Preparation method of full-biomass sepiolite aerogel and application of full-biomass sepiolite aerogel in oil-water separation
By preparing all-biomass sepiolite aerogel, using non-fluorinated coating technology and chitosan carrier, the problems of high cost and low efficiency in oil-water separation are solved, and efficient and environmentally friendly oil-water separation effect is achieved. Maintain adsorption capacity in harsh environments.
Patent Information
- Application Number
- CN202411215194.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-12
AI Technical Summary
The prior art has problems of high cost, low efficiency and poor selectivity in oil-water separation, making it difficult to effectively solve the problem of water pollution.
The multifunctional aerogel is prepared by non-fluorinated coating technology, using chitosan as a carrier, combined with sepiolite and polydimethylsiloxane for hydrophobization, and a full biomass sepiolite aerogel is prepared, using Separate from oil and water.
It achieves efficient and low-cost oil-water separation, has excellent adsorption ability and chemical stability, can be reused in harsh environments, and has environmentally friendly materials and low production costs.
Smart Images

Figure CN118925680A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of super-hydrophobic materials, and particularly relates to a preparation method of all-biomass sepiolite aerogel and application thereof in oil-water separation. Background Art
[0002] With the rapid development of society, water pollution has become one of the most serious environmental problems. It not only poses a huge threat to the underwater ecological environment, but also seriously affects the ecosystem and human health, thus attracting widespread attention from the society. At present, oil / organic solvents are one of the main water pollutants, which comes from oil / organic solvent leakage and abundant industrial wastewater discharge. However, response methods, such as in situ combustion, bioremediation and oxidative degradation, have disadvantages such as high cost, poor effective separation and selectivity, which seriously limit their wide practical application. Therefore, the development of a cost-effective and environmentally friendly wastewater remediation technology has become a focus of attention.
[0003] Zhai et al. mixed the purchased hydrophobic SiO2 with Sep particles and fixed them on a sponge with an adhesive PDMS to obtain a super hydrophobic sponge with an oil-water mixture separation efficiency greater than 99.85%. The adsorption method is one of the strategies that has attracted the most public attention due to its advantages of low cost, simple operation, high efficiency, and time saving. In recent years, aerogels, a three-dimensional material, have attracted widespread attention due to their advantages of low density, low cost, large surface area, easy processing, and high recyclability, especially chitosan aerogels. Chitosan has abundant oxygen-containing functional groups, is biodegradable, and non-toxic, and has been widely studied as a potential candidate material for water remediation. The present invention modifies the aerogel so that it can selectively absorb oil or water, thereby achieving oil-water separation. Summary of the invention
[0004] The present invention adopts non-fluorinated coating technology to prepare multifunctional aerogel, uses chitosan as a carrier to support sepiolite, and polydimethylsiloxane is used for hydrophobic treatment. The obtained aerogel has a high adsorption capacity for oil.
[0005] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0006] A full-biomass sepiolite aerogel, the preparation method of which comprises the following steps:
[0007] 1) Add chitosan CS to deionized water, gradually add acetic acid solution, and stir continuously under heating conditions to obtain a highly viscous solution;
[0008] 2) adding Sepiolite to the highly viscous solution, stirring vigorously until a homogeneous solution is formed, and freeze-drying to obtain Sep / CS aerogel;
[0009] 3) Take the hydrophobic material, add the curing agent, dissolve it in the organic solvent, stir to obtain a uniform suspension, immerse the Sep / CS aerogel in the suspension, and then vacuum dry the mixed system to obtain the all-biomass sepiolite aerogel PDMS@Sep / CS.
[0010] Furthermore, in the above preparation method, in step 1), the volume ratio of deionized water to acetic acid is 50:1.
[0011] Furthermore, in the above preparation method, in step 1), heating is performed at 60° C. with continuous stirring for 2 h.
[0012] Furthermore, in the above preparation method, the mass ratio of chitosan to sepiolite is 3 to 10:1.
[0013] Furthermore, in the above preparation method, in step 3), the hydrophobic material is selected from polydimethylsiloxane.
[0014] Furthermore, in the above preparation method, in step 3), the curing agent is diphenylbutyl carbamate.
[0015] Furthermore, in the above preparation method, in step 3), the organic solvent is n-hexane.
[0016] Application of the all-biomass sepiolite aerogel prepared by any of the above methods as an adsorbent in oil-water separation.
[0017] Furthermore, the above application method is as follows: adding the full-biomass sepiolite aerogel into the oil-water mixture and allowing it to stand for adsorption.
[0018] Furthermore, in the above application, the oil includes n-hexane, N,N-dimethylformamide, dichloromethane, chloroform, ethyl acetate, motor oil, peanut oil or olive oil.
[0019] The beneficial effects of the present invention are:
[0020] 1. Compared with pure chitosan aerogel, the PDMS@Sep / CS of the present invention has a higher specific surface area, provides more active sites during the adsorption process, and the internal pore volume of the material after freeze-drying is larger, which is more conducive to adsorption.
[0021] 2. The PDMS@Sep / CS of the present invention can separate oil and water and still has excellent adsorption effect in harsh environments such as strong acids and strong salts.
[0022] 3. The PDMS@Sep / CS of the present invention has excellent mechanical strength and chemical stability, and can realize multiple cycles of oil-water separation experiments. This multifunctional aerogel provides a new strategy for removing oil, heavy metal ions and other new pollutants in complex and harsh water environments.
[0023] 4. The super-hydrophobic modifier used in the present invention is a fluorine-free environmentally friendly reagent. The entire preparation method is very simple, does not require the use of expensive reagents, equipment and harsh experimental conditions, the raw materials are green and environmentally friendly, the production cost is low, the synthesized material has good stability, high separation efficiency and strong circulation performance, and solves the problem of high production cost in the existing method for preparing super-hydrophobic materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 Schematic diagram of the synthesis of PDMS@Sep / CS aerogel.
[0025] Figure 2 are the scanning electron microscope images of chitosan CS (a1, a2), Sep / CS aerogel (b1, b2), and PDMS@Sep / CS aerogel (c1, c2).
[0026] Figure 3 A photo of PDMS@Sep / CS aerogel on pine leaves (a) and digital photos of the designed and fabricated PDMS@Sep / CS aerogel in an ideal shape (bc).
[0027] Figure 4 The XRD spectrum (a), FT-IR spectrum (b) and XPS graph (c) of PDMS@Sep / CS.
[0028] Figure 5 Comparison photo of CS aerogel and PDMS@Sep / CS aerogel in water (a); photo of water droplets on PDMS@Sep / CS aerogel (b); photo of different liquid droplets on PDMS@Sep / CS aerogel (c); diagram of the dynamic contact process of water droplets on the surface of PDMS@Sep / CS aerogel (d); silver mirror phenomenon of PDMS@Sep / CS aerogel (e); waterproof performance of PDMS@Sep / CS aerogel (f).
[0029] Figure 6 This is the absorption performance diagram of PDMS@Sep / CS aerogel for different oils and organic solvents.
[0030] Figure 7 These are photos of the absorption process of n-hexane by PDMS@Sep / CS aerogel (a); and photos of the absorption process of dichloromethane by PDMS@Sep / CS aerogel (b).
[0031] Figure 8 These are photos of dynamic oil-water separation (pump separation) of oils of different densities using PDMS@Sep / CS, where the heavy oil / water is a dichloromethane / water mixture (a) and the light oil / water is a n-hexane / water mixture (b).
[0032] Fig. 9Schematic diagrams of the sand impact test (a1, a2), water impact test (b1, b2) and sandpaper abrasion test (c1, c2) and the water contact angle of PDMS@Sep / CS aerogel after the test.
[0033] Fig.10 It is the hydrophobic performance diagram of PDMS@CZIF-67 / CS in different harsh environments. DETAILED DESCRIPTION
[0034] Example 1 All-biomass Sepiolite aerogel (PDMS@Sep / CS)
[0035] (I) The preparation method is as follows:
[0036] PDMS@Sep / CS synthesis route Figure 1 .
[0037] 1) Preparation of CS:
[0038] 5 g of chitosan (CS) was added to 100 mL of deionized water, and 2 mL of acetic acid solution was gradually added, and the mixture was stirred continuously at 60 °C for 2 h to obtain a highly viscous solution.
[0039] 2) Preparation of Sep / CS aerogel:
[0040] 1.0 g Sep was added to the highly viscous solution and stirred vigorously until a homogeneous solution was formed; the solution was transferred to a 2 cm × 2 cm × 2 cm cubic mold, frozen at -20 ° C for 12 h, freeze-dried at -80 ° C for 24 h, soaked in anhydrous ethanol for 24 h to remove residual acetic acid, and dried to obtain Sep / CS aerogel.
[0041] 3) Preparation of PDMS@Sep / CS:
[0042] 0.847 g PDMS (polydimethylsiloxane) and 0.0847 g curing agent (butyl diphenylcarbamate) were dissolved in 50 mL n-hexane and stirred for 5 min to obtain a uniform suspension. The Sep / CS aerogel was soaked in the solution for 30 min, and the mixed system was placed in a vacuum oven at 120 ° C and dried for 2 h to synthesize the PDMS@Sep / CS aerogel.
[0043] (II) Testing
[0044] 1) The microstructures of chitosan (CS), Sep / CS aerogel and PDMS@Sep / CS aerogel were observed using a scanning electron microscope (test voltage: 10.0 kV, scale: 100 μm). Figure 2 .
