Catalyst for catalytic combustion of chlorine-containing organic waste gas as well as preparation method and application of catalyst
By using vanadium and tungsten elements in the catalyst, combining elements such as cerium and ruthenium to form a catalyst with polyvalent characteristics, the efficiency and cost problems of existing catalysts when treating halogen-containing volatile organic matter are solved, and high efficiency and low energy are achieved catalytic effects and long-lived industrial applications.
Patent Information
- Application Number
- CN202411048763.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-12
AI Technical Summary
When existing catalysts treat volatile organic compounds containing a variety of halogen, they are difficult to maintain high efficiency, have weak anti-toxicity, have short service life, and are relatively high in preparation costs, which cannot meet the needs of industrial-scale production.
Vanadium and tungsten elements are used as transition metals, combined with cerium, ruthenium and other elements, and a catalyst with polyvalent characteristics is formed through a specific preparation method, which improves the anti-toxicity and service life of the catalyst and reduces the preparation cost.
It achieves efficient catalytic oxidation under low temperature conditions, extends the service life of the catalyst, reduces energy consumption, improves corrosion and poisoning resistance, and has relatively low production cost, which is suitable for industrial-scale applications.
Abstract
Description
Technical Field
[0001] The present application relates to a catalyst for catalytic combustion of chlorine-containing organic waste gas, a preparation method and application thereof, and belongs to the technical field of waste gas treatment. Background Art
[0002] Volatile organic compounds (VOCs) are a type of harmful organic chemical substances that pose potential risks to the ecological environment and human health. Common VOCs include benzene, toluene, xylene, styrene, trichloroethylene, trichloromethane, trichloroethane, diisocyanate (TDI), diisocyanatoluene, etc. There are many types of VOCs, and they are difficult to degrade at low temperatures.
[0003] The existing treatment technology is mainly catalytic combustion at high temperature. Due to the high energy consumption, incomplete catalytic effect, and part of the tail gas after treatment does not meet the emission standards of relevant national laws, it cannot be completed in the project acceptance. Therefore, the development of a catalyst that can reduce the temperature, has high catalytic efficiency, and has a single tail gas product has become one of the mainstream directions of industrial catalyst research and development.
[0004] At present, the mainstream catalyst types can be divided into precious metal catalysts and non-precious metal catalysts. Precious metal catalysts have high catalytic efficiency, less by-products, complete combustion, and long service life, but they are usually expensive, and in the case of complex exhaust gas components, the catalyst is easily deactivated by halogen elements such as sulfur / chlorine during operation. The advantage of non-precious metal catalysts is that they are low in cost and are usually used in industries that do not have high requirements for exhaust emissions. However, their catalytic effect is far inferior to that of precious metal catalysts.
[0005] The patent with publication number CN113426458A discloses a catalyst for catalytic combustion of halogen-containing mixed organic matter, and the catalyst mainly includes a monolithic or granular carrier and an active coating with high viscosity. Due to its good catalytic effect, but weak resistance to chlorine poisoning, after long-term operation for a period of time, the catalyst is poisoned and cannot be used continuously. The catalyst needs to be replaced regularly, and there is a problem of high cost. The patent with publication number CN117772817A discloses a method for preparing a catalyst. Its catalyst cost is relatively low, but the catalytic temperature is high, and catalysis cannot be completed at low temperatures, so the physical cost of catalysis is high, there is no high economic value, and the catalyst has a weak ability to resist poisoning, which is not applicable to complex industrial conditions and catalysts with high requirements. Patent publication number CN115591548A discloses a low-temperature oxidation, low calorific value, high-efficiency Pt / Pd bimetallic catalyst and a preparation method thereof. Although the catalyst has a long life, it cannot resist the presence of various volatile organic compounds such as chlorine and other halogens. