Non-stick metal ware and non-stick pan
By applying PVD multi-metal film on non-stick metal utensils and pots to form a micro-nano-scale porous oil locking structure and aluminum homogenized layer, the problem of anti-stick coating falling off and physical non-stick structure easily destroyed at high temperatures is solved. It achieves high wear resistance and long-term non-stick effect, ensuring cooking safety.
Patent Information
- Application Number
- CN202310968560.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-07-14
- Filing Date
- 2023-08-03
- Publication Date
- 2024-11-12
AI Technical Summary
The anti-stick coating of existing non-stick pans is easy to fall off when used at high temperatures, which may release toxic gases. The physical non-stick structure is easily damaged in the heating environment, making it impossible to achieve a long-term non-stick effect.
A PVD multi-metal film is used to form a micro-nano-scale porous oil-locking structure with low surface energy on the micro-scale roughened surface, and an aluminum heat-hospital layer is installed on the inner layer of the pot to uniformly receive heat and extend the non-stick life.
It significantly improves the wear resistance and non-stick effect of non-stick metal utensils and pots, extends service life, and maintains non-stick properties at high temperatures, avoids the release of toxic substances, and ensures cooking safety.
Smart Images

Figure CN118924138A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of kitchenware, and in particular to a non-stick metal utensil and a non-stick cookware, which significantly improve the non-stick effect of the metal utensil. Background Art
[0002] The non-stick pans in the prior art are usually coated with a layer of anti-stick coating on the inner wall of the pan. The most commonly used coating material is Teflon, scientifically known as polytetrafluoroethylene, which solves the problem of sticking to the pan and brings some convenience to people's lives. However, the anti-stick coating on the inner wall of the pan is easy to fall off during use, especially during high-temperature stir-frying. If the non-stick pan is burned empty, it is more likely to cause the anti-stick coating to fall off. Although polytetrafluoroethylene itself is non-toxic, when the pan is in a high-temperature stir-frying or empty burning state, polytetrafluoroethylene will carbonize and crack, releasing trace amounts of toxic gases and substances, contaminating the food, thereby causing problems such as food sticking to the pan and accidental ingestion of chemical coatings.
[0003] On this basis, a non-stick pan has appeared in the prior art, which uses the lotus leaf effect to make an anti-stick structure on the inner wall of the pot. The anti-stick structure is a periodically distributed convex part or / and concave part on the inner wall, and the size of the convex part and the concave part is between a few microns and tens of microns. The inner wall surface of the non-stick pan becomes a rough surface with a roughness of micrometer level, and the contact surface between the cooked food and the inner wall surface of the non-stick pan becomes a composite contact surface. The concave areas between the convex parts of the anti-stick structure and the concave areas of the concave parts are adsorbed with gas, forming an air cushion layer, which effectively reduces the contact area between the cooked food and the inner wall surface of the non-stick pan, does not stick to the cooked food, and realizes physical anti-sticking and zero coating; even if the food is fried at high temperature and the pot is burned empty, the zero-coating non-stick pan does not release any toxic substances and gases, and will not pollute the cooked food and the kitchen environment, making cooking safer.
[0004] However, it is far from enough to apply this structure to the surface of a non-stick pan to form a physical non-stick layer. Because the non-stick pan needs to be heated when used, the air cushion layer formed in the recessed area recorded in the above scheme will be destroyed in the heating environment, thereby failing to achieve the purpose of physical non-stick.
[0005] In addition, if only the above-mentioned physical non-stick method is set on the surface of the pot body, it is not enough to achieve long-term non-stick. Because each time cooking is performed, the spatula needs to be rubbed against the surface of the pot repeatedly many times, then the long-term friction will wear out the physical non-stick layer, and thus the long-term non-stick effect cannot be achieved. This problem also needs to be solved urgently. Summary of the invention
[0006] The technical problem to be solved by the present invention is to overcome the deficiencies of the above-mentioned prior art and provide a non-stick metal utensil and non-stick cookware with high wear resistance and capable of achieving persistent non-stick properties. The PVD multi-metal film has a micron-scale roughened surface with a low surface energy micro-nano structure composed of multi-metals, which significantly improves the non-stick effect.
[0007] In order to achieve the above-mentioned purpose, the present invention provides a non-stick metal utensil, including a body; the inner surface of the body is constructed as a micron-scale roughened surface; wherein a PVD multi-metal film is attached to the micron-scale roughened surface, and the PVD multi-metal film is configured to form a micro-nano porous oil-locking structure with low surface energy on the micron-scale roughened surface. The micron-scale roughened surface is formed by sandblasting, preferably by multi-stage sandblasting, and can also be made into a micron-scale roughened surface by other methods. The roughness of the micron-scale roughened surface formed by sandblasting can usually reach Rz25~100μm, and the roughness Rz refers to the ten-point height of microscopic roughness, which refers to the sum of the average value of the five largest contour peak heights and the average value of the five largest contour valley depths within the sampling length L.
[0008] The above technical solution can be further improved through the following measures.
[0009] In one embodiment, the thickness h value of the PVD multi-metal film is less than the roughness Rz value of the micron-scale roughened surface. The thickness range of the PVD multi-metal film is 0.7 to 4.0 μm. The body includes a first metal layer, a heat-sinking layer, and a second metal layer from the inside to the outside, and the first metal layer and the second metal layer are combined into one by the heat-sinking layer so that the first metal layer is evenly heated. The first metal layer is a stainless steel layer, the heat-sinking layer is an aluminum layer, and the second metal layer is a stainless steel layer.
[0010] In one embodiment, the PVD multi-metal film includes a bottom layer, an intermediate layer and a surface layer deposited in sequence from bottom to top. The bottom layer contains metal titanium and / or metal chromium. The intermediate layer contains chromium nitride and aluminum nitride, wherein the content of chromium nitride is 60-80wt%, wherein the content of aluminum nitride is 20-40wt%; or, the intermediate layer contains chromium carbide, wherein the content of chromium carbide is 85-95wt%. The surface layer contains metal copper and aluminum oxide, wherein the content of metal copper is 1.0-10wt%. The surface layer also contains iron oxide, wherein the iron oxide is 3-15wt%. The thickness of the bottom layer is 0.1-1.0μm, the thickness of the intermediate layer is 0.5-3.8μm, and the thickness of the surface layer is 0.1-1.0μm. The hardness range of the PVD multi-metal film is HV1100-3500. The thickness range of the PVD multi-metal film is 0.7-4.0μm. The surface energy of the PVD multi-element metal film is less than 40 dynes, and the water drop angle thereof is greater than 95°.
[0011] Specifically, the PVD multi-element metal film was subjected to 5000 times of plane wear resistance test according to the Chinese national standard GB / T32095.2-2015, and the fried egg non-stickiness test result was evaluated as Grade I.
[0012] The present invention also provides a non-stick cookware, which is configured as the non-stick metal utensil.
[0013] Due to the adoption of the above technical solution, the present invention has the following beneficial effects:
[0014] The non-stick metal utensils and non-stick cookware of the present invention further deposit a low surface energy PVD multi-metal film on the roughened surface of the inner metal layer, and control the thickness of the PVD multi-metal film, so that a micro-nano porous oil-locking structure with low surface energy can be formed on the micron-level roughened surface, which has an excellent non-stick effect. At the same time, it can also significantly improve the adhesion of the PVD multi-metal film on the bottom layer, thereby increasing the service life of the non-stick metal utensils. In addition, in order to solve the technical problem that metal utensils are prone to local overheating and damage to the metal film during cooking, the cookware of the present invention also has an aluminum heat-dissipating layer between the two layers of metal. The aluminum heat-dissipating layer can make the bottom of the cookware heated more evenly, thereby extending the non-stick life of the non-stick cookware.
[0015] The PVD multi-metal film of the present invention has a low surface energy micro-nano porous oil-locking structure composed of nitrides, carbides and oxides of multi-metals (chromium and aluminum, and may also contain titanium, copper, iron, etc.), and its bottom layer is mainly metal titanium and / or metal chromium, which can improve the adhesion of the PVD multi-metal film on the body, thereby improving the service life of the metal film. Its surface layer is metal copper and aluminum oxide, so that a layer of oxide film is formed on the surface of the PVD multi-metal film to prevent the PVD multi-metal film from oxidative discoloration during use. At the same time, the metal copper can play an effective antibacterial role, especially against Escherichia coli and Staphylococcus aureus, with an antibacterial effect of more than 99.99%. In addition, it also has a good non-stick effect when the copper content is less than 10wt%. The surface energy of the PVD multi-element metal film in the present invention can reach less than 40 dynes, the water drop angle can reach more than 95 degrees, and it has a micro-nano porous oil-locking structure, so that it has excellent wear resistance and non-stick properties. After 5000 times of plane wear resistance test using the Chinese national standard GB / T32095.2~2015, the non-stick level can still reach Class I non-stick. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings of the embodiments will be briefly introduced below. Obviously, the drawings in the following description only relate to some embodiments of the present invention, but are not intended to limit the present invention.
[0017] Figure 1 It is a cross-sectional view of the non-stick metal container in Example 1.
[0018] Figure 2 yes Figure 1 Magnified view at A in the middle.
[0019] Figure 3 It is a schematic diagram of the non-stick structure of the non-stick metal container in Example 1.
[0020] Figure 4 This is a surface morphology image of the non-stick metal vessel in Example 1 (500 times).
[0021] Figure 5 This is a surface morphology image of the non-stick metal container in Example 1 (1000 times).
[0022] Figure 6 This is a surface morphology image of the non-stick metal vessel in Example 1 (5000 times).
[0023] Description of reference numerals:
[0024] 100. Non-stick cookware (non-stick metal utensil); 101. First metal layer; 102. Second metal layer; 103. Heat-saturating layer; 104. PVD multi-metal film. DETAILED DESCRIPTION
[0025] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the present invention will be further described in detail below with reference to the accompanying drawings. The components of the embodiments of the present invention described and shown in the accompanying drawings can be arranged and designed in various configurations. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] It should be noted that similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, further definition and explanation thereof is not required in subsequent drawings.
[0027] Unless otherwise defined, the technical terms or scientific terms used in this patent document shall have the usual meanings understood by people with ordinary skills in the field to which the invention belongs. The words "first", "second" and similar words used in the patent specification and claims of the present invention do not indicate any order, quantity or importance, but are only used to distinguish different components. Similarly, words such as "one", "an" or "the" do not indicate a quantity limitation, but indicate the existence of at least one. Words such as "include" or "comprise" mean that the elements or objects appearing before "include" or "comprise" include the elements or objects listed after "include" or "comprise" and their equivalents, and do not exclude other elements or objects. "Center", "up", "down", "left", "right", "vertical", "horizontal", "inside", "outside", "far", "near" and the like are only used to indicate relative positional relationships. When the absolute position of the described object changes, the relative positional relationship may also change accordingly. It is only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation of the present invention.
[0028] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be an indirect connection through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0029] Some embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. In the absence of conflict, the features of the following embodiments can be combined with each other.
[0030] Embodiment 1:
[0031] like Figures 1 to 6A non-stick metal utensil 100 is shown, comprising a first metal layer 101 and a second metal layer 102, wherein the first metal layer 101 is configured as an inner layer, and the inner surface of the first metal layer 101 is constructed as a micron-scale roughened surface having micron-scale holes, wherein the micron-scale roughened surface is formed by sandblasting, preferably by multi-stage sandblasting. Knurling treatment may also be used in other embodiments. Among them, a PVD multi-element metal film 104 is plated on the micron-scale roughened surface, and micro-nano-scale holes are distributed on the PVD multi-element metal film 104 to form a porous oil-locking structure; the first metal layer 101 and the second metal layer 102 are composited into one by a heat-dissipating layer 103, and the heat-dissipating layer 103 has a higher thermal conductivity than the first metal layer 101 to prevent the first metal layer 101 from being locally overheated and damaging the PVD multi-element metal film 104.