[0045] like Figure 2As shown, the original CS aerogel has a highly interconnected porous network ( Figure 2 a1); CS aerogel surface is smooth ( Figure 2 The Sep fiber-like structures are well distributed in the aerogel framework, forming a rough and uneven surface ( Figure 2 b1), Sep in aerogel presents a rod-like crystal structure ( Figure 2 b2). PDMS treatment resulted in the formation of a PDMS layer around Sep, forming an uneven and rough structure similar to a film ( Figure 2 (c1, c2).
[0046] 2) PDMS@Sep / CS aerogel is ultra-light, such as Figure 3 As shown in Figure a, it can be placed on a relatively light substrate (pine leaves) without losing its shape. In addition, the simple and controllable method ensures that aerogels can be easily designed and manufactured into ideal shapes for various applications, such as cubes and other complex three-dimensional shapes ( Figure 3 (b, c).
[0047] 3) If Figure 4 As shown in Figure a, the chemical composition of PDMS@Sep / CS aerogel was analyzed by XRD. The typical peaks of synthesized Sep / CS appear at 2θ=7.35°, 20.7°, and 35.0°. In the Sep / CS spectrum, there are identifiable Sep / CS peaks. After hydrophobic modification, the crystal structure of the aerogel has no obvious changes. XRD results show that the aerogel was successfully prepared.
[0048] 4) If Figure 4 As shown in b, in the FTIR spectrum, at 1006 cm -1 and 469cm -1 The peaks at 802 cm-1 belong to the asymmetric stretching vibration of the O-Si-O bond and the Si-O-Si bending vibration in the tetrahedral silica sheet. The Sep / CS aerogel exhibits the characteristic peaks of CS and Sep, indicating the successful preparation of Sep / CS aerogel. -1 、1091cm -1 and 1260cm -1 The broad peaks are Si-C stretching vibration, Si-O-Si and Si-CH3 stretching vibration, indicating that PDMS is successfully deposited on the sample.
[0049] 5) If Figure 4 As shown in c, the XPS spectrum shows that the sample is mainly composed of C, N, O and Si atoms ( Figure 4In (c), the peaks of Si 2s and Si 2p were detected, corresponding to Si-O and Si-C bonds, respectively. These phenomena confirmed that PDMS was successfully modified. The results of XPS analysis further proved the successful synthesis of aerogel.
[0050] Example 2 Application of all-biomass sepiolite aerogel PDMS@Sep / CS in oil-water separation
[0051] The application of aerogel as adsorbent material in oil-water separation was investigated.
[0052] Adsorption capacity is a standard for evaluating the performance of oil-absorbing materials and can be measured by the following procedure. A single aerogel is weighed and then placed in different types of oils and organic solvents for adsorption tests. After adsorption saturation, it is taken out and the oil and organic solvent on the surface are wiped off with filter paper, and then the aerogel after oil absorption is weighed. The adsorption capacity (Q) is calculated by the following formula:
[0053]
[0054] Among them, m0 and m1 are the weights of aerogel before and after adsorption, respectively.
[0055] (I) Wetting ability of PDMS@Sep / CS
[0056] Pure chitosan aerogel is hydrophilic, and its hydrophobicity increases after adding PDMS and Sep ( Figure 5 (a). The water droplet maintains a stable spherical shape on the PDMS@Sep / CS surface ( Figure 5 (b) Different liquid droplets maintain a stable spherical shape on the PDMS@Sep / CS surface ( Figure 5 (c). Water droplets can make dynamic contact on the PDMS@Sep / CS surface ( Figure 5 (d) A large number of bubbles appear around the surface of PDMS@Sep / CS in water, resulting in mirror reflection ( Figure 5 e). PDMS@Sep / CS also exhibits strong repellency to the impinging water flow ( Figure 5 (f)
[0057] (II) Saturated adsorption of PDMS@Sep / CS on different oils and organic solvents
[0058] The saturated adsorption capacity of PDMS@Sep / CS for three oils (motor oil, peanut oil, and olive oil) and organic solvents (n-hexane, N,N-dimethylformamide, dichloromethane, chloroform, and ethyl acetate) was investigated.
[0059] Depend on Figure 6It can be seen that the absorption capacity depends on the density and viscosity of the oils and organic solvents. When the organic solvent is chloroform, the absorption capacity is the highest, reaching 12 times its own weight. The recyclability of these oils and organic solvents was evaluated, and after 12 cycles of adsorption and desorption, the absorption capacity did not decrease significantly. This excellent recyclability is mainly due to the chemical durability, porous structure and strong layered roughness of the PDMS layer.
[0060] (III) Practical Application
[0061] The practical application of PDMS@Sep / CS in oil spill cleanup was investigated, simulating the separation of mixed oil from a mixture under natural conditions. The selective adsorption experiments were conducted using Sudan III-dyed n-hexane (light oil) and dichloromethane (heavy oil) mixed with water.
