Positive electrode for solid-state secondary battery and solid-state secondary battery including same
By optimizing the proportion and particle size distribution of positive electrode active substances and solid electrolytes in the positive electrode active substance layer of an all-solid secondary battery, the problem of increasing internal resistance of positive electrodes is solved, and the balance of high energy density and low internal resistance is achieved , meets the high capacity and high output requirements of the battery.
Patent Information
- Application Number
- CN202380026080.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-01-06
- Filing Date
- 2023-01-06
- Publication Date
- 2024-11-08
AI Technical Summary
In all-solid secondary batteries, although increasing the amount of positive electrode active substances or particle size increases the energy density and charging rate, it leads to a decrease in lithium ion and electron conductivity, an increase in internal resistance, and an increase in negative electrode thickness will also lead to a positive The internal resistance of the electrode rises.
By increasing the amount of positive electrode active substance in the positive electrode active substance layer and adjusting the volume density after pressing, combining the ratio of positive electrode active substances and solid electrolytes of different particle sizes, the lithium ion and electron conductivity is optimized and the internal resistance is reduced by reducing internal resistance. . Specific measures include the use of 85 wt%~92 wt% positive electrode active material, 7 wt%~15 wt% solid electrolyte, 0.1 wt%~10 wt% conductive additive in the 100 wt% positive electrode active material layer, and control the particle size distribution to improve the contact area. .
It realizes the suppression of the internal resistance of the battery while increasing the energy density, meets the requirements of high capacity and high output, improves the lithium ion conductivity and electron conductivity, and ensures the high-efficiency energy density and low internal resistance of the battery.
Smart Images

Figure CN118922956A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a positive electrode for a solid-state secondary battery and a solid-state secondary battery including the same. Background Art
[0002] In order to further popularize and develop electric vehicles, the cruising range must be extended, and all-solid-state secondary batteries used in electric vehicles require higher energy density (e.g., 800Wh / L or higher).
[0003] As a method of increasing the energy density of an all-solid-state secondary battery to a higher energy density than before, the amount of positive electrode active material in the positive electrode of the all-solid-state secondary battery is increased, or the particle size of the positive electrode active material is increased, thereby improving the density and charging rate of the positive electrode active material in the positive electrode.
[0004] Additionally, it is conceivable to increase the thickness of the positive electrode to obtain a higher capacity positive electrode.
[0005]
Prior art documents
[0006] (Patent Document 1) Japanese Patent Application Publication No. 2003-036848
[0007] (Non-patent document 1) Naoki Suzuki et al., "Synthesis and Electrochemical Properties of I4-type Li 1+2x Zn 1-x PS4 Solid Electrolyte (I4--Type Li 1+2x Zn 1-x Synthesis and electrochemical properties of PS4 solid electrolytes), Chemistry of Materials, published on March 9, 2018, No. 30, 2236-2244 (2018). Summary of the invention
[0008] However, when the amount of the positive electrode active material in the positive electrode increases or the particle size of the positive electrode active material increases, the density and charging rate of the positive electrode active material in the positive electrode increase, but the contact area between the positive electrode active material and the solid electrolyte or conductive material is small. If so, there is a problem that the lithium ion conductivity and the electron conductivity in the positive electrode decrease and the internal resistance of the positive electrode increases.
[0009] And, if the thickness of the negative electrode increases, the internal resistance of the positive electrode also increases. The present invention is made in consideration of these problems, and provides a positive electrode for an all-solid-state secondary battery that satisfies high levels of both capacity and output by suppressing the internal resistance of the battery while sufficiently increasing the energy density of the all-solid-state secondary battery.
[0010] That is, the positive electrode for a solid-state secondary battery according to an embodiment includes a positive electrode current collector and a positive electrode active material layer,
[0011] The positive electrode active material layer includes a positive electrode active material, a solid electrolyte, a binder and a conductive aid.
[0012] The amount of the positive electrode active material is greater than or equal to 85 wt % and less than or equal to 92 wt % based on 100 wt % of the positive electrode active material layer,
[0013] The amount of the solid electrolyte is greater than or equal to 7 wt % and less than or equal to 15 wt % based on 100 wt % of the positive electrode active material layer.
[0014] When the amount of the positive electrode active material in the positive electrode active material layer is 100 wt %, the amount of the binder in the positive electrode active material layer is greater than or equal to 0.1 wt % and less than or equal to 1.0 wt %, and
[0015] When the amount of the solid electrolyte in the positive electrode active material layer is 100 wt %, the amount of the conductive aid in the positive electrode active material layer is greater than or equal to 0.1 wt % and less than or equal to 10 wt %.
[0016] According to the positive electrode for a solid-state secondary battery constructed in this way, the amount of the positive electrode active material in the positive electrode can be increased as much as possible, and the balance of the positive electrode active material, the solid electrolyte, the binder and the conductive aid can be optimally achieved. As a result, by increasing the amount of the positive electrode active material, the lithium ion conductivity and the electronic conductivity can be optimized, thereby achieving a high energy density in the positive electrode and suppressing an increase in internal resistance.
[0017] It is desirable that the secondary particles of the positive electrode active material have a D50 based on a volume-based particle size distribution obtained by a laser diffraction / scattering particle size distribution measurement method of greater than or equal to 1 μm and less than or equal to 20 μm.
[0018] Meanwhile, D50 of the positive electrode active material based on volume-based particle size distribution obtained by a laser diffraction / scattering particle size distribution measurement method was measured using water as a dispersion medium and a particle size distribution measurement device (MT3000) from Microtrac Systems, Inc.
[0019] The positive electrode active material may include two types of positive electrode active materials having different D50s, and one of the two types of positive electrode active materials, the small particle size positive electrode active material, has a D50 of greater than or equal to 1 μm and less than 10 μm, and the other, the large particle size positive electrode active material, has a D50 of greater than or equal to 10 μm and less than or equal to 20 μm.
[0020] The small particle size positive electrode active material may have a D50 of greater than or equal to 2 μm and less than 8 μm, and the large particle size positive electrode active material may have a D50 of greater than or equal to 8 μm and less than or equal to 20 μm. The small particle size positive electrode active material may have a D50 of greater than or equal to 2 μm and less than 8 μm, and the large particle size positive electrode active material may have a D50 of greater than or equal to 10 μm and less than or equal to 20 μm.
[0021] The positive electrode active material may satisfy any one of Chemical Formula 1 or Chemical Formula 2.
[0022] [Chemical Formula 1]
[0023] Li a Ni x Co y M 1-x-y O2
[0024] [Chemical Formula 2]
[0025] Li a Ni x Co y O2
[0026] Meanwhile, M in Chemical Formula 1 is one or more metal elements selected from aluminum and manganese. In addition, a, x, y, and 1 - x - y in Chemical Formula 1 and Chemical Formula 2 are numbers that satisfy 0.20 ≤ a ≤ 1.20, 0.80 ≤ x < 1.00, 0 < y ≤ 0.20, and 0 < 1 - x - y ≤ 0.10, respectively.
[0027] The solid electrolyte may be a sulfide - based solid electrolyte including lithium, phosphorus, and sulfur, and
[0028] the D50 of the primary particles and / or secondary particles of the solid electrolyte based on the volume - based particle size distribution obtained by the laser diffraction / scattering particle size distribution measurement method may be greater than or equal to 0.1 μm and less than or equal to 3 μm.
[0029] To further suppress the internal resistance of the positive electrode, it is desirable that the volume density of the positive electrode active material layer after pressing is greater than or equal to 3.2 g / cm 3 .
[0030] In the case of a solid-state secondary battery equipped with a positive electrode for a solid-state secondary battery according to the present embodiment, the discharge energy density ratio obtained by dividing the discharge energy density when the discharge current is 1C by the discharge energy density when the discharge current is 0.1C can be set to be greater than or equal to 0.70 and less than 1.00. The discharge energy density ratio is an indicator that the larger the value, the smaller the internal resistance of the battery. This value is greater than or equal to 0.70, indicating that the solid-state secondary battery has a sufficiently small internal resistance, that is, has a high output.
[0031] As described above, according to the embodiment, a positive electrode for a solid-state secondary battery that satisfies high levels of both capacity and output by suppressing the internal resistance of the battery while sufficiently increasing the energy density of the solid-state secondary battery can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 is a cross-sectional view showing a schematic configuration of an all-solid-state secondary battery according to an embodiment.
[0033] Figure 2 Graph showing the relationship between the particle size distribution of the positive electrode active material and the density of the positive electrode active material. DETAILED DESCRIPTION
[0034] The embodiments will be described in detail below.
[0035] <1. Basic Configuration of Solid-State Secondary Battery According to the Present Embodiment>
[0036] Below, we will refer to Figure 1 A solid-state secondary battery is described. Figure 1 is a cross-sectional view showing a schematic configuration of an all-solid-state secondary battery according to an embodiment.
[0037] refer to Figure 1 The all-solid-state secondary battery 1 according to the present embodiment is an all-solid-state lithium-ion battery including a positive electrode 10 , a negative electrode 20 , and a solid electrolyte layer 30 between the positive electrode and the negative electrode.
[0038] (1-1, positive electrode)
[0039] The positive electrode 10 includes a positive electrode current collector 11 and a positive electrode active material layer 12 .
[0040] The positive electrode current collector 11 may be, for example, a plate-like body or a thin body made of one or more materials selected from indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li) or their alloys.
[0041] The positive electrode active material layer 12 is a layer including a positive electrode active material that reversibly intercalates and deintercalates lithium ions. Since the positive electrode active material layer has the features of the above embodiment, it will be described in detail later.
[0042] (1-2, negative electrode)
[0043] The negative electrode 20 includes a negative electrode current collector 21 and a negative electrode active material layer 22 .
[0044] The negative electrode current collector 21 is desirably made of a material that does not react with lithium (i.e., does not form any alloy or compound with lithium). The material constituting the negative electrode current collector may have, for example, a plate-like body or a thin body made of one or more metals selected from copper (Cu), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), and nickel (Ni), an alloy, or a coating material.
[0045] The negative electrode active material layer 22 includes a negative electrode active material.
[0046] The negative electrode active material may include, for example, amorphous carbon and an alloy-forming element that forms an alloy with lithium. Examples of alloy-forming elements include one or more selected from gold, platinum, palladium, silicon, silver, aluminum, bismuth, tin, and zinc. In this article, examples of amorphous carbon may include carbon black, graphene, and graphite. Examples of carbon black may include acetylene black, furnace black, and Ketjen black. In addition, in order to improve electronic conductivity, the surface of silicon may be covered with a carbon layer having a thickness of 1 nm to 10 nm.
[0047] In this article, when any one or more of gold, platinum, palladium, silicon, silver, aluminum, bismuth, tin and zinc are used as alloy forming elements, these negative electrode active materials are, for example, in the form of particles, and the particle size is desirably 4 μm or less, more desirably 300 nm or less. In this case, the characteristics of the all-solid-state secondary battery are further improved. In this article, the particle size of the secondary particles of the negative electrode active material may be, for example, a median diameter (so-called D 50 ). On the other hand, D50 of the negative electrode active material based on the volume-based particle size distribution obtained by the laser diffraction / scattering particle size distribution measurement method can be measured using a particle size distribution measurement device (MT3000) manufactured by Microtrac Systems, Inc. using N-methylpyrrolidone (NMP) as a dispersion medium.
[0048] The negative electrode active material layer may be appropriately blended with additives used in conventional all-solid lithium ion secondary batteries (such as a binder, a filler, a dispersant, and an ion conduction aid) in addition to the above-mentioned negative electrode active material.
[0049] (1-3. Solid electrolyte layer)
[0050] The solid electrolyte layer includes a solid electrolyte.
[0051] The solid electrolyte is composed of, for example, a sulfide-based solid electrolyte material. The sulfide-based solid electrolyte material may include, for example, Li2S-P2S5, Li2S-P2S5-LiX (wherein X is a halogen element such as I or Cl), Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-SiS2, Li2S-SiS2-LiI, Li2S-SiS2-LiBr, Li2S-SiS2-LiCl, Li2S-SiS2-B2S3-LiI, Li2S-SiS2-P2S5-LiI, Li2S-B2S3, Li2S-P2S5-Z m S n (where m and n are positive numbers, and Z is Ge, Zn or Ga), Li2S-GeS2, Li2S-SiS2-Li3PO4, Li2S-SiS2-Li p MO q (where p and q are positive numbers, and M is any one of P, Si, Ge, B, Al, Ga or In), Li6PS5Cl, etc. The sulfide-based solid electrolyte material is produced by treating the raw materials (e.g., Li2S, P2S5, etc.) by melt quenching or mechanical grinding. In addition, heat treatment may be further performed after these treatments. The solid electrolyte may be amorphous, crystalline, or a mixture of the two.
[0052] Furthermore, as a solid electrolyte, among the sulfide solid electrolyte materials mentioned above, it is desired to use a sulfide solid electrolyte material including at least sulfur (S), phosphorus (P) and lithium (Li) as constituent elements, and in particular to use a sulfide solid electrolyte material including Li2S-P2S5.
[0053] When a material including Li2S-P2S5 is used as a sulfide-based solid electrolyte material forming a solid electrolyte, the mixing molar ratio of Li2S and P2S5 can be selected from, for example, the range of Li2S:P2S5=50:50 to 90:10. In addition, the solid electrolyte layer may further include a binder. The binder included in the solid electrolyte layer may include, for example, styrene-butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, and polyethylene.
[0054] <2. Configuration of Solid State Secondary Battery According to the Present Embodiment>
[0055] The positive electrode active material layer constituting the positive electrode of the all-solid-state lithium ion secondary battery according to the present embodiment includes a positive electrode active material, a solid electrolyte, a conductive auxiliary agent, and a binder.
[0056] Examples of the positive electrode active material may include lithium salts such as lithium cobalt oxide (hereinafter referred to as LCO), lithium nickel oxide, lithium nickel cobalt oxide, lithium nickel cobalt aluminum oxide (hereinafter referred to as NCA), lithium nickel cobalt manganese oxide (hereinafter also referred to as NCM), lithium manganese oxide, or lithium iron phosphate, nickel sulfide, copper sulfide, lithium sulfide, sulfur, iron oxide, vanadium oxide, etc. These positive electrode active materials may be used alone or in combination of two or more types.
[0057] Among them, it is desirable to use a compound represented by Chemical Formula 1 or Chemical Formula 2 as the positive electrode active material. These materials are called high-Ni positive electrode active materials, and by adopting such a positive electrode active material, the cycle stability and energy density can be further improved.
[0058] [Chemical Formula 1]
[0059] Li a Ni x Co y M 1-x-y O2
[0060] [Chemical Formula 2]
[0061] Li a Ni x Co y O2
[0062] Meanwhile, M in Chemical Formula 1 is one or more metal elements selected from aluminum and manganese. In addition, a, x, y, and 1 - x - y in Chemical Formula 1 and Chemical Formula 2 are numbers satisfying 0.20 ≤ a ≤ 1.20, 0.80 ≤ x < 1.00, 0 < y ≤ 0.20, and 0 < 1 - x - y ≤ 0.10, respectively.
[0063] The positive electrode active material may be coated. As the coating, a known coating for the positive electrode active material of an all-solid-state secondary battery may be used, and for example, Li2O-ZrO2 may be used.
[0064] In addition, when the positive electrode active material is formed of a lithium salt of a ternary transition metal oxide such as NCA or NCM and the positive electrode active material includes nickel (Ni), the capacity density of the all-solid-state lithium-ion secondary battery increases, and the metal dissolution from the positive electrode active material during the charged state can be reduced. Accordingly, the all-solid-state secondary battery according to the present embodiment can improve the long-term reliability and cycle characteristics during the charged state. To further demonstrate these characteristics, it is more desirable that the nickel (Ni) content in the positive electrode active material is high. The nickel content in the positive electrode active material is desirably greater than or equal to 60 mol%, and more desirably greater than or equal to 80 mol%. On the other hand, if the nickel content in the positive electrode active material is less than or equal to 95 mol%, it is desirable because this can suppress the reduction of the battery capacity during charge and discharge evaluation.
[0065] The shape of the positive electrode active material is desirably, for example, a particle shape such as a true spherical shape or an ellipsoidal shape.
[0066] The particle size of the secondary particles of the positive electrode active material may have a D50 of greater than or equal to 1 μm and less than or equal to 20 μm, greater than or equal to 2 μm and less than or equal to 19 μm, greater than or equal to 3 μm and less than or equal to 18 μm based on a volume-based particle size distribution obtained by a laser diffraction / scattering particle size distribution measurement method.
[0067] More specifically, it is desirable to use a mixture of two types of positive electrode active materials having different D50 as the positive electrode active material. Of the two types of positive electrode active materials, the D50 of the small particle size positive electrode active material having a relatively small particle size may desirably be greater than or equal to 1 μm and less than 10 μm, and the D50 of the large particle size positive electrode active material having a relatively large particle size may desirably be greater than or equal to 10 μm and less than or equal to 20 μm, greater than or equal to 11 μm and less than or equal to 19 μm, greater than or equal to 12 μm and less than or equal to 18 μm.
[0068] Also, D50 of the small particle size positive electrode active material is more desirably greater than or equal to 2 μm and less than 8 μm, and more desirably greater than or equal to 3 μm and less than or equal to 7 μm.
[0069] When the D50 of the small particle size positive electrode active material is greater than or equal to 2 μm and less than 8 μm, the D50 of the large particle size positive electrode active material may desirably be greater than or equal to 8 μm and less than or equal to 20 μm, more desirably be greater than or equal to 9 μm and less than or equal to 19 μm, and particularly desirably be greater than or equal to 10 μm and less than or equal to 18 μm.
[0070] These small particle size positive electrode active materials and large particle size positive electrode active materials may have the same composition or different compositions.
[0071] The amount of the positive electrode active material in the positive electrode active material layer may be greater than or equal to 85 wt % and less than or equal to 92 wt %, greater than or equal to 85 wt % and less than or equal to 91 wt %, or greater than or equal to 87 wt % and less than or equal to 91 wt %.
[0072] As a solid electrolyte, a solid electrolyte made of one or more solid electrolyte materials selected from the examples given in the description of the solid electrolyte layer can be widely used. Among them, a solid electrolyte material (argentum type) Li6PS5Cl having a argyrodite crystal structure is desirable because it is easy to control the particle size, can be highly charged by miniaturization, and can form a good interface with the positive electrode active material. In addition, a solid electrolyte material (argentum type) Li6PS5Cl having a argyrodite crystal structure may be an ideal material because it has a wide potential window and excellent voltage resistance, and a large-scale production manufacturing process has been established so that it is a material that can be expected in terms of cost.
[0073] As solid electrolyte materials, in addition to those mentioned above, argyrodite-type Li6PS5Br x Cl 1-x , glass ceramics Li2S-P2S5-LiX (X=Br or I), etc.
[0074] Examples of the shape of the solid electrolyte include particle shapes such as a spherical shape and an ellipsoidal shape.
[0075] When the solid electrolyte is in a particle shape, the particle size of the primary particles desirably has a D50 greater than or equal to 0.1 μm and less than or equal to 3.0 μm based on a volume-based particle size distribution obtained by a laser diffraction / scattering particle size distribution measurement method. The D50 of the solid electrolyte is more desirably greater than or equal to 0.2 μm and less than or equal to 2.8 μm, and greater than or equal to 0.3 μm and less than or equal to 2.5 μm. On the other hand, the D50 of the solid electrolyte based on a volume-based particle size distribution obtained by a laser diffraction / scattering particle size distribution measurement method is measured using xylene as a dispersion medium and a particle size distribution measurement device (PSA1090) manufactured by Anton Paar.
[0076] The amount of the solid electrolyte based on the total positive electrode active material layer (i.e., when the mass of the positive electrode active material layer is 100%) may be greater than or equal to 7 wt % and less than or equal to 15 wt %, more desirably greater than or equal to 8 wt % and less than or equal to 13 wt %, and particularly desirably greater than or equal to 9 wt % and less than or equal to 13 wt %.
[0077] The conductive auxiliary agent is one or more substances selected from the group consisting of graphite, carbon black, acetylene black, Ketjen black, carbon fiber, metal powder and the like.
[0078] When the amount of solid electrolyte in the positive electrode active material layer is 100wt%, the amount of conductive aid in the positive electrode active material layer may be greater than or equal to 0.1wt% and less than or equal to 10wt%, desirably greater than or equal to 0.2wt% and less than or equal to 9wt%, more desirably greater than or equal to 0.3wt% and less than or equal to 8wt%, and particularly desirably greater than or equal to 0.5wt% and less than or equal to 7wt%.
[0079] The amount of the conductive aid may be greater than or equal to 0.05 wt % and less than or equal to 1.0 wt %, greater than or equal to 0.1 wt % and less than or equal to 0.8 wt %, based on the total positive electrode active material layer.
[0080] The binder may be one or more materials selected from styrene butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, and the like.
[0081] When the amount of positive electrode active material in the positive electrode active material layer is 100wt%, the amount of binder in the positive electrode active material layer may desirably be greater than or equal to 0.1wt% and less than or equal to 1.0wt%, desirably be greater than or equal to 0.1wt% and less than or equal to 0.9wt%, more desirably be greater than or equal to 0.1wt% and less than or equal to 0.8wt%, and particularly desirably be greater than or equal to 0.1wt% and less than or equal to 0.7wt%.
[0082] The amount of the binder in the total positive electrode active material layer may desirably be greater than or equal to 0.05 wt % and less than or equal to 1.0 wt %, and more desirably greater than or equal to 0.1 wt % and less than or equal to 0.9 wt %.
[0083] In the positive electrode active material layer, in addition to the above substances, fillers, dispersants, ion conduction aids, etc. can be appropriately added within the range that can demonstrate the effects of the present embodiment (for example, based on the total positive electrode active material layer, less than or equal to 6wt%, more desirably less than or equal to 3wt%, and particularly desirably less than or equal to 1wt%).
[0084] <3. Method for Manufacturing Solid-State Secondary Battery According to the Present Embodiment>
[0085] Hereinafter, a method for manufacturing an all-solid-state lithium ion secondary battery according to the present embodiment will be described. The all-solid-state lithium ion secondary battery according to the present embodiment can be manufactured by separately manufacturing a positive electrode, a negative electrode and a solid electrolyte layer, then stacking each layer, and finally covering with an outer body.
[0086] (3-1. Positive electrode manufacturing process)
[0087] In this embodiment, instead of using a wet method of forming the positive electrode active material layer by suspending the material constituting the positive electrode active material layer in a solvent and then coating it on a current collector and drying it, a dry method of forming the positive electrode active material layer by pressing a mixture of the materials constituting the positive electrode active material layer is used.
[0088] Specifically, the materials constituting the positive electrode active material layer (positive electrode active material, solid electrolyte, conductive additive, binder, etc.) are kneaded, and the kneaded material mass is pressed to form a positive electrode mixture sheet that becomes the positive electrode active material layer. The positive electrode is manufactured by stacking the positive electrode mixture sheet on the base layer using roller pressing, etc. At this time, when the all-solid-state lithium-ion secondary battery is completed (after pressing), it is expected that the volume density of the positive electrode active material layer is adjusted to be greater than or equal to 3.2 g / cm 3 And less than or equal to 3.6g / cm 3 .
[0089] Needless to say, the positive electrode active material layer can also be produced using a wet method.
[0090] (3-2. Negative electrode manufacturing process)
[0091] The slurry is prepared by adding the negative electrode active material layer material (negative electrode active material, non-alloying element, binder, etc.) constituting the negative electrode active material layer to a polar solvent or a non-polar solvent. Next, the obtained slurry is coated on the negative electrode current collector and dried. Next, the obtained laminate is pressed (for example, using hydrostatic pressure to pressurize) to produce a negative electrode. Because the above-mentioned pressurization treatment is not a necessary process, it can be omitted.
[0092] (3-3. Solid Electrolyte Layer Manufacturing Process)
[0093] The solid electrolyte layer can be produced by forming a film of a solid electrolyte formed of a sulfide-based solid electrolyte material. The specific manufacturing sequence is as follows.
[0094] First, the solid electrolyte material is produced by a melt quenching method or a mechanical grinding method.
