Capacitor and manufacturing method thereof

By using specific electrode materials and diaphragm structures in capacitors, including fine pore size distribution and reduction reaction products of porous substrates, the problem of low energy density at high voltages is solved, and the improvement of high energy density and capacity is achieved.

CN118922902APending Publication Date: 2024-11-08PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380028991.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-29
Filing Date
2023-03-28
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The energy density of existing capacitors is still low at high voltages, and it is difficult for the diaphragm to achieve high energy density at high voltages, limiting its application range.

Method used

The first electrode containing the first active substance, the second electrode containing the second active substance, and the separator between the two is used. The electrolyte contains an ionic liquid, and the pore size of the separator has a volume of 0.1 μm to 2 μm. 0.4 cm3/g or above, or contains a porous substrate and an ionic liquid reduction reaction product bonded thereto, the energy density of the capacitor is increased by these structures.

Benefits of technology

The high energy density and capacity of capacitors at high voltages are achieved, which improves the application potential of capacitors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922902A_ABST
    Figure CN118922902A_ABST
Patent Text Reader

Abstract

The present invention pertains to a capacitor provided with a first electrode containing a first active material, a second electrode containing a second active material, a separator interposed between the first electrode and the second electrode, and an electrolyte solution containing an ionic liquid, and in the pore diameter distribution of the separator, the total volume Va in the range of pore diameters of 0.1 [mu] m to 2 [mu] m is 0.4 cm3 / g or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a capacitor and a method for manufacturing the same. Background Art

[0002] In recent years, capacitors with high energy density have been desired. Since the higher the operating voltage of a capacitor, the higher the energy density can be, the combination of electrolyte and electrode materials that can operate at high voltage has been explored.

[0003] Patent Document 1 proposes a graphene sheet film, characterized in that two or more graphene sheets are aggregated in parallel via carbon nanotubes, and the graphene sheet aggregates are electrically and mechanically connected to each other in a three-dimensional form via carbon nanotubes. The film was used for an electrode, and a capacity of 290.6 F / g was reported.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application No. 2012 / 073998 Summary of the invention

[0007] Problems to be solved by the invention

[0008] Although the capacitor described in Patent Document 1 has a higher output density than a lithium-ion battery, its energy density is still low and its applications are limited. In order to expand the applications of capacitors, it is required to further increase the energy density of capacitors.

[0009] The higher the operating voltage of a capacitor, the higher the energy density that can be obtained. Therefore, the combination of electrolyte and electrode materials that can operate at high voltage is being explored. However, in addition to electrolyte and electrode materials, it is also important to explore a separator that can achieve high energy density even at high voltage.

[0010] Means for solving problems

[0011] In view of the above, one embodiment of the present invention relates to a capacitor comprising: a first electrode containing a first active material, a second electrode containing a second active material, a separator between the first electrode and the second electrode, and an electrolyte, wherein the electrolyte contains an ionic liquid, and in the pore size distribution of the separator, the total volume Va of the pores in the range of 0.1 μm to 2 μm is 0.4 cm 3 / g or above.

[0012] In view of the above situation, another embodiment of the present invention relates to a capacitor, comprising: a first electrode containing a first active material, a second electrode containing a second active material, a separator between the first electrode and the second electrode, and an electrolyte, wherein the electrolyte contains an ionic liquid, and the separator contains a porous substrate and a reduction reaction product of the ionic liquid adhered to the porous substrate.

[0013] In view of the above situation, another embodiment of the present invention relates to a method for manufacturing a capacitor, which is a method for manufacturing a capacitor comprising a first electrode containing a first active material, a second electrode containing a second active material, a diaphragm between the first electrode and the second electrode, and an electrolyte, wherein the manufacturing method includes: a step of preparing a porous substrate and an ionic liquid, and a step of obtaining the diaphragm by bonding a reduction reaction product of the ionic liquid to the porous substrate.

[0014] Effects of the Invention

[0015] According to the present invention, a capacitor with high energy density can be realized.

[0016] The novel features of the present invention are described in the appended claims, but the present invention both in terms of configuration and content will be more clearly understood from the following detailed description taken in conjunction with other objects and features of the present invention with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 It is a partially cutaway perspective view of a capacitor according to the present invention.

[0018] Figure 2 It is a graph showing the charge and discharge efficiency of the capacitors of Examples 7 and 8 and Comparative Example 5. DETAILED DESCRIPTION

[0019] Hereinafter, the embodiments of the present disclosure will be described. In addition, in the following description, the embodiments of the present disclosure will be described as an example, but the present disclosure is not limited to the examples described below. In the following description, specific numerical values, materials, etc. are sometimes exemplified, but other numerical values, materials, etc. may also be applied as long as the effects of the present disclosure can be obtained. In this specification, the description of "numerical value A to numerical value B" includes numerical value A and numerical value B, which can be replaced by "numerical value A or more and numerical value B or less". In the following description, when the lower limit and upper limit of the numerical value related to specific physical properties and conditions are exemplified, as long as the lower limit is not above the upper limit, any one of the exemplified lower limits can be arbitrarily combined with any one of the exemplified upper limits. When multiple materials are exemplified, one of them can be selected and used alone, or two or more can be used in combination.

[0020] In addition, the present disclosure includes a combination of matters described in two or more claims arbitrarily selected from the plurality of claims recorded in the attached claims. In other words, matters described in two or more claims arbitrarily selected from the plurality of claims recorded in the attached claims can be combined as long as no technical contradiction occurs.

[0021] Hereinafter, the capacitor includes capacitors having various power storage mechanisms, and refers to power storage devices such as double-layer capacitors and lithium-ion capacitors that at least partially have power storage mechanisms. The power storage device or capacitor includes a pair of capacitor electrodes and an electrolyte. The electrodes contain an active material.

[0022] Active materials exhibit capacity, for example, by doping and dedoping ions. The so-called doping of ions into active materials includes concepts such as adsorption of ions into active materials, embedding of ions based on active materials, chemical interactions between active materials and ions, etc. In addition, the so-called dedoping of ions from active materials includes concepts such as desorption of ions from active materials, deintercalation of ions from active materials, and release of chemical interactions between active materials and ions. However, the so-called doping of ions into active materials mainly refers to the adsorption of ions into active materials, and the so-called dedoping of ions from active materials mainly refers to the desorption of ions from active materials. If the active material adsorbs ions, a double layer is formed and capacity is exhibited. In other words, electrodes for capacitors mainly refer to polarizing electrodes, but they can also be electrodes that have the properties of polarizing electrodes while Faraday reactions also contribute to capacity.

[0023] A capacitor according to one embodiment of the present disclosure comprises: a first electrode containing a first active material, a second electrode containing a second active material, a separator between the first electrode and the second electrode, and an electrolyte. One of the first electrode and the second electrode is a positive electrode of the capacitor, and the other is a negative electrode. The first electrode and the second electrode may also be the same electrode. The electrolyte contains an ionic liquid.

[0024] In the pore size distribution of the separator, the total volume Va of the pores in the range of 0.1 μm to 2 μm is 0.4 cm 3 / g or above.

[0025] Between the first electrode and the second electrode of the capacitor, a high voltage of, for example, 4.0 V or more may be applied. In this case, if a separator having a Va satisfying the above conditions is used, a capacitor having a high capacity and a high energy density can be realized.

[0026] About Va is 0.4cm 3 The reason why the capacitance of the capacitor is significantly increased when the capacitance is greater than 100 / g is currently under investigation, and it is considered to be as follows. However, the present invention is not limited to this.

[0027] The cations or anions contained in the ionic liquid are reduced or oxidized by applying a high voltage, and reaction products of reduction or oxidation reaction can be generated in the electrolyte. If these reaction products are present near the positive electrode or negative electrode, the formation of a double electric layer is sometimes hindered, which can be considered to be a reason for the reduction in capacity.

[0028] For example, the reaction product reacts with the components constituting the electrode layer (e.g., the functional groups of the active material and the side chains of the binder, etc.) to generate side reaction products. If the side reaction products are deposited near the positive electrode or the negative electrode and in the pores of the electrode layer, the active sites of the active material are reduced, or the movement (diffusion) of cations or anions is hindered, thereby sometimes hindering the formation of a double electric layer.

[0029] On the other hand, the diaphragm can adsorb the reaction products. The reaction products adsorbed by the diaphragm will not hinder the formation of the double electric layer in the positive and negative electrodes, and can maintain high capacity. However, if the pore size of the diaphragm is larger than 2μm, the reaction products can easily pass through the pores, and the effect of adsorbing the reaction products is low. In contrast, tiny pores with a pore size of less than 2μm can easily capture the reaction products in the pores, and the effect of adsorbing and fixing the reaction products is high. If Va is 0.4cm 3 / g or more, the separator has sufficient micropores with a pore diameter of 2 μm or less, and the reaction product is easily fixed. As a result, it is considered that when Va is 0.4 cm 3 / g or more, a significantly high capacity can be maintained.

[0030] In this case, in the pore size distribution of the separator, the total volume Vm of the pores in the range of 0.01 μm to 6 μm is more preferably 0.7 cm 3 / g or above.

[0031] Specifically, for example, when 1-ethyl-3-methylimidazolium tetrafluoroborate (EMIBF4) is used as the ionic liquid, when charged at a voltage of 4.0 V or more, the 1-ethyl-3-methylimidazolium cation (EMI + ) is reduced at the negative electrode, and EMI radicals can be generated through the reaction shown in the following reaction formula 1.

[0032] Reaction 1:

[0033] [Chemical formula 1]

[0034]

[0035] On the other hand, during discharge, the reverse reaction of chemical formula 1 is carried out, so that the EMI radical releases an electron and returns to the EMI +Reaction of cations (oxidation reaction). Therefore, in addition to the capacity exhibited by the adsorption of cations or anions, the capacitor also exhibits additional capacity through oxidation-reduction reactions, and as a result, it is believed that significantly higher capacity can be obtained.

[0036] EMI radicals can be converted into carbene by the reaction shown in the following reaction formula 2. In addition, dimers can be generated by the reaction shown in the following reaction formula 3. The reactions shown in reaction formulas 2 and 3 are equilibrium reactions. If the concentration of the ionic liquid (EMIBF4) contained in the electrolyte is low, it becomes difficult to carry out the reaction shown in reaction formula 3, and the reaction shown in reaction formula 2 mainly proceeds. On the other hand, if EMIBF4 is present in a high concentration in the electrolyte, it becomes easy to carry out the reaction shown in reaction formula 3. Furthermore, regarding EMI dimers, by subjecting the electrolyte to a reaction based on 1 The presence of EMI radicals and carbenes cannot be confirmed by NMR, but can be confirmed by ESR (electron spin resonance).

[0037] Reaction 2:

[0038] [Chemical formula 2]

[0039]

[0040] Reaction 3:

[0041] [Chemical formula 3]

[0042]

[0043] If the reaction product, i.e., carbene and dimer, is present near the positive electrode or the negative electrode, the reaction product hinders the formation of the double electric layer as described above, sometimes reducing the capacity. However, the separator has the function of adsorbing and fixing the reaction product, which can inhibit the reaction product from hindering the formation of the double electric layer, thereby inhibiting the decrease in capacity.

[0044] In addition, during discharge, the EMI free radicals are oxidized and returned to the EMI cations, which contributes to the capacity. On the other hand, if it is in the state of carbene and dimer, it does not directly contribute to the capacity. Therefore, the capacity of the capacitor is reduced accordingly to the extent of carbene and dimer generated by the reaction of EMI free radicals. However, in a capacitor according to an embodiment of the present disclosure, by making the carbene and dimer adhere to the diaphragm, the concentration of carbene and dimer near the negative electrode can be increased, and the balance of reaction formulas 2 and 3 can be moved to the left. Thus, the generation of carbene and dimer can be suppressed, so that most EMI free radicals are oxidized during discharge and can return to EMI cations, thereby being able to maintain a high capacity expressed by the redox reaction.

[0045] The pore volumes Va and Vm can be obtained by measuring the differential pore volume distribution or the logarithmic differential pore volume distribution of the diaphragm and integrating them in the range of pore diameters of 0.1 μm to 2 μm and 0.01 μm to 6 μm, respectively. In the measurement of the pore volume distribution, a mercury porosimeter based on the mercury intrusion method or a pore size distribution measuring instrument (permporometer) based on the bubble point method or the gas permeation method can be used.

[0046] The volume Va of the separator with a pore diameter of 0.1 μm to 2 μm may be 0.6 cm 3 / g or more. The volume Va can also be 1.0cm 3 / g or less, 0.8cm 3 / g or less or 0.7cm 3 / g or less.

[0047] The porosity of the separator is preferably 60% or more, more preferably 65% ​​or more, and further preferably 70% or more.

[0048] The porosity of the separator can be calculated by setting the mass per unit area of ​​the separator to W (g / cm 2 ), the true density of the material constituting the diaphragm is set to ρ (g / cm 3 ), the thickness of the diaphragm is set to t (cm), and the following formula is used to calculate it. The thickness t can be measured using a micrometer. Regarding the thickness measurement method, the thickness of each diaphragm is calculated from the thickness when 10 diaphragms are stacked and a fixed load is applied.

[0049] Porosity (%) = 100 - (W / (ρ×t)) × 100

[0050] The porosity of the separator can also be measured by, for example, a pure water porosimeter.

[0051] The density of the separator is, for example, 0.3 g / cm 3 Above and 0.8g / cm 3 Below, can also be 0.35g / cm 3 Above and 0.7g / cm 3 Here, the density of the separator refers to the bulk density, which can be obtained by the following formula.

[0052] (Density of diaphragm) = (Weight of diaphragm) / [(Area of ​​diaphragm) × (Thickness of diaphragm)]

[0053] As a material for the separator, it is preferred to contain cellulose or a derivative thereof. Cellulose is relatively stable to both acids and alkalis, and is stable even in an environment where a high voltage is applied. In addition, it has high tensile strength, and has sufficient strength even when the first electrode and the second electrode are wound to form a wound electrode group. As the form of the separator, for example, a microporous film, a woven fabric or a non-woven fabric can be used. The thickness of the separator is, for example, 8 to 50 μm, preferably 12 to 35 μm, and more preferably 14 to 35 μm or 16 to 35 μm.

[0054] In addition, another embodiment of the present disclosure relates to a capacitor comprising: a first electrode containing a first active material, a second electrode containing a second active material, a separator between the first electrode and the second electrode, and an electrolyte. Either the first electrode or the second electrode is a positive electrode of the capacitor, and the other is a negative electrode. The first electrode and the second electrode may also be the same electrode. The electrolyte contains an ionic liquid. The separator contains a porous substrate and a reduction reaction product of the ionic liquid bonded to the porous substrate.

[0055] Furthermore, in the above, the ionic liquid contained in the electrolyte of the capacitor and the ionic liquid before the reduction reaction product adhered to the diaphragm reacts may be the same or different. Hereinafter, the ionic liquid before the reduction reaction product reacts is sometimes referred to as the "first ionic liquid", and the ionic liquid contained in the electrolyte of the capacitor is referred to as the "second ionic liquid".

[0056] In addition, a method for manufacturing a capacitor involved in one embodiment of the present disclosure is a method for manufacturing a capacitor having a first electrode containing a first active material, a second electrode containing a second active material, a separator between the first electrode and the second electrode, and an electrolyte, which includes: a step of preparing a porous substrate and an ionic liquid, and a step of obtaining a separator by bonding a reduction reaction product of the ionic liquid to the porous substrate.

[0057] By adopting a diaphragm formed by bonding the reduction reaction product of the ionic liquid to a porous substrate, the capacity of the capacitor using the ionic liquid in the electrolyte can be increased. It can be considered that this is because: in addition to the capacity of the capacitor by the doping and dedoping of the ions constituting the ionic liquid into the active material, the additional capacity is also exhibited by the redox reaction of the ions constituting the ionic liquid. By bonding the reduction reaction product to the diaphragm in advance, the redox reaction is efficiently generated, thereby increasing the capacity. In addition, the charge and discharge efficiency is also improved.

[0058] Specifically, for example, when 1-ethyl-3-methylimidazolium tetrafluoroborate (EMIBF4) is used as the ionic liquid, when charging at a voltage of 4.0 V or more, the 1-ethyl-3-methylimidazolium cation (EMI +) is reduced at the negative electrode, and EMI radicals are generated through the reaction shown in the above reaction formula 1. On the other hand, during discharge, the reverse reaction to reaction formula 1 is performed, and the EMI radicals are returned to the EMI by releasing an electron. + Reaction of cations (oxidation reaction): EMI radicals can be converted into carbenes by the reaction shown in the above reaction formula 2. In addition, dimers can be generated by the reaction shown in the above reaction formula 3.

[0059] During discharge, the capacitor exhibits additional capacity by oxidizing the EMI radicals and returning to the EMI cations. However, if it is in the state of carbenes and dimers, it is difficult to release an electron and cannot directly contribute to the capacity. Therefore, if the number of carbenes and dimers generated by the reaction of EMI radicals increases, the capacity increase based on the redox reaction is correspondingly suppressed. In addition, part of the electricity provided during charging is consumed by the generation of reduction reaction products, so the charge and discharge efficiency is reduced.

[0060] In contrast, according to a capacitor and a method for manufacturing a capacitor involved in one embodiment of the present disclosure, by making most of the reduction reaction products (such as carbenes and dimers) adhere to the diaphragm, the concentration of the reduction reaction products near the negative electrode in the capacitor using the diaphragm is increased. As a result, the balance of reaction formula 2 and reaction formula 3 can be moved to the left, and the generation of reduction reaction products can be suppressed when the capacitor is charged. Therefore, during discharge, most EMI radicals are oxidized and can return to EMI cations, which can maintain the capacity expressed by the redox reaction at a high level, while improving the charge and discharge efficiency.

[0061] In addition, if the reduction reaction product exists near the positive electrode or the negative electrode, it hinders the formation of the double electric layer, sometimes reducing the capacity. However, by suppressing the generation of the reduction reaction product, the reduction reaction product can be suppressed from hindering the formation of the double electric layer, thereby suppressing the decrease in capacity.

[0062] In addition, by suppressing the generation of reduction reaction products, the concentration of reduction reaction products in the electrolyte can be suppressed even after repeated charge and discharge cycles, and the viscosity of the electrolyte can be suppressed. Thus, the capacity drop after repeated charge and discharge cycles can be suppressed.

[0063] The process of obtaining the diaphragm includes, for example, the process of placing a porous substrate impregnated with the first ionic liquid between a pair of electrodes to make a battery (cell), and the process of applying voltage to the battery to generate a reduction reaction product. Then, the porous substrate is taken out from the battery and cleaned to obtain a diaphragm in which the reduction reaction product and the porous substrate are bonded. The first ionic liquid can also be mixed with other liquids (solvents) and the obtained electrolyte is impregnated in the porous substrate. The voltage applied to the battery is above the voltage that produces the reduction reaction of the first ionic liquid, and although it depends on the first ionic liquid, it is, for example, above 4.0V. The application time is, for example, more than 5 hours. The voltage application cycle can also be repeated multiple times in a manner that the total voltage application time becomes more than 5 hours.

[0064] The composition of the battery used to bond the reduction reaction product to the porous substrate (composition, size, etc. of the electrodes and the electrolyte) may be the same as or different from the composition of the capacitor to be manufactured. For example, the active material used in the positive and negative electrodes of the battery may be the same as or different from the active material used in the positive and negative electrodes of the capacitor to be manufactured. The electrolyte used in the battery and the electrolyte used in the capacitor to be manufactured both contain ionic liquids, but the concentration of the ionic liquid in the electrolyte may be different. In addition, the first ionic liquid contained in the electrolyte used in the battery and the ionic liquid (second ionic liquid) contained in the electrolyte used in the capacitor to be manufactured may be different. As described above, as long as the reduction reaction products are the same, the first ionic liquid and the second ionic liquid may contain the same cations, and the anions constituting the ionic liquids may be different.

[0065] As a porous substrate, it is preferred to contain at least one selected from cellulose and its derivatives. Cellulose is relatively stable to both acids and alkalis, and is stable even in an environment where a high voltage is applied. In addition, it has high tensile strength and has sufficient strength even when it is wound together with the first electrode and the second electrode of the capacitor to form a wound electrode group. As the form of the porous substrate, for example, a microporous film, a woven fabric or a non-woven fabric can be used. The thickness of the porous substrate is, for example, 8 to 50 μm, preferably 12 to 35 μm, and more preferably 14 to 35 μm or 16 to 35 μm.

[0066] As a porous substrate, a porous substrate having a structure with more fine pores is preferred in that it is easy to make the reduction reaction product adhere to the pores. More specifically, a porous substrate with well-developed fine pores with a pore diameter of less than 2 μm is preferred. Pores with a pore diameter of 2 μm or more are difficult to adhere to the reduction reaction product because the reduction reaction product easily passes through the pores. In the pore diameter distribution of the porous substrate, the total volume Va of the pore diameter range of 0.1 μm to 2 μm can also be 0.4 cm3 In addition, the total volume Vm of the pore diameter in the range of 0.01 μm to 6 μm is preferably 0.7 cm 3 / g or more. Va is 0.4cm 3 / g or more of the porous substrate has a high effect of fixing the reduction reaction product, and it is easy to realize a capacitor with high energy density. Furthermore, the pore volumes Va and Vm can be obtained by measuring the differential pore volume distribution or the logarithmic differential pore volume distribution of the diaphragm, and integrating them in the range of pore diameters of 0.1μm to 2μm and 0.01μm to 6μm, respectively. In the measurement of the pore volume distribution, a mercury porosimeter based on the mercury intrusion method, or a pore size distribution measuring instrument based on the bubble point method or the gas permeation method can be used.

[0067] As the first ionic liquid, a salt compound that exists in a liquid state at normal temperature (25°C) and normal pressure (atmospheric pressure) can be preferably used. Examples of cations constituting the salt compound include imidazolium cations, pyrrolidinium cations, pyridinium cations, piperidinium cations, ammonium cations, and phosphonium cations. Examples of anions include halide ions (Cl - Br - etc.), tetrafluoroborate ion (BF4 - ), hexafluorophosphate ion (PF6 - ), bis(fluorosulfonyl)imide ion ((FSO2)2N - ), bis(trifluoromethylsulfonyl)imide ion ((CF3SO2)2N - )wait.

[0068] Among these cations, when cations having an aromatic heterocyclic ring are used, a capacitor having a very high capacity can be realized when a separator is used and a carbon material having a graphene layer is used as an active material. The reason for this is currently under investigation, but it is believed that the nonlocalized π orbital from the aromatic ring easily bonds with the π orbital of graphene, thereby forming a specific and stable adsorption state.

[0069] The cation having an aromatic heterocyclic ring may be an imidazolium cation. The imidazolium cation may be a cation in which a part of hydrogen atoms in the imidazole skeleton is replaced by an alkyl group or the like.