[0062] Depend on Figure 7 As can be seen from a1-a4, PDMS@Sep / CS can selectively adsorb n-hexane. When the material comes into contact with n-hexane in the upper layer of water, n-hexane can be quickly absorbed into the material within seconds, and static separation of n-hexane and water can be achieved. No red pollutants are observed in the water. Figure 7 As can be seen from b1-b4, when the material comes into contact with dichloromethane in the water layer, dichloromethane can be quickly absorbed into the material within seconds, and static separation of water and dichloromethane can be achieved, and no red pollutants are observed in the water. In summary, it can be shown that the material has high separation efficiency and is pollution-free.
[0063] (IV) Continuous oil-water separation capability of PDMS@Sep / CS
[0064] The continuous oil-water separation capability of PDMS@Sep / CS was investigated. Figure 8 .
[0065] One end of the peristaltic pump catheter was inserted into PDMS@Sep / CS and placed in a dichloromethane / water mixture ( Figure 8 a) or n-hexane / water mixture ( Figure 8 In b), the organic phase is gradually transferred to the beaker at the other end of the conduit under the drive of the peristaltic pump. After the separation, there is no residue in the aqueous phase and the organic phase.
[0066] (V) Investigation of the mechanical stability of all-biomass sepiolite aerogel PDMS@Sep / CS
[0067] The chemical stability of PDMS@Sep / CS was investigated. The surface stability and durability of PDMS@Sep / CS play a vital role in practical applications.
[0068] like Fig. 9As shown in the figure, the mechanical stability of PDMS@Sep / CS aerogel was tested by sand impact test, water impact test and sandpaper grinding test. After 20 cycles of grinding test, the aerogel can still maintain superhydrophobicity, which is attributed to the reaction of PDMS chain with hydroxyl groups on the surface of aerogel to form polysiloxane and the presence of binder, which synergistically promotes the firmness of the coating.
[0069] like Fig.10 As shown, when exposed to various harsh environments such as strong acid, strong salt, high temperature and freezing, PDMS@Sep / CS will not lose its superhydrophobicity and maintain good water resistance, and the contact angle can still be maintained above 150°, proving that they have good chemical stability.
Claims
1. A full-biomass sepiolite aerogel, characterized in that: The preparation method thereof comprises the following steps: 1) Add chitosan CS to deionized water, gradually add acetic acid solution, and stir continuously under heating conditions to obtain a highly viscous solution; 2) adding Sepiolite to the highly viscous solution, stirring vigorously until a homogeneous solution is formed, and freeze-drying to obtain Sep / CS aerogel; 3) Take the hydrophobic material, add the curing agent, dissolve it in the organic solvent, stir to obtain a uniform suspension, immerse the Sep / CS aerogel in the suspension, and then vacuum dry the mixed system to obtain the all-biomass sepiolite aerogel PDMS@Sep / CS.
2. The all-biomass sepiolite aerogel according to claim 1, characterized in that: In step 1), the volume ratio of deionized water to acetic acid is 50:
1.
3. The all-biomass sepiolite aerogel according to claim 1, characterized in that: In step 1), heat at 60°C with continuous stirring for 2 h.
4. The all-biomass sepiolite aerogel according to claim 1, characterized in that: By mass ratio, chitosan: sepiolite = 3-10:
1.
5. The all-biomass sepiolite aerogel according to claim 1, characterized in that: In step 3), the hydrophobic material is selected from polydimethylsiloxane.
6. The all-biomass sepiolite aerogel according to claim 1, characterized in that: In step 3), the curing agent is diphenylbutyl carbamate.
7. The all-biomass sepiolite aerogel according to claim 1, characterized in that: In step 3), the organic solvent is n-hexane.
8. Use of the all-biomass sepiolite aerogel according to any one of claims 1 to 7 as an adsorbent in oil-water separation.
9. The use according to claim 8, characterized in that: The method is as follows: add all-biomass sepiolite aerogel into the oil-water mixture and let it stand for adsorption.
10. The use according to claim 9, characterized in that: The oil includes n-hexane, N,N-dimethylformamide, dichloromethane, chloroform, ethyl acetate, motor oil, peanut oil or olive oil.
Citation Information
Patent Citations
Application of composite adsorbent in treating oily wastewater
CN108439523A
Preparation method of fuel thickener capable of being degraded and recycled easily
CN109762525A
Nano chitin composite aerogel as well as preparation method and application thereof
CN112646240A
Sepiolite-graphene oxide / chitosan composite gel ball as well as preparation method and application thereof
CN116037069A
Oil-water separator filter combining nanoparticles and soot impregnated on sponges, and method for preparing the same
WO2023084298A1