Nanofiltration membrane as well as preparation method and application thereof
By using triglycidyl isocyanurate and sucralose for interfacial polymerization, a nanofiltration membrane without active hydrogen groups was prepared, which solved the problem of functional layer destruction of nanofiltration membrane in sodium hypochlorite solution in the prior art, and achieved the goal of achieving the High chlorine resistance and stable ion retention rate.
Patent Information
- Application Number
- CN202411214246.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-31
- Publication Date
- 2024-11-12
AI Technical Summary
After the existing nanofiltration membrane is soaked in sodium hypochlorite solution, the active hydrogen groups in the polyamine-triformyl chloride system are prone to react, resulting in a significant reduction in functional layer integrity and ion retention.
The organic phase solution containing epoxy compounds and the aqueous phase solution containing hydroxy compounds were polymerized interfacially to prepare a nanofiltration membrane without active hydrogen groups, and specifically polymerized using triglycidyl isocyanurate and sucralose. , form a functional layer with good chlorine resistance.
The chlorine resistance of the nanofiltration membrane is improved, so that its retention rate in aqueous sodium hypochlorite solution does not change significantly, and a high ion retention rate and flux are maintained.
Smart Images

Figure BDA0005021083320000031 
Figure BDA0005021083320000041 
Figure BDA0005021083320000051
Abstract
Description
Technical Field
[0001] The invention belongs to the field of separation, and specifically relates to a nanofiltration membrane and a preparation method and application thereof. Background Art
[0002] Membrane separation technology is widely used in water treatment, material separation, purification, concentration and other fields. At present, membrane technology has gradually replaced traditional water treatment processes due to its energy saving, high efficiency, simple process and convenient operation. Nanofiltration membrane, as a kind of membrane separation technology, can effectively screen and intercept specific substances by using steric hindrance effect and charge repulsion effect.
[0003] Nanofiltration membranes usually include a nanofiltration base membrane and a functional layer; in the prior art, the functional layer is generally prepared by interfacial polymerization of polyamine aqueous phase monomers (such as polyethyleneimine, diethylenetriamine, m-phenylenediamine, p-phenylenediamine, etc.) and organic phase monomers (such as trimesoyl chloride). The acyl chloride groups present in the polyamine-trimesoyl chloride system are easily hydrolyzed into carboxyl groups during the reaction process, which improves the hydrophilicity of the nanofiltration membrane obtained by the polyamine-trimesoyl chloride, and therefore, it usually has a large flux. However, after being soaked in a sodium hypochlorite solution, the polyamide functional layer obtained by the polyamine-trimesoyl chloride system contains active hydrogen groups (such as -NH-CO-), which are easily oxidized by active chlorine such as hypochlorite to produce aromatic substitution reactions or N-chlorination reactions, resulting in the destruction of the integrity of the functional layer and a significant reduction in the ion interception rate. Summary of the invention
[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a nanofiltration membrane and a preparation method and application thereof.
[0005] To achieve the above object, the technical solution adopted by the present invention is:
[0006] A nanofiltration membrane comprises a nanofiltration base membrane and a functional layer arranged on the surface of the nanofiltration base membrane; the functional layer is obtained by polymerizing an organic phase solution containing an epoxy compound and an aqueous phase solution containing a hydroxyl compound.
[0007] The epoxy group-containing compound is triglycidyl isocyanurate.
[0008] The hydroxyl-containing compound is sucralose.
[0009] The nanofiltration base membrane is one of polysulfone, polyvinylidene fluoride, or polyvinyl chloride.
[0010] The present invention also includes a method for preparing the nanofiltration membrane, comprising the following steps: 1) immersing the nanofiltration base membrane in an aqueous solution containing a hydroxyl compound, and using a fan to sweep the surface of the nanofiltration base membrane, so that the aqueous solution containing the hydroxyl compound is evenly distributed on the surface of the nanofiltration base membrane; 2) continuing to immerse the nanofiltration base membrane in an organic solution containing an epoxy compound; 3) performing a high-temperature interfacial polymerization reaction to obtain the nanofiltration membrane.
[0011] The specific steps include:
[0012] Under room temperature conditions, the prepared nanofiltration base membrane filaments are first immersed in a stainless steel tank of an aqueous solution containing hydroxyl compounds by a drawing machine to control the full wetting of the outer surface of the membrane filaments. Then, the nanofiltration base membrane filaments are pulled into the pipeline from top to bottom at an angle perpendicular to the ground, and the surface of the hollow fiber membrane is purged from bottom to top by a blower to ensure that the aqueous solution containing hydroxyl compounds on the surface of the hollow fiber membrane is evenly distributed; then, the purged membrane filaments are pulled into a stainless steel tank filled with an organic solution containing epoxy compounds to ensure that the outer surface of the membrane filaments is fully wetting; finally, the completely wetted hollow fiber membrane is pulled into an oven for drying and high-temperature polymerization to obtain a hollow fiber nanofiltration membrane, and the prepared hollow fiber nanofiltration membrane is immersed in deionized water for standby use.
