viewpoint of facilitating the alignment for reconstructing the slice image into a three-dimensional image, the roughened copper foil 10 is subjected to the following treatment before the slice image is obtained. For reference, an example of a slice image of the roughened copper foil of Example 9 subjected to the treatment is shown in FIG. Figure 7. First, a thermosetting resin 14 (EPOXY (G-2), manufactured by Gatan, Inc.) is applied to the roughened surface of the roughened copper foil 10 to completely bury the roughened particles 12 (coating thickness: 2.0 μm or more and 4.5 μm or less). The thermosetting resin 14 is cured by vacuum heating the roughened copper foil 10 coated with the resin at 120°C for 20 minutes, and then cooled to room temperature. The cooled roughened copper foil 10 is placed in the above-mentioned FIB-SEM device, and a platinum film 16 (thickness 1.0 μm or more and 1.5 μm or less) for marking is formed on the surface of the cured thermosetting resin 14 using the deposition function of the FIB. Then, using the etching function of the FIB, the surface (xz plane) of the platinum film 16 is processed along the z-axis direction to form a mark M, so that marks of the same shape (three wedge shapes) can be visually identified in each slice image. At this time, the processing depth in the y-axis direction is set to be less than two-thirds of the thickness of the formed platinum film 16. Then, in order to protect the formed mark M, a carbon film 18 (thickness of about 1 μm) is formed on the surface of the platinum film 16 using the deposition function of the FIB. Hereinafter, the platinum film 16 and the carbon film 18 are collectively referred to as "protective film 20".

[0144] <Three-dimensional analysis of slice images>

[0145] The slice image data of the roughened copper foil obtained by FIB-SEM was three-dimensionally analyzed using the three-dimensional image processing software "Dragonfly (version 2022.1.0.1259)" (manufactured by Object Research System) to calculate the number of micrometers per 1 μm. 2 The volume of the roughened particles. At this time, the analysis area is x:z = 4.5 μm:4.5 μm, and y is arbitrary (depending on the size of the roughened particles). In addition, the number of analysis fields is set to 1. The three-dimensional analysis is described in detail below, and the following steps (1) to (6) are performed in sequence.

[0146] (1) Slice image reading and alignment

[0147] (2) Trimming of sliced ​​images

[0148] (3) Creation of segmentation model based on machine learning

[0149] (4) Extraction of Cu from Roughened Copper Foil

[0150] (5) Extraction of roughened particles

[0151] (6) Trimming of the analysis area and calculation of the volume of the roughened particles

[0152] (1) Slice image reading and alignment

[0153] The slice image data of the roughened copper foil obtained by FIB-SEM was read into the above-mentioned three-dimensional image processing software. At this time, "X:Y:Z=0.005:0.005:0.01" was input as the voxel size in "Image Spacing (in μm)".

[0154] In order to perform alignment for three-dimensional reconstruction, "Slice Registration" is selected on the read image data. Then, "Template Matching" is selected in "Registration method" to include only the portion of the protective film 20 where the mark M is formed ( Figure 7 Specify the template range by selecting "Apply" and automatically aligning. After checking all images, manually align only the parts that are significantly offset. Manual alignment is performed as follows: After changing the above-mentioned "Registration method" to "Manual", move the next slice image indicated in red toward the indicated slice image data to perform manual alignment.

[0155] (2) Trimming of sliced ​​images

[0156] In order to shorten the processing time, the protective film 20 portion that is not necessary for calculating the volume of the roughened particle 12 is removed by trimming. This trimming is performed as follows: After selecting "Crop..." of "Modify and Transform", the frames of the XY section and YZ section represented in the three-dimensional reconstructed image are moved so as to exclude the protective film 20 portion from the range, thereby trimming. Select the "Create new" checkbox, select "Apply" and "Close" in sequence, and the unnecessary portion is deleted.

[0157] (3) Creation of segmentation model based on machine learning

[0158] In order to extract the Cu portion derived from the roughened copper foil described below, a segmentation model based on machine learning was prepared as follows. As described below, the segmentation model based on machine learning can be prepared only for representative samples among the samples to be analyzed.

