Fuel transport pipe
By adopting a laminated structure of inner layer, intermediate layer and reinforcement layer in the fuel delivery pipe, and using thermoplastic resin and vulcanized rubber with high load deflection temperature, the dissolution of sulfur to the conveyor and interlayer peeling problems are solved, and the pipe is improved Durability and stability.
Patent Information
- Application Number
- CN202280094099.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-31
- Filing Date
- 2022-12-16
- Publication Date
- 2024-11-08
AI Technical Summary
During use, existing fuel conveying pipes are prone to dissolution of sulfur to the conveying substance and interlayer peeling problems, which affects its service life and performance.
The inner layer, the intermediate layer, the reinforcement layer and the outer layer are sequentially stacked, wherein the inner layer contains the first thermoplastic resin with a load deflection temperature of 75°C or above and the second thermoplastic resin with a load deflection temperature of less than 75°C, and the middle The layer contains vulcanized rubber, and the inner layer is bonded to the intermediate layer through an adhesive layer, and the thickness ratio and adhesion of the inner layer to the intermediate layer are controlled to inhibit sulfur dissolution and interlayer peeling.
It effectively inhibits the dissolution of sulfur and interlayer peeling, improves the durability and stability of fuel delivery pipes, and ensures performance under different temperatures and deformation conditions.
Smart Images

Figure CN118922663A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a pipe for transporting fuels, and more particularly to a pipe for transporting fuels such as gasoline, light oil, kerosene, and liquefied petroleum gas. Background Art
[0002] Pipes used for conveying fuel etc. can have a layer of vulcanized rubber on the inside.
[0003] Patent Document 1 discloses a low gas permeability tube comprising an inner layer, a reinforcement layer and an outer layer, wherein the inner layer has an innermost water-resistant layer formed of vulcanized rubber and a gas barrier layer formed on the outer side of the water-resistant layer.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2004-176908 Summary of the invention
[0007] Problems to be solved by the invention
[0008] An object of the present invention is to provide a fuel transport tube which can suppress the elution of sulfur into a transported object and suppress interlayer delamination of the tube.
[0009] Means for solving problems
[0010] The present inventors have discovered that the above-mentioned subject can be accomplished by the following means:
[0011] Plan 1
[0012] A fuel transportation pipe is a fuel transportation pipe comprising an inner layer, an intermediate layer, a reinforcement layer and an outer layer stacked in sequence.
[0013] The inner layer contains a thermoplastic resin composition, wherein the thermoplastic resin composition contains a first thermoplastic resin having a deflection temperature under load of 75° C. or higher and a second thermoplastic resin having a deflection temperature under load of less than 75° C.,
[0014] The intermediate layer contains a rubber composition, and the rubber composition contains nitrile rubber.
[0015] The inner layer and the intermediate layer are bonded directly or via an adhesive layer.
[0016] Plan 2
[0017] In the fuel transporting pipe according to claim 1, a mass ratio of the first thermoplastic resin to a total of the first thermoplastic resin and the second thermoplastic resin is 0.05 to 0.95.
[0018] Plan 3
[0019] In the fuel transporting pipe according to claim 1 or 2, the first thermoplastic resin has an aromatic ring in its main chain.
[0020] Plan 4
[0021] According to the fuel transport pipe according to embodiment 3, the aromatic ring has 6 to 10 carbon atoms.
[0022] Plan 5
[0023] In the fuel transporting pipe according to any one of aspects 1 to 4, the first thermoplastic resin is an aromatic polyamide resin.
[0024] Plan 6
[0025] In the fuel transporting pipe according to any one of aspects 1 to 5, the second thermoplastic resin is an aliphatic polyamide.
[0026] Plan 7
[0027] According to any one of aspects 1 to 6, the fuel transport pipe has a free sulfur content of 1.0% by mass or less relative to the inner layer, or contains no free sulfur content.
[0028] Plan 8
[0029] According to any one of aspects 1 to 7 of the fuel transport pipe, a ratio of the thickness of the inner layer to the thickness of the intermediate layer is 0.01 to 2.00.
[0030] Plan 9
[0031] The fuel transport pipe according to any one of claims 1 to 8, wherein the swelling degree of the inner layer after immersion in a fuel at a temperature of 23° C. for 7 days is 35.0% or less.
[0032] The fuel contains 42.5% by volume of isooctane, 42.5% by volume of toluene, and 15% by volume of ethanol based on the entire fuel.