[0095] For example, when using the melt quenching method, a predetermined amount of raw materials (e.g., Li2S, P2S5, etc.) are mixed to form a pellet, reacted in a vacuum at a predetermined reaction temperature, and then quenched to prepare a sulfide-based solid electrolyte material. On the other hand, the reaction temperature of the mixture of Li2S and P2S5 is desirably 400°C to 1000°C, and more desirably 800°C to 900°C. Moreover, the reaction time is desirably 0.1 hour to 12 hours, and more desirably 1 hour to 12 hours. In addition, the quenching temperature of the reactant is generally less than or equal to 10°C, desirably less than or equal to 0°C, and the quenching rate is generally about 1°C to 10000°C, and desirably about 1°C to 1000°C.
[0096] When the mechanical grinding method is used, the sulfide-based solid electrolyte material can be manufactured by stirring and reacting the raw materials (e.g., Li2S, P2S5, etc.) using a ball mill, etc. Meanwhile, the stirring speed and stirring time in the mechanical grinding method are not particularly limited, but the faster the stirring speed, the faster the production rate of the sulfide-based solid electrolyte material, and the longer the stirring time, the higher the conversion rate of the raw material into the sulfide-based solid electrolyte material.
[0097] Thereafter, the mixed raw materials obtained by the melt quenching method or the mechanical grinding method are heat-treated at a predetermined temperature and then pulverized to produce a granular solid electrolyte. When the solid electrolyte has a glass transition point, the solid electrolyte can be changed from amorphous to crystalline by heat treatment.
[0098] Subsequently, the solid electrolyte obtained by the above method is formed into a film using, for example, a known film forming method (such as an aerosol deposition method, a cold spray method, or a sputtering method) to form a solid electrolyte layer. On the other hand, the solid electrolyte layer can be produced by pressing the solid electrolyte particles alone. In addition, the solid electrolyte layer can be produced by mixing a solid electrolyte, a solvent, and a binder, coating, drying, and pressing.
[0099] (3-4. Assembly process of all-solid-state secondary batteries)
[0100] The positive electrode, negative electrode and solid electrolyte layer produced by the above method are stacked so that the positive electrode and the negative electrode sandwich the solid electrolyte layer in the middle and are covered on both sides of them with the laminate film forming the above-mentioned outer body, and then pressed (for example, by using hydrostatic pressure) to manufacture an all-solid-state lithium-ion secondary battery according to this embodiment.
[0101] <4. Effects of the present embodiment>
[0102] According to the all-solid-state lithium ion secondary battery constructed in this manner, a positive electrode for a solid-state secondary battery can be provided, which satisfies high levels of both capacity and output by suppressing the internal resistance of the battery while sufficiently increasing the energy density of the solid-state secondary battery.
[0103] As the positive electrode active material, because a mixture of two types of positive electrode active materials with different D50 is used, the small particle size positive electrode active material enters the gaps between the large particle size positive electrode active material to increase the volume density of the positive electrode as much as possible, and a sufficient contact area between the positive electrode active material and the solid electrolyte in the positive electrode active material layer can be ensured, thereby improving the lithium ion conductivity.
[0104] Since the positive electrode active material layer is formed by a dry method, the amount of the binder included in the positive electrode active material layer can be reduced as much as possible, and the energy density in the positive electrode active material layer can be increased as much as possible.
[0105] Although the preferred embodiments have been described in detail above, the present specification is not limited to these embodiments. It is clear to a person skilled in the art to which the present invention belongs that various changes or modifications can be made within the scope of the technical ideas described in the patent claims, and these changes or modifications are naturally understood to fall within the technical scope of the present specification.
[0106] [Example]
[0107] Hereinafter, the solid-state secondary battery according to the above embodiment will be described in more detail through examples, but the present description is not limited to these examples.
[0108] (Example 1)
[0109] [Manufacturing of positive electrode]
[0110] LiNi 0.8 Co 0.15 Mn 0.05O2 (NCM) was prepared as a positive electrode active material. The positive electrode active material was coated with Li2O-ZrO2 by the method described in non-patent document 1. For the coated positive electrode active material, the D50 of the secondary particles was measured based on the volume-based particle size distribution obtained by the laser diffraction / scattering particle size distribution measurement method, and it was found to be 6 μm. As a solid electrolyte, argyrodite-type crystals Li6PS5Cl were prepared. In addition, polytetrafluoroethylene (Teflon (registered trademark) binder manufactured by DuPont) was prepared as a binder. In addition, carbon nanofibers (CNF) were prepared as conductive additives. Next, these materials were mixed in a weight ratio of positive electrode active material: solid electrolyte: conductive additive: binder = 87: 12.8: 0.1: 0.1, and a positive electrode mixture sheet was prepared by a dry method in which the mixture was stretched into a sheet shape. At this time, the thickness of the positive electrode mixture sheet was such that the area capacity (i.e., the current density at 1C discharge) was 7 mA / cm 2 In addition, the positive electrode mixture sheet was cut into a prescribed shape with a Thompson blade. The positive electrode current collector foil was a 10 μm thick aluminum foil coated with a 1 μm thick primer layer, which was cut into the same size as the positive electrode sheet using a Pinnacle die.
[0111] [Manufacturing of negative electrode]
[0112] A nickel foil current collector with a thickness of 10 μm was prepared as the negative electrode current collector.
[0113] In addition, as the negative electrode active material, CB1 (nitrogen adsorption specific surface area of about 339 m 2 / g, DBP oil consumption is about 193ml / 100g) and CB2 manufactured by Asahi Carbon (nitrogen adsorption specific surface area is about 52m 2 / g, DBP oil amount is about 193 ml / 100 g), and silver particles with a particle size of 60 nm are prepared. Meanwhile, the particle size of the silver particles is based on the D50 of the volume-based particle size distribution measured using, for example, a laser particle size distribution instrument.
