Resin composition for back surface polishing film substrate, back surface polishing film substrate, and back surface polishing film

The composition of ethylene unsaturated ester copolymer, ethylene alpha-olefin copolymer and styrene-based resin is solved, and high softness and excellent tear properties are achieved. The backside abrasive film reduces chips and milling chips during the grinding process.

CN118922916APending Publication Date: 2024-11-08DOW MITSUI POLYCHEMICALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380026908.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-14
Filing Date
2023-03-08
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing backside abrasive film is insufficient in flexibility and tear, which leads to easy generation of chips and milling chips during the grinding process, resulting in contamination and adverse effects.

Method used

The composition of ethylene·unsaturated ester copolymer, ethylene·α-olefin copolymer and styrene-based resin is used to improve the flexibility and tearability of the backside abrasive film by adjusting its composition ratio and structure.

Benefits of technology

It is achieved to significantly improve the tearability of the back abrasive film while maintaining high flexibility, reduce the generation of chips and milling chips, and improve the quality and efficiency of the grinding process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005037843990000231
    Figure BDA0005037843990000231
Patent Text Reader

Abstract

The resin composition for a back surface polishing film base material comprises: an ethylene unsaturated ester copolymer (A); and at least one selected from the group consisting of an ethylene / alpha-olefin copolymer (B) having a melt flow rate of 0.1 g / 10 minutes or more and less than 25 g / 10 minutes as measured under the conditions of 190 DEG C and a load of 2160 g, and a styrene resin (C). When the total amount of the ethylene-unsaturated ester copolymer (A), the ethylene-alpha-olefin copolymer (B), and the styrene resin (C) is taken as 100 parts by mass, the content of the ethylene-unsaturated ester copolymer (A) is more than 60 parts by mass and less than 100 parts by mass.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a resin composition for a back grinding film substrate, a back grinding film substrate and a back grinding film. Background Art

[0002] In the manufacturing process of semiconductor devices such as ICs, in order to thin the semiconductor wafer formed with a circuit pattern, a back grinding process is usually performed to grind the back side of the semiconductor wafer. In the back grinding process, in order to protect the circuit pattern surface of the semiconductor wafer from contamination and to maintain the thinned semiconductor wafer, an adhesive film (back grinding film) is attached to the circuit pattern surface. In addition, after the back grinding process, a film for wafer processing (dicing film) having elasticity is usually attached to the back side of the ground semiconductor wafer to implement a dicing process to divide the semiconductor wafer into chip units.

[0003] Since a circuit pattern is formed on the surface of the semiconductor wafer, there are bumps and depressions. Therefore, if the softness of the back grinding film is low, a gap is generated between the semiconductor wafer surface and the back grinding film, and the semiconductor wafer and the back grinding film may be peeled off during back grinding. Therefore, in order to closely adhere to the semiconductor wafer even if there are bumps and depressions, the back grinding film is required to have softness (bump and depression followability).

[0004] In addition, after the back grinding process, the back grinding film is peeled off from the surface of the semiconductor wafer. However, if a part of the back grinding film remains on the surface of the semiconductor wafer during the peeling, the semiconductor wafer may be contaminated. The situation where a part of the back grinding film remains on the semiconductor wafer is also called residual adhesive. Therefore, the back grinding film is required to be releasable so that there is no residual adhesive.

[0005] In addition, the back grinding film is also required to be resistant to deformation such as strain and warping (heat shrinkage resistance) due to the frictional heat generated when grinding the semiconductor wafer, the heat applied when the adhesive is applied to the back grinding film substrate, and the heat applied when the grinding chips are washed with water and dried.

[0006] As the back grinding film substrate, ethylene-vinyl acetate copolymer (hereinafter, sometimes abbreviated as EVA) is used as an example from the viewpoints of flexibility, releasability, and resistance to deformation.

[0007] For example, Patent Document 1 describes an adhesive tape for back grinding, which is an adhesive tape for back grinding in which an adhesive layer for bonding and fixing a wafer is provided on a base film, wherein the base film is a single-layer film, and the single-layer film is formed by a mixture of 60 to 98 weight % of one or more ethylene-vinyl acetate copolymer resins having a vinyl acetate content of 15 to 30 weight % and 2 to 40 weight % of one or more polyolefin resins having a melting point of 100° C. or higher. It is also described that such an adhesive tape for back grinding has sufficient flexibility to prevent the wafer from being damaged during the back grinding process of the wafer, and has heat shrinkage resistance that is not easy to shrink even against the heat received in each process.

[0008] In addition, Patent Document 2 describes an adhesive film containing (A) 60 parts by weight of an ethylene-propylene-diene copolymer and (B) 40 parts by weight of an ethylene-vinyl acetate copolymer, which exhibits adhesiveness by heating to a temperature of 50 to 90° C. It is also described that the adhesiveness of such an adhesive film can be increased or decreased depending on the use temperature conditions, and can be easily peeled off by cooling.

[0009] Prior art literature

[0010] Patent Literature

[0011] Patent Document 1: Japanese Patent Application Publication No. 2005-33000

[0012] Patent Document 2: Japanese Patent Application Laid-Open No. 2-129282 Summary of the invention

[0013] Problems to be solved by the invention

[0014] However, due to the high flexibility of EVA, when the back grinding film is cut into the shape of a semiconductor wafer, cuttings and milling chips are sometimes generated. If cuttings and milling chips are generated, the semiconductor wafer may be contaminated or may cause adverse effects in the process after the back grinding process. That is, it is desired to improve the tearing property.

[0015] In contrast, from the viewpoint of film forming properties, the adhesive film of Patent Document 2 has an ethylene-propylene-diene copolymer as a main component, and therefore has insufficient flexibility. In addition, although the base film of Patent Document 1 has EVA as a main component, it contains a polyolefin-based resin with a melting point of 100° C. or higher, and therefore has insufficient flexibility. In addition, these documents do not mention the reduction in tearing properties caused by the high flexibility of EVA.

[0016] The present invention has been made in view of the above problems and has an object to provide a resin composition for a back grinding film substrate, a back grinding film substrate, and a back grinding film capable of realizing a back grinding film substrate having excellent flexibility and excellent tearing properties.

[0017] Means for solving problems

[0018] That is, the present invention provides the following resin composition for a back grinding film substrate.

[0019] [1] A resin composition for a back grinding film substrate, comprising:

[0020] an ethylene·unsaturated ester copolymer (A); and

[0021] At least one selected from the group consisting of an ethylene-α-olefin copolymer (B) having a melt flow rate of 0.1 g / 10 min or more and less than 25 g / 10 min as measured under the conditions of 190° C. and a load of 2160 g according to JIS K 7210:1999, and a styrene resin (C),

[0022] When the total amount of the ethylene-unsaturated ester copolymer (A), the ethylene-α-olefin copolymer (B) and the styrene resin (C) is 100 parts by mass, the content of the ethylene-unsaturated ester copolymer (A) is greater than 60 parts by mass and less than 100 parts by mass.

[0023] [2] The resin composition for a back grinding film substrate according to [1], wherein the content of the structural unit derived from the unsaturated ester in the ethylene-unsaturated ester copolymer (A) is 15% by mass or more and 46% by mass or less.

[0024] [3] A resin composition for a back grinding film substrate as described in [1] or [2], wherein the melt flow rate of the ethylene-unsaturated ester copolymer (A) measured at 190°C and a load of 2160 g in accordance with JIS K 7210:1999 is from 0.1 g / 10 min to 100 g / 10 min.

[0025] [4] The resin composition for a back grinding film substrate according to any one of [1] to [3], wherein the melting point of the ethylene / α-olefin copolymer (B) is lower than 100°C.

[0026] [5] A resin composition for a back grinding film substrate as described in any one of [1] to [4], wherein the melt flow rate of the styrene resin (C) measured at 190°C and a load of 2160 g in accordance with JIS K 7210:1999 is 0.01 g / 10 min or more and 50 g / 10 min or less.

[0027] [6] The resin composition for a back grinding film substrate according to any one of [1] to [5], wherein the styrene-based resin (C) is a styrene-based elastomer.

[0028] [7] A resin composition for a back grinding film substrate as described in any one of [1] to [6], wherein, when the total amount of the resin composition for the back grinding film is set to 100 mass%, the total amount of the aforementioned ethylene·unsaturated ester copolymer (A), the aforementioned ethylene·α-olefin copolymer (B) and the styrene resin (C) is more than 70 mass% and less than 100 mass%.

[0029] [8] The resin composition for a back grinding film substrate according to any one of [1] to [7], wherein the ethylene-unsaturated ester copolymer (A) is an ethylene-vinyl acetate copolymer.

[0030] The present invention provides the following back grinding film substrate and back grinding film.

[0031] [9] A back grinding film substrate having at least one layer comprising the resin composition for a back grinding film substrate according to any one of [1] to [8].

[0032]

[10] The back grinding film substrate according to [9], wherein the initial value of the hardness (Shore A) of the layer comprising the resin composition for back grinding film substrate measured in accordance with JIS K 7215:1996 is 75 or less.

[0033]

[11] A back grinding film substrate as described in [9] or

[10] , wherein the hardness (Shore A) of the layer comprising the resin composition for the back grinding film substrate measured in accordance with JIS K 7215:1996 is 72 or less 15 seconds after the start of the measurement.

[0034]

[12] A back grinding film comprising: the back grinding film substrate according to any one of [9] to

[11] ; and an adhesive layer laminated on at least one surface of the back grinding film substrate.

[0035] Effects of the Invention

[0036] According to the resin composition for a back grind film substrate of the present invention, a back grind film substrate having excellent flexibility and excellent tearing properties can be realized. DETAILED DESCRIPTION

[0037] In this specification, the numerical range expressed by "to" means a range including the numerical values ​​before and after "to" as the lower limit and the upper limit. In addition, "(meth)acrylic acid" is an expression used to include both "acrylic acid" and "methacrylic acid", and "(meth)acrylate" is an expression used to include both "acrylate" and "methacrylate".

[0038] 1. About the resin composition for back grinding film substrate

[0039] The resin composition for a back grinding film substrate of the present invention (hereinafter, also simply referred to as "resin composition") is mainly used for a back grinding film substrate, but the application of the resin composition is not limited to the back grinding film substrate.

[0040] As described above, the substrate of the back grinding film is required to have not only flexibility to follow the irregularities of the semiconductor wafer surface but also improved tearing properties to prevent chips and milling chips from being generated when the substrate is cut into the shape of a semiconductor wafer.

[0041] In this regard, the inventors of the present application conducted in-depth research and found that the following resin composition has softness and can improve tear resistance, and the resin composition comprises:

[0042] an ethylene·unsaturated ester copolymer (A); and

[0043] At least one selected from an ethylene-α-olefin copolymer (B) having a melt flow rate of 0.1 g / 10 min or more and less than 25 g / 10 min as measured at 190° C. and a load of 2160 g, and a styrene-based resin (C),

[0044] The content of the ethylene-unsaturated ester copolymer (A) is more than 60 parts by mass and less than 100 parts by mass, based on 100 parts by mass of the total amount of the ethylene-unsaturated ester copolymer (A), the ethylene-α-olefin copolymer (B) and the styrene resin (C).

[0045] The reasons are as follows. That is, ethylene-unsaturated ester copolymers (A) such as EVA have high flexibility, so when the layer of the resin composition containing it is cut into the shape of a semiconductor wafer, it is easy to produce chips, milling chips, etc. On the contrary, the ethylene-α-olefin copolymer (B) with a low melt flow rate and the styrene resin (C) with a relatively rigid structure are well compatible with the ethylene-unsaturated ester copolymer (A) and can give the resin composition a moderate strength. It is believed that the high flexibility from the ethylene-unsaturated ester copolymer (A) can be maintained, and the tearing property can be improved, and the generation of chips and milling chips when cut into a specified shape can be suppressed.

[0046] As described above, the resin composition according to the present application comprises: an ethylene·unsaturated ester copolymer (A); and at least one selected from an ethylene·α-olefin copolymer (B) and a styrene-based resin (C).

[0047] In the above resin composition, when the total amount of the ethylene·unsaturated ester copolymer (A), the ethylene·α-olefin copolymer (B) and the styrene resin (C) is set to 100 parts by mass, the content of the ethylene·unsaturated ester copolymer (A) is greater than 60 parts by mass and less than 100 parts by mass, preferably 65 parts by mass or more and 95 parts by mass or less, more preferably 70 parts by mass or more and 90 parts by mass or less, and further preferably 75 parts by mass or more and 85 parts by mass or less. If the content of the ethylene·unsaturated ester copolymer (A) is greater than the lower limit, it is easy to further improve the softness of the resin composition, and if it is less than the upper limit, it is not easy to damage the tearing property of the resin composition.

[0048] In the above resin composition, when the total amount of the ethylene·unsaturated ester copolymer (A), the ethylene·α-olefin copolymer (B), and the styrene resin (C) is set to 100 parts by mass, the total amount of the ethylene·α-olefin copolymer (B) and the styrene resin (C) is greater than 0 parts by mass and less than 40 parts by mass, preferably 5 parts by mass to 35 parts by mass, more preferably 10 parts by mass to 30 parts by mass, and further preferably 15 parts by mass to 25 parts by mass. If the total amount of the ethylene·α-olefin copolymer (B) and the styrene resin (C) is greater than the lower limit, the tearing property of the resin composition is easily further improved, and if it is less than the upper limit, the flexibility of the resin composition is not easily impaired.

[0049] The total amount of the ethylene·unsaturated ester copolymer (A), the ethylene·α-olefin copolymer (B) and the styrene resin (C) in the above-mentioned resin composition is not particularly limited. When the resin composition as a whole is set to 100 mass%, it is preferably from 70 mass% to 100 mass%, more preferably from 80 mass% to 100 mass%, further preferably from 90 mass% to 100 mass%, particularly preferably from 95 mass% to 100 mass%, particularly preferably from 98 mass% to 100 mass%, and extremely preferably from 99 mass% to 100 mass%.

[0050] Hereinafter, each component contained in the resin composition will be described, and then the physical properties of the resin composition will be described.

[0051] <Ethylene-unsaturated ester copolymer (A)>

[0052] The ethylene-unsaturated ester copolymer (A) is a polymer obtained by copolymerizing ethylene and an unsaturated ester.

[0053] Examples of unsaturated esters include vinyl esters such as vinyl acetate, vinyl propionate, vinyl butyrate, and vinyl stearate; and unsaturated carboxylic acid esters such as alkyl (meth)acrylates. Among them, vinyl esters are preferred, and vinyl acetate is more preferred.

[0054] That is, the ethylene-unsaturated ester copolymer (A) is preferably, for example, an ethylene-vinyl acetate copolymer, an ethylene-vinyl propionate copolymer, an ethylene-vinyl butyrate copolymer, or an ethylene-vinyl stearate copolymer, and more preferably an ethylene-vinyl acetate copolymer.

[0055] The content of the structural unit of ethylene·unsaturated ester copolymer (A) and from ethylene is preferably 54% by mass or less and 85% by mass or less relative to all structural units of ethylene·unsaturated ester copolymer (A), more preferably 58% by mass or less and 80% by mass or less, further preferably 62% by mass or less and 74% by mass or less, especially preferably 65% ​​by mass or less and 72% by mass or less, especially preferably 66% by mass or less and 69% by mass or less. If the content of the structural unit from ethylene is above the lower limit, the resin composition will not become too soft, and therefore it is easy to further suppress stickiness, residual glue, etc. If the content of the structural unit from ethylene is below the upper limit, it is not easy to damage the flexibility of the resin composition.

[0056] The content of the structural unit from the unsaturated ester of the ethylene·unsaturated ester copolymer (A) is preferably 15% by mass or more and 46% by mass or less, more preferably 20% by mass or more and 42% by mass or less, further preferably 26% by mass or more and 38% by mass or less, especially preferably 28% by mass or more and 35% by mass or less, and particularly preferably 31% by mass or more and 34% by mass or less. If the content of the structural unit from the unsaturated ester is above the lower limit, it is easy to further improve the flexibility of the resin composition, and it is easy to further improve the uneven tracking property when used as the substrate of the back grinding film. If the content of the structural unit from the unsaturated ester is below the upper limit, it is easy to further suppress the stickiness, residual glue, etc. of the resin composition.

[0057] The ethylene-unsaturated ester copolymer (A) may further contain a structural unit derived from other monomers in addition to ethylene and unsaturated esters. Examples of such other monomers include olefins such as propylene, butene, and hexene.

[0058] The melt flow rate of the ethylene-unsaturated ester copolymer (A), measured at 190°C and a load of 2160 g according to JIS K 7210:1999, is preferably from 0.1 g / 10 min to 100 g / 10 min, more preferably from 1 g / 10 min to 70 g / 10 min, further preferably from 15 g / 10 min to 50 g / 10 min, and particularly preferably from 25 g / 10 min to 35 g / 10 min. If the melt flow rate of the ethylene-unsaturated ester copolymer (A) is at least the lower limit, the flexibility of the resin composition can be further improved, and the unevenness tracking property when used as a substrate of a back grinding film can be further improved. If the melt flow rate of the ethylene-unsaturated ester copolymer (A) is at most the upper limit, the stickiness and adhesive residue of the resin composition can be further suppressed.

[0059] The ethylene-unsaturated ester copolymer (A) may be used alone or in combination of two or more.

[0060] The method for producing the ethylene-unsaturated ester copolymer (A) according to the present embodiment is not particularly limited, and can be produced by a known method. For example, it can be obtained by subjecting each polymer component to free radical copolymerization at high temperature and high pressure. In addition, the ethylene-unsaturated ester copolymer (A) can use commercially available materials.

[0061] <Ethylene·α-olefin copolymer (B)>

[0062] The ethylene·α-olefin copolymer (B) is a copolymer of ethylene and an α-olefin having 3 or more carbon atoms.

[0063] As the α-olefin, an α-olefin having 3 to 20 carbon atoms is preferred. Examples of the α-olefin having 3 to 20 carbon atoms include linear α-olefins such as propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, 1-tridecene, 1-tetradecene, 1-pentadecene, 1-hexadecene, 1-heptadecene, 1-octadecene, 1-nonadecene, and 1-eicosene; and branched α-olefins such as 3-methyl-1-butene, 3-methyl-1-pentene, 4-methyl-1-pentene, 2-ethyl-1-hexene, and 2,2,4-trimethyl-1-pentene. These may be used alone or in combination of two or more. Among them, the α-olefin preferably has 3 to 10 carbon atoms from the viewpoint of versatility (cost, mass productivity, or availability), and more preferably has 4 to 8 carbon atoms from the viewpoint of less likely to reduce the flexibility of the resin composition.

[0064] The ethylene·α-olefin copolymer (B) is preferably an ethylene·propylene copolymer, an ethylene·1-butene copolymer, an ethylene·4-methyl-1-pentene copolymer, an ethylene·1-hexene copolymer, or an ethylene·1-octene copolymer. From the viewpoint of better maintaining the flexibility of the resin composition, an ethylene·1-butene copolymer is more preferred.

[0065] When the content of all structural units constituting the ethylene·α-olefin copolymer (B) is set to 100 mass%, the content of the structural unit derived from the α-olefin is preferably 5 mass% or more and less than 50 mass%, more preferably 10 mass% or more and 40 mass% or less, and more preferably 10 mass% or more and 30 mass% or less. If the content of the structural unit derived from the α-olefin is within the above range, the flexibility of the resin composition is less likely to be impaired.

[0066] The melt flow rate of the ethylene α-olefin copolymer (B) measured under the conditions of 190°C and a load of 2160 g according to JIS K 7210:1999 is 0.1 g / 10 min or more and less than 25 g / 10 min, preferably 0.3 g / 10 min or more and 15 g / 10 min or less, more preferably 0.5 g / 10 min or more and 10 g / 10 min or less, and further preferably 0.7 g / 10 min or more and 5 g / 10 min or less. If the melt flow rate of the ethylene α-olefin copolymer (B) is above the lower limit, the flexibility of the resin composition is not easily impaired. If the melt flow rate of the ethylene α-olefin copolymer (B) is below the upper limit, appropriate strength can be imparted to the resin composition, so it is easy to further improve the tearing property.

[0067] The density of the ethylene / α-olefin copolymer (B) measured in accordance with JIS K7112:1999 is preferably 840 kg / m 3 Above 930kg / m 3 Below, more preferably 850kg / m 3 Above 910kg / m 3 Below, especially preferably 860kg / m 3 Above 890kg / m 3 Below, particularly preferably 865kg / m 3 Above 880kg / m 3 the following.

[0068] The melting point of the ethylene·α-olefin copolymer (B) is preferably less than 100°C, more preferably 90°C or less, further preferably 80°C or less, and particularly preferably 70°C or less. If the melting point of the ethylene·α-olefin copolymer (B) is within the above range, the softness of the resin composition is well maintained and the tear resistance is easily further improved. The melting point of the ethylene·α-olefin copolymer (B) can be measured, for example, using a differential scanning calorimeter (DSC) in accordance with JIS K 7121 (1987).

[0069] The melting point of the ethylene·α-olefin copolymer (B) can be adjusted, for example, by the type and content of the α-olefin. For example, the melting point of the ethylene·α-olefin copolymer (B) is more likely to be lowered as the number of carbon atoms of the α-olefin constituting the ethylene·α-olefin copolymer (B) and the content thereof are greater.

[0070] The ethylene·α-olefin copolymer (B) may be used alone or in combination of two or more.

[0071] <Styrene resin (C)>

[0072] As long as the styrene resin (C) is a resin having at least styrene as a structural unit, it can be a homopolymer of styrene or a polymer of styrene and other monomers. Examples of styrene resins (C) include styrene elastomers, ABS resins as copolymers of acrylonitrile and styrene, polystyrene, etc. Among these, styrene elastomers are preferred. Styrene elastomers refer to styrene polymers that are rubber elastomers at room temperature.

[0073] Examples of styrene-based elastomers include: block copolymers comprising a hard segment formed by a styrene block (styrene polymer) and a soft segment formed by an alkylene block, or their hydrogenates; random copolymers of styrene and an alkylene group, or their hydrogenates; or acid-modified styrene-based elastomers obtained by acid-modifying the styrene-based elastomer, etc.

[0074] The styrene block in the block copolymer may be a site formed by polymerizing two or more styrenes, and the alkylene block may be a site formed by polymerizing two or more olefins. The alkylene block may be a homopolymer of one olefin or a copolymer of two or more olefins.

[0075] Examples of the above block copolymers include styrene-butadiene block copolymers (SB), styrene-butadiene-styrene block copolymers (SBS), styrene-isoprene block copolymers (SI), and styrene-isoprene-styrene block copolymers (SIS).

[0076] As described above, the styrene-based elastomer may be a hydrogenated product of the block copolymer. In the hydrogenated product, both the styrene block and the alkylene block may be hydrogenated, or only one of the styrene block and the alkylene block may be hydrogenated, or only a part of the styrene block and the alkylene block may be hydrogenated.

[0077] Examples of hydrogenated products of the above block copolymers include: styrene-ethylene·butylene block copolymer (SEB) which is a hydrogenated product of styrene-butadiene block copolymer (SB); styrene-ethylene·butylene-styrene block copolymer (SEBS) which is a hydrogenated product of styrene-butadiene-styrene block copolymer (SBS); styrene-ethylene·propylene-styrene block copolymer (SEPS) which is a hydrogenated product of styrene-isoprene-styrene block copolymer (SIS), etc.

[0078] As mentioned above, examples of styrene-based elastomers also include random copolymers of styrene and alkylene. Examples thereof include styrene-butadiene random copolymers, styrene-isoprene random copolymers, styrene-ethylene-butylene random copolymers, styrene-ethylene-propylene random copolymers, styrene-isobutylene random copolymers, styrene-ethylene-isoprene random copolymers, etc.

[0079] As described above, the styrene-based elastomer may be a hydrogenated product of the above-mentioned random copolymer, and examples thereof include a hydrogenated product of a styrene-butadiene random copolymer (HSBR) and the like.

[0080] Among the styrene-based elastomers that have not been acid-modified, hydrogenated products are preferred among the above, and styrene-ethylene·butylene-styrene block copolymers (SEBS) and styrene-ethylene·propylene-styrene block copolymers (SEPS) are more preferred. From the perspective of being able to provide good tear properties without damaging the flexibility of the substrate of the back grinding film obtained from the resin composition, styrene-ethylene·butylene-styrene block copolymers (SEBS) are particularly preferred.

[0081] On the other hand, the styrene-based elastomer may be an acid-modified styrene-based elastomer obtained by graft-modifying an elastomer formed from the block copolymer or random copolymer or a hydrogenated product thereof with an unsaturated carboxylic acid or a derivative thereof as described above. The acid-modified styrene-based elastomer may be a product obtained by graft-modifying an elastomer formed from the block copolymer or random copolymer or a hydrogenated product thereof with one unsaturated carboxylic acid or a derivative thereof, or may be a product obtained by graft-modifying an elastomer formed from the block copolymer or random copolymer or a hydrogenated product thereof with two or more unsaturated carboxylic acids or derivatives thereof.

[0082] Examples of unsaturated carboxylic acids used in graft modification include (meth) acrylic acid, 2-ethyl acrylic acid, crotonic acid, maleic acid, fumaric acid, itaconic acid, and the like. On the other hand, examples of unsaturated carboxylic acid derivatives used in graft modification include anhydrides such as maleic anhydride, phthalic anhydride, and itaconic anhydride; acid esters such as monomethyl maleate and monoethyl maleate; amides; acid halides; and the like. Among these, maleic acid or maleic anhydride is preferred from the viewpoint of reactivity with styrene elastomers.

[0083] The acid-modified styrene-based elastomer is obtained by graft-polymerizing an unsaturated carboxylic acid or a derivative thereof to the above block copolymer, random copolymer, etc. in the presence of a radical initiator. The radical initiator may be any initiator for graft reaction of polyolefin, and a known compound may be used.

[0084] The acid value of the acid-modified styrene elastomer is preferably greater than 0 mgCH3ONa / g and less than 20 mgCH3ONa / g, more preferably greater than 0 mgCH3ONa / g and less than 11 mgCH3ONa / g, and further preferably from 0.5 mgCH3ONa / g to 11 mgCH3ONa / g.

[0085] In addition, examples of styrene resins (C) also include ABS resins. ABS resins are resins containing structural units derived from acrylonitrile and structural units derived from styrene, and examples thereof include rubber-reinforced styrene polymers synthesized by various manufacturing methods such as blending, grafting, or grafting and blending. Specific examples of ABS resins include materials obtained by grafting styrene and acrylonitrile, and other monomers such as methyl methacrylate, α-methylstyrene, ethylene bismaleimide, and maleimide added as needed onto rubber components such as polybutadiene, styrene-butadiene rubber, and ethylene-propylene-diene rubber.

[0086] Examples of styrene resins (C) also include polystyrenes obtained by polymerizing styrene. Examples of polystyrenes include general-purpose polystyrenes synthesized by production methods such as suspension polymerization and continuous polymerization, and impact-resistant polystyrenes obtained by graft polymerization of styrene onto rubber components such as butadiene rubber.

[0087] The content of the structural unit from styrene is relative to all structural units of styrene resin (C), preferably 1 mass % or more and 85 mass % or less, more preferably 5 mass % or more and 75 mass % or less, and further preferably 5 mass % or more and 65 mass % or less. If the content of the structural unit from styrene is more than the lower limit, it is easy to give appropriate intensity to the resin combination, so it is easy to further improve tearing property. If the content of the structural unit from styrene is below the upper limit, it is not easy to damage the flexibility of the resin combination.

[0088] The melt flow rate of the styrene resin (C) measured at 190°C and a load of 2160 g according to JIS K 7210:1999 is preferably 0.01 g / 10 min to 50 g / 10 min, more preferably 0.1 g / 10 min to 10 g / 10 min, and further preferably 0.2 g / 10 min to 5 g / 10 min. In addition, the melt flow rate measured at 230°C and a load of 2160 g according to JIS K 7210:1999 is preferably 0.1 g / 10 min to 100 g / 10 min, more preferably 0.3 g / 10 min to 50 g / 10 min, and further preferably 0.5 g / 10 min to 15 g / 10 min. When the melt flow rate of the styrene resin (C) is at least the lower limit, the flexibility of the resin composition is not easily impaired. When the melt flow rate of the styrene resin (C) is equal to or less than the upper limit value, appropriate strength can be easily imparted to the resin composition, and therefore the tearing property can be easily further improved.

[0089] The styrene-based resin (C) may be used alone or in combination of two or more.

[0090] <Other polymers and additives>

[0091] The resin composition may contain other polymers, various additives, tackifier resins, antistatic agents, ultraviolet absorbers, fillers, etc. in addition to the above-mentioned ethylene·unsaturated ester copolymer (A) and ethylene·α-olefin copolymer (B) as needed within the range not impairing the effects of the present invention.

[0092] Examples of other polymers include polyolefins such as polyethylene and polypropylene. The amount of other polymers in the resin composition is preferably 30 parts by mass or less, more preferably 20 parts by mass or less, relative to 100 parts by mass of the total of the ethylene·unsaturated ester copolymer (A), the ethylene·α-olefin copolymer (B) and the styrene resin (C).

[0093] On the other hand, examples of additives include antioxidants, heat stabilizers, light stabilizers, pigments, dyes, lubricants, anti-blocking agents, mildew inhibitors, antibacterial agents, flame retardants, flame retardant aids, crosslinking agents, crosslinking aids, foaming agents, foaming aids, fiber reinforcement materials, etc.

[0094] As the tackifier resin, a hydrocarbon resin selected from the group consisting of aliphatic hydrocarbon resins, alicyclic hydrocarbon resins, and coumarone-indene resins, or a terpene resin is preferably used.

[0095] When the resin composition contains a tackifier resin, when the total amount of the ethylene-unsaturated ester copolymer (A) and the tackifier resin is set to 100 parts by mass, the content of the tackifier resin is preferably 4 parts by mass or less, more preferably 3 parts by mass or less, further preferably 2 parts by mass or less, and particularly preferably 0.1 parts by mass or less.

[0096] In addition, when the total amount of the ethylene-unsaturated ester copolymer (A), the styrene resin (C) and the tackifier resin is set to 100 parts by mass, the content of the tackifier resin is preferably 2 parts by mass or less, more preferably 1 part by mass or less, further preferably 0.5 parts by mass or less, and particularly preferably 0.1 parts by mass or less.

[0097] In addition, the example of antistatic agent includes low molecular antistatic agent, polymer antistatic agent, preferably polymer antistatic agent. The example of polymer antistatic agent includes vinyl copolymer, alkyl sulfonate, alkyl benzene sulfonate, betaine etc. having sulfonate in molecule. In addition, other examples of polymer antistatic agent also include salt of inorganic protonic acid of polyether, polyamide elastomer, polyester elastomer, polyether amide or polyether ester amide etc. As salt of inorganic protonic acid, alkali metal salt, alkaline earth metal salt, zinc salt or ammonium salt can be enumerated.

[0098] Examples of the ultraviolet absorber include benzophenone-based, benzoate-based, benzotriazole-based, cyanoacrylate-based, hindered amine-based, and the like.

[0099] Examples of filler materials include silica, clay, calcium carbonate, barium sulfate, glass beads, talc, and the like.

[0100] The amounts of additives, antistatic agents, ultraviolet absorbers, and fillers are appropriately selected depending on their types.

[0101] <Method for producing resin composition and physical properties of resin composition>

[0102] The method for producing the resin composition of the present invention is not particularly limited as long as it is a method that can mix the ethylene-unsaturated ester copolymer (A), the ethylene-α-olefin copolymer (B), the styrene resin (C) and other polymers and additives added as needed. For example, all the components may be dry-blended and then melt-kneaded, or a part of the components may be kneaded first and then the subsequent components may be added.

[0103] The shape of the resin composition after kneading is not particularly limited, and it may be in the form of pellets, or in the form of long strips or single sheets.

[0104] As described above, the resin composition has high flexibility derived from the ethylene-unsaturated ester copolymer (A). Specifically, the initial value of the hardness (Shore A) of the layer containing the resin composition measured according to JIS K 7215:1996 is not particularly limited, but is preferably 75 or less, more preferably 73 or less, and further preferably 71 or less.

[0105] The hardness (Shore A) of the layer containing the resin composition measured in accordance with JIS K 7215:1996 after 15 seconds from the start of the measurement is not particularly limited, but is preferably 72 or less, more preferably 69 or less, and further preferably 67 or less. If the initial value and the value after 15 seconds of the hardness (Shore A) of the layer containing the resin composition are each within the above range, the layer containing the resin composition has higher flexibility, so when used as a substrate of a back grinding film, the unevenness tracking property becomes better.

[0106] The hardness (Shore A) of the layer containing the resin composition can be adjusted, for example, by the types of the ethylene·unsaturated ester copolymer (A), the ethylene·α-olefin copolymer (B), and the styrene resin (C), the melt flow rate, and their composition ratio. For example, if the content of the structural unit derived from the unsaturated ester in the ethylene·unsaturated ester copolymer (A) is increased, or the melt flow rate is increased, the hardness of the layer containing the resin composition is likely to decrease. In addition, if the relative content of the ethylene·unsaturated ester copolymer (A) is increased, or the melt flow rate is increased, the hardness of the layer containing the resin composition is likely to decrease.

[0107] The melt flow rate of the layer containing the resin composition, measured under the conditions of 190°C and a load of 2160 g according to JIS K 7210:1999, is not particularly limited, and is preferably, for example, 0.1 g / 10 minutes to 100 g / 10 minutes, more preferably 1 g / 10 minutes to 70 g / 10 minutes, further preferably 5 g / 10 minutes to 50 g / 10 minutes, and particularly preferably 10 g / 10 minutes to 40 g / 10 minutes. If the melt flow rate of the layer containing the resin composition is within the above range, not only the moldability is good, but also the flexibility and tearing properties are further improved.

[0108] The tear strength of the layer containing the resin composition in the MD direction (Machine Direction) and the TD direction (Transverse Direction) per 1 mm thickness is preferably 20 N / mm or less, more preferably 15 N / mm or less. If the tear strength of the layer containing the resin composition is within the above range, it has good tearing properties, so when used as a substrate for a back grinding film, it is easy to cut into the shape of a semiconductor wafer, and chips, milling chips, etc. are also less likely to be generated.

[0109] The tear strength can be measured by the following procedure.

[0110] Using a tape casting machine, the resin composition is tape cast at a processing temperature of 200°C to prepare a 250μm thick film. The obtained film is cut into a size of 150mm×50mm, and a 75mm incision is made from the center of the 50mm width along the length direction. Using Autograph, under the conditions of a distance between chucks of 75mm and a speed of 1000mm / min, the sample with the incision is torn up and down to find its average strength. Then, the average strength is divided by the thickness measurement value of the sample, and the strength per 1mm thickness (unit is N / mm) is calculated as the tear strength.

[0111] The tear strength of the layer containing the resin composition can be adjusted, for example, by the type, melt flow rate, content, etc. of the ethylene α-olefin copolymer (B) and the styrene resin (C). For example, if the content of the ethylene α-olefin copolymer (B) or the styrene resin (C) is increased or the melt flow rate is decreased, the tear strength of the layer containing the resin composition is easily reduced, and the tear property becomes better.

[0112] 2. About back grinding film substrate

[0113] The back grinding film substrate can be any substrate having at least one layer of the above-mentioned layer containing the resin composition. The back grinding film substrate has the above-mentioned layer containing the resin composition, so it has excellent flexibility and tearing properties. The back grinding film substrate is suitable for use as a substrate for a back grinding film, but is not limited to this use.

[0114] The structure of the back grinding film substrate is not particularly limited, and the back grinding film substrate may have only one layer containing the resin composition, or may have two or more layers containing the resin composition. In addition, other resin layers may be laminated as needed.

[0115] Examples of the back grinding film substrate include: a laminate having a one-layer structure consisting only of the above-mentioned layer containing the resin composition; a laminate having a two-layer structure consisting of the above-mentioned layer containing the resin composition and other resin layers; a laminate having a three-layer structure consisting of the above-mentioned layer containing the resin composition / other resin layer / the above-mentioned layer containing the resin composition, etc. In addition, the back grinding film substrate may include a layer containing an adhesive, an adhesive sheet, etc. in addition to the above.

[0116] Here, the above-mentioned layer containing the resin composition may be a layer formed only by the above-mentioned resin composition, or may be a layer comprising the above-mentioned resin composition and other components added within the scope that does not impair the purpose and effect of the present invention. From the viewpoint of the softness and tear resistance of the back grinding film substrate, it is preferably a layer substantially formed by the above-mentioned resin composition.

[0117] The thickness of the above-mentioned layer containing the resin composition is not particularly limited. From the perspective of improving the retention and heat shrinkage resistance of the semiconductor chip brought about by the back grinding film substrate, it is preferably moderately thick, preferably from 50 μm to 500 μm, and more preferably from 60 μm to 400 μm.

[0118] The initial value and the value after 15 seconds of the hardness (Shore A) of the layer containing the resin composition measured in accordance with JIS K 7215: 1996 are preferably as described above. The tear strength of the layer containing the resin composition in the MD direction and the TD direction per 1 mm thickness is also preferably as described above.

[0119] On the other hand, examples of other resin layers include layers containing linear low-density polyethylene (LLDPE), low-density polyethylene (LDPE), ethylene·α-olefin copolymer, polypropylene, ethylene·unsaturated carboxylic acid copolymer or its ionomer, ethylene·unsaturated carboxylic acid·unsaturated carboxylic acid alkyl ester terpolymer or its ionomer, ethylene·unsaturated carboxylic acid alkyl ester copolymer, ethylene·vinyl ester copolymer, ethylene·unsaturated carboxylic acid alkyl ester·carbon monoxide copolymer, unsaturated carboxylic acid grafts thereof, polyvinyl chloride, etc. Other resin layers may contain only one of these resins, or may contain two or more of them.

[0120] The thickness of the other resin layer is not particularly limited, but is preferably 10 μm to 100 μm, more preferably 15 μm to 80 μm, from the viewpoint of not impairing the flexibility and tear properties of the layer containing the resin composition.

[0121] Here, the thickness of the back grinding film substrate as a whole is preferably 50 μm or more from the viewpoint of improving the retention and heat shrinkage resistance of the semiconductor wafer during back grinding, and preferably 600 μm or less from the viewpoint of improving the unevenness followability of the circuit surface of the semiconductor wafer, if it is considered that it is used as a component of the back grinding film. Among them, the thickness of the back grinding film substrate as a whole is more preferably 60 μm or more and 480 μm or less.

[0122] The surface of the back grinding film substrate may be subjected to various treatments, for example, corona treatment, etc. Alternatively, electron beam irradiation may be performed.

[0123] The manufacturing method of the back grinding film substrate is not particularly limited, and it can be manufactured by a known molding method. For example, in the case of manufacturing a back grinding film substrate formed only by the above-mentioned layer containing the resin composition, the above-mentioned resin composition can be molded by using a conventionally known T-die casting molding method, a T-die roll molding method, an inflation molding method, an extrusion lamination method, a calendering molding method, etc.

[0124] On the other hand, in the case where the back grinding film substrate is a laminate of the above-mentioned layer containing the resin composition and other resin layers, the above-mentioned resin composition and other resins can be molded by co-extrusion lamination method or the like. In addition, the above-mentioned layer containing the resin composition and other resin layers can be made separately and independently, and they can be bonded together by adhesives, adhesive sheets, etc. Examples of materials of adhesives and adhesive sheets include various ethylene copolymers, or their unsaturated carboxylic acid grafts, etc. In addition, in the case where the back grinding film substrate is a laminate of the above-mentioned layer containing the resin composition and other resin layers, any one of the above-mentioned layer containing the resin composition and other resin layers can be formed first, and another layer can be formed on this layer by using a T-die film molding machine, an extrusion coating molding machine, etc., so as to be laminated.

[0125] 3. About back grinding film

[0126] The back grinding film of the present invention only needs to have the above-mentioned back grinding film substrate and an adhesive layer laminated on at least one side thereof, and may include other structures as required. It should be noted that when the above-mentioned back grinding film substrate includes multiple layers, it is preferred that the layer containing the resin composition in the back grinding film substrate is laminated with the adhesive layer.

[0127] The adhesive constituting the adhesive layer may be an adhesive used for the adhesive layer of a conventional back grinding film. Examples of the adhesive include: rubber-based, acrylic-based, silicone-based, and polyvinyl ether-based adhesives; radiation-curable adhesives; and heat-foamable adhesives. Among them, in consideration of the releasability of the back grinding film from the semiconductor wafer, the adhesive layer preferably includes a radiation-curable adhesive, and more preferably includes an ultraviolet-curable adhesive.

[0128] UV-curable adhesives generally contain a radically polymerizable compound (which may be any monomer, oligomer, or polymer) capable of free radical polymerization and a photopolymerization initiator, and may also contain additives such as a crosslinking agent, a tackifier, a filler, an anti-aging agent, a colorant, etc. as required.

[0129] Examples of free radical polymerizable compounds include: monomers or oligomers of alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, and isononyl (meth)acrylate; monomers or oligomers of hydroxyalkyl (meth)acrylates such as hydroxyethyl (meth)acrylate, hydroxybutyl (meth)acrylate, and hydroxyhexyl (meth)acrylate; copolymers of the above alkyl (meth)acrylates and / or hydroxyalkyl (meth)acrylates with other monomers (e.g., (meth)acrylic acid, itaconic acid, maleic anhydride, (meth)acrylamide, N-hydroxymethyl (meth)acrylate, alkylamino (meth)acrylate ester monomers formed by (meth)acrylic acid and polyols such as glycidyl (meth)acrylate trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, tetraethylene glycol di(meth)acrylate, 1,6-hexanediol (meth)acrylate, neopentyl glycol di(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and oligomers thereof; isocyanurates such as 2-propylene di-3-butenyl cyanurate, 2-hydroxyethyl bis(2-acryloyloxyethyl) isocyanurate, tris(2-methacryloyloxyethyl) isocyanurate, and tris(2-methacryloyloxyethyl) isocyanurate, and the like.

[0130] Examples of photopolymerization initiators include: benzoin alkyl ethers such as benzoin methyl ether, benzoin isopropyl ether, and benzoin isobutyl ether; aromatic ketones such as α-hydroxycyclohexyl phenyl ketone; aromatic ketals such as benzyl dimethyl ketal; thioxanthones such as polyvinyl benzophenone, chlorothioxanthone, dodecylthioxanthone, dimethylthioxanthone, and diethylthioxanthone.

[0131] Examples of the cross-linking agent include polyisocyanate compounds, melamine resins, urea resins, polyamines, carboxyl group-containing polymers, and the like.

[0132] The thickness of the adhesive layer is appropriately selected depending on the type of the adhesive, and is preferably 3 to 100 μm, and more preferably 3 to 50 μm.

[0133] In addition, the adhesive layer of the back grinding film can be protected by a diaphragm. If the adhesive layer is protected by the diaphragm, the surface of the adhesive layer can be kept smooth. In addition, the handling and transportation of the back grinding film become easy, and label processing can also be performed on the diaphragm. The diaphragm is peeled off when the back grinding film is used.

[0134] The separator may be paper, or a synthetic resin film such as polyethylene, polypropylene, or polyethylene terephthalate. In addition, the surface of the separator in contact with the adhesive layer may be subjected to a release treatment such as silicone treatment or fluorine treatment as required to improve the peelability from the adhesive layer. The thickness of the separator is generally 10 to 200 μm, preferably about 25 to 100 μm.

[0135] The manufacturing method of the back grinding film is not particularly limited, for example, it can be manufactured by applying an adhesive on the above-mentioned cut substrate using a known method. At this time, the coating of the adhesive can be carried out using a gravure roll coater, a reverse roll coater, a kiss roll coater, an immersion roll coater, a rod coater, a knife coater, a spray coater, etc. In addition, an adhesive can also be applied to the release sheet to form an adhesive layer, and the adhesive layer is transferred to the back grinding film substrate, and the back grinding film substrate and the adhesive layer are stacked. In addition, the back grinding film substrate and the adhesive layer can also be formed simultaneously by coextrusion, etc.

[0136] Example

[0137] The present invention will be described below with reference to Examples. The scope of the present invention is not to be construed limitatively by the Examples. The melt flow rate (MFR) is measured in accordance with JIS K 7210: 1999. The melting point is measured in accordance with JIS K 7121 (1987).

[0138] [Material preparation]

[0139] The following materials were used as the respective components.

[0140] <Ethylene-unsaturated ester copolymer (A)>

[0141] EVA: ethylene-vinyl acetate copolymer (content of structural units derived from ethylene: 67% by mass, content of structural units derived from vinyl acetate: 33% by mass, MFR (190° C., 2160 g load): 30 g / 10 min)

[0142] <Ethylene·α-olefin copolymer (B)>

[0143] PO1: ethylene-1-butene copolymer (manufactured by Mitsui Chemicals, Inc., TAFMER DF710 (trade name), MFR (190°C, 2160 g load) 1.2 g / 10 min, density 870 kg / m 3 , melting point 55°C)

[0144] <Styrene resin (C)>

[0145] Styrene resin 1: hydrogenated styrene thermoplastic elastomer SEBS (content of structural units derived from styrene: 30% by mass, manufactured by Asahi Kasei Corporation, Tuftec H1041 (trade name), MFR (190°C, 2160 g load) 0.3 g / 10 min, MFR (230°C, 2160 g load) 5 g / 10 min)

[0146] Styrene resin 2: hydrogenated styrene thermoplastic elastomer SEBS (content of structural units derived from styrene: 18% by mass, manufactured by Asahi Kasei Corporation, Tuftec H1062 (trade name), MFR (190°C, 2160 g load) 0.7 g / 10 min, MFR (230°C, 2160 g load) 4.5 g / 10 min)

[0147] Styrene resin 3: hydrogenated styrene thermoplastic elastomer SEBS (content of structural units derived from styrene: 13% by mass, manufactured by Krayton Polymer Corporation, Krayton G1657MS (trade name), MFR (190°C, 2160 g load) 1.6 g / 10 min, MFR (230°C, 2160 g load) 8.5 g / 10 min)

[0148] Styrene resin 4: hydrogenated styrene thermoplastic elastomer acid-modified SEBS (content of structural units derived from styrene 30% by mass, manufactured by Asahi Kasei Corporation, Tuftec M1913 (trade name), MFR (190°C, 2160 g load) 0.3 g / 10 min, MFR (230°C, 2160 g load) 5 g / 10 min, acid value 10 mgCH3ONa / g)

[0149] Styrene resin 5: hydrogenated styrene thermoplastic elastomer SEBS (content of structural units derived from styrene: 62% by mass, manufactured by Asahi Kasei Corporation, Tuftec SOE1611 (trade name), MFR (190° C., 2160 g load) 4 g / 10 min)

[0150] Styrene elastomer 6: hydrogenated styrene-based thermoplastic elastomer SEBS (content of structural units derived from styrene: 10% by mass, manufactured by JSR Corporation, DYNARON 1320P (trade name), MFR (190° C., 2160 g load) 0.7 g / 10 min, MFR (230° C., 2160 g load) 3.5 g / 10 min)

[0151] <Other resins>

[0152] PO2: Ethylene-1-butene copolymer (manufactured by Mitsui Chemicals, TAFMER DF7350 (trade name), MFR (190°C, 2160 g load) 25 g / 10 min, density 870 kg / m 3 , melting point 55°C)

[0153] LDPE: High-pressure low-density polyethylene (MFR (190°C, 2160g load) 1.1g / 10min, density 917kg / m 3 )

[0154] EMAA: ethylene-methacrylic acid copolymer (content of structural units derived from ethylene 91% by mass, content of structural units derived from methacrylic acid 9% by mass), MFR (190°C, 2160g load) 2.5g / 10min, density 930kg / m 3 )

[0155] [Examples 1 to 7 and Comparative Examples 1 to 4]

[0156] The ethylene-unsaturated ester copolymer (A) and the ethylene-α-olefin copolymer (B) or the styrene resin (C) were dry-blended in the ratio (mass ratio) shown in Table 1 so that the charge amount was 10 kg. The dry-blended mixture was charged into a resin inlet of a twin-screw extruder (L / D=32), and melt-kneaded at a processing temperature of 160° C. to obtain a resin composition for a back grinding film substrate.