[0033] Plan 10
[0034] The fuel transport pipe according to any one of claims 1 to 9, wherein the fuel permeability of the inner layer after immersion in a fuel at a temperature of 23° C. for 7 days is 5.00 mg·mm / 24h·cm 2 the following,
[0035] The fuel contains 42.5% by volume of isooctane, 42.5% by volume of toluene, and 15% by volume of ethanol based on the entire fuel.
[0036] Plan 11
[0037] In the fuel transport pipe according to any one of aspects 1 to 10, the storage elastic modulus E of the inner layer at -30°C is 1,500 to 3,500 MPa.
[0038] Plan 12
[0039] The fuel transport pipe according to any one of aspects 1 to 11, wherein the inner layer further contains rubber and / or an elastomer.
[0040] Plan 13
[0041] According to the fuel transport pipe according to claim 12, the elastomer is a polyester elastomer, a polyamide elastomer, or a modified styrene elastomer.
[0042] Plan 14
[0043] According to the fuel transport pipe according to the twelfth or thirteenth aspect, the inner layer has a sea-island structure of the thermoplastic resin composition and the rubber and / or elastomer.
[0044] Plan 15
[0045] According to any one of aspects 1 to 14, the fuel transporting pipe, wherein the nitrile rubber contained in the intermediate layer contains 25 to 50% by mass of acrylonitrile based on the nitrile rubber.
[0046] Effects of the Invention
[0047] According to the present invention, it is possible to provide a fuel transport tube which can suppress the elution of sulfur into a transported object and suppress delamination of the tube. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] Figure 1 It is a schematic diagram which viewed the fuel delivery pipe 10 according to the first embodiment of the present invention from the side.
[0049] Figure 2 It is a schematic diagram showing a cross section of the fuel transport pipe 10 according to the first embodiment of the present invention. DETAILED DESCRIPTION
[0050] Hereinafter, embodiments of the present disclosure will be described in detail. It should be noted that the present disclosure is not limited to the following embodiments, and various modifications can be made within the scope of the disclosed gist.
[0051] The fuel transportation pipe of the present invention is a fuel transportation pipe in which an inner layer, an intermediate layer, a reinforcing layer and an outer layer are laminated in this order, the inner layer contains a thermoplastic resin composition, the above-mentioned thermoplastic resin composition contains a first thermoplastic resin with a load deflection temperature of 75°C or more, and a second thermoplastic resin with a load deflection temperature of less than 75°C, the intermediate layer contains a rubber composition, the above-mentioned rubber composition contains vulcanized rubber, and the inner layer and the intermediate layer are bonded directly or via an adhesive layer.
[0052] Here, the inner layer, the intermediate layer, the reinforcing layer, and the outer layer are laminated in this order, which means that these layers are laminated in this order from the inside to the outside of the fuel transporting pipe.
[0053] Generally speaking, as the inner layer of the fuel transport pipe, a layer containing a vulcanized rubber composition is used. When such a fuel transport pipe is used to transport a transported object such as fuel, a part of the sulfur or sulfur compound added to the rubber composition is sometimes dissolved in the transported object. From the viewpoint of suppressing the dissolution of such sulfur components, it can be considered to configure an inner layer containing a thermoplastic resin composition as a barrier layer on the innermost side of the fuel transport pipe. It can be considered that the bonding of the inner layer and the layer containing the rubber composition, i.e., the intermediate layer, is carried out by utilizing the heat during vulcanization to soften or flow the thermoplastic resin composition and the rubber composition, thereby contacting and entanglement between the two at the interface, and the bonding strength is improved, but depending on the composition of the thermoplastic resin composition, it may not be easy to soften or flow, and the adhesion becomes insufficient. In such a fuel transport pipe with insufficient adhesion, if repeated or large deformation is given, interlayer peeling occurs between the inner layer and the intermediate layer. In addition, depending on the composition of the thermoplastic resin composition, it may soften or flow significantly during vulcanization, and the thickness of the inner layer becomes uneven due to the flow and deformation of the rubber composition.
[0054] Although not limited by the principle, it is considered that when the deflection temperature under load of the thermoplastic resin composition is high, if the tube is repeatedly or greatly deformed after vulcanization, peeling is likely to occur between the inner layer and the intermediate layer. On the other hand, it is considered that when the deflection temperature under load of the thermoplastic resin composition is low, when the rubber composition is vulcanized, the inner layer deforms following the deformation of the intermediate layer, and the thickness of the inner layer tends to become non-uniform.