[0114] First, 1.5 g of CB1, 1.5 g of CB2 and 1 g of silver particles were placed in a container, and 4 g of N-methylpyrrolidone (NMP) solution including 5 wt % of a binder (#9300 manufactured by Kureha Corporation) was added thereto. Next, a negative electrode active material layer coating solution was prepared by stirring the mixed solution while gradually adding a total amount of 30 g of NMP to the mixed solution. The negative electrode active material layer coating solution was coated on a nickel foil using a blade coater and dried in air at 80° C. for about 20 minutes to form a negative electrode active material layer. The resulting laminate was vacuum dried at 100° C. for about 12 hours and drilled with a Pinnacle mold (registered trademark). Through the above steps, a negative electrode was manufactured.
[0115] [Manufacturing of Solid Electrolyte Layer]
[0116] First, a solid electrolyte layer coating solution is prepared.
[0117] To the amorphous powder of Li2S-P2S5 (80:20mol%) as a sulfide solid electrolyte, an SBR binder dissolved in dehydrated xylene is added to 1wt% based on the solid electrolyte to prepare a first mixed slurry. In addition, an appropriate amount of dehydrated xylene and dehydrated diethylbenzene for viscosity adjustment are added to the first mixed slurry to prepare a second mixed slurry. In addition, in order to improve the dispersibility of the mixed powder, zirconia balls with a diameter of 5mm are added to the second mixed slurry so that the voids, the mixed powder and the zirconia balls each occupy 1 / 3 of the total volume of the mixing container. The third liquid mixture prepared in this way is placed in a rotary mixer and stirred at 3000rpm for 3 minutes to produce a solid electrolyte layer coating solution.
[0118] The prepared solid electrolyte layer coating solution was coated on a PET film whose surface had been subjected to release treatment with a scraper, dried on a hot plate at 40°C for 10 minutes, and then vacuum dried at 40°C for 12 hours to obtain a solid electrolyte sheet. The thickness of the dried solid electrolyte layer was about 65 μm. The dried solid electrolyte sheet was pierced with a Thompson blade and processed into a predetermined size.
[0119] [Fabrication of electrolyte-negative electrode structure]
[0120] The solid electrolyte sheet was placed on the surface of the negative electrode so that the solid electrolyte layer and the negative electrode active material layer were in contact, and placed on an aluminum plate (support material) with a thickness of 3 mm attached to a release film, and vacuum laminated (including the support material). The solid electrolyte layer on the solid electrolyte sheet was integrated with the negative electrode by immersion in a pressurized medium and hydrostatic pressure treatment at 50 MPa (combination process using an isostatic press).
[0121] [Manufacturing of all-solid-state battery cells]
[0122] On the electrolyte-negative electrode structure obtained by stripping the PET film from the solid electrolyte sheet, the positive electrode is placed so that the positive electrode active material layer is in contact with the solid electrolyte layer, and a laminate as a pressurized all-solid-state lithium ion secondary battery is obtained. The all-solid-state lithium ion secondary battery is vacuum laminated and packaged before pressurization. It is placed on a 3 mm thick aluminum plate (support material) with a release film, covered with a release film, and vacuum laminated and packaged (including support material). It is immersed in a pressurized medium and subjected to hydrostatic pressure treatment (using a merging process of an isostatic press) at 490 MPa to obtain a single battery cell (test battery cell) of an all-solid-state lithium ion secondary battery.
[0123] Meanwhile, in this example, an aluminum plate and a metal plate made of SUS are used as supporting materials, but the materials of these supporting materials are not particularly limited as long as they have strength capable of withstanding pressurization by isostatic pressing.
[0124] [Evaluation of discharge load characteristics]
[0125] The manufactured test battery cells were measured and evaluated by using a charge and discharge evaluation device (TOSCAT-3100 manufactured by Toyo Systems Co., Ltd.). The charge and discharge of the battery cells were performed at 45 environment. Charge to 4.15V at a constant current of 0.1C, and then charge to a current of 0.05C at a constant potential. Discharge to 2.5V at constant currents of 0.1C and 1C to measure the discharge energy density. Subsequently, the ratio of the discharge energy density of 1C to the discharge energy density of 0.1C (1C / 0.1C) is used as an indicator of load characteristics. The higher the ratio, the smaller the internal resistance, but the better the battery characteristics. The results of other embodiments and comparative examples are shown in Table 1.
[0126] (Example 2)
[0127] In the positive electrode manufacturing process, the positive electrode is manufactured in the same manner as in Example 1, except that the positive electrode active material layer is formed to include 85wt% of the positive electrode active material, 14.1wt% of the solid electrolyte, 2.1wt% of the conductive aid based on 100wt% of the solid electrolyte and 0.7wt% of the binder based on 100wt% of the positive electrode active material.
[0128] (Example 3)
[0129] In the positive electrode manufacturing process, a positive electrode was manufactured in the same manner as in Example 1, except that the positive electrode active material layer was formed to include 12.4 wt % of a solid electrolyte and 0.6 wt % of a binder based on 100 wt % of the positive electrode active material.
[0130] (Example 4)
[0131] In the positive electrode manufacturing process, a positive electrode was manufactured in the same manner as in Example 1, except that the positive electrode active material layer was formed to include 12.05 wt % of the solid electrolyte and 1.0 wt % of the binder based on 100 wt % of the positive electrode active material.
[0132] (Example 5)
[0133] In the positive electrode manufacturing process, the positive electrode is manufactured in the same manner as in Example 1, except that the positive electrode active material layer is formed to include 88 wt % of the positive electrode active material, 11.3 wt % of the solid electrolyte, 1.8 wt % of the conductive aid based on 100 wt % of the solid electrolyte and 0.6 wt % of the binder based on 100 wt % of the positive electrode active material.
[0134] (Example 6)
[0135] In the positive electrode manufacturing process, the positive electrode is manufactured in the same manner as in Example 1, except that the positive electrode active material layer is formed to include 89 wt % of the positive electrode active material, 10.3 wt % of the solid electrolyte, 1.9 wt % of the conductive aid based on 100 wt % of the solid electrolyte and 0.6 wt % of the binder based on 100 wt % of the positive electrode active material.
[0136] (Example 7)
[0137] In the positive electrode manufacturing process, the positive electrode is manufactured in the same manner as in Example 1, except that the positive electrode active material layer is formed to include 85 wt % of the positive electrode active material (the positive electrode active material is prepared by mixing two types of positive electrode active materials with D50 of 6 μm and D50 of 14 μm in a weight ratio of 1:3), 13.8 wt % of the solid electrolyte, 5.8 wt % of the conductive aid based on 100 wt % of the solid electrolyte and 0.5 wt % of the binder based on 100 wt % of the positive electrode active material.