[0032] Physical vapor deposition (PVD) technology refers to the technology of using physical methods to vaporize the surface of the material source (solid or liquid) into gaseous atoms or molecules, or partially ionize into ions under vacuum conditions, and deposit a thin film with some special functions on the surface of the body through a low-pressure gas (or plasma) process. Physical vapor deposition is one of the main surface treatment technologies. PVD (physical vapor deposition) coating technology is mainly divided into three categories: vacuum evaporation coating, vacuum sputtering coating and vacuum ion coating. The main methods of physical vapor deposition are: vacuum evaporation, sputtering coating, arc plasma coating, ion coating and molecular beam epitaxy. The corresponding vacuum coating equipment includes vacuum evaporation coating machine, vacuum sputtering coating machine and vacuum ion coating machine. According to different uses, PVD (physical vapor deposition) coating technology can also be divided into tool plating and decorative plating. In order to ensure the thickness of the PVD multinary metal film, tool plating is used in the present application, so that the PVD multinary metal film can reach 0.7 to 4.0 microns. Preferably, the thickness of the PVD multinary metal film is 1.0 to 2.5 microns. Specifically, the thickness of the PVD multinary metal film is 2.0 microns, and in another embodiment, it can be 3 microns or 4 microns. It should be emphasized that the thickness of the PVD multinary metal film should be compatible with the micron-scale roughened surface. The thickness of the PVD metal film needs to be less than the Rz value of the micron-scale roughened surface, so that the PVD metal film can adhere to the micron-scale roughened surface to form a micro-nano porous oil-locking structure, and does not cover the micron-scale roughened surface. In the present application, the micro-nano porous oil-locking structure is formed on the basis of the micron-scale roughened surface.
[0033] It should also be noted that the micro-nano porous oil-locking structure refers to the deposition of nitrides, carbides and oxides of multiple metals (including at least chromium and aluminum, and further including titanium, copper and iron) on the micron-scale roughened surface by PVD coating technology, further forming micro-nano pores, the pore size of which is in the range of 0.1 to 3.0 microns, and in this embodiment, 0.1 to 1.0 microns. The specific size of the micron-scale pores can be measured by Zeiss's microscope Axioplan2imaging (model), and the size of the nano-scale pores can be measured by the scanning electron microscope Nova 400NanoSEM (model) of FEI (manufacturer) in the United States.
[0034] In a preferred embodiment, in order to further improve the service life of the PVD coating 104, the non-stick metal vessel adopts a steel-aluminum-steel composite structure, wherein the first metal layer 101 is a stainless steel layer, the heat-saturating layer 103 is an aluminum layer, and the second metal layer 102 is a stainless steel layer, such as SUS430. The selected stainless steel is preferably food grade, especially the first metal layer 101, such as SUS304. The second metal layer 102 mainly has a protective function. In addition to stainless steel, other metals can also be selected, such as titanium alloys. In order to further improve the non-stick effect of the inner surface, a plurality of etched grooves arranged in an array can be etched on the inner surface first, and then sandblasted. The grooves can be made by chemical etching or laser etching technology, or by knurling or biting, and a micron-level roughened surface is formed on the surface of the etched grooves. The array-arranged grooves can form a lotus leaf structure inside the non-stick metal vessel 100, thereby improving the non-stick effect.
[0035] In this embodiment, the micro-nano pores can shrink and expand as the heating temperature changes. When animal fats or vegetable oils are used to heat the pot, the micro-nano pores expand as the temperature of the pot body rises, and shrink as the temperature of the pot body drops. It is further explained that when the user heats the pot body, the micro-nano pores expand to facilitate the entry and exit of grease. When the heating of the pot body stops, the temperature of the pot body gradually cools down, the micro-nano pores shrink, and the grease that enters the holes is locked inside, thereby achieving the oil locking function and maintaining the non-stick performance of the pot surface. In this embodiment, the micro-nano pores with a pore diameter or opening width in the range of 0.1 to 1 μm have good oil storage and oil locking functions, thereby improving the non-stick effect of the pot surface. For specific views of the micro-nano pores, please refer to Figure 3 After oil accumulation, the hydrophobic contact angle of the PVD multi-element metal film micro-nano porous structure of the present invention can reach above 95, so that the present invention has an excellent non-stick effect.
[0036] In this embodiment, the PVD multi-metal film mainly comprises titanium, chromium and aluminum. The chromium content is 20-50at%, the aluminum content is 50-70at%, and the titanium content is 1-10at%. When the content of titanium is between 1-10at%, the surface energy can be effectively reduced, thereby improving the anti-sticking effect. Preferably, the content of titanium is 3-6at%, specifically, the content of titanium can be 3at%. The aluminum element contained in the PVD multi-metal film can reduce its surface energy, thereby improving the anti-sticking effect, and the aluminum content is preferably about 30at%. In addition to reducing the surface energy, the chromium element contained can also improve corrosion resistance and prevent the precipitation of heavy metals. The chromium content is preferably 50at%. The PVD multi-metal film includes a bottom layer, an intermediate layer and a surface layer deposited from bottom to top. The bottom layer contains metallic titanium and / or metallic chromium. In the bottom layer, titanium and chromium are both present in the form of metal, which is used to improve the adhesion of the PVD multi-metal film to the roughened surface, and can also prevent the precipitation of heavy metal substances from the first metal layer, affecting health. It is also noted that in the bottom layer, titanium and chromium can exist alone or at the same time, and both can achieve the purpose of preventing sticking and preventing the precipitation of heavy metals, but the performance of having both titanium and chromium will be better.
[0037] In the middle layer, nitrides and / or carbides of chromium aluminum are contained, and nitrides and / or carbides of titanium may be further contained. Specifically, it may be titanium nitride (TiN), chromium nitride (CrN), aluminum nitride (AlN), titanium carbide (TiC), chromium carbide (CrC), aluminum carbide (AlC), aluminum titanium nitride (AlTiN) and aluminum chromium nitride (AlCrN), aluminum titanium nitride (AlTiN), aluminum chromium nitride (AlCrN) and aluminum chromium carbide (Cr2AlC). Regarding the specific content of multi-metal, technicians in the relevant field can adjust it within the above range. It should be pointed out that nitrides and carbides of chromium aluminum can exist alone or at the same time. In particular, chromium carbide can significantly improve the hardness and wear resistance of PVD multi-metal film, as well as corrosion resistance, and can also improve the hydrophobicity of PVD multi-metal film. In another embodiment, chromium carbide can be added to the surface layer to further improve the hydrophobicity of PVD multi-metal film. Among nitrides, titanium nitride has good thermal stability and good thermal shock resistance. Aluminum nitride is in a ceramic state and has excellent thermal conductivity, which can prevent the PVD film from being destroyed due to local overheating. Chromium nitride has good corrosion resistance and can reduce the friction coefficient of the PVD film, making it have excellent wear resistance. Therefore, the combination of titanium chromium aluminum nitride and carbide has higher hardness and wear resistance. In addition, the intermediate layer can also make the PVD film of the present invention have good mechanical shock resistance and thermal shock resistance. Even when cooking directly with tools such as metal shovels, or when local overheating occurs, the PVD film is not easily damaged. The PVD multi-metal film in this embodiment has low surface energy, extremely high hardness and non-occupying performance. Specifically, its hardness can reach HV1000~5000, the surface energy can reach below 40 dynes, and the water drop angle is above 95 degrees.
[0038] Specifically, the middle layer in this embodiment contains chromium nitride and aluminum nitride, wherein the content of chromium nitride is 60-80wt%, specifically 75wt%, wherein the content of aluminum nitride is 20-40wt%, specifically 25wt%. In another embodiment, the middle layer contains chromium carbide, wherein the content of chromium carbide is 85-95wt%, and the remaining components are one or a combination of aluminum nitride and titanium nitride, and may also contain components such as aluminum carbide. The surface layer contains metallic copper and aluminum oxide, wherein the content of metallic copper is 1.0-10wt%, specifically 5wt%. The surface layer also contains iron oxide, wherein the content of iron oxide is 3-15wt%, specifically 10wt%, and may also be 5wt% or 12wt%. wt% is mass percentage. In the surface layer, except for metallic copper, aluminum oxide and iron oxide, the content of other components and impurities is less than 5wt%.