[0055] The fuel transport pipe of the present invention has an inner layer containing a thermoplastic resin composition containing a first thermoplastic resin having a deflection temperature under load of 75° C. or higher and a second thermoplastic resin having a deflection temperature under load of less than 75° C., so that even if the rubber composition is vulcanized, the thickness of the inner layer is unlikely to change, and the adhesion between the inner layer and the intermediate layer is also excellent.
[0056] Figure 1 and 2Schematic diagram of a fuel delivery pipe 10 according to a first embodiment of the present invention. Figure 1 FIG. 1 is a diagram showing a fuel transport pipe 10 according to a first embodiment of the present invention as viewed from the side. Figure 2 1 is a cross-sectional view in the radial direction of the fuel delivery pipe 10 according to the first embodiment of the present invention. Figure 1 and 2 None of them is intended to limit the present invention.
[0057] like Figure 1 and 2 As shown in the figure, the fuel transporting pipe 10 according to the first embodiment of the present invention is a fuel transporting pipe 10 in which an inner layer 11, an intermediate layer 12, a reinforcing layer 13 and an outer layer 14 are sequentially stacked. Here, the so-called sequential stacking means that each layer is sequentially stacked from the inside of the fuel transporting pipe 10, that is, the pipe interior 15 toward the outside of the fuel transporting pipe 10.
[0058] The inner layer 11 contains a thermoplastic resin composition containing a first thermoplastic resin having a deflection temperature under load of 75° C. or higher and a second thermoplastic resin having a deflection temperature under load of less than 75° C. The middle layer 12 contains a rubber composition containing vulcanized rubber. The inner layer 11 and the middle layer 12 are bonded directly or via an adhesive layer (not shown).
[0059] Inner Layer
[0060] The inner layer contains a thermoplastic resin composition and optionally contains other ingredients such as a softening ingredient.
[0061] In the fuel transport pipe, the inner layer containing the thermoplastic resin composition is arranged on the inner diameter side of the intermediate layer containing the vulcanized rubber composition, thereby suppressing the elution of sulfur components from the intermediate layer into the transported object such as fuel.
[0062] The inner layer preferably contains a free sulfur component of 1.0% by mass or less relative to the inner layer, or contains no free sulfur component.
[0063] The reason is that the less free sulfur components are contained in the inner layer, the more the elution of sulfur components into the transported material such as fuel can be suppressed. Therefore, it is more preferable that the free sulfur components are contained in the inner layer as little as possible.
[0064] The inner layer may contain a small amount of free sulfur due to migration of sulfur or sulfur compounds from the adjacent intermediate layer or adhesive layer, and may contain free sulfur in an amount of preferably 1.0 mass % or less, more preferably 0.5 mass % or less, and further preferably 0.2 mass % or less.
[0065] Here, the so-called free sulfur component refers to sulfur or sulfur compounds that can be extracted from the inner layer by the fuel. The content of the free sulfur component contained in the inner layer can be obtained by sealing the test fuel inside the tube cut into a specified length, and after standing for more than 48 hours in an atmosphere of 23°C, the sulfur component contained in the test fuel is quantified. The sulfur component in the test fuel can be detected by oxidative decomposition coulometric titration using a commercially available sulfur analyzer in accordance with JIS K2541-2 Crude Oil and Petroleum Products-Sulfur Content Test Method Part 2 Microcoulometric Titration Acidification Method (Crude Oil and Petroleum Products-Sulfur Test Method Part 2 Microcoulometric Titration Oxidation Method). It should be noted that the so-called test fuel here is a fuel containing 42.5% by volume of isooctane, 42.5% by volume of toluene, and 15% by volume of ethanol relative to the whole.
[0066] The ratio of the thickness of the inner layer to the thickness of the intermediate layer is preferably 0.01 to 2.00.
[0067] When the ratio of the thickness of the inner layer to the thickness of the intermediate layer is within such a range, it is possible to achieve both variation in the thickness of the inner layer accompanying the flow of the rubber composition of the intermediate layer during vulcanization and adhesion to the intermediate layer.
[0068] The ratio of the thickness of the inner layer to the thickness of the intermediate layer may be 0.01 to 2.00, 0.10 to 1.80, or 0.50 to 1.40.
[0069] The inner layer preferably has a swelling degree of 35.0% or less after being immersed in a fuel at a temperature of 23° C. for 7 days.