[0138] (Example 8)
[0139] In the positive electrode manufacturing process, the positive electrode was manufactured in the same manner as in Example 7, except that the positive electrode active material layer was formed to include 89 wt % of the positive electrode active material, 10.0 wt % of the solid electrolyte and 5.8 wt % of the conductive aid based on 100 wt % of the solid electrolyte.
[0140] (Example 9)
[0141] In the positive electrode manufacturing process, a positive electrode was manufactured in the same manner as in Example 8, except that carbon black was used as a conductive auxiliary agent.
[0142] (Example 10)
[0143] In the positive electrode manufacturing process, the positive electrode was manufactured in the same manner as in Example 8, except that the positive electrode active material layer was formed to include 90 wt % of the positive electrode active material, 9.15 wt % of the solid electrolyte and 0.3 wt % of the binder based on 100 wt % of the positive electrode active material.
[0144] (Example 11)
[0145] In the positive electrode manufacturing process, the positive electrode was manufactured in the same manner as in Example 10, except that the area capacity of the positive electrode was 8 mAh / cm 2 .
[0146] (Example 12)
[0147] The positive electrode was manufactured in the same manner as in Example 10, except that the area capacity of the positive electrode was 9 mAh / cm 2 .
[0148] (Example 13)
[0149] In the positive electrode manufacturing process, the positive electrode was manufactured in the same manner as in Example 10, except that the positive electrode active material layer was formed to include 91 wt % of the positive electrode active material, 8.2 wt % of the solid electrolyte and 6.7 wt % of the conductive aid based on 100 wt % of the solid electrolyte.
[0150] (Example 14)
[0151] In the positive electrode manufacturing process, a positive electrode was manufactured in the same manner as in Example 3, except that the D50 of the positive electrode active material was 14 μm.
[0152] (Example 15)
[0153] In the positive electrode manufacturing process, the positive electrode is manufactured in the same manner as in Example 3, except that the positive electrode active material layer is formed to include 88 wt % of the positive electrode active material (the positive electrode active material is prepared by mixing two types of positive electrode active materials with D50 of 3 μm and D50 of 10 μm in a weight ratio of 1:3), 11.15 wt % of the solid electrolyte, 5.4 wt % of the conductive aid based on 100 wt % of the solid electrolyte and 0.3 wt % of the binder based on 100 wt % of the positive electrode active material.
[0154] (Example 16)
[0155] In the positive electrode manufacturing process, a mixture of two positive electrode active materials with a D50 of 6 μm and a D50 of 14 μm in a weight ratio of 1:3 is used as the positive electrode active material. As a solid electrolyte, a glass ceramic solid electrolyte Li2-P2S5-LiBr is used. The D50 of the solid electrolyte is set to 1.2 μm. The positive electrode is manufactured in the same manner as in Example 1, except that the positive electrode active material layer is formed to have 90 wt% of the positive electrode active material, 9.15 wt% of the solid electrolyte, 6.6 wt% of the conductive aid based on 100 wt% of the solid electrolyte, and 0.3 wt% of the binder based on 100 wt% of the positive electrode active material.
[0156] (Example 17)
[0157] In the positive electrode manufacturing process, a mixture of two positive electrode active materials with a D50 of 6 μm and a D50 of 14 μm in a weight ratio of 1:3 is used as the positive electrode active material. As a solid electrolyte, a argyrodite solid electrolyte Li6-PS5X (a combination of X = Cl and Br) is used. The D50 of the solid electrolyte is set to 0.8 μm. The positive electrode is manufactured in the same manner as in Example 1, except that the positive electrode active material layer is formed to have 90 wt% of the positive electrode active material, 9.15 wt% of the solid electrolyte, 6.6 wt% of the conductive aid based on 100 wt% of the solid electrolyte, and 0.3 wt% of the binder based on 100 wt% of the positive electrode active material.
[0158] (Example 18)
[0159] In the positive electrode manufacturing process, the positive electrode is manufactured in the same manner as in Example 1, except that the positive electrode active material layer is formed to have 85wt% of the positive electrode active material, 12.8wt% of the solid electrolyte with a D50 of 2μm, 6.3wt% of the conductive aid based on 100wt% of the solid electrolyte and 0.5wt% of the binder based on 100wt% of the positive electrode active material.
[0160] (Comparative Example 1)
[0161] In the positive electrode manufacturing process, a positive electrode was manufactured in the same manner as in Example 1 except that the positive electrode active material layer was formed to have 11.4 wt % of the solid electrolyte and 1.7 wt % of the binder based on 100 wt % of the positive electrode active material.
[0162] (Comparative Example 2)
[0163] In the positive electrode manufacturing process, the positive electrode is manufactured in the same manner as in Example 10, except that the positive electrode active material layer is formed to include 8.2 wt % of a solid electrolyte, 11.0 wt % of a conductive aid based on 100 wt % of the solid electrolyte, and 1.0 wt % of a binder based on 100 wt % of the positive electrode active material.
[0164] (Comparative Example 3)
[0165] In the positive electrode manufacturing process, a positive electrode was manufactured in the same manner as in Example 13, except that the positive electrode active material layer was formed to include 93 wt % of the positive electrode active material and 6.2 wt % of the solid electrolyte.
[0166] (Comparative Example 4)
[0167] In the positive electrode manufacturing process, the positive electrode is manufactured in the same manner as in Example 8, except that the positive electrode active material layer is formed to include 8.95wt% of a solid electrolyte, 20.1wt% of a conductive aid based on 100wt% of the solid electrolyte, and 0.3wt% of a binder based on 100wt% of the positive electrode active material.
[0168] (Comparative Example 5)
[0169] In the positive electrode manufacturing process, a positive electrode was manufactured in the same manner as in Example 8, except that the positive electrode active material layer was formed to include 10.75 wt % of a solid electrolyte and 0.3 wt % of a binder based on 100 wt % of the positive electrode active material, but did not include a conductive aid.