[0039] In this embodiment, the PVD film is a non-stick metal film layer with chromium and aluminum as main elements. The aluminum element contained in the PVD multi-element metal film can reduce its surface energy, thereby improving the anti-stick effect. In addition to reducing the surface energy, the chromium element contained can also improve the corrosion resistance and prevent the precipitation of heavy metals. In the PVD multi-element metal film in this embodiment, the main metal components are titanium, aluminum, chromium, iron and copper, and the non-metallic components mainly include oxygen, carbon, nitrogen and silicon.
[0040] The surface layer may also contain oxides of titanium and chromium, specifically, at least one of the oxides of titanium and chromium, such as titanium oxide, or a combination of titanium oxide and chromium oxide. The combination of metallic copper and aluminum oxide (combination of metallic copper and aluminum iron oxide) enables the surface layer to have good non-stick properties. The surface layer may form an oxide film on the surface of the PVD film, thereby preventing discoloration problems during later use. At the same time, aluminum oxide may prevent metallic copper from oxidizing to produce toxic copper oxide.
[0041] Adding metallic copper to the PVD multi-element metal film makes the PVD multi-element metal film have antibacterial effect. When the copper content is below 10wt%, the anti-sticking effect of the PVD multi-element metal film can be further improved.
[0042] In this embodiment, the bottom layer is attached to the micron-scale roughened surface, and the surface layer is attached to the surface of the middle layer. The thickness of the surface layer and the bottom layer are both small, specifically 0.1 to 1 μm, specifically 0.3 μm in this embodiment, and may also be 0.5 μm or 0.8 μm in other embodiments. The thickness of the middle layer is 5 to 6.8 μm, specifically 6.4 μm.
[0043] The inner surface of the PVD multi-element metal film 104 is a polished surface, for example, polished by high pressure water polishing or other methods. The thickness of the PVD multi-element metal film 104 ranges from 0.7 to 6.0 μm, preferably from 2 to 5 μm, and specifically from 2 μm.
[0044] On the basis of the above technical content, in order to construct a porous oil-locking structure with low surface energy, technicians in the relevant field can adjust the proportions of various components according to actual needs, or add other metal or non-metal components on the basis of the above multi-metal, such as further adding silicon element to form high melting point iron silicide. After testing, the hardness range of the PVD multi-metal film 104 is HV1000~5000, preferably the hardness range of the PVD multi-metal film 104 is HV1100~3500, and more preferably HV2000~3500. In addition, the PVD multi-metal film has a lower surface energy, but its hardness and wear resistance are extremely excellent, so that the present invention has good anti-sticking effect, high hardness, good wear resistance, and long service life.
[0045] In this embodiment, the wear resistance of the PVD multi-element metal film 104 is measured as follows: after 5000 wear tests according to the Chinese national standard "GB / T32095.2-2015 Non-stick surface performance and test specifications for household food metal cooking utensils Part 2: Non-stick and wear resistance test specifications", the oil-free frying egg test can reach Class I non-stick. Class I means that the egg can be taken out without damage and without leaving residue with a plastic spatula. Class II means that the egg cannot be taken out without damage with a plastic spatula, but the residue can be removed by wiping it lightly with a wet sponge or rag. The non-stick performance of the non-stick metal utensil 100 in the present invention is Class I. According to the long-term laboratory test results, the number of first-class eggs can reach 7 to 9, and the highest record is 20 first-class eggs, which greatly exceeds the Chinese standard requirement of 3 eggs.
[0046] The present invention also provides a PVD multi-element metal film 104 non-stick cookware 100, which is the above non-stick metal vessel 100. The non-stick cookware can be used as a frying pan, and the one with chromium carbide as the surface layer can be used as the inner pot of an electric rice cooker, a pressure cooker, etc.