[0070] When the swelling degree of the inner layer is smaller than the above value, deformation of the inner layer when the fuel is transported through the fuel transport pipe can be further suppressed.
[0071] The swelling degree may be 35.0 to 0.0%, 30.0 to 1.0%, or 15.0 to 2.0%.
[0072] In addition, the inner layer preferably has a fuel permeability of 5.00 mg·mm / 24h·cm after being immersed in a fuel at a temperature of 23°C for 7 days. 2 the following.
[0073] When the fuel permeability of the inner layer is less than the above value, it is beneficial to the transportation of the fuel.
[0074] The above fuel permeability can be 5.00 to 0.01 mg·mm / 24h·cm 2 4.50~0.02mg·mm / 24h·cm 2 、3.50~0.10mg·mm / 24h·cm 2 , or 2.50~0.50mg·mm / 24h·cm2 .
[0075] It should be noted that the fuel used for the measurement of the swelling degree and the fuel permeability in the present invention is a fuel containing 42.5 volume % of isooctane, 42.5 volume % of toluene, and 15 volume % of ethanol relative to the entire fuel. It should be noted that the fuel that can be transported by the fuel transport pipe of the present invention is not limited to the above-mentioned composition.
[0076] The storage elastic modulus E of the inner layer at -30°C is preferably 1,500 to 3,500 MPa.
[0077] When the storage elastic modulus E' at -30°C is within the above range, it is advantageous to use the fuel transport pipe in a low temperature environment.
[0078] The storage elastic modulus E′ may be 1,500 to 3,500 MPa, 1,700 to 3,200 MPa, 2,000 to 3,000 MPa, or 2,200 to 2,500 MPa.
[0079] <Thermoplastic resin composition>
[0080] The thermoplastic resin composition contains a first thermoplastic resin having a deflection temperature under load of 75°C or higher and a second thermoplastic resin having a deflection temperature under load of less than 75°C.
[0081] The mass ratio of the first thermoplastic resin to the total of the first thermoplastic resin and the second thermoplastic resin is preferably 0.05 to 0.95.
[0082] When the mass ratio of the first thermoplastic resin to the total of the first thermoplastic resin and the second thermoplastic resin is within such a range, both the variation in thickness of the inner layer accompanying the flow of the rubber composition of the intermediate layer during vulcanization and the adhesion to the intermediate layer can be achieved.
[0083] The mass ratio of the first thermoplastic resin to the total of the first thermoplastic resin and the second thermoplastic resin may be 0.05 to 0.95, 0.10 to 0.90, 0.20 to 0.80, 0.30 to 0.70, or 0.40 to 0.60.
[0084] (First thermoplastic resin)
[0085] The first thermoplastic resin is a thermoplastic resin having a deflection temperature under load of 75° C. or higher.
[0086] Here, the load deflection temperature can be measured by fixing the two ends in the longitudinal direction of a test piece (vertical width 80 mm, horizontal width 10 mm, and thickness 4 mm) produced using an injection molding machine (Centriel Novel Products Co., Ltd.) in accordance with JIS K 7191 "Plastics - Test method for deflection temperature under load (Plastics - Test method for deflection temperature under load)", applying a load of 1.8 MPa to the center, and raising the temperature at 2°C / min.
[0087] The deflection temperature under load of the first thermoplastic resin may be 75 to 150°C, 80 to 140°C, or 90 to 130°C.
[0088] The first thermoplastic resin preferably has an aromatic ring in the main chain. If the thermoplastic resin composition contains a thermoplastic resin having a deflection temperature under load of 75°C or higher and an aromatic ring in the main chain, swelling of the inner layer and changes in physical properties are unlikely to occur when in contact with fuel.
[0089] The aromatic ring preferably has 6 to 10 carbon atoms. That is, the aromatic ring may be, for example, a 6-membered ring, an 8-membered ring, or a 10-membered ring.
[0090] The first thermoplastic resin is preferably an aromatic polyamide resin.
[0091] Examples of thermoplastic resins having a deflection temperature under load of 75° C. or higher include, but are not limited to, nylon MXD6 (MXD6), nylon 6T (Ny6T), nylon 6I (Ny6I), nylon 9T (Ny9T), polybutylene naphthalate (PBN), or polyphenylene sulfide (PPS).