[0070] As an example of an imidazolium cation, a cation having an aromatic heterocyclic ring may also be 1-C 1-3 Alkyl-3-C 1-3 The alkyl imidazolium cation, more specifically, may contain a 1-ethyl-3-methylimidazolium cation. 80 mol % or more of the cation may be 1-C 1-3 Alkyl-3-C 1-3An alkylimidazolium cation or a 1-ethyl-3-methylimidazolium cation.

[0071] The content of the reduction reaction product fixed in the diaphragm (i.e., the ratio of the mass of the reduction reaction product to the total mass of the diaphragm) is, for example, 2% by mass or more, and may be 5% by mass or more, 10% by mass or more, 20% by mass or more, or 30% by mass or more. In the capacitor, a part of the reduction reaction product fixed in the diaphragm may be dissolved in the electrolyte, but most of it remains fixed to the diaphragm.

[0072] The amount of the reduction reaction product fixed to the separator can be analyzed, for example, by the following method.

[0073] First, the diaphragm to which the reaction product is bonded is taken out, the surface is cleaned with dimethyl carbonate (DMC), and it is dried for more than 2 hours at room temperature under reduced pressure (e.g., 0.1 MPa or less, preferably 10 Pa or less). Then, the liquid containing the reaction product is fully extracted from the inside of the diaphragm by centrifugal separation.

[0074] By performing ESR analysis on the extract, the concentration of the reaction product, i.e., free radicals, etc., can be analyzed to determine the minimum amount of the reaction product bound. The reaction product, i.e., free radicals, can be quantified by drawing a calibration curve using a spin quantitative standard sample solution (TEMPOL).

[0075] In addition, by implementing 1 H-NMR analysis can separate and detect the ions caused by cations (EMI + ) and a peak due to dimers. The ratio of dimers contained in the extract can be quantified from the areas of the two peaks.

[0076] As the ionic liquid or the second ionic liquid contained in the electrolyte of the capacitor, the compounds listed as the first ionic liquid can be exemplified. The second ionic liquid contains the same cations as those constituting the first ionic liquid. The second ionic liquid may be the same as the first ionic liquid.

[0077] Between the first electrode and the second electrode of the capacitor, a high voltage of, for example, 4.0 V or more may be applied. In this case, a significantly high capacity can be achieved.

[0078] In order to adjust the viscosity of the electrolyte and improve the output characteristics, a solvent may be mixed in the second ionic liquid and used as the electrolyte. As the solvent, any solvent (non-aqueous solvent) used in the past as the electrolyte of capacitors may be used as long as it can be uniformly mixed with the ionic liquid.

[0079] As the non-aqueous solvent, a high boiling point solvent is preferred. For example, lactones such as γ-butyrolactone, carbonates such as propylene carbonate, polyvalent alcohols such as ethylene glycol and propylene glycol, cyclic sulfones such as sulfolane, amides such as N-methylacetamide, N,N-dimethylformamide, and N-methyl-2-pyrrolidone, esters such as methyl acetate, ethers such as 1,4-dioxane, ketones such as methyl ethyl ketone, formaldehyde, etc. can be used.

[0080] When the electrolyte solution contains a solvent other than the ionic liquid, the proportion of the ionic liquid in the entire electrolyte solution may be 75% by mass or more, 80% by mass or more, or even 90% by mass or more.

[0081] As the material of the first active material and / or the second active material, a carbon material having a layered structure can be used. That is, the carbon material contains a layered structure in which carbon atoms are bonded in a hexagonal mesh in a plane (generally referred to as a graphene layer or a graphene sheet). The carbon material may also contain graphene. The graphene may also be reduced graphene oxide or graphene having a three-dimensional structure.

[0082] Graphene is a carbon material with a graphene sheet having a thickness equivalent to one carbon atom as the smallest unit, and usually constitutes a laminate of multiple graphene sheets. A graphene sheet is an aggregate or molecule composed of sp2 bonded carbon having a thickness equivalent to one carbon atom, and has a honeycomb lattice structure extending in a sheet shape.

[0083] At least the first active material among the first active material and the second active material may contain a carbon material having a layer structure.

[0084] The carbon material having a layered structure can be used as either an active material on the positive electrode side or an active material on the negative electrode side. However, in one embodiment, by using an electrode (the first electrode or the second electrode) containing the above-mentioned carbon material in the active material as the negative electrode, the capacity is increased dramatically. Here, at least the first electrode of the first electrode and the second electrode is an electrode containing the above-mentioned carbon material in the active material (the first active material) for explanation.

[0085] The carbon material may also include reduced graphene oxide. Reduced graphene oxide can be obtained by reducing graphene oxide.

[0086] Graphene oxide (hereinafter also referred to as "GO") has a structure in which oxygen-containing groups are bonded to graphene sheets. It is believed that the oxygen-containing groups are mainly bonded to the edge planes of the graphene sheet stack. The oxygen-containing groups are hydrophilic groups such as hydroxyl groups, carbonyl groups, and carboxyl groups. Graphene oxide (GO) is generally dispersible in polar solvents such as water. Graphene oxide (GO) generally has insulating properties because it contains sp3 bonded carbon.

[0087] By reducing graphene oxide (GO), oxygen-containing groups can be removed to obtain reduced graphene oxide (hereinafter also referred to as "rGO"). Reduced graphene oxide (rGO) is a graphene analogue with conductivity. Reduced graphene oxide may contain oxygen-containing groups that are not removed by the reduction process. By the presence of functional groups such as oxygen atoms in the graphene layer, the crystal structure of the carbon material deviates from the ideal graphene or graphite structure, and sp2 bonds and sp3 bonds are mixed in the carbon atoms in the graphene layer. As a result, the graphene interlayer becomes easy to expand by applying a high voltage, cations and anions are easily embedded in the graphene interlayer, and the formation area of ​​the double electric layer becomes easy to expand. Therefore, by using reduced graphene oxide in the active material, the capacity of the capacitor can be increased dramatically.

[0088] In addition, the presence of functional groups such as oxygen atoms can generate strain in the planar structure of graphene, and a three-dimensional structure can be formed by disorder of the layer structure (or disorder of the interlayer distance) or by bending or curving of the graphene layer. Thus, the effective surface area for adsorbing cations and anions is increased, thereby achieving high capacity.

[0089] Ordinary graphene usually has a flat sheet-like form. On the other hand, the graphene used in the capacitor of this embodiment may not be a flat sheet, but may be a graphene sheet stack with a disordered layer structure (or disordered interlayer spacing) (or a three-dimensional structure) in various forms. By using a graphene (graphene sheet stack) with a three-dimensional structure in the active material, the capacity of the capacitor is increased dramatically.

[0090] The so-called three-dimensional structure mainly refers to the microscopic three-dimensional structure (i.e., fine structure) formed in the flaky particles. By having a three-dimensional structure, the overlap of graphene sheets can be significantly suppressed compared with flat sheet-like graphene, and the large surface area of ​​graphene can be effectively utilized. On the main surface (mainly on the 002 plane (basal plane)) of the graphene sheet stack with a three-dimensional structure, a plurality of protrusions or a plurality of pits (i.e., wrinkles) are formed. Through such a three-dimensional structure, the distance between the graphene sheets can be appropriately controlled, thereby effectively reducing the overlap of the graphene sheets.

[0091] The three-dimensional structure may include a bent structure formed by bending a wrinkled graphene sheet. A stacked body may be formed by folding a graphene sheet in a direction intersecting the surface of the sheet through the bent portion. The radius of curvature of the bent portion in the bent structure is, for example, in the range of 10 to 1000 nm. The interval between wrinkles is, for example, in the range of 10 to 100 nm.

[0092] The bending structure in the three-dimensional structure includes, for example, a wrinkled structure or a folded structure in the sheet portion between the curved portions. At this time, each graphene sheet stack itself may have a fine porous structure (microporous structure). Therefore, the diffusion of ions near the surface of the stack becomes better. The presence of the wrinkled structure and the folded structure (i.e., the wrinkled portion) can be confirmed by an electron microscope (SEM, TEM, etc.) photograph of the graphene sheet stack.

