Composite structures comprising single crystal thin layers on polycrystalline silicon carbide support substrates and related methods of manufacture
By adopting preferred crystal orientation and nitrogen doping on the polycrystalline SiC support substrate, combined with molecular adhesion bonding technology and intermediate layer, the resistivity and curvature problems of the support substrate are solved, and high-quality single crystal silicon carbide thinness is achieved Transfer of layers and versatility of supporting substrates are suitable for power electronic applications.
Patent Information
- Application Number
- CN202380026936.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-30
- Filing Date
- 2023-03-10
- Publication Date
- 2024-11-08
AI Technical Summary
The prior art is difficult to manufacture high-quality single crystal SiC thin layers on low-cost polycrystalline SiC support substrates, and the mechanical, electrical and thermal characteristics of the support substrate are not suitable for power electronic applications, especially vertical conductivity and In occasions where thermal conductivity is high.
Using preferred crystal orientation and nitrogen-doped polycrystalline SiC support substrate, combined with molecular adhesion bonding technology and the use of intermediate layers, transfer single crystal silicon carbide thin layer, and optimize the resistance of the support substrate through chemical vapor deposition technology Rate and curvature characteristics.
The high-quality single crystal silicon carbide thin layer is achieved on low-cost polycrystalline SiC supporting substrate, meeting the vertical conductivity and thermal conductivity requirements for power electronic applications, while ensuring the mechanical properties of the support substrate and the stability of component manufacturing.
Smart Images

Figure CN118922912A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor materials for microelectronic components. The invention relates in particular to a composite structure comprising a single-crystalline thin layer arranged on a support substrate made of polycrystalline silicon carbide. The single-crystalline thin layer is preferably made of silicon carbide, the composite structure being intended for power electronics applications. Background Art
[0002] SiC is increasingly being used to create innovative power components to meet the needs of growing electronics applications, especially electric vehicles. In fact, power components and integrated power systems based on single-crystal silicon carbide are able to handle much higher power densities than conventional silicon equivalents and require a smaller active area.
[0003] Nevertheless, high-quality single-crystal SiC (c-SiC) substrates for the microelectronics industry are still expensive and difficult to supply in large quantities. Therefore, layer transfer solutions for the manufacture of composite structures, which usually contain a thin layer made of single-crystal SiC (obtained from a high-quality c-SiC substrate) on a lower-cost support substrate (for example made of polycrystalline SiC (p-SiC)), are advantageous. Electronic components can then be manufactured on and / or in this thin layer.
[0004] A well-known thin layer transfer solution is Smart Cut TM The method is based on light ion implantation and direct bonding assembly at the bonding interface between a single-crystalline donor substrate and a supporting substrate.
[0005] Currently, p-SiC substrates are available on the market as support substrates. However, their mechanical, electrical and even thermal properties are not necessarily optimal for high-quality composite structures obtained by thin-layer transfer methods and intended for power applications.
[0006] As mentioned above, power electronics applications require excellent vertical conductivity of the composite structure. Therefore, the single-crystalline thin layer can be doped according to the application requirements: for example, with N-type doping, a resistivity less than or equal to 30mOhm.cm, 10mOhm.cm, or even less than 1mOhm.cm. However, it is also necessary to ensure good conductivity in the supporting substrate of the composite structure. For this purpose, the polycrystalline substrate is usually heavily doped (in particular, N-type doping) to achieve a resistivity of less than 30mOhm.cm. In addition, the assembly interface of the composite structure must be designed in a form that the vertical resistance does not increase (or only increases slightly).
[0007] However, there are other applications that do not require vertical conductivity but require a high resistivity of the supporting substrate: this is especially the case for RF applications. The other properties of the supporting substrate listed below (mechanical and even thermal) are necessary for these RF applications as well as for power applications.
[0008] Thin-layer transfer methods based on direct molecular adhesion bonding are highly dependent on the surface quality of the assembled substrates. In particular, a roughness of less than or equal to 1 nm RMS (root mean square roughness) is required, as well as a very low level of surface defects (particles, pores, etc. or other undulations that could produce bonding defects), both for the support substrate and the donor substrate.
[0009] The hardness of SiC and the presence of grains on the surface of the single crystal support substrate make surface preparation very complicated and difficult to achieve perfect quality.
[0010] Finally, it is necessary to use a support substrate that exhibits low curvature or low deformation. The curvature corresponds to a deflection or "warp", which is equivalent to the algebraic difference of the deviation of the substrate relative to the reference plane. On the one hand, low curvature is required so that these support substrates are compatible with high-quality direct assembly and high bonding energy, and on the other hand, so that the support substrate is not easily damaged in the single crystal thin layer due to high mechanical stress during or after the transfer method. Low curvature is also important for ensuring the performance of the manufacturing steps (e.g., lithography) of the components on / in the composite structure thin layer. The radius of curvature of the p-SiC support substrate (proportional to the inverse of the warp) is generally intended to be greater than about 25m, that is, for example, for a 150mm diameter substrate, the curvature ("warp") is less than or equal to 100 microns (for simplicity, μm is referred to as "micrometer" in the rest of this article).
[0011] Furthermore, in order to effectively dissipate the heat generated, in particular by power components, it is generally important that the support substrate ensures good thermal conductivity.
[0012] Achieving all these specifications on a p-SiC substrate is very complex.
[0013] Document US10934634 proposes a p-SiC substrate, the grain size variation between the two surfaces of the substrate is less than 0.43%, resulting in a curvature radius greater than 142m. In addition, at least one surface of the substrate exhibits an arithmetic mean roughness of less than 1nm.
[0014] However, this method is still expensive, energy- and material-intensive, since a considerable portion of the p-SiC initially deposited on the graphite substrate is removed and lost to obtain the proposed p-SiC substrate (typically 2 mm initially deposited to form a 350 micron p-SiC substrate). Summary of the invention
[0015] The invention proposes a composite structure comprising a thin layer made of a single-crystalline material, in particular c-SiC, arranged on a p-SiC support substrate. The invention also relates to a method for producing such a composite structure. SUMMARY OF THE INVENTION
[0017] The invention relates to a composite structure for producing a microelectronic component, comprising a single-crystalline thin layer arranged on a support substrate made of polycrystalline silicon carbide, the support substrate having a preferred crystal orientation, wherein:
[0018] -C 422 A texture coefficient of less than 30%, in particular less than 20%; and
[0019] -C 220 Texture coefficient greater than 60%, or C 111 +C 222 +C 511 The sum of the texture factors is greater than 70%, in particular greater than 80%.
[0020] Other advantages and non-limiting features according to the invention (which may be considered individually or in any technically feasible combination) are:
[0021] The support substrate has nitrogen doping and a resistivity of less than 30 mOhm.cm;
[0022] The thin layer is made of silicon carbide;
[0023] The thin layer is made of diamond;
[0024] The composite structure comprises a continuous or discontinuous intermediate layer, which is arranged between the thin layer and the supporting substrate and is composed of at least one metal or semiconductor material;
[0025] The intermediate layer is composed of silicon, silicon carbide, tungsten, and / or titanium;
[0026] ·C 422 The texture coefficient is less than 15%, or even less than 10%;
[0027] The thickness of the support substrate ranges between 50 micrometers and 800 micrometers, preferably between 60 micrometers and 500 micrometers.
[0028] The composite structure comprises electronic components on and / or in the thin layer and optionally electrical contacts on the back side of the supporting substrate.
[0029] The invention also relates to a method for producing a composite structure comprising a single-crystalline thin layer arranged on a supporting substrate made of polycrystalline silicon carbide, the method comprising the following steps:
[0030] a) providing a support substrate made of polycrystalline silicon carbide, the support substrate having a preferred crystal orientation, wherein:
[0031] -C 422 A texture factor of less than 30%, in particular less than 20%; and
[0032] -C 220 Texture coefficient greater than 60%, or C 111 +C 222 +C 511 The sum of the texture coefficients is greater than 70%, in particular greater than 80%;
[0033] b) providing a donor substrate made of a single crystal material;
[0034] c) Transferring the thin layer from the donor substrate to a supporting substrate.
[0035] Other advantages and non-limiting features according to the invention (which may be considered individually or in any technically feasible combination) are:
[0036] The transfer step c) comprises:
[0037] c1) forming a weakened buried surface in the donor substrate to define the thin layer between the weakened buried surface and the front surface of the donor substrate;
[0038] c2) assembling the donor substrate to the support substrate directly or through an intermediate layer by molecular adhesion bonding;
[0039] c3) separation along the weakened buried surface to result in transfer of the thin layer to the supporting substrate;
[0040] Before bonding the two substrates, step c2) comprises:
[0041] - before or after step c1), forming an intermediate layer on the donor substrate; and / or
[0042] - forming an intermediate layer on a supporting substrate,
[0043] The intermediate layer (30) is formed of at least one metal or semiconductor material selected from silicon, silicon carbide, tungsten and titanium;
[0044] The single crystal material forming the donor substrate is silicon carbide;
[0045] The manufacturing method further comprises manufacturing electronic components on and / or in the thin layer of the composite structure;
[0046] The production of electronic components includes, in particular, homoepitaxial or heteroepitaxial steps on thin layers. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] Further features and advantages of the present invention will become apparent from the following detailed description of the invention provided with reference to the accompanying drawings, in which:
[0048] [ Figure 1 ] Figure 1 The composite substrate of the present invention is shown;
[0049] [ Figure 2 ] Figure 2 shows a list of 10 diffraction peaks classified according to ascending Miller indices (hkl), considered in 3C polytype SiC substrates and measurable by X-ray diffraction; the table also shows the positions of the peaks and their theoretical intensities;
[0050] [ Figure 3a ]
[0051] [ Figure 3b ]
[0052] [ Figure 3c ] Figure 3a , 3b 3c shows micrographs (SEM) of support substrates manufactured under different conditions and having different preferred crystal orientations or textures, which are implemented to manufacture the composite structure of the present invention;
[0053] [ Figure 4 ] Figure 4 The composite substrate of the present invention is shown;
[0054] [ Figure 5a ]
[0055] [ Figure 5b ]
[0056] [ Figure 5c ]
[0057] [ Figure 5c ']
[0058] [ Figure 5c” ]
[0059] [ Figure 5d ] Figure 5a , 5b , 5c, 5c', 5c" and 5d show the steps of the manufacturing method of the present invention;
[0060] [ Figure 6 ] Figure 6 Production conditions and related features of five types of support substrates are shown, of which support substrates 2, 3 and 4 are suitable for the composite structure of the present invention.
[0061] The same reference numerals may be used for components of the same type in the figures. For the purpose of readability, some of the figures are schematic diagrams that are not drawn to scale. In particular, the thickness of the layers along the z-axis is not proportional to the lateral dimensions along the x-axis and the y-axis; and the relative thickness of the layers is not necessarily drawn as shown in the figures. DETAILED DESCRIPTION
[0062] The invention relates to a composite structure 100 particularly suitable for manufacturing a microelectronic component, comprising a single-crystalline thin layer 10, in particular made of silicon carbide, diamond, silicon, a II-VI or III-V semiconductor compound (for example AlN, GaN, etc.) or even gallium oxide (Ga2O3), which is arranged on a supporting substrate 20 made of polycrystalline silicon carbide ( Figure 1 ).
[0063] In the main plane (x, y), the composite structure 100 is preferably in the form of a circular wafer with a diameter of 100 mm, 150 mm, 200 mm or even larger. However, it may be in any other form that allows it to be processed to manufacture components. The thickness of the composite structure 100 extends along the z axis in the figure.
[0064] The thickness of the thin layer 10 of the composite structure 100 typically ranges from tens of nm to hundreds of nm, for example, from 50 nm to 800 nm. As will be seen below, an epitaxial step can be performed on the thin layer 10 to thicken it (homoepitaxy) or grow other materials (heteroepitaxy) to meet the requirements of the electronic component to be manufactured.
[0065] The thin layer 10 exhibits a resistivity suitable for the application and the target component. For example, for power components, the resistivity of the thin layer is typically less than 30 mOhm.cm, 10 mOhm.cm or even 1 mOhm.cm, and has N-type doping (nitrogen doping). For RF components, the resistivity of the thin layer can be greater than 100 Ohm.cm or even 10 kOhm.cm, for example without specific doping or addition of vanadium.
[0066] The support substrate 20, as its name implies, acts as a mechanical support for the composite structure 100. The lateral dimensions of the main planes (x, y) of the support substrate 20, and in particular its diameter, are identical to those of the composite structure 100. It should be noted that, due to the transfer method, the thin layer 10 may have slightly smaller lateral dimensions: in fact, the peripheral ring of the support substrate 20 is usually free of the thin layer 10, since flanges or chamfers at the edges of the substrate 20 would hinder the assembly and effective application of said layer 10.
[0067] In the composite structure 100 , the thickness of the support substrate 20 typically ranges between a few hundred micrometers and about 50 micrometers, for example, between 800 micrometers and 50 micrometers, in particular between 500 micrometers and 60 micrometers, or even between 350 micrometers and 100 micrometers.
[0068] When good vertical conductivity is required (power applications), the support substrate 20 has a resistivity of less than 30 mOhm.cm, 15 mOhm.cm or even less than 10 mOhm.cm. When the thin layer 10 is N-type, the support substrate 20 is usually doped with the same type, typically nitrogen. In order to achieve the aforementioned low resistivity, the nitrogen concentration (which can be measured by secondary ion mass spectrometry) is usually greater than 5E19 atoms / cm 3 , preferably greater than or equal to 1E20 atoms / cm 3 , or even greater than or equal to 1.5E20 atoms / cm 3 .
[0069] When a high resistivity is required for the support substrate (greater than 100 Ohm.cm, or even greater than 10 kOhm.cm, or even greater), the p-SiC support substrate 20 is made from very pure precursors (eg, methyltrichlorosilane) and / or with added impurities (such as vanadium).
[0070] The support substrate 20 made of 3C polytype p-SiC also has a preferred crystal orientation. In this case, the preferred crystal orientation is characterized by specific ratios of various texture coefficients.
[0071] The texture coefficient can be expressed as a percentage, which can quantify the preferred average orientation of the crystallites of the supporting substrate 20 relative to the normal of the surface of the substrate 20. As a reminder, the texture coefficient can be measured by the method described by G. Harris ("X. Quantitative measurement of preferred orientation in rolled uranium bars", Philosophical Magazine Series 7, 43: 336, 113-123, 1952). In practice, the texture coefficient is measured by the diffraction peaks collected by an X-ray diffractometer, which uses the θ-2θ method (2θ scale) in the angle range of 10° to 135°. Within this range, the 3C polytype SiC substrate can be considered in the table ( Figure 2 Ten diffraction peaks are listed and classified according to increasing Miller indices (hkl).
[0072] Texture coefficient C hkl Based on the peak intensity I hkl(which is proportional to the area under the sample peak) and the theoretical strength of the powder, I0 hkl (It can be calculated based on the theoretical percentage published by ICDD (International Center for Diffraction Data). Texture coefficient C hkl It is expressed as follows:
[0073] C hkl =(I hkl / I0 hkl ) / (1 / N xΣ(I hkl / I0 hkl )), where N is the number of peaks considered.
[0074] According to a first alternative embodiment, the preferred crystal orientation of the support substrate 20 is characterized by C 422 The texture coefficient is less than 30% and C 220 The texture coefficient is greater than 60%.
[0075] According to a second alternative embodiment, the preferred crystal orientation of the support substrate 20 is characterized by C 422 The texture coefficient is less than 30%, and C 111 +C 222 +C 511 The fact that the sum of the texture coefficients is greater than 70%.
[0076] Preferably, for any of the alternative embodiments, C 422 The texture factor is less than 20%, less than 15%, or even less than 10%.
[0077] Preferably, according to a second alternative embodiment, C 111 +C 222 +C 511 The sum of the texture coefficients is greater than 80%.
[0078] Figure 3a , 3b 3c show three examples of the texture of the support substrate 20 of the composite structure 100 of the present invention. These images were obtained by scanning electron microscopy (SEM) in the transverse plane (y, z) (i.e., in the cross section of the support substrate 20). Figure 3a and 3b On the right, as an illustration, the texture triangle contains certain facets marked with different white symbols; as an illustration, the symbols are also applied to certain textures in the SEM image. The relevant main texture coefficient percentages are shown in the three Figure 3a , 3b and the right side of the SEM image in 3c.
[0079] The preferred texturing (according to the two alternative embodiments described above) combined with high doping (when vertical conduction is required) allows obtaining a support substrate 20 that meets the desired physical, mechanical and electrical specifications in the composite structure 100, namely:
[0080] -Excellent flatness (low curvature);
[0081] - low resistivity (when required for application and manufacturing of components on the composite structure 100); and
[0082] - Good thermal conductivity (especially in the case of the first mentioned alternative embodiment).
[0083] The radius of curvature of the support substrate 20 is greater than 25 m, advantageously greater than or equal to 50 m. For example, a support substrate 20 with a diameter of 150 mm has a curvature (or "warp") less than or equal to 100 microns, or even 50 microns, while a support substrate 20 with a diameter of 200 mm has a curvature (or "warp") less than or equal to 150 microns, or even 70 microns.
[0084] The radius of curvature of the support substrate 20 is in such a range that the substrate is perfectly compatible with the specifications of the composite structure 100 provided with the single-crystalline thin layer 10, the method for manufacturing such a structure 100, and the subsequent manufacture of microelectronic components on and / or in the thin layer 10. It should be noted that the curvature of the composite structure 100 remains close to the curvature of the support substrate 20.
[0085] According to a specific embodiment of the present invention, the composite structure 100 includes a continuous or discontinuous intermediate layer 30, which is disposed between the thin layer 10 and the supporting substrate 20 and is composed of at least one metal material or semiconductor material ( Figure 4 As described below, with reference to a method for manufacturing the composite structure 100 , the intermediate layer 30 may be formed on one side of the thin layer 10 , one side of the supporting substrate 20 , or both sides before assembly along the bonding interface 40 .
[0086] For example, the intermediate layer 30 may be made of silicon, silicon carbide, tungsten and / or titanium. Its thickness generally ranges between a few nm and several hundred nm, preferably between 2 nm and 50 nm.
[0087] The present invention also relates to a method for producing a composite structure 100 .
[0088] The method comprises a first step a) of providing a support substrate 20 made of polycrystalline silicon carbide having a preferred crystal orientation, wherein:
[0089] -C 422 A texture factor of less than 30%, in particular less than 20%, less than 15% or even less than 10%; and
[0090] -C 220 Texture coefficient greater than 60%, or C 111 +C 222 +C 511 The sum of the texture factors is greater than 70%, in particular greater than 80%.
[0091] Preferably, in order to address power electronics applications, the support substrate 20 has a nitrogen doping such that a resistivity of less than 30 mOhm.cm, 15 mOhm.cm or even less than 10 mOhm.cm is reached.
[0092] The radius of curvature of the support substrate 20 is greater than 25 m, advantageously greater than or equal to 50 m.
[0093] Step a) implements Chemical Vapour Deposition (CVD) technology. This technology involves a gas mixture that includes at least one silicon precursor gas (such as silane or chlorosilane) and / or at least one carbon precursor gas (such as alkane or olefin), and / or at least one silicon and carbon precursor gas (such as methyltrichlorosilane, abbreviated as MTCS) and, if necessary, at least one nitrogen-containing (e.g., NH3, N2H4, N2) doping gas. The doping gas may also be a carbon and / or silicon precursor (e.g., an amine, such as H2NCH3). Such gases may be diluted in a carrier, which may be a reducing gas such as hydrogen and / or an inert gas such as argon.
[0094] This gas mixture enters the reactor at high temperature, where the precursor gases decompose and react on the surface of the seed crystals, which are preferably made of fine-grained and purified isostatic graphite, to form a 3C-SiC polytype whose mechanical and thermal resistance, thermal expansion coefficient and purity are perfectly compatible with the specifications of the composite structure 100. In addition, the 3C-SiC polytype can be doped with very high levels of nitrogen, typically 10 20 Atom / cm 3 , thus exhibiting a resistivity of less than 30 mOhm.cm without degrading the substrate quality, which would be detrimental to the quality of the composite structure and subsequently the performance capabilities of the microelectronic assembly. Finally, it is a material that can withstand the high temperature methods to which the support substrate 20 must be subjected when manufacturing the composite structure 100 and the assembly.
[0095] The reactor temperature during the CVD deposition of SiC should be between about 1000° C. and about 1600° C., preferably between about 1100° C. and about 1400° C. In this temperature range, the deposition rate can vary within a fairly wide range, from 1 micron / hour to more than 100 microns / hour. Advantageously, the total pressure in the reactor does not exceed 350 mbar or even 300 mbar.
[0096] By varying the parameters of the CVD process, such as temperature, partial pressures of the precursors and possibly the percentage of doping gases, the crystal orientation / texture of the deposited p-SiC layer can be varied.
[0097] After deposition, the graphite seeds coated with the thick SiC deposit are machined and subsequently oxidized in air, typically at 900° C., in order to remove any graphite residues. It should be noted that the removal of the graphite seeds can also be performed solely by machining techniques or even essentially by combustion / oxidation.
[0098] A raw p-SiC wafer is recovered from each face of the seed. The raw p-SiC wafer exhibits curvature due to stress release from the deposited layer. This curvature can be measured using a confocal white light sensor that scans the surface of the p-SiC wafer.
[0099] Subsequently, the p-SiC bare wafer is thinned by rough grinding and then fine grinding, and surface treatment is performed by polishing to obtain a p-SiC support substrate 20 having the key features described above when describing the composite structure 100. In particular, the grinding step aims to remove sufficient thickness from the side of the wafer face in contact with graphite. This removes the initial crystal growth area that generates significant stress.
[0100] It is important that the curvature of the p-SiC bare wafer is kept within a reasonable range so that a low-curvature support substrate 20 can be manufactured from a bare wafer with an economically feasible thickness. For example, the curvature ("warp") target of a p-SiC bare wafer with a diameter of 150 mm and a thickness of less than 900 microns is less than or equal to 250 microns. Therefore, after grinding and polishing, a support substrate 20 with a thickness of typically less than 500 microns and a curvature ("warp") of less than 100 microns, or less than 50 microns, or even less than 30 microns can be obtained.
[0101] Figure 6 A table showing various p-SiC deposition conditions (temperature, precursor gas, pressure, mole fraction of doping gas) and the resulting mechanical, electrical and thermal properties is shown. Samples 2, 3 and 4 represent the support substrate 20 of the composite structure 100 of the present invention; their textures are as follows: Figure 3c , 3a and 3b.
[0102] Samples 1 and 5 do not meet the specifications (resistivity, curvature) required to manufacture a high quality composite structure 100 and therefore do not fall within the scope of the present invention. The texture of these samples is not conducive to low curvature, and the grain size on the surface 20a is larger and more non-uniform than that of samples 2, 3 and 4, making it more difficult to prepare their surfaces and obtain the surface finish required for direct assembly.
[0103] The surface 20a ( Figure 5a ) preferably exhibits a roughness of less than or equal to 1 nm RMS (measured by atomic force microscopy with a 20 micron x 20 micron scan), and even more preferably less than or equal to 0.5 nm RMS. The surface of the support substrate 20 intended to form the back side of the composite structure 100 may exhibit a higher surface roughness, for example of the order of 10 nm RMS.
[0104] Step a) of the method may optionally include a heat treatment applied to the support substrate 20 at a temperature greater than or equal to 1500° C., typically between 1500° C. and 2000° C., in order to stabilize the polycrystalline structure. In fact, these temperature ranges are likely to be applied later in the method for manufacturing the composite structure 100.
[0105] The manufacturing method of the invention then comprises a step b) of providing a donor substrate 1 made of a single-crystalline material from which the thin layer 10 is to be obtained ( Figure 5a ). As mentioned above, with reference to the composite structure 100, the single crystal material may be 4H, 6H or 3C polytype silicon carbide, diamond, silicon, II-IV or III-V semiconductor compounds (particularly GaN), etc. The donor substrate 1 is preferably in the form of a wafer having a diameter of 100 mm, 150 mm, 200 mm or even larger (the same as or very close to the diameter of the support substrate 20) and a thickness typically ranging between 300 microns and 800 microns. It has a front side 1a and a back side 1b. The surface roughness of the front side 1a is advantageously selected to be less than 1 nm RMS or even less than 0.5 nm RMS, as measured by atomic force microscopy (AFM) with a scan of 20 microns x 20 microns. The doping type and resistivity of the donor substrate 1 are determined according to the requirements of the components to be manufactured on and / or in the thin layer 10 of the composite structure 100.
[0106] Finally, the method comprises a step c of transferring the thin layer 10 from the donor substrate 1 onto the support substrate 20). Various options for layer transfer are known in the prior art (mechanical, chemical or mechanochemical thinning, separation on the porous layer of the donor substrate 1, etc.) and will not be described in detail here.
[0107] According to a preferred embodiment, step c) of the method involves TM The principle of the method is to inject lightweight elements and assemble them by direct bonding.
[0108] The first step c1) corresponds to introducing a light element into the donor substrate 1 to form a weakened buried surface 11 which delimits, with the front surface 1a of the donor substrate 1, a thin layer 10 to be transferred ( Figure 5b). It should be noted that, although the thin layer 10 to be transferred is shown as a continuous layer, it may also consist of discontinuous areas such as prepared on the surface of the donor substrate 1 .
[0109] The light elements are preferably hydrogen, helium or a combination of these two elements and are implanted at a predetermined depth in the donor substrate 1, consistent with the target thickness of the thin layer 10. These light elements will form microcavities around the predetermined depth, which are distributed in a very thin layer (fine layer) parallel to the free surface 1a of the donor substrate 1 (i.e., parallel to the plane (x, y) in the figure). For simplicity, this very thin layer is called a weakened buried surface 11.
[0110] The implantation energy of the light element is selected so as to reach a predetermined depth. For example, at an energy level in the range of 10 keV to 250 keV and at an energy level in the range of 5 E 16 / cm 2 with 1 E 17 / cm 2 Hydrogen ions are implanted at a dose of between 100 nm and 1500 nm so as to define a thin layer 10 having a thickness of about 100 nm to 1500 nm. It should be noted that, before the ion implantation step, a protective layer may be deposited on the front side 1 a of the donor substrate 1. This protective layer may consist of a material such as silicon oxide or silicon nitride. The protective layer is removed before the next stage.
[0111] Subsequently, the transfer step c) includes a second stage c2), that is, assembling the front side 1a of the donor substrate 1 to the first side 20a of the support substrate 20 along the bonding interface 40 by molecular adhesion bonding ( Figure 5c ).
[0112] Optionally, before or after the stage c1) of introducing the light element, in any case before the assembly stage, an intermediate layer 30 may be formed on the front side 1a of the donor substrate 1. This intermediate layer 30 may be made of a semiconductor material (e.g. silicon or silicon carbide) or a metal material (such as tungsten, titanium, etc.). The thickness of the intermediate layer 30 is advantageously generally limited to between a few nanometers and tens of nanometers.
[0113] In the case where the intermediate layer 30 is formed before the first stage c1), the implantation energy (and possible dose) of the light elements can be adjusted at the intersection of this additional layer. In the case where the intermediate layer 30 is formed after the first stage c1), this layer is formed with care by applying a thermal budget lower than the thermal budget for blistering, which corresponds to the appearance of bubbles on the surface of the donor substrate 1 due to excessive growth and pressurization of the microcavities in the weakened buried surface 11.
[0114] Optionally, before the assembly stage, an intermediate layer 30 may also be deposited on the face of the support substrate 20 to be assembled; it may be chosen to be of the same nature or different nature than the intermediate layer 4 mentioned for the donor substrate 1. The intermediate layer 30 may optionally be deposited on either of the two substrates 1, 10 to be assembled.
[0115] The purpose of one or more intermediate layers is essentially to increase the bonding energy (especially in the temperature range below 1100° C.), due to the formation of covalent bonds at lower temperatures than in the case of two directly assembled SiC surfaces; another advantage of this (these) intermediate layer(s) is that the vertical conductivity of the bonding interface 40 can be improved.
[0116] One or more intermediate layers 30 are expected to be embedded in the bonding assembly 50 after assembly ( Figure 5c ', 5c") and is finally buried in the composite structure 100. Even if the intermediate layer 30 is continuous when it is formed on one and / or the other substrate 1, 20, it may be segmented and have a discontinuous nature during the subsequent heat treatment. This is basically the case when the initial thickness of the layer is very low, typically less than 10 nm.
[0117] With further reference to the description of the assembly stage c2), it is well known that direct molecular adhesion bonding does not require an adhesive material, since the bond is established at the atomic level between the assembled surfaces. There are many types of molecular adhesion bonding, which differ in particular in their temperature conditions, pressure conditions, atmosphere conditions or treatments before the surfaces are brought into contact. One may cite room temperature bonding (with or without prior plasma activation of the surfaces to be assembled), atomic diffusion bonding (ADB), surface activated bonding (SAB), etc.
[0118] The assembly stage c2) may include conventional procedures of chemical cleaning (e.g. RCA cleaning), surface activation (e.g. by oxygen or nitrogen plasma) or other surface treatments (such as cleaning by brushing (scrubbing)) before bringing the surfaces 1a, 20a to be assembled into contact, which may improve the quality of the bonding interface 40 (low defect rate, high adhesion energy).
[0119] Finally, the third phase c3) consists in the separation along the weakened buried surface 11, which results in the thin layer 10 being applied to the supporting substrate 20 ( Figure 5d ).
[0120] The separation along the weakened buried surface 11 is usually carried out by applying a heat treatment in a temperature range between 800° C. and 1200° C. This heat treatment leads to the creation of cavities and microcracks in the weakened buried surface 11, subjecting them to the pressure of light elements present in gaseous form until the cracks are transmitted along the weak plane 11. Alternatively, or together, mechanical stresses can be applied to the bonded components (in particular to the weakened buried surface 11) to transmit or assist the mechanical transmission of the fracture that leads to the separation. After completing this separation, on the one hand, a composite structure 100 including the support substrate 20 and the transferred thin layer 10 is obtained, and on the other hand, the remaining part 1 ' of the donor substrate is obtained. The degree and type of doping of the thin layer 10 are defined by the choice of the properties of the donor substrate 1, or can be subsequently adjusted by known techniques for doping semiconductor layers.
[0121] The free surface 10a of the thin layer 10 is usually rough after separation: for example, its roughness is between 5nm and 100nm RMS. Cleaning and / or smoothing stages can be applied to restore a good surface finish (usually, the roughness is less than a few angstroms RMS). In particular, these stages may include a mechanochemical smoothing treatment of the free surface of the thin layer 20. Removing 50nm to 300nm can effectively restore the surface finish of the layer 10. The stage may also include at least one thermal treatment in the temperature range of 1200°C to 1800°C. This thermal treatment is applied to remove the residual light elements on the thin layer 10 and promote the rearrangement of the crystal lattice of the thin layer 10. It can also strengthen the bonding interface 40. The thermal treatment may also include or correspond to epitaxy on the thin layer 10 to increase its thickness (for example, c-SiC homoepitaxy on the c-SiC thin layer 10, GaN heteroepitaxy on the c-SiC thin layer 10, etc.).
[0122] Finally, it is noted that the transfer step c) may include a reconditioning step of the remaining portion 1' of the donor substrate to serve again as the donor substrate 1 for the new composite structure 100. Mechanical and / or chemical treatments similar to those applied to the composite structure 100 may be applied to the front side 1 of the remaining substrate 1'.