[0092] (Second thermoplastic resin)
[0093] The second thermoplastic resin is a thermoplastic resin having a deflection temperature under load of less than 75°C.
[0094] Here, the deflection temperature under load of the second thermoplastic resin can be measured by the same method as the measurement of the deflection temperature under load of the first thermoplastic resin.
[0095] The deflection temperature under load of the second thermoplastic resin may be 10°C or more and less than 75°C, 15 to 70°C, 30 to 65°C, or 40 to 60°C.
[0096] The second thermoplastic resin is preferably an aliphatic polyamide. When the thermoplastic resin composition contains an aliphatic polyamide having a deflection temperature under load of less than 75°C, the composition will not be excessively rigid and the occurrence of cracks in the inner layer due to deformation and repeated fatigue can be suppressed.
[0097] Examples of thermoplastic resins having a deflection temperature under load of less than 75° C. include, but are not limited to, nylon 6 (Ny6), nylon 6.66 (Ny6.66), nylon 6.10 (Ny6.10), nylon 6.12 (Ny6.12), nylon 10.10 (Ny10.10), nylon 11 (Ny11), nylon 12 (Ny12), nylon 66 (Ny66), polybutylene terephthalate (PBT), and ethylene vinyl alcohol copolymer (EVOH). In addition, the thermoplastic resin having a deflection temperature under load of less than 75° C. may be a copolymer of these resins.
[0098] 〈Softening ingredients〉
[0099] The inner layer preferably further contains rubber and / or an elastomer as a soft component.
[0100] Examples of the rubber include, but are not limited to, butyl rubber, EPDM rubber, nitrile rubber, hydrogenated nitrile rubber, acrylic rubber, fluororubber, epichlorohydrin rubber, epoxidized natural rubber, and mixtures thereof. The rubber may be vulcanized.
[0101] As the elastomer, for example, polyester elastomer, polyamide elastomer, polystyrene elastomer, polyolefin elastomer, polyurethane elastomer, or vinyl chloride elastomer and their modified products can be cited, but it is not limited to these. In addition, from the viewpoints of not easily swelling with respect to fuels and affinity with thermoplastic resins, polyester elastomer, polyamide elastomer, and polystyrene elastomer are particularly preferred.
[0102] When the inner layer contains rubber and / or elastomer, the inner layer may have a sea-island structure of the thermoplastic resin composition and the rubber and / or elastomer.
[0103] Middle Layer
[0104] The intermediate layer contains a rubber composition, and the rubber composition contains vulcanized rubber.
[0105] The vulcanized rubber may be a vulcanized rubber such as nitrile rubber (NBR), a nitrile rubber (NBR) / polyvinyl chloride (PVC) blend, chlorosulfonated polyethylene (CSM), butyl rubber (IIR), or a mixture thereof.
[0106] From the viewpoint of oil resistance, the nitrile rubber may contain 25 to 50% by mass of acrylonitrile relative to the entire nitrile rubber. The nitrile rubber may contain 25 to 50% by mass, 30 to 45% by mass, or 35 to 40% by mass of acrylonitrile relative to the entire nitrile rubber.
[0107] The rubber composition may further contain additives such as a crosslinking agent, an antioxidant, a plasticizer, a processing aid, a crosslinking accelerator, a crosslinking accelerator, a reinforcing agent (filler), a scorch retardant, a peptizer, an organic modifier, a softener, and a tackifier.
[0108] Adhesive layer
[0109] The adhesive layer is a layer containing an arbitrary material capable of adhering the inner layer and the intermediate layer.
[0110] Examples of the adhesive layer include phenolic resin adhesives, urethane resin adhesives, epoxy resin adhesives, resorcinol resin adhesives, urea resin adhesives, melamine resin adhesives, and modified silicone adhesives.
[0111] Enhancement Layer
[0112] The reinforcement layer may have, for example, at least one organic fiber layer or a metal wire layer.
[0113] The arrangement relationship between the organic fiber layer and the metal wire layer in the reinforcement layer is not particularly limited, but it is preferred that the organic fiber layer is arranged on the inner layer side and the metal wire layer is arranged on the outer layer side, and in particular, the metal wire layer is arranged on the outermost layer side of the reinforcement layer. Thus, the expansion and contraction of the inner layer of the fuel delivery pipe during use can be cushioned by the organic fiber layer on the inner layer side of the reinforcement layer, while high durability can be ensured by the metal wire layer on the outer layer side of the reinforcement layer.