[0159] (3-1) Material allocation

[0160] Select "Segmentation Wizard" and "Continue" on the trimmed image data in sequence to enlarge the sliced ​​image in a manner that represents a portion of the roughened copper foil 10, roughened particles 12, and other parts (thermosetting resin 14, etc.). Select the above-mentioned enlarged image from "Add new frame" as the object area for machine learning. In "Classes and labels", enter "Cu" as the name of the area made of copper (roughened copper foil 10 and roughened particles 12), and enter "Resin" as the name of the area made of materials other than copper (such as resin). It should be noted that in order to easily distinguish between the various areas, the colors of the "Cu" area and the "Resin" area are specified as different colors (such as pink and green).

[0161] (3-2) Machine Learning

[0162] The regions of each material are subjected to machine learning as follows. For reference, Figure 8 An example of the display screen after material assignment is shown in FIG. First, select "Round Brush" from "2D view tools". At this time, set "Brush type" to "Full". In order to make the software recognize the "Resin" area, mark it with ○ so that it does not deviate from the thermosetting resin 14 ( Figure 8 Next, in order to allow the software to recognize the "Cu" area, the roughened copper foil 10 or the roughened particles 12 are marked with a circle ( Figure 8 "10a" in the figure) roughly specifies the range. It should be noted that in this process, as long as the range is specified in a way that does not deviate from the area of ​​​​each material, the thickness of the "Brush" (the size of the ○ mark) will not affect the machine learning. Then, select "Train" to start machine learning. In the "Model Generation Strategy" represented, select "High Accuracy". Select "Random Forest", "U-net" and "Sensor3D" from the three segmentation models for image processing. Select "Continue" to generate the first inference image. It should be noted that in the initial inference image generation, "U-net" and "Sensor 3D" are skipped.

[0163] (3-3) Creation of teacher images

[0164] Select the inferred images of "Cu" and "Resin" generated in "Random Forest". For reference, an example of the initial inferred image is shown in Fig. 9. Compare the inferred image with the original slice image, and for the parts where the offset occurs in the "Cu" area and the "Resin" area, enlarge the part until 1 pixel can be confirmed. Then, make a teacher image by manually correcting the area. The correction method is the same as the range specification method for the "Cu" and "Resin" areas mentioned above, but this time the correction is accurately performed in units of 1 pixel. After that, select "Train" and perform machine learning again using the three segmentation models "Random Forest", "U-net" and "Sensor 3D".

[0165] (3-4) Creation of segmentation model

[0166] Confirm the "Score" of the "Models" tab, and select the inferred image with the highest "Score" among "Random Forest", "U-net", and "Sensor3D". Compare the inferred image with the original slice image, and for the parts where the offset occurs in the "Cu" area and the "Resin" area, enlarge the part until 1 pixel can be confirmed. Then, generate a new teacher image by manually correcting the area again. Then, move to other slice images, enlarge the slice image in a manner that represents a part of the roughened copper foil 10, roughened particles 12, and other parts (thermosetting resin 14, etc.), and select the above-mentioned enlarged image from "Add newframe" as the object area for machine learning. Then, select "Predict" to generate an inferred image reflecting the results of the above-mentioned new teacher image. By repeating the above operations until the "Score" of the inferred image becomes greater than 0.98, a segmentation model is created. This time, the following is used. Fig. 10A The roughened bottom surface B of the roughened copper foil 10 and the roughened particles 12 are continuous (connected) as shown in FIG. Fig. 10B As shown in the figure, the roughened bottom surface B of the roughened copper foil 10 and the roughened particles 12 are discontinuous (not connected) to create a segmentation model. Then, as the final inference image, that is, the segmentation model, the model with the highest "Score" among "U-net" and "Sensor 3D" is used.

[0167] (4) Extraction of Cu from Roughened Copper Foil

[0168] The extraction of the "Cu" area originating from the roughened copper foil 10 and the roughened particles 12 is performed as follows. Select the prepared segmentation model and the slice image data reflecting the segmentation model. Select "Preview" to confirm whether the generated image properly identifies the "Cu" area and the "Resin" area. Then, select "All Slices" from "Segment" to apply the segmentation model to all slice image data. It should be noted that when the segmentation model is appropriate, the "Cu" area and the "Resin" area are colored with designated heterogeneous colors (such as pink and green). When the segmentation model is inappropriate, a segmentation model is again prepared for the image data of the sample in the same way as above (3). This time, segmentation models were prepared for Examples 1, 5, 7, and 11.