[0013] The mass concentration of the aqueous phase solution is 0.2-1.4%, preferably 0.5-1.0%.
[0014] The mass concentration of the organic phase solution is 0.05-0.3%, preferably 0.15%. The solvent of the organic phase solution is dimethyl sulfoxide.
[0015] In step 3), the temperature of high temperature polymerization is 60-100° C., preferably 80° C.; the polymerization time is 2-20 min; preferably 5-10 min.
[0016] The time for immersing in the aqueous phase solution in step 1) is 5-60 s, preferably 30 s; the time for immersing in the organic phase solution in step 3) is 40-120 s, preferably 60 s.
[0017] The present invention also includes an application of the nanofiltration membrane.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] The technical solution of the present application eliminates the presence of active hydrogen-containing groups in the composite nanofiltration membrane obtained by polymerizing an organic phase solution containing an epoxy compound with an aqueous phase solution containing a hydroxyl compound, thereby improving the chlorine resistance of the nanofiltration membrane. It can also be seen from the test data that the retention rate of the composite nanofiltration membrane does not change significantly after being immersed in an aqueous sodium hypochlorite solution, indicating that the membrane itself has significant chlorine resistance. DETAILED DESCRIPTION
[0020] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with embodiments.
[0021] A nanofiltration membrane comprises a nanofiltration base membrane and a functional layer arranged on the surface of the nanofiltration base membrane; the functional layer is obtained by polymerizing an organic phase solution containing an epoxy compound and an aqueous phase solution containing a hydroxyl compound. The epoxy compound is triglycidyl isocyanurate. The hydroxyl compound is sucralose. The nanofiltration base membrane is one of polysulfone, polyvinylidene fluoride, or polyvinyl chloride.
[0022] In this application, interfacial polymerization of triglycidyl isocyanurate and sucralose is used as an example, and PVDF is selected as the nanofiltration base membrane. The specific nanofiltration membrane is prepared in the following manner:
[0023] Example 1
[0024] At room temperature, the prepared PVDF hollow fiber nanofiltration membrane was immersed in a stainless steel tank containing 0.5 wt% sucralose aqueous solution by a drawing machine. The outer surface of the hollow fiber membrane was wetted for 30 seconds by process control. Then, the hollow fiber membrane was pulled from top to bottom at a perpendicular angle to the ground to a cross-sectional area of 0.25 m 2 The pipe is filled with air and the fan is used to blow air at 0.5m 3 The surface of the hollow fiber membrane is purged from bottom to top at a flow rate of 15 seconds at a flow rate of / min to ensure that the sucralose aqueous solution is evenly distributed on the surface of the hollow fiber membrane; the purged membrane fibers are then pulled into a stainless steel tank filled with a 0.05wt% triglycidyl isocyanurate organic solution with dimethyl sulfoxide as a solvent, and the outer surface of the hollow fiber membrane is ensured to be wetted for 60 seconds through process control; finally, the completely wetted hollow fiber membrane is pulled into an oven at 80°C and dried for 5 minutes to obtain a hollow fiber nanofiltration membrane, and the prepared hollow fiber nanofiltration membrane is immersed in deionized water for standby use.
[0025] The main difference between other embodiments and embodiment 1 is that the concentrations of the sucralose aqueous solution and the triglycidyl isocyanurate organic solution are different, and the infiltration time is adjusted accordingly to ensure sufficient infiltration, as shown in Table 1.
[0026] Table 1
[0027]
[0028] The main difference between Comparative Examples 1 and 2 and the embodiment is that the polymerization is carried out using a polyamine aqueous solution and a trimesoyl chloride organic solution, and the specific steps are as follows:
[0029] Comparative Example 1
[0030] At room temperature, the prepared PVDF hollow fiber membrane was immersed in a stainless steel tank containing 2.0 wt% polyethyleneimine aqueous solution by a drawing machine. The outer surface of the hollow fiber membrane was ensured to be wetted for 30 seconds by process control. Then, the hollow fiber membrane was pulled from top to bottom at an angle perpendicular to the ground to a cross-sectional area of 0.25 m 2 The pipe is filled with air and the fan is used to blow air at 0.5m 3 The surface of the hollow fiber membrane is purged from bottom to top at a flow rate of 100 μg / min for 15 seconds to ensure that the polyethyleneimine aqueous solution on the surface of the hollow fiber membrane is evenly distributed; the purged membrane fibers are then pulled into a stainless steel tank filled with a 0.5 wt% organic solution of trimesoyl chloride using n-hexane as a solvent, and the outer surface of the hollow fiber membrane is ensured to be wetted for 60 seconds through process control; finally, the completely wetted hollow fiber membrane is pulled into an oven at 40°C and dried for 5 minutes to obtain a hollow fiber nanofiltration membrane, and the prepared hollow fiber nanofiltration membrane is immersed in deionized water for standby use.
[0031] Comparative Example 2
[0032] At room temperature, the prepared PVDF hollow fiber membrane was immersed in a stainless steel tank containing 3.0 wt% polyethyleneimine aqueous solution by a drawing machine. The outer surface of the hollow fiber membrane was wetted for 30 seconds by process control. Then, the hollow fiber membrane was pulled from top to bottom at an angle perpendicular to the ground to a cross-sectional area of 0.25 m 2 The pipe is filled with air and the fan is used to blow air at 0.5m 3 The surface of the hollow fiber membrane is purged from bottom to top at a flow rate of 100 μg / min for 15 seconds to ensure that the polyethyleneimine aqueous solution on the surface of the hollow fiber membrane is evenly distributed; the purged membrane fibers are then pulled into a stainless steel tank filled with a 0.7 wt % organic solution of trimesoyl chloride using n-hexane as a solvent, and the outer surface of the hollow fiber membrane is ensured to be wetted for 60 seconds through process control; finally, the completely wetted hollow fiber membrane is pulled into an oven at 40°C and dried for 5 minutes to obtain a hollow fiber nanofiltration membrane, and the prepared hollow fiber nanofiltration membrane is immersed in deionized water for standby use.
[0033] The nanofiltration membrane obtained in the above embodiment was made into a membrane assembly by static casting. The membrane assembly was fixed on a cross-flow filtration test device, pure water passed through the membrane assembly under external pressure mode, and the pressure of the cross-flow filtration test device was set to pre-press for 1h under 0.4MPa pressure to fully compact the membrane, and then the following tests were performed: ① The cross-flow filtration test device was used as the feed liquid under an operating pressure of 0.3MPa, and the pure water passed through the membrane assembly under external pressure mode, and the water obtained within 10min was collected, and the pure water flux was tested using a weighing method. ② The cross-flow filtration test device was tested under an operating pressure of 0.3MPa with a 1000mg / L MgCl2 solution as the feed liquid, and the salt solution passed through the membrane assembly under external pressure mode. The salt concentration in the produced water was tested using a conductivity meter every 10min until it was stable and unchanged to obtain the retention rate. ③ The membrane assembly was fully soaked in a 1000mg / L NaClO aqueous solution for 1h, and then taken out and the retention rate of the 1000mg / L MgCl2 solution was tested in the same manner as in ②. The pure water flux and retention rate measured by the above steps are shown in Table 2 below.
[0034] Table 2
[0035]
[0036]
[0037] Result analysis:
[0038] It can be seen from Examples 1 to 5 that when the content of triglycidyl isocyanurate in the organic phase is increased from 0.05% to 0.15%, the retention rate of the prepared composite nanofiltration membrane for MgCl2 increases while the membrane flux decreases. Due to the increase in the concentration of triglycidyl isocyanurate, sucralose is more likely to undergo polymerization reaction with triglycidyl isocyanurate, which can not only increase the rate of the polymerization reaction, but also help to improve the network cross-linking degree of the obtained polymer, and the formed functional layer is more complete; however, when triglycidyl isocyanurate When the content is further increased to 0.3%, the retention rate of MgCl2 by the prepared hollow fiber nanofiltration membrane decreases instead of increases. This is because the concentration of triglycidyl isocyanurate is too high, resulting in a too fast polymerization reaction rate. The epoxy groups of triglycidyl isocyanurate are not fully reacted with sucralose, resulting in a disordered polymer. Moreover, with the rapid accumulation of the thickness of the functional layer, the resistance of sucralose to diffuse into the organic phase increases, which in turn leads to a decrease in the polymerization rate and the degree of cross-linking of the polymer, resulting in a decrease in the ion retention rate of the nanofiltration membrane and an increase in the flux.
[0039] It can be seen from Examples 3 and 6 to 12 that when the sucralose content in the aqueous phase is increased from 0.3% to 1.0%, the interception rate of the composite nanofiltration membrane for MgCl2 increases and the membrane flux decreases. As the concentration of sucralose in the solution increases, more sucralose molecules are easily polymerized with triglycidyl isocyanurate, which accelerates the polymerization reaction rate and improves the cross-linking degree of the polymer network, making the functional layer more uniform and dense, and the ion interception rate of the composite nanofiltration membrane is improved. However, when the sucralose content in the aqueous phase is further increased from 1.0% to 1.4%, the interception rate of the composite nanofiltration membrane decreases instead. This is because the excessive concentration of sucralose in the aqueous phase causes the prepared polymer to be sparse and disordered, and with the rapid superposition of the thickness of the functional layer, the resistance of sucralose diffusion into the organic phase increases, which in turn leads to a decrease in the polymerization rate and the degree of cross-linking of the polymer, so that the ion interception rate of the nanofiltration membrane decreases and the flux increases.
[0040] It can be seen from Example 3, Example 10 and Comparative Examples 1 and 2 that the nanofiltration membrane prepared by the polyethyleneimine-trimecyl chloride system and the nanofiltration membrane prepared by the sucralose-triglycidyl isocyanurate system have equivalent retention rates for MgCl2, and the acyl chloride groups present in the polyethyleneimine-trimecyl chloride system are easily hydrolyzed into carboxyl groups during the reaction, which improves the hydrophilicity of the nanofiltration membrane obtained by polyethyleneimine-trimecyl chloride and improves the flux compared with the nanofiltration membrane prepared by sucralose-triglycidyl isocyanurate. However, after being soaked in sodium hypochlorite solution, since the polyamide functional layer prepared by the polyethyleneimine-trimethylenediamine chloride system contains active hydrogen groups (such as -NH-CO-), it is easily oxidized by active chlorine such as hypochlorite to produce aromatic substitution reaction or N-chlorination reaction, resulting in the destruction of the integrity of the functional layer and a significant reduction in ion retention rate. The nanofiltration membranes prepared in Comparative Examples 1 and 2 have a significant reduction in retention rate after being soaked in sodium hypochlorite aqueous solution, which also confirms this conclusion. However, there are no groups containing active hydrogen in the composite nanofiltration membrane prepared by sucralose-triglycidyl isocyanurate, which improves the chlorine resistance of the nanofiltration membrane. It can also be seen from the test data that the retention rate of the composite nanofiltration membrane prepared by sucralose-triglycidyl isocyanurate has no significant change after being soaked in sodium hypochlorite aqueous solution, indicating that the membrane itself has obvious chlorine resistance.
[0041] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A nanofiltration membrane, characterized in that: The invention comprises a nanofiltration base membrane and a functional layer arranged on the surface of the nanofiltration base membrane; the functional layer is obtained by polymerizing an organic phase solution containing an epoxy compound and an aqueous phase solution containing a hydroxyl compound.
2. The nanofiltration membrane according to claim 1, characterized in that The epoxy group-containing compound is triglycidyl isocyanurate.
3. The nanofiltration membrane according to claim 1, characterized in that The hydroxyl-containing compound is sucralose.
4. The nanofiltration membrane according to claim 1, characterized in that The nanofiltration base membrane is one of polysulfone, polyvinylidene fluoride, or polyvinyl chloride.
5. A method for preparing a nanofiltration membrane according to any one of claims 1 to 4, characterized in that: The method comprises the following steps: 1) immersing a nanofiltration base membrane into an aqueous solution containing a hydroxyl compound, and using a fan to sweep the surface of the nanofiltration base membrane, so that the aqueous solution containing the hydroxyl compound is evenly distributed on the surface of the nanofiltration base membrane; 2) continuing to immerse the nanofiltration base membrane into an organic solution containing an epoxy compound; and 3) performing a high-temperature interfacial polymerization reaction to obtain a nanofiltration membrane.
6. The preparation method according to claim 5, characterized in that: The mass concentration of the aqueous phase solution is 0.2-1.4%, preferably 0.5-1.0%.
7. The preparation method according to claim 5, characterized in that: The mass concentration of the organic phase solution is 0.05-0.3%, preferably 0.15%. The solvent of the organic phase solution is dimethyl sulfoxide.
8. The preparation method according to claim 5, characterized in that: In step 3), the temperature of high temperature polymerization is 60-100° C., preferably 80° C.; the polymerization time is 2-20 min; preferably 5-10 min.
9. The preparation method according to claim 5, characterized in that: The time for immersing in the aqueous phase solution in step 1) is 5-60 s, preferably 30 s; the time for immersing in the organic phase solution in step 3) is 40-120 s, preferably 60 s.
10. Use of the nanofiltration membrane according to any one of claims 1 to 4.