[0114] 〈Organic fiber layer〉
[0115] The organic fiber layer may contain a poly(p-phenylene benzobis(2-hydroxyethyl)benzene) selected from Fibers of at least one of azoles, polyesters, polyamides, and polyketones.
[0116] Furthermore, the organic fiber layer can be a layer woven from threads formed by organic fibers. The organic fiber layer has a braid structure or a spiral structure, preferably a braid structure. The braid structure is a structure with higher elasticity than the spiral structure. Therefore, when the organic fiber layer is a braid structure, it is more flexible and has excellent operability.
[0117] 〈Metal Wire Layer〉
[0118] The metal wire layer may be a layer woven from metal wires such as steel wires, copper and copper alloy wires, aluminum and aluminum alloy wires, magnesium alloy wires, titanium and titanium alloy wires, etc. The metal wire layer is particularly preferably a layer woven from steel wires. Examples of the steel wires include stainless steel wires and zinc-plated steel wires.
[0119] The metal wire layer may be a layer having a braid structure or a spiral structure, preferably a braid structure. The braid structure is a woven form with higher elasticity than the spiral structure. Therefore, when the metal wire layer is a braid structure, it has a certain elasticity and thus maintains operability while having high durability.
[0120] Outer Layer
[0121] The outer layer is typically formed from a rubber composition, a thermoplastic elastomer, or a thermoplastic elastomer composition.
[0122] The rubber composition is not limited and includes rubbers such as nitrile rubber (NBR), nitrile rubber (NBR) / polyvinyl chloride (PVC) blends, chlorosulfonated polyethylene (CSM), butyl rubber (IIR), etc., to which crosslinking agents, antioxidants, plasticizers, processing aids, crosslinking accelerators, crosslinking accelerators, reinforcing agents (fillers), scorch retardants, plasticizers, organic modifiers, softeners, tackifiers and other additives are added.
[0123] Examples of the thermoplastic elastomer include olefin-based thermoplastic elastomers, styrene-based thermoplastic elastomers, polyamide elastomers, polyester elastomers, and polyurethane elastomers.
[0124] Examples of the thermoplastic elastomer composition include those composed of a matrix comprising a thermoplastic resin such as a polyamide resin, a polyester resin, an ethylene-vinyl alcohol resin, a polyolefin resin, a polyketone resin, a polyacetal resin, a polyphenylene sulfide resin, a polyphenylene ether resin, a fluorine-based resin, and a structural domain comprising a rubber such as butyl rubber, modified butyl rubber, an olefin-based thermoplastic elastomer, a styrene-based thermoplastic elastomer, an ethylene-unsaturated carboxylic acid ester copolymer, a polyamide elastomer, a polyester elastomer, and a polyurethane elastomer.
[0125] The thickness of the outer layer is preferably 0.2 to 5.0 mm, more preferably 0.2 to 4.0 mm, and even more preferably 0.2 to 3.0 mm.
[0126] Example
[0127] 《Examples 1 to 22 and Comparative Examples 1 to 4》
[0128] 〈Tube Production〉
[0129] On a core rod, the first thermoplastic resin, the second thermoplastic resin, and the elastomer, which were dry-blended in the mixing ratio (mass %) shown in Tables 1-1 and 1-2, were extruded using an extruder in a manner to have the thickness (thickness of the inner layer) described in Tables 4-1 and 4-2 to form an inner layer.
[0130] Next, the rubber composition prepared at the compounding ratio (parts by mass) shown in Table 2 was extruded using a Banbury mixer to the outer side of the inner layer so as to have the thickness (thickness of the intermediate layer) shown in Tables 4-1 and 4-2, thereby forming an intermediate layer.
[0131] A phenolic resin adhesive was applied to the outer side of the intermediate layer, and steel wires were braided using a braiding machine to form a reinforcement layer.
[0132] On the outside of the reinforcing layer, a rubber composition prepared at the compounding ratio (parts by mass) shown in Table 3 was extruded using a Banbury mixer to have a thickness of 2.0 mm to form an outer layer.
[0133] Then, steam vulcanization was performed at 143° C. for 60 minutes, and the mandrel was withdrawn to produce a tube having an inner diameter of 22.5±0.5 mm and an outer diameter of 31.7±0.5 mm.