[0169] Confirm the three-dimensional reconstructed image. If there is a part in the "Resin" area that is mistakenly identified as "Cu", manually identify it as the "Resin" area. The identification method of this area is the same as the range specification method of the "Cu" area and the "Resin" area in (3-1) above, but this time it is identified in units of 1 pixel. Then, select "Resin" from "Classes and labels" in "2D view tools" and delete "Resin" by "Remove". In "Data Properties and Settings", select "New ROI" on the image with "Resin" deleted to generate an "ROI" that only extracts the "Cu" part. Here, "ROI" refers to the "region of interest in the image" to which filtering or recognition processing is applied. In the case where there are holes (uncolored parts) in "Cu", it is impossible to accurately extract the roughened particles 12, so select the generated "ROI", select "Apply" in "Fill inner areas: 3D" in "ROI tools", and fill the holes.

[0170] (5) Extraction of roughened particles

[0171] Select the "ROI" that fills the voids in "Cu". Select "Invert" from "ROI Tools" in the "Segment" tab to invert the measurement object from the "Cu" part to the space part, thereby generating an "ROI" for "Air" (the space part other than "Cu" other than "Resin"). Select "Fill Connected Pores with a Diameter Smaller Than..." in "Refine Region of Interest" on the generated "ROI" of "Air". In the window shown, input the root diameter of the above-mentioned roughened particles 12 as the threshold value, and separate the roughened bottom surface B of the roughened copper foil 10 from the roughened particles 12. In this way, an "ROI" of the roughened particles 12 including "Air" is generated. It should be noted that when the above-mentioned threshold value is too large, the roughened particles 12 are cut in a state including the roughened bottom surface B of the roughened copper foil 10, which is inappropriate. On the other hand, when the threshold value is too small, the cut portion enters the interior of the roughened particles 12, which is inappropriate. Therefore, as described above, the maximum value excluding outliers in the box plot is used as the root diameter of the roughened particle 12. In order to fill the voids of the generated "ROI" including the roughened particle 12 of "Air", "Apply" of "Fillinner areas: 3D" is selected.

[0172] Only the roughened particles 12 are extracted from the roughened particles 12 containing "Air" as follows. "Erode" of "Morphological operations" is selected from "ROI Tools" in the "Segment" tab to finely adjust the segmentation of the roughened particles 12 and the roughened bottom surface B. At this time, the conditions are as follows.

[0173] (Slicing conditions)

[0174] -Dimensionality:2D(Z)

[0175] -Shape:Square

[0176] -Range: Not entered

[0177] -Kernel size:3

[0178] It should be noted that the “2D (Z)” in the above condition means that the selected “ROI” is processed along the z-axis.

[0179] After the above segmentation, in order to fill the hole of one pixel, select "Apply" of "Fill inner areas: 3D". Repeat the above segmentation operation and hole filling operation, and perform fine adjustment of the roughened particles 12 and the roughened bottom surface B twice in total. This fine adjustment is always performed twice in total for each case. Select the "ROI" generated after this adjustment as "(A)", select the "ROI" of "Air" as "(B)", and then select "AB", thereby making an "ROI" in which only the roughened particles 12 are extracted.

[0180] (6) Trimming of the analysis area and calculation of the volume of the roughened particles

[0181] In the "ROI" where only the roughened particles 12 are extracted, select "Crop..." in "Modify and Transform". Then, enter values ​​for "Min" and "Max" with "Size" of "X" as 900 (= 4.5μm) and "Size" of "Z" as 450 (= 4.5μm) to determine the analysis area (X:Z = 4.5μm: 4.5μm). At this time, set "Min" and "Max" so that the analysis area does not include the ends. After selecting the "Create new" checkbox, select "Apply" to trim the analysis area. Then, read the value (μm) represented by "Volume (Labeled voxels)" in "Statistical properties". 3 ) is taken as the total volume V of the roughened particles. The total volume V of the roughened particles is divided by the area A of the analysis region (=20.25 μm 2 )(=V / A), from which the value per 1μm is calculated 2 The results are shown in Table 3.

[0182] <Peel Strength for Thermoplastic Resins (Liquid Crystal Polymers)>

[0183] As a thermoplastic resin substrate, a liquid crystal polymer (LCP) film (Kuraray Co., Ltd., VECSTARCT-Q, thickness 50μm×1 sheet) was prepared. The roughened copper foil obtained was laminated on the thermoplastic resin substrate in a manner that its roughened surface was in contact with the resin substrate, and a vacuum press was used to press under the conditions of a pressing pressure of 4MPa, a temperature of 330°C, and a pressing time of 10 minutes to produce a copper-clad laminate. For the copper-clad laminate, a copper chloride etching solution was used to form a circuit using a subtractive method to produce a test substrate with a 3mm wide straight line circuit. For the produced test substrate, a desktop precision universal testing machine (manufactured by Shimadzu Corporation, AGS-50NX) was used to peel the formed straight line circuit from the thermoplastic resin substrate according to the A method (90° peeling) of JIS C5016-1994, and the normal peel strength (kgf / cm) was measured. The peel strength was judged to be qualified when it was 0.60kgf / cm or more. The results are shown in Table 3.