[0093] The so-called wrinkled structure, for example, is a structure having a plurality of randomly formed wrinkled (pleated) shaped protrusions and concave portions. In addition, the so-called folded structure is a structure having a folded portion formed by locally folding a graphene sheet stack multiple times, which is included in the category of the wrinkled structure. The height of the protrusion or the depth of the concave portion formed in the folded portion may be greater than the thickness of the carbon portion of the graphene sheet stack having the structure, and may be more than twice the thickness of the carbon portion.

[0094] In the logarithmic differential pore volume distribution, graphene having such a three-dimensional structure may have a peak in the range of pore diameters from 2nm to 4nm, and further in the range of pore diameters from 4nm to 50nm, the volume increases as a quadratic function as the pore diameter increases. The total pore volume of mesopores in the range of pore diameters from 2nm to 50nm may be, for example, 0.20cm 3 / g or more. The total pore volume of the mesopores can also be 0.20cm 3 / g~0.5cm 3 / g range, 0.25cm 3 / g~0.4cm 3 / g range, or 0.25cm 3 / g~0.35cm 3 The total volume of pores having a pore diameter of 4 nm to 50 nm may be, for example, 15 times or more the total volume of pores having a pore diameter of 2 nm to 4 nm.

[0095] The specific surface area and pore size distribution of graphene can be measured using a BELSORP 28SA device available from BEL Co., Ltd. of Japan. As an analytical theory of mesopores, the Dollimore Heal method (DH method) based on capillary condensation theory (Kelvin formula) is used.

[0096] By having such a three-dimensional graphene structure, a capacitor electrode having a maximum peak in a range of 0.3 μm or more and 6 μm or less in the logarithmic differential pore volume distribution measured by a mercury porosimeter can be obtained. By having a three-dimensional structure, the overlap of graphene sheets can be significantly suppressed compared to flat sheet-like graphene, and the surface area of ​​graphene can be effectively applied in ion adsorption. By forming a three-dimensional structure of multiple protrusions or multiple pits on the base surface, the distance between the graphene sheets can be properly controlled, and the overlap of the graphene sheets can be effectively reduced. Therefore, the active sites of the active material can be increased without suppressing the movement (diffusion) of ions, and high capacity can be exhibited. In addition, since the reaction product can be moved more, it can contribute to the performance of high capacity.

[0097] According to a capacitor involved in one embodiment of the present disclosure, specifically, it is possible to achieve a capacitor in which the electrostatic capacitance per unit mass of the active material is 300F / g or more when a voltage of 4.0V or more is applied. A capacitor in which the electrostatic capacitance per unit mass of the active material is 400F / g or more, 500F / g or more, 800F / g or more, or 1000F / g or more can also be achieved. Furthermore, the electrostatic capacitance per unit mass of the active material when a voltage of 4.0V or more is 300F / g or more means that when the capacitor is charged with a voltage of 4.0V or more and then discharged, there is a voltage range in which the electrostatic capacitance becomes 300F / g or more in a certain voltage range. Regarding the voltage range in which the electrostatic capacitance becomes 300F / g or more, it is not particularly limited as long as it is above 4.0V. The electrostatic capacitance is 300F / g or more in the voltage range above 4.0V, and the electrostatic capacitance can also be 300F / g or more in a certain voltage range below 4.0V.

[0098] The average number of stacked graphene sheet layers is, for example, 10 or less, or 5 or less. The graphene sheet stack is preferably closer to a minimum unit graphene sheet having a thickness equivalent to one carbon atom (ie, a single-layer sheet).

[0099] The average number of stacking layers can be inferred from the interplanar spacing (d002) calculated from the diffraction peak of the 002 plane (basal plane) belonging to the X-ray diffraction profile (for example, the summary of the 2015 Autumn Conference of the Physical Society of Japan, p1014). Alternatively, it can be an inferred value obtained from an electron microscope (SEM, etc.) photo of graphene. For example, the number of stacking layers of a graphene sheet can be inferred from the scale of the SEM photo of graphene and the interplanar spacing of the 002 plane (basal plane) of the graphene sheet. For example, select any 20 graphene sheet stacks, infer the number of stacking layers respectively, omit the values ​​from the maximum side to the 5th and the values ​​from the minimum side to the 5th, and take the average of the 10 values ​​in the middle as the average number of stacking layers.

[0100] The interlayer spacing (i.e., basal plane spacing) between graphene sheets can also vary randomly. Random changes in interlayer spacing mean that the crystallinity of the graphene sheet stack is low. The greater the disorder of the stacking structure in the stack, the more significant the change in interlayer spacing.

[0101] The X-ray diffraction profile of graphene generally has a diffraction peak B attributed to the 002 plane. The greater the overlap of graphene sheets and the higher the crystallinity of graphene, the sharper the diffraction peak B becomes.

[0102] On the other hand, when graphene has a three-dimensional structure, the diffraction peak B becomes broad and can be waveform-separated into a plurality of peaks. A halo pattern attributed to the amorphous phase can also be observed at a higher angle than the diffraction peak B.

[0103] The interplanar spacing d002 of the 002 plane of graphene calculated from the X-ray diffraction profile is greater than 0.330nm and less than 0.360nm. d002 can be calculated by waveform separation of the diffraction peak observed in the region near 2θ=26.38°, calculating d002 for each component, and calculating the average thereof. The distance d002 of the 002 plane of graphene is preferably 0.340nm More preferably 0.360nm More preferably, 0.370 nm above.

[0104] The graphene having the above structure is used in the active material to manufacture the first electrode and / or the second electrode as the capacitor electrode. The capacitor electrode may also contain a binder. The binder has the function of assisting the bonding of the graphenes to each other and the bonding of the graphene to the collector when the graphene having the above three-dimensional structure is formed into an electrode layer.

[0105] Hereinafter, an example of a method for producing graphene according to an embodiment of the present disclosure and a method for producing a capacitor electrode using the graphene produced thereby will be described.

[0106] 《How to make graphene》

[0107] (i) Dispersion Preparation Step

[0108] First, an aqueous dispersion containing graphene oxide is prepared. In addition to graphene oxide and water, the aqueous dispersion may also contain a dispersant such as carboxymethyl cellulose (CMC). Graphene oxide can be generated, for example, by peeling off from graphite in a single or multilayer state after oxidation of graphite.

[0109] The oxidation of graphite can be carried out, for example, using an oxidant in water. As the oxidant, sulfuric acid, potassium permanganate, chromic acid, sodium dichromate, sodium nitrate, peroxide, persulfate, organic peroxy acid, etc. can be used. A water-soluble solvent can also be added to the water. As the water-soluble solvent, ketones such as alcohols, acetone, dioxane, ethers such as tetrahydrofuran, etc. can be exemplified. An aqueous dispersion of graphene oxide is generated by an oxidation reaction in water.

[0110] The oxygen content of graphene oxide may be, for example, 10 to 60% by mass, 20 to 50% by mass, or 30 to 50% by mass.

[0111] (ii) Reduction process

[0112] Next, the graphene oxide is reduced in an aqueous dispersion containing graphene oxide to generate reduced graphene oxide (first reduction step). As a reduction method, for example, hydrothermal treatment is preferred. For example, a gel-like product can be generated by sealing the aqueous dispersion in an autoclave and performing hydrothermal treatment. The temperature of the hydrothermal treatment is, for example, above 150° C., and can also be above 170° C. and below 200° C.

[0113] Reduced graphene oxide with a three-dimensional structure can also be obtained by hydrothermal treatment alone, but in order to further reduce it, the gel-like product can also be contacted with a reducing agent (second reduction step). As a reducing agent, for example, metal hydrides, borohydrides, boranes, hydrazines or hydrazides, ascorbic acid, thioglycolic acid, cysteine, sulfurous acid, thiosulfate, dithionite, etc. can be exemplified. For example, the gel-like product can be immersed in an aqueous solution containing a water-soluble reducing agent such as sodium ascorbate. The temperature of the aqueous solution can be, for example, 20 to 110°C, 40 to 100°C, or 50 to 100°C. The amount of the reducing agent used can be appropriately adjusted according to the type of reducing agent, the oxygen content of the first carbon raw material (graphene oxide), the amount of the gel-like product, etc.

[0114] Then, the gel-like product can also be freeze-dried. By freeze-drying, a dried gel (xerogel) in which the three-dimensional structure of graphene is highly maintained can be obtained. Freeze-drying can be performed at, for example, -50°C to 0°C, preferably at -50°C to -20°C and under reduced pressure of less than 100 Pa and more preferably less than 1 Pa.

[0115] Next, the dried gel is thermally reduced in a non-oxidizing atmosphere to remove the remaining functional groups (third reduction step).

[0116] The non-oxidizing atmosphere can also be a reduced pressure atmosphere (for example, below 0.1 MPa (preferably below 10 Pa)), a reducing atmosphere (for example, a hydrogen atmosphere below 0.01 MPa), an inert gas atmosphere (for example, a circulating atmosphere of N2, Ar, Ne, He, etc.), etc.

[0117] The heating temperature in the non-oxidizing atmosphere is 700°C or more, 800°C or more, 900°C or more, 1000°C or more, or 1200°C or more. However, the reduction of the oxygen content of the reduced graphene oxide has a limit. Considering the production cost, the heating temperature in the non-oxidizing atmosphere may be 1800°C or less, 1400°C or less, or 1200°C or less. When specifying the temperature range, the upper and lower limits thereof may be arbitrarily combined. The temperature range may be, for example, 1000°C to 1800°C.

[0118] The heating time in the non-oxidizing atmosphere can be appropriately selected depending on the heating conditions and the amount of carbon to be treated, and may be, for example, about 0.1 to 5 hours.

[0119] The oxygen content of the dried gel after thermal reduction is less than 5% by mass, and may be less than 4% by mass, or less than 3% by mass, preferably less than 2.6% by mass, or less than 2% by mass or less than 1.5% by mass. If the oxygen content is reduced to less than 5% by mass, the reactants generated by the redox reaction of the oxygen-containing group and the electrolyte component are reduced. Such reactants block the pores of the electrode, reduce the diffusivity of the ions, and also reduce the adsorption sites of the ions. Therefore, the fewer the reactants, the less the diffusivity of the ions will be reduced, and the less the adsorption sites of the ions will be reduced, so that high capacity can be exhibited.

[0120] The dried gel after thermal reduction is crushed to obtain reduced graphene oxide powder (rGO powder).

[0121] By the above method, graphene (reduced graphene oxide) having a three-dimensional structure can be produced. Using the produced graphene, a capacitor electrode can be produced by the following method, for example.

[0122] 《Method for manufacturing capacitor electrode》

[0123] (iii) Electropolarization process

[0124] For example, rGO powder is dispersed in a dispersion medium such as water together with a binder to prepare a slurry. The obtained slurry is applied to a conductive substrate (collector), and the coating is dried to form an electrode layer supported on the collector to obtain a capacitor electrode. Then, the electrode layer can also be rolled.

[0125] As the binder, for example, fluororesins such as polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), vinylidene fluoride-hexafluoropropylene copolymer (PVdF-HFP), carboxymethyl cellulose (CMC), polyethylene oxide (PEO), polyethylene glycol (PEG), polyacrylonitrile (PAN), polymethyl methacrylate (PMMA), polyvinyl alcohol (PVA), polyvinyl pyrrolidone (PVP), polyacrylic acid (PAA), polyvinyl acetate and other water-soluble resins can be used.

[0126] The electrode layer may contain other active materials such as activated carbon in addition to the above-mentioned graphene. In addition, the electrode layer may also contain carbon particles such as carbon fibers such as carbon nanotubes (CNT), carbon black, and graphite. However, from the viewpoint of taking both high capacity and high reliability into account, it is preferred that graphene constitutes more than 50% by mass of the electrode layer, and more preferably more than 65% by mass.

[0127] As the current collector, metal foil, metal porous body, etc. can be used. As the material of the current collector, aluminum, copper, nickel, iron, stainless steel, platinum, etc. can be used. An alloy with these metals as the main component can also be used. The metal foil can also be a smooth foil, but it can also be a foil roughened by etching, etc. and a foil treated with plasma, etc. The metal porous body has, for example, a three-dimensional network structure.

[0128] The mass per unit area of ​​the porous metal body may be, for example, 500 g / m 2 Below, can also be 150g / m 2 The porosity of the porous metal body may be, for example, 80% by volume to 98% by volume, or 90% by volume to 98% by volume.

[0129] The average pore diameter of the pores of the porous metal body may be, for example, 50 μm to 1000 μm, 400 μm to 900 μm, or 450 μm to 850 μm.

[0130] Capacitor

[0131] Next, an example of a capacitor including the above-described capacitor electrodes as first and second electrodes will be described. Figure 1 1 is a partially cutaway perspective view of capacitor 10 .

[0132] The capacitor 10 shown in the figure has a wound capacitor element 1. The capacitor element 1 is formed by winding the sheet-shaped first electrode 2 and the second electrode 3 through the separator 4. The first electrode 2 and the second electrode 3 respectively have a first collector made of metal, a second collector, and a first electrode layer and a second electrode layer supported on the surface thereof, and exhibit capacity by adsorbing and desorbing ions. As the first and second collectors, aluminum foil can be used, for example. The surface of the collector can also be roughened by etching or other methods. The separator 4 can use, for example, a non-woven fabric with cellulose as the main component. Leads 5a and 5b are connected to the first electrode 2 and the second electrode 3 as lead-out members. The capacitor element 1 is housed in a cylindrical outer packaging shell 6 together with an electrolyte (not shown). The material of the outer packaging shell 6 can be, for example, a metal such as aluminum, stainless steel, copper, iron, and brass. The opening of the outer packaging shell 6 is sealed by a sealing member 7. The leads 5a and 5b are led out to the outside in a manner that passes through the sealing member 7. The sealing member 7 can be made of a rubber material such as butyl rubber.

[0133] The electrode layer contains an active material as an essential component and may contain a binder, a conductive aid, etc. as an optional component. The active material, for example, includes graphene having the characteristics described above. The electrode layer can be obtained, for example, by the following method: the active material, a binder (for example, carboxymethyl cellulose (CMC)), etc. are kneaded together with water in a mixer to obtain a slurry, the obtained slurry is applied on the surface of the collector, the coating is dried, and then rolled.

[0134] The above-mentioned Va obtained from the pore size distribution of the separator is preferably 0.4 cm 3 The reduction reaction product may also be bonded to the diaphragm.

[0135] In the above embodiment, a winding type capacitor is described, but the application scope of the present invention is not limited to the above content, and it can also be applied to capacitors of other structures, such as stacked type or coin type capacitors.

[0136] Hereinafter, the present invention will be described in more detail based on Examples, but the present invention is not limited to the Examples.

[0137] <Examples 1 to 6, Comparative Examples 1 to 4>

[0138] (1) Fabrication of capacitor electrodes

[0139] Graphite was oxidized in water using potassium permanganate as an oxidant to obtain graphene oxide. A water dispersion containing 1% by mass of graphene oxide was hydrothermally treated at 180° C. for 6 hours to obtain a gel-like product (first reduction step).

[0140] Next, the gel product was immersed in a reducing agent, namely, an aqueous sodium ascorbate solution (sodium ascorbate concentration: 1.0 mol / L), and heated to 100° C. and maintained for 2 hours to fully reduce the carbon (second reduction step).

[0141] The gel product was then freeze-dried at -20°C and 100 Pa under reduced pressure to obtain a dry gel. The dry gel was then heat-treated at 1200°C for 2 hours in a nitrogen atmosphere (third reduction step). The heat-treated dry gel was then pulverized to obtain reduced graphene oxide powder.

[0142] 100 parts by mass of reduced graphene oxide powder and 10 parts by mass of a binder, namely CMC, were dispersed in an appropriate amount of water to prepare a slurry. The obtained slurry was coated on a collector consisting of an Al foil having a thickness of 30 μm, the coating was vacuum dried at 110°C, and then rolled to form an electrode layer, thereby obtaining a capacitor electrode.

[0143] (2) Preparation of diaphragm

[0144] Nonwoven fabric separators a1 to a4 made of cellulose fibers, nonwoven fabric separators a5, a6, b1, and b2 made of synthetic fibers including cellulose fibers, a nonwoven fabric separator c1 made of polypropylene (PP), and a polyolefin-based nonwoven fabric separator d1 were prepared.

[0145] Table 1 shows the thickness, porosity, and density (bulk density) of each separator a1 to a6, b1, b2, c1, and d1. In addition, Table 1 also shows the total volume Va of the pore diameter range of 0.1 μm to 2 μm and the total volume Vm of the pore diameter range of 0.01 μm to 6 μm measured by a mercury porosimeter.

[0146] Table 1

[0147]

[0148] (3) Fabrication of capacitors

[0149] Prepare a pair of capacitor electrodes and punch them into a 20 mm × 20 mm square shape. Connect leads to the capacitor electrodes respectively, overlap the capacitor electrodes by clamping the diaphragm a1 so that the coated surfaces of the electrode layers face each other, and obtain a laminated capacitor element. The capacitor element and the electrolyte are placed in an outer packaging shell made of Al lamination, and sealed with a sealing member to complete the capacitor A1 of Example 1. Then, an aging treatment is performed at 60°C for 6 hours while applying a voltage of 2.5 V.

[0150] As the electrolyte solution of the capacitor A1, 1-ethyl-3-methylimidazolium tetrafluoroborate (EMIBF4) as an ionic liquid was used. The chemical formula of EMIBF4 is shown below.

[0151] [Chemical formula 4]

[0152]

[0153] Similarly, capacitors A2 to A6, B1, B2, C1 and D1 were prepared using diaphragms a2 to a6, b1, b2, c1 and d1 instead of diaphragm a1. Capacitors A1 to A6 correspond to Examples 1 to 6, respectively, and capacitors B1, B2, C1 and D1 correspond to Comparative Examples 1 to 4, respectively.

[0154] The following evaluations were performed on capacitors A1 to A6, B1, B2, C1, and D1, respectively.

[0155] <Evaluation>

[0156] The capacitance of each capacitor A1 to A6, B1, B2, C1 and D1 is evaluated by the following method.

[0157] The manufactured capacitor was charged with a constant current of 0.1 to 1 A / g relative to the weight of the battery active material (the total of the positive electrode active material mass and the negative electrode active material mass) until the set voltage V1 (=2.8 V) was reached. Then, constant voltage charging was performed for 8 minutes at the set voltage V1.

[0158] After the constant voltage charge is completed, the battery is discharged at a constant current of 0.1 to 1 A / g relative to the weight of the battery active material to 0 V. The capacity is calculated from the slope of the voltage change from 2.1 V to 0.1 V during discharge. The capacity can be calculated by the following formula when the constant current value during discharge is set to I (A) and the discharge time from 2.1 V to 0.1 V is set to t (sec).

[0159] Capacity (F) = It / (2.1-0.1)

[0160] From the calculated capacity, calculate the single-electrode capacity when the positive and negative electrode capacities (mass of positive and negative electrode active materials) are set to the same, and find the single-electrode capacity C1 (F / g) per 1g mass of positive and negative electrode active materials when 2.8V is applied.

[0161] The set voltage is changed to V2 (=4.4V), and the capacitor is charged and discharged in the above-mentioned charge and discharge cycle in the same manner as before. The single-electrode capacity C2 (F / g) per 1g of positive and negative electrode active material mass when 4.4V is applied is calculated.

[0162] Table 2 shows the evaluation results of the single-electrode capacitance C1 and C2 and the ratio C2 / C1 of C2 to C1 in each of capacitors A1 to A6, B1, B2, C1 and D1 together with the total volume Va of the pore diameter of the used separator in the range of 0.1 μm to 2 μm.

[0163] Table 2

[0164]

[0165] As can be seen from Table 2, if the applied voltage of the capacitor is 2.8V, the difference in capacitance C1 among capacitors A1 to A6, B1, B2, C1, and D1 is small. In contrast, if the applied voltage of the capacitor is 4.4V, the difference in capacitance C2 among capacitors A1 to A6, B1, B2, C1, and D1 is significantly increased. However, when the Va of the diaphragm is set to 0.4cm 3 Capacitors A1 to A6 with a capacitance of 0.1 V or more can achieve high capacitance even when a voltage of 4.0 V or more is applied.

[0166] <Example 7>

[0167] (1) Fabrication of capacitor electrodes

[0168] In the same manner as in Example 1, a capacitor electrode was obtained.

[0169] (2) Preparation of test battery

[0170] A cellulose nonwoven fabric separator (porous substrate) X1 is prepared.

[0171] Prepare a pair of capacitor electrodes and punch them into a 20 mm × 20 mm square shape. Connect leads to the capacitor electrodes respectively, overlap the capacitor electrodes by clamping the diaphragm X so that the coated surfaces of the electrode layers face each other, and obtain a stacked capacitor element. The capacitor element and the electrolyte are placed in an outer packaging shell made of Al lamination, sealed with a sealing member, and the test battery is completed. As the electrolyte, 1-ethyl-3-methylimidazolium tetrafluoroborate (EMIBF4) as an ionic liquid is used.

[0172] Then, a voltage of 4.4 V to 4.6 V was applied to the test battery for 5 hours.

[0173] The separator (porous substrate) was removed from the test cell after voltage application, washed with dimethyl carbonate (DMC), and dried for 2 hours at room temperature under reduced pressure to obtain a separator Y1 having a reduction reaction product adhered thereto. The electrolyte of the test cell after voltage application turned brown, and the separator Y1 was also colored brown.

[0174] The electrolyte removed from the test cell was subjected to 1H-NMR, 13 C-NMR, 11 B-NMR and 19 F-NMR analysis. 1 H-NMR and 13 The results of C-NMR confirmed the presence of the EMI dimer shown in Chemical Formula 3. 11 B-NMR and 19 The results of F-NMR showed that no oxidation product was found to be generated by the anion of the ionic liquid, and it was confirmed to be BF4 - The state of the electrolyte taken out from the test battery was maintained without change. In addition, the electrolyte solution was analyzed by ESR, and the presence of EMI radicals and EMI carbenes was confirmed.

[0175] The mass of the separator Y1 was measured and found to have increased by 33% compared to the state before voltage application (separator X1). The degree of mass increase is considered to depend on the fixed reduction reaction product.

[0176] (3) Fabrication of capacitors

[0177] A pair of capacitor electrodes was prepared. Using EMIBF4, which was not used as an electrolyte, and separator Y1, a capacitor element was produced in the same manner as in the production of a test cell, thereby obtaining a capacitor A7.

[0178] <Example 8>

[0179] A nonwoven fabric separator (porous base material) X2 composed of mixed fibers containing cellulose is prepared.

[0180] In the same manner as in Example 7, a separator Y2 to which the reduction reaction product was fixed was obtained from the separator X2, and a capacitor element was produced using the separator Y2, thereby obtaining a capacitor A8.

[0181] <Comparative Example 5>

[0182] A pair of capacitor electrodes was prepared. Using EMIBF4 and separator X1, which were not used as an electrolyte, a capacitor element was produced in the same manner as in the production of a test cell, thereby obtaining a capacitor E1.

[0183] In other words, the test battery using the separator X1 before the 4.4 V to 4.6 V applied voltage treatment was used as the capacitor E1 and evaluated.

[0184] <Comparative Example 6>

[0185] A pair of capacitor electrodes was prepared. Using EMIBF4, which was not used as an electrolyte, and separator X2, a capacitor element was produced in the same manner as in the production of a test cell, thereby obtaining a capacitor E2.

[0186] In other words, the test battery using the separator X2 before the 4.4 V to 4.6 V applied voltage treatment was used as the capacitor E2 to be evaluated.

[0187] The capacitors A7 and A8 correspond to the seventh and eighth embodiments, respectively, and the capacitors E1 and E2 correspond to the fifth and sixth comparative examples, respectively.

[0188] The capacitors A7, A8, E1, and E2 were evaluated as shown below.

[0189] (Monopolar Capacitance Measurement)

[0190] The manufactured capacitor was charged at a constant current of 0.1 A / g to 1 A / g relative to the weight of the battery active material (the total of the positive electrode active material mass and the negative electrode active material mass) to a set voltage (4.6 V). Then, constant voltage charging was performed at the set voltage for 8 minutes.

[0191] After the constant voltage charge is completed, the battery is discharged at a constant current of 0.1A / g to 1A / g relative to the weight of the battery active material to 0V. The capacity is calculated from the slope of the voltage change from 2.1V to 0.1V during discharge. The capacity can be calculated by the following formula when the constant current value during discharge is set to I (A) and the discharge time from 2.1V to 0.1V is set to t (sec).

[0192] Capacity (F) = It / (2.1-0.1)

[0193] From the calculated capacity, the positive and negative electrode capacities (mass of positive and negative electrode active materials) were set to be the same and the single electrode capacity was calculated, and the single electrode capacity C0 (F / g) per 1g mass of positive and negative electrode active materials when 4.6V was applied was obtained.

[0194] (Charge and discharge efficiency)

[0195] For the manufactured capacitor, the following charging 1 and discharging 1 were regarded as one cycle, and this cycle was repeated 250 times.

[0196] [Charge 1]

[0197] Until the set voltage (=4.6V), constant current charging is performed at a current of 0.1A / g to 1A / g relative to the weight of the battery active material (the total mass of the positive electrode active material and the negative electrode active material), and then constant voltage charging is performed at the set voltage for 8 minutes.

[0198] [Discharge 1]

[0199] The battery was discharged at a constant current of 0.1 A / g to 1 A / g relative to the weight of the battery active material to 0 V.

[0200] In each cycle, the charge quantity Q1 in charge 1 and the discharge quantity Q2 in discharge 1 were measured, and the charge and discharge efficiency was evaluated as R=(Q2 / Q1)×100.

[0201] Table 3 shows the evaluation results of the single-electrode capacity C0 and the charge-discharge efficiency Q2 / Q1 of the 250th cycle in each capacitor A7, A8, E1 and E2. Figure 2 The change in the charge and discharge efficiency Q2 / Q1 per cycle is also shown for each of the capacitors A7, A8 and E1.

[0202] Table 3

[0203]

[0204] From Table 3 and Figure 2 It is found that the capacitors A7 and A8 using the separator to which the reduction reaction product is fixed in advance have a larger capacity C0 and improved charge and discharge efficiency than the capacitors E1 and E2 in which the reduction reaction product is not fixed to the separator.

[0205] Industrial Applicability

[0206] According to the present invention, a capacitor with high energy density can be obtained.

[0207] The present invention has been described with respect to the currently preferred embodiments, but such disclosure is not to be construed in a limiting sense. Various modifications and changes will become apparent to those skilled in the art of the present invention upon reading the above disclosure. Therefore, the appended claims should be construed to include all modifications and changes without departing from the true spirit and scope of the present invention.

[0208] Explanation of symbols:

[0209] 1: capacitor element, 2: first electrode, 3: second electrode, 4: separator, 5a: first lead, 5b: second lead, 6: outer case, 7: sealing member, 10: capacitor

Claims

1. A capacitor comprising: a first electrode including a first active material, a second electrode including a second active material, a separator between the first electrode and the second electrode, and Electrolyte, in, The electrolyte comprises an ionic liquid, In the pore size distribution of the separator, the total volume Va of pores in the range of 0.1 μm to 2 μm is 0.4 cm 3 / g or above.

2. The capacitor according to claim 1, wherein: A voltage of 4.0 V or more is applied between the first electrode and the second electrode.

3. The capacitor according to claim 1 or 2, wherein: In the pore size distribution of the separator, the total volume Vm of pores in the range of 0.01 μm to 6 μm is 0.7 cm 3 / g or above.

4. The capacitor according to any one of claims 1 to 3, wherein: The porosity of the separator is greater than 60%.

5. The capacitor according to any one of claims 1 to 4, wherein: Among the first active material and the second active material, at least the first active material contains reduced graphene oxide.

6. The capacitor according to claim 5, wherein: The reduced graphene oxide has a peak in the range of pore diameters of 2nm to 4nm in the logarithmic differential pore volume distribution, and has a distribution in which the volume increases as a quadratic function with the increase of the pore diameter in the range of 4nm to 50nm.

7. The capacitor according to any one of claims 1 to 6, wherein: The ionic liquid contains a cation having an aromatic heterocyclic ring.

8. The capacitor according to claim 7, wherein: The cation includes a 1-ethyl-3-methylimidazolium cation.

9. The capacitor according to any one of claims 1 to 8, wherein: The electrostatic capacitance per unit mass of the first active material when a voltage of 4.0 V or higher is applied is 300 F / g or higher.

10. A capacitor comprising: a first electrode including a first active material, a second electrode including a second active material, a separator between the first electrode and the second electrode, and Electrolyte, in, The electrolyte comprises an ionic liquid, The separator includes a porous substrate and a reduction reaction product of an ionic liquid fixed to the porous substrate.

11. The capacitor according to claim 10, wherein: The content of the reduction reaction product fixed to the separator is 2% by mass or more.

12. The capacitor according to claim 10 or 11, wherein: At least one of the first active material and the second active material contains reduced graphene oxide.

13. The capacitor according to claim 12, wherein: The reduced graphene oxide has a peak in the range of pore diameters of 2nm to 4nm in the logarithmic differential pore volume distribution, and has a distribution in which the volume increases as a quadratic function with the increase of the pore diameter in the range of 4nm to 50nm.

14. The capacitor according to any one of claims 10 to 13, wherein: The electrostatic capacitance per unit mass of the first active material when a voltage of 4.0 V or higher is applied is 300 F / g or higher.

15. A method for manufacturing a capacitor, comprising: a first electrode containing a first active material, a second electrode containing a second active material, a separator between the first electrode and the second electrode, and an electrolyte solution, wherein: The manufacturing method comprises: a step of preparing a porous substrate and an ionic liquid, and A step of obtaining a separator by bonding the reduction reaction product of the ionic liquid to the porous substrate.

16. The method for manufacturing a capacitor according to claim 15, wherein: The process of obtaining the diaphragm comprises: a step of placing the porous substrate impregnated with the ionic liquid between a pair of electrodes to produce a battery; and A step of applying a voltage to the battery to generate the reduction reaction product.

17. The method for manufacturing a capacitor according to claim 15 or 16, wherein: The porous substrate contains at least one selected from cellulose and its derivatives.

18. The method for manufacturing a capacitor according to any one of claims 15 to 17, wherein: The ionic liquid contains a cation having an aromatic heterocyclic ring.

19. The method for manufacturing a capacitor according to claim 18, wherein: The cation includes a 1-ethyl-3-methylimidazolium cation.