[0134] <Determination of deflection temperature under load>
[0135] The deflection temperature under load of the first thermoplastic resin and the second thermoplastic resin used in each example was measured in accordance with JIS K7191 “Plastics - Test method for deflection temperature under load”. Test pieces (vertical width 80 mm×lateral width 10 mm×thickness 4 mm) of these resins were produced using an injection molding machine (Centriel Novel Products Co., Ltd.). Both ends of the test pieces were fixed, and a load of 1.8 MPa was applied to the center portion, and the temperature was raised at 2°C / min.
[0136] <Measurement of swelling degree, fuel permeability, and storage elastic modulus of the inner layer>
[0137] (Preparation of sample)
[0138] The first thermoplastic resin, the second thermoplastic resin, and the elastomer were used at the blending ratio (mass %) shown in Tables 1-1 and 1-2, and a Φ40 mm single-screw extruder (Protec Co., Ltd.) with a T-die of 550 mm width was used to produce a sheet having the same composition as the inner layer. The temperature of the barrel and the die was set to 240 to 265° C., and the temperature of the cooling roll and the pulling speed were set to arbitrary conditions to obtain a sheet having an average thickness of 0.15 to 0.20 mm.
[0139] (Determination of swelling degree of inner layer)
[0140] The obtained sheet was cut into a size of 1.2 cm in vertical width × 3.0 cm in horizontal width, and the specific gravity was calculated using an automatic densimeter in accordance with JIS K 6258-2016 "Volume change measurement (volume change measurement)". The measured sample was immersed in a test fuel (isooctane / toluene / ethanol = 42.5 / 42.5 / 15 volume %) for 7 days, and the specific gravity of the sample after immersion was calculated by the same procedure, and the swelling degree was calculated from the change before and after immersion.
[0141] (Measurement of fuel permeability)
[0142] In an aluminum cup used in JIS Z0208 "Moisture-proof packaging material's permeation humidity test method (Moisture-proof packaging material's permeation humidity test method)", 20 mL of the test fuel (isooctane / toluene / ethanol = 42.5 / 42.5 / 15 volume %) was sealed, and the obtained sheet was cut out so that the permeation surface became a circle with a diameter of 60 mm, and then installed. The sheet was left to stand at 23°C with the sheet facing downward so that the sheet and the test fuel were always in contact, and the weight of the cup was measured every day. The fuel permeability was calculated from the weight loss until 7 days later.
[0143] (Determination of storage elastic modulus)
[0144] The obtained sheet was cut into a size of 0.5 cm in vertical width×10.0 cm in horizontal width, and the viscoelasticity at -30°C was measured with a dynamic strain of ±0.1%, a frequency of 20 Hz, and a static strain of 2%.
[0145] <Evaluation of vulcanization resistance>
[0146] The tube of each example produced was cut at right angles to the longitudinal direction of the tube, and the thickness of the inner layer was measured at 30 points on the circumference using an optical microscope to determine the coefficient of variation (CV value). The same measurement was performed at 5 points in the longitudinal direction of a tube of 10 m in length to determine the deviation, and when the CV value of Comparative Example 2 was expressed as an index of 100, less than 80 was considered "excellent", 80 or more and less than 90 was considered "good", 90 or more and less than 98 was considered "acceptable", and 98 or more was considered "unacceptable", and the resistance to the change in the circumferential thickness due to vulcanization was evaluated.
[0147] <Evaluation of Adhesion Between Inner Layer and Intermediate Layer>
[0148] The tube of each example was cut into a predetermined length to prepare a ring-shaped test piece, and the end of the peeled test piece was fixed to the jig of the tester so that the peeling angle was about 90°, and the peeling force between the inner layer and the middle layer was measured. When the peeling force in the tube of Comparative Example 1 was expressed as an index with 100, 130 or more was regarded as "excellent", 100 or more and less than 130 was regarded as "good", 80 or more and less than 100 was regarded as "acceptable", and less than 80 was regarded as "unacceptable".
[0149] <result>
[0150] The composition of the inner layer is shown in Table 1-1 and Table 1-2, the composition of the intermediate layer is shown in Table 2, and the composition of the outer layer is shown in Table 3. In addition, the configuration and test results of the tube of each example are shown in Table 4-1 and Table 4-2. It should be noted that "Ny6.66" in Table 1-1 and Table 1-2 refers to a copolymer of nylon 6 and nylon 66. Other "Ny6.12", "Ny6.10" and the like are also copolymers of two types of nylon.