[0157] The melt flow rate (MFR) of the obtained back grinding film substrate resin composition was measured under the conditions of 190° C. and a load of 2160 g in accordance with JIS K 7210: 1999. The measurement results are shown in Table 1.

[0158] [Evaluation of Softness]

[0159] For the obtained back grinding film substrate resin composition, a hot press set at 160°C was used to prepare a 150mm×150mm×3mm thick back grinding film substrate. The prepared back grinding film substrate was punched into a strip of 20mm in width×100mm in length as a test piece, and the obtained test piece was stored in an atmosphere of 23°C and 50% relative humidity for 2 weeks. Then, two back grinding film substrates were overlapped and the hardness (Shore A) was measured using an Asker automatic rubber hardness meter P1-D. The measured values ​​read the initial value and the value after 15 seconds. The measurement conditions comply with JIS K 7215:1996. The measurement results are shown in Table 1.

[0160] Regarding the initial value of hardness (Shore A), flexibility was evaluated based on the following criteria.

[0161] A (good): 71 or less

[0162] B (slightly good): greater than 71 and less than 75

[0163] C (bad): more than 75

[0164] Regarding the value of hardness (Shore A) after 15 seconds, the flexibility was evaluated based on the following criteria.

[0165] A (good): 67 or less

[0166] B (slightly good): greater than 67 and less than 72

[0167] C (bad): more than 72

[0168] [Evaluation of tearing properties]

[0169] The obtained resin composition for back grinding film substrate is used The tape casting machine is used to perform tape casting at a processing temperature of 200°C, a rotation speed of 100 rpm, and a processing speed of 3m / min to produce a 250μm thick back grinding film substrate. A 150mm×50mm sample is cut from the obtained back grinding film substrate, and a 75mm incision is made from the center of the 50mm width along the length direction. Using Autograph, the incised sample is torn up and down under the conditions of a distance between chucks of 75mm and a speed of 1000mm / min to determine its average strength. The average strength is divided by the measured thickness of the sample, and the strength N / mm per 1mm thickness is calculated as the tear strength. The tear strength is measured in the MD direction (Machine Direction) and TD direction (Transverse Direction) of the back grinding film substrate. The measurement results are shown in Table 1.

[0170] The tear strength was evaluated based on the following criteria: The criteria were the same in the MD direction and the TD direction.

[0171] A (good): 15N / mm or less

[0172] B (slightly good): greater than 15 N / mm and less than 20 N / mm

[0173] C (bad): greater than 20N / mm

[0174] [Table 1]

[0175]

[0176] As can be seen from Table 1, the back grinding film substrates using the back grinding film substrate resin compositions of Examples 1 to 7 have excellent tear properties while maintaining the softness of EVA. In contrast, the back grinding film substrates using the back grinding film substrate resin compositions of Comparative Examples 1 to 4 cannot maintain the softness of EVA, or even if they maintain the softness of EVA, the tear properties are poor.

[0177] From the above, it was confirmed that the resin composition for a back grind film substrate according to the present embodiment can realize a back grind film substrate having excellent tearing properties while maintaining the flexibility of EVA.

[0178] This application claims priority based on Japanese Patent Application No. 2022-39221 filed on March 14, 2022. The contents described in the specification of that application are incorporated herein by reference in their entirety.

[0179] Industrial Applicability

[0180] The resin composition for a back grinding film substrate of the present invention can realize a back grinding film substrate having excellent flexibility and excellent tearing properties, and is therefore very useful in the field of semiconductor device manufacturing.

Claims

1. A resin composition for a back grinding film substrate, comprising: an ethylene·unsaturated ester copolymer (A); and At least one selected from the group consisting of an ethylene-α-olefin copolymer (B) having a melt flow rate of 0.1 g / 10 min or more and less than 25 g / 10 min as measured under the conditions of 190° C. and a load of 2160 g according to JIS K 7210:1999, and a styrene resin (C), When the total amount of the ethylene·unsaturated ester copolymer (A), the ethylene·α-olefin copolymer (B) and the styrene resin (C) is 100 parts by mass, the content of the ethylene·unsaturated ester copolymer (A) is greater than 60 parts by mass and less than 100 parts by mass.

2. The resin composition for a back grinding film substrate according to claim 1, wherein The content of the structural unit derived from the unsaturated ester in the ethylene-unsaturated ester copolymer (A) is 15% by mass or more and 46% by mass or less.

3. The resin composition for a back grinding film substrate according to claim 1, wherein The ethylene-unsaturated ester copolymer (A) has a melt flow rate of 0.1 g / 10 min to 100 g / 10 min, as measured at 190° C. and a load of 2160 g in accordance with JIS K 7210:1999.

4. The resin composition for a back grinding film substrate according to claim 1, wherein The melting point of the ethylene·α-olefin copolymer (B) is lower than 100°C.

5. The resin composition for a back grinding film substrate according to claim 1, wherein The styrene resin (C) has a melt flow rate of 0.01 g / 10 min to 50 g / 10 min as measured at 190° C. and a load of 2160 g in accordance with JIS K 7210:1999.

6. The resin composition for a back grinding film substrate according to claim 1, wherein The styrene-based resin (C) is a styrene-based elastomer.

7. The resin composition for a back grinding film substrate according to claim 1, wherein When the entire back grinding film resin composition is taken as 100 mass %, the total amount of the ethylene·unsaturated ester copolymer (A), the ethylene·α-olefin copolymer (B) and the styrene resin (C) is 70 mass % or more and 100 mass % or less.

8. The resin composition for a back grinding film substrate according to claim 1, wherein The ethylene-unsaturated ester copolymer (A) is an ethylene-vinyl acetate copolymer. 9 . A back grinding film substrate comprising at least one layer comprising the resin composition for a back grinding film substrate according to claim 1 .

10. The back grinding film substrate according to claim 9, wherein The initial value of the hardness (Shore A) of the layer including the resin composition for a back grinding film substrate measured in accordance with JIS K 7215:1996 is 75 or less.

11. The back grinding film substrate according to claim 9, wherein The hardness (Shore A) of the layer including the resin composition for a back grinding film substrate measured in accordance with JIS K 7215:1996 is 72 or less 15 seconds after the start of the measurement.

12. A back grinding film having: The back grinding film substrate according to claim 9; and An adhesive layer is laminated on at least one side of the back grinding film substrate.