[0047] From the above description, it can be seen that the present invention has the following beneficial effects:
[0048] The PVD multi-element metal film 104 non-stick metal vessel 100 and the PVD multi-element metal film 104 non-stick cookware 100 of the present invention, because the PVD multi-element metal film 104 is further deposited on the roughened surface of the inner metal layer, and the thickness of the PVD multi-element metal film 104 is controlled, the micron-level holes on the micron-level roughened surface can be turned into micro-nano-level holes, so that the inner metal surface has a good non-stick effect. However, during use, the bottom of the cookware is prone to local overheating and damages the PVD multi-element metal film 104, so that the cookware loses its non-stick performance. In order to solve this technical problem, the cookware of the present invention uses an aluminum heat-dissipating layer 103 between two layers of metal. The aluminum heat-dissipating layer 103 can make the bottom of the cookware heated more evenly, thereby extending the non-stick life of the cookware.
[0049] In summary, the non-stick metal utensil (non-stick cookware) 100 of the present invention has excellent non-stick performance. After 5000 times of wear resistance test, its non-stick level can still reach Class I non-stick. In addition, the present invention further prolongs the life of the non-stick performance because the bottom of the cookware is heated evenly. In addition, the materials used in the present invention meet the requirements of food hygiene indicators, do not contain heavy metal elements harmful to the human body, and are safe and healthy.
[0050] The above are only specific embodiments of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the protection scope of the claims.
Claims
1. A non-stick metal container, comprising a body; characterized in that: The inner surface of the body is configured as a micron-scale roughened surface; Wherein, a PVD multi-element metal film is attached to the micron-scale roughened surface, and the PVD multi-element metal film is configured to form a micro-nano-scale porous oil-locking structure with low surface energy on the micron-scale roughened surface.
2. The non-stick metal container according to claim 1, characterized in that: The PVD multi-element metal film comprises a bottom layer, an intermediate layer and a surface layer which are deposited in sequence from bottom to top.
3. The non-stick metal container according to claim 2, characterized in that: The base layer comprises metallic titanium and / or metallic chromium.
4. The non-stick metal container according to claim 3, characterized in that: The intermediate layer comprises chromium nitride and aluminum nitride, wherein the content of chromium nitride is 60-80wt%, and the content of aluminum nitride is 20-40wt%; or, The intermediate layer comprises chromium carbide, wherein the content of the chromium carbide is 85-95 wt %.
5. The non-stick metal container according to claim 4, characterized in that: The surface layer comprises metallic copper and aluminum oxide, wherein the content of the metallic copper is 1.0 to 10 wt %.
6. The non-stick metal container according to any one of claims 2 to 5, characterized in that: The thickness of the PVD multi-element metal film ranges from 0.7 to 4.0 μm.
7. The non-stick metal container according to any one of claims 2 to 5, characterized in that: The thickness of the surface layer is 0.1-1.0 μm.
8. The non-stick metal container according to any one of claims 2 to 5, characterized in that: The hardness range of the PVD multi-element metal film is HV1100-3500.
9. The non-stick metal container according to any one of claims 2 to 5, characterized in that: The surface energy of the PVD multi-element metal film is less than 40 dynes, and the hydrophobic angle after oil storage is greater than 95°.
10. The non-stick metal container according to any one of claims 2 to 5, characterized in that: The PVD multi-element metal film was subjected to 5000 times of plane wear resistance test according to the Chinese national standard GB / T32095.2-2015, and the fried egg non-stickiness test result was evaluated as Grade I.
11. The non-stick metal container according to claim 1, characterized in that Grooves are distributed on the inner side of the body, and the roughened surface is formed on the grooves.
12. The non-stick metal container according to claim 1, characterized in that The body includes a first metal layer, a heat-saturating layer, and a second metal layer in sequence from the inside to the outside. The first metal layer and the second metal layer are combined into one by the heat-saturating layer, so that the first metal layer is heated evenly.
13. The non-stick metal container according to claim 12, characterized in that: The first metal layer is a stainless steel layer, the heat-absorbing layer is an aluminum layer, and the second metal layer is a stainless steel layer.
14. A PVD multi-element metal film non-stick cookware, which is configured as the non-stick metal utensil according to any one of claims 1 to 13.
Citation Information
Cited By
Continuous production equipment for PVD (Physical Vapor Deposition) coating of pot
CN120844045A
Cookware coating equipment
CN223892838U