[0184] <Evaluation of transmission characteristics>

[0185] As an insulating resin substrate, a high-frequency substrate (manufactured by Panasonic Corporation, MEGTRON6N, thickness 45μm×2 sheets) was prepared. The roughened copper foil obtained was laminated on both sides of the insulating resin substrate in such a manner that its roughened surface was in contact with the insulating resin substrate, and a vacuum press was used to press it under the conditions of a pressing pressure of 3MPa, a temperature of 190°C, and a pressing time of 90 minutes to obtain a copper-clad laminate. Then, a copper chloride etching solution was used to form a circuit based on the subtractive method on the copper-clad laminate (circuit height: 18μm, circuit width 300μm, circuit length: 300mm). In this way, a transmission loss measurement substrate with a microstrip line formed in such a manner that the characteristic impedance becomes 50Ω±2Ω was obtained. For the obtained transmission loss measurement substrate, a network analyzer (manufactured by Keysight Technology, N5225B) was used to measure the transmission loss L1 (dB) at 50GHz under the following setting conditions. Then, the increase rate of the transmission loss L1 relative to the transmission loss L0 (dB) at 50 GHz of Example 7 (Comparative Example) was calculated (= L1 / L0). The transmission loss increase rate was determined to be acceptable when it was 1.10 or less. The results are shown in Table 3.

[0186] (Setting conditions)

[0187] -IF Bandwidth:100Hz

[0188] -Frequency:10MHz~50GHz

[0189] -Data points:501point

[0190] -Average:Off

[0191] -Calibration method: SOLT (e-cal) [Table 3]

[0192]

Claims

1. A roughened copper foil having a roughened surface on at least one side, The peak density Sds of the roughened surface is 1.57 μm -2 Above and 2.64μm -2 the following, The roughened surface has a plurality of roughened particles, each 1 μm 2 The volume of the roughening particles is 0.11 μm 3 Above and 0.25μm 3 the following, The Sds is a value measured according to EUR15178N without performing cutoff by the S filter and the L filter. Each 1 μm 2 The volume of the roughened grains is a value calculated by obtaining an image of the roughened surface using FIB-SEM and performing three-dimensional analysis on the image.

2. The roughened copper foil according to claim 1, wherein: The skewness Ssk of the roughened surface is greater than 0.35, The Ssk is a value measured in accordance with JIS B0681-2:2018 under the conditions that no cutoff by an S filter is performed and the cutoff wavelength by an L filter is 1.0 μm.

3. The roughened copper foil according to claim 1 or 2, wherein: The kurtosis Sku of the roughened surface is greater than or equal to 2.70 and less than or equal to 4.90, The Sku is a value measured in accordance with JIS B0681-2:2018 under the condition where cutoff by the S filter and the L filter is not performed.

4. The roughened copper foil according to claim 1 or 2, wherein: The load area ratio Smr1 of the separation protruding peak portion and the center portion of the roughened surface is 11.2% or more, The Smr1 is a value measured in accordance with JIS B0681-2:2018 under the conditions that no cutoff by an S filter is performed and the cutoff wavelength by an L filter is 1.0 μm.

5. The roughened copper foil according to claim 1 or 2, wherein: The roughened surface is further provided with a rust-proofing layer and / or a silane coupling agent layer. 6 . A copper foil with a carrier, comprising: a carrier, a release layer provided on the carrier, and the roughened copper foil according to claim 1 or 2 provided on the release layer with the roughened surface facing the outside. 7 . A copper-clad laminate comprising the roughened copper foil according to claim 1 .

8. A printed wiring board comprising the roughened copper foil according to claim 1 or 2.

Citation Information

Patent Citations

  • Blackened surface-treated copper foil, method for manufacturing blackened surface-treated copper foil, copper-clad laminate and flexible printed circuit board

    WO2014133164A1

  • Roughened copper foil and printed wiring board

    WO2016174998A1