[0170] (Table 1)
[0171]
[0172]
[0173] Referring to the results of Table 1, if the positive electrode active material layer is formed to include a positive electrode active material in an amount greater than or equal to 85wt% and less than or equal to 92wt%, a solid electrolyte in an amount greater than or equal to 7wt% and less than or equal to 15wt%, a conductive aid in an amount greater than or equal to 0.1wt% and less than or equal to 10wt% based on 100wt% of the solid electrolyte, and a binder in an amount greater than or equal to 0.1wt% and less than or equal to 1.0wt% based on 100wt% of the positive electrode active material, a 1C / 0.1C discharge energy ratio of 0.70 or more and a high discharge energy density, that is, high power, are achieved compared to a comparative example including each component outside the aforementioned range. On the other hand, because the 1C discharge energy becomes less than the 0.1C discharge energy, the 1C / 0.1C discharge energy ratio has an upper limit of less than 1.00.
[0174] Referring to the results of Table 1, it is confirmed that the D50 of the positive electrode active material is desirably greater than or equal to 1 μm and less than or equal to 20 μm. In addition, compared with Example 4 and Example 14, it is considered particularly desirable to contain two types of positive electrode active materials having different D50. Thus, if two types of positive electrode active materials having different D50 are contained, for example, Figure 2 As shown, not only the small particle size positive electrode active material is inserted into the space between the large particle size positive electrode active material to increase the positive electrode density, but also the positive electrode active material sufficiently ensures the contact area with the solid electrolyte layer.
[0175] In addition, referring to the results of Example 15, the small particle size positive electrode active material has a particle size greater than or equal to 1 μm and less than 10 μm, and the large particle size positive electrode active material has a particle size greater than or equal to 10 μm and less than or equal to 20 μm.
[0176] Referring to the results of Example 6, even if the type of the conductive auxiliary agent is changed, the effect of the present invention is achieved without problem. Referring to the results of Examples 16 and 17, even if the type of the solid electrolyte is changed, the effect of the present invention is achieved without problem.
[0177] Furthermore, although not described here, it can be easily inferred that results having the same tendency are obtained even if the type of the positive electrode active material and the type of the binder are changed.
[0178] Although the embodiments have been described in detail above, the scope of rights is not limited thereto, and various modifications and improvements made by those skilled in the art using the basic concept defined in the claims also fall within the scope of rights.
Claims
1. A positive electrode for a solid-state secondary battery, comprising: positive electrode current collector and positive electrode active material layer, The positive electrode active material layer comprises a positive electrode active material, a solid electrolyte, a binder and a conductive aid, The amount of the positive electrode active material based on 100 wt % of the positive electrode active material layer is greater than or equal to 85 wt % and less than or equal to 92 wt %, The amount of the solid electrolyte based on 100 wt % of the positive electrode active material layer is greater than or equal to 7 wt % and less than or equal to 15 wt %, When the amount of the positive electrode active material in the positive electrode active material layer is 100 wt %, the amount of the binder in the positive electrode active material layer is greater than or equal to 0.1 wt % and less than or equal to 1.0 wt %, and When the amount of the solid electrolyte in the positive electrode active material layer is 100 wt %, the amount of the conductive aid in the positive electrode active material layer is greater than or equal to 0.1 wt % and less than or equal to 10 wt %.
2. The positive electrode for a solid-state secondary battery according to claim 1, wherein The positive electrode active material has a D50 greater than or equal to 1 μm and less than or equal to 20 μm based on a volume-based particle size distribution obtained by a laser diffraction / scattering particle size distribution measurement method.
3. The positive electrode for a solid-state secondary battery according to claim 2, wherein The positive electrode active material includes two types of positive electrode active materials with different D50, wherein one of the two types of positive electrode active materials, a small particle size positive electrode active material, has a D50 greater than or equal to 1 μm and less than 10 μm, and the other, a large particle size positive electrode active material has a D50 greater than or equal to 10 μm and less than or equal to 20 μm.
4. The positive electrode for a solid-state secondary battery according to claim 3, wherein The small particle size positive electrode active material has the D50 greater than or equal to 2 μm and less than 8 μm, and the large particle size positive electrode active material has the D50 greater than or equal to 8 μm and less than or equal to 20 μm.
5. The positive electrode for a solid-state secondary battery according to claim 3, wherein The small particle size positive electrode active material has the D50 greater than or equal to 2 μm and less than 8 μm, and the large particle size positive electrode active material has the D50 greater than or equal to 10 μm and less than or equal to 20 μm.
6. The positive electrode for a solid-state secondary battery according to claim 1, wherein The positive electrode active material satisfies any one of Chemical Formula 1 or Chemical Formula 2: [Chemical formula 1] Li a Ni x Co y M 1-x-y O2 [Chemical formula 2] Li a Ni x Co y O2 (wherein M in Chemical Formula 1 is one or more metal elements selected from aluminum and manganese, and a, x, y, and 1 - x - y in Chemical Formula 1 and Chemical Formula 2 are numbers satisfying 0.20 ≤ a ≤ 1.20, 0.80 ≤ x < 1.00, 0 < y ≤ 0.20, and 0 < 1 - x - y ≤ 0.10).
7. The positive electrode for a solid - state secondary battery according to claim 1, wherein the solid electrolyte is a sulfide - based solid electrolyte including lithium, phosphorus, and sulfur, and the D50 of the volume - based particle size distribution obtained by the laser diffraction / scattering particle size distribution measurement method is greater than or equal to 0.1 μm and less than or equal to 3 μm.
8. The positive electrode for a solid - state secondary battery according to claim 1, wherein the volume density of the positive electrode active material layer after pressing is greater than or equal to 3.2 g / cm 3 .
9. A solid - state secondary battery, comprising the positive electrode according to any one of claims 1 to 8, the discharge energy density ratio obtained by dividing the discharge energy density at a discharge current of 1C by the discharge energy density at a discharge current of 0.1C is greater than or equal to 0.70 and less than 1.
00.
10. A method for manufacturing a positive electrode for a solid - state secondary battery, comprising forming the positive electrode active material layer by a dry method to manufacture the positive electrode for a solid - state secondary battery according to any one of claims 1 to 8.