[0151] [Table 1-1]
[0152]
[0153] [Table 1-2]
[0154] [Table 2]
[0155] Table 2
[0156] The composition of the middle layer Mass NBR 10 0.0 Carbon Black 10 0.0 sulfur 1.5 Vulcanization accelerator 1.0 Antioxidant 1.0 Zinc Oxide 5.0 Stearic acid 2.0 Plasticizers 6.0 total 216.5
[0157] [Table 3]
[0158] Table 3
[0159] Composition of the outer layer Mass NBR 10 0.0 Carbon Black 90.0 sulfur 1.5 Vulcanization accelerator 1.0 Antioxidant 1.0 Zinc Oxide 5.0 Stearic acid 2.0 Plasticizers 6.0 total 206.5
[0160] [Table 4-1]
[0161]
[0162] [Table 4-2]
[0163]
[0164] As shown in Tables 4-1 and 4-2, the pipes of Examples 1 to 22 have both vulcanization resistance and adhesion between the inner layer and the intermediate layer. On the other hand, in Comparative Examples 1 to 4, both vulcanization resistance and adhesion between the inner layer and the intermediate layer are not achieved.
[0165] Explanation of symbols
[0166] 10 Fuel delivery pipe
[0167] 11 Inner layer
[0168] 12 Middle Layer
[0169] 13 Enhancement Layer
[0170] 14 Outer layer
[0171] 15 Tube interior.
Claims
1. A fuel transportation pipe, which is a fuel transportation pipe having an inner layer, an intermediate layer, a reinforcement layer and an outer layer laminated in sequence. The inner layer contains a thermoplastic resin composition, wherein the thermoplastic resin composition contains a first thermoplastic resin having a deflection temperature under load of 75° C. or higher and a second thermoplastic resin having a deflection temperature under load of less than 75° C., The intermediate layer contains a rubber composition, and the rubber composition contains vulcanized rubber. The inner layer and the middle layer LB are bonded directly or via an adhesive layer. 2 . The fuel transporting pipe according to claim 1 , wherein a ratio of the mass of the first thermoplastic resin to the total mass of the first thermoplastic resin and the second thermoplastic resin is 0.05 to 0.
95. 3 . The fuel transport pipe according to claim 1 , wherein the first thermoplastic resin has an aromatic ring in its main chain. 4 . The fuel transport pipe according to claim 3 , wherein the aromatic ring has 6 to 10 carbon atoms. 5 . The fuel transporting pipe according to claim 1 , wherein the first thermoplastic resin is an aromatic polyamide resin. 6 . The fuel transporting pipe according to claim 1 , wherein the second thermoplastic resin is an aliphatic polyamide. 7 . The fuel transport pipe according to claim 1 , wherein the free sulfur content of the inner layer is 1.0% by mass or less relative to the inner layer, or the inner layer contains no free sulfur content. 8 . The fuel transport pipe according to claim 1 , wherein a ratio of a thickness of the inner layer to a thickness of the intermediate layer is 0.01 to 2.
00.
9. The fuel transport pipe according to any one of claims 1 to 8, wherein the swelling degree of the inner layer after immersion in a fuel at a temperature of 23°C for 7 days is 35.0% or less. The fuel contains 42.5% by volume of isooctane, 42.5% by volume of toluene, and 15% by volume of ethanol, based on the entire fuel.
10. The fuel transport pipe according to any one of claims 1 to 9, wherein the fuel permeability of the inner layer after immersion in a fuel at a temperature of 23°C for 7 days is 5.00 mg·mm / 24h·cm 2 the following, The fuel contains 42.5% by volume of isooctane, 42.5% by volume of toluene, and 15% by volume of ethanol, based on the entire fuel. 11 . The fuel transport pipe according to claim 1 , wherein the storage elastic modulus E of the inner layer at -30° C. is 1,500 to 3,500 MPa. 12 . The fuel transport pipe according to claim 1 , wherein the inner layer further contains rubber and / or elastomer. 13 . The fuel transporting pipe according to claim 12 , wherein the elastomer is a polyester elastomer, a polyamide elastomer, or a modified styrene elastomer. 14 . The fuel transport pipe according to claim 12 , wherein the inner layer has a sea-island structure of the thermoplastic resin composition and the rubber and / or elastomer. 15 . The fuel transporting pipe according to claim 1 , wherein the vulcanized rubber is a vulcanized nitrile rubber, and the nitrile rubber contains 25 to 50% by mass of acrylonitrile based on the entire nitrile rubber.