[0123] The resulting composite structure 100 is extremely robust to very high temperature heat treatments that may be used to improve the quality of the thin layer 10 or to fabricate components on and / or in the layer 10. The support substrate 20 in the composite structure 100 is stable and its curvature does not increase excessively during high temperature heat treatments applied to it during and after fabrication of the composite structure 100.
[0124] The composite structure 100 of the present invention is particularly suitable for manufacturing one (or more) high voltage microelectronic components, such as Schottky diodes, MOSFET transistors, etc. More generally, it is suitable for power microelectronic applications, achieving excellent vertical thermal conductivity, good thermal conductivity and providing high quality c-SiC thin layers.
[0125] With a resistive support substrate 20, the composite structure 100 may also be suitable for radio frequency applications, with its physical and potential thermal properties being well suited for fabricating RF electronic components.
[0126] Of course, the invention is not limited to the embodiments and examples that have been described, and other embodiments may be added without departing from the scope of the invention as defined in the claims.
Claims
1. A composite structure (100) for producing a microelectronic component, comprising a single-crystal thin layer (10) arranged on a support substrate (20) made of polycrystalline silicon carbide, the support substrate (20) having a preferred crystal orientation, wherein: -C 422 A texture factor of less than 30%, in particular less than 20%; and -C 220 Texture coefficient greater than 60%, or C 111 +C 222 +C 511 The sum of the texture factors is greater than 70%, in particular greater than 80%.
2. The composite structure (100) according to the preceding claim, wherein: The support substrate (20) has nitrogen doping and a resistivity of less than 30 mOhm.cm.
3. The composite structure (100) according to any one of the preceding claims, wherein: The thin layer (10) is made of silicon carbide.
4. The composite structure (100) according to any one of claims 1 and 2, wherein: The thin layer (10) is made of diamond.
5. A composite structure (100) as claimed in any one of the preceding claims, comprising a continuous or discontinuous intermediate layer (30), which is arranged between the thin layer (10) and the supporting substrate (20) and is composed of at least one metallic material or semiconductor material.
6. The composite structure (100) according to the preceding claim, wherein: The intermediate layer (30) is made of silicon, silicon carbide, tungsten and / or titanium.
7. The composite structure (100) according to any one of the preceding claims, wherein: The C 422 The texture coefficient is less than 15%, or even less than 10%.
8. The composite structure (100) according to any one of the preceding claims, wherein: The thickness of the support substrate (20) is 50 micrometers to 800 micrometers, preferably 60 micrometers to 500 micrometers.
9. A composite structure (100) as claimed in any one of the preceding claims, comprising electronic components on and / or in the thin layer (10) and optionally electrical contacts on the back side of the supporting substrate (20).
10. A method for manufacturing the composite structure (100), the composite structure (100) comprising a single crystal thin layer (10) arranged on a support substrate (20) made of polycrystalline silicon carbide, the manufacturing method comprising the following steps: a) providing a support substrate (20) made of polycrystalline silicon carbide, said support substrate having a preferred crystal orientation, wherein: -C 422 A texture factor of less than 30%, in particular less than 20%; and -C 220 Texture coefficient greater than 60%, or C 111 +C 222 +C 511 The sum of the texture coefficients is greater than 70%, in particular greater than 80%; b) providing a donor substrate (1) made of a single-crystalline material; c) transferring the thin layer (10) from the donor substrate (1) to the support substrate (20).
11. The manufacturing method according to the preceding claim, wherein: The transfer step c) comprises: c1) forming a weakened buried surface (11) in the donor substrate (1) to define the thin layer (10) between the weakened buried surface (11) and the front surface (1a) of the donor substrate (1); c2) assembling the donor substrate (1) onto the support substrate (20) directly or through an intermediate layer (30) by molecular adhesion bonding; c3) separation along the weakened buried surface (11), thereby causing the thin layer (10) to be transferred to the supporting substrate (20).
12. A method of manufacturing as claimed in the preceding claim, wherein: Before assembling the two substrates (1, 20), the step c2) comprises: - before or after step c1), forming an intermediate layer (30) on the donor substrate (1); and / or - forming an intermediate layer (30) on the support substrate (20), The intermediate layer (30) is formed of at least one metal material or semiconductor material selected from silicon, silicon carbide, tungsten and titanium.
13. The manufacturing method according to any one of the two preceding claims, wherein: The single crystal material forming the donor substrate (1) is silicon carbide.
14. The manufacturing method according to any one of claims 10 to 13, further comprising manufacturing electronic components on and / or in the thin layer (10) of the composite structure (100).
15. A method of production as claimed in the preceding claim, wherein: The production of the electronic component comprises in particular a homoepitaxial or heteroepitaxial step on the thin layer (10).
Citation Information
Patent Citations
Polycrystalline SiC substrate and method for manufacturing same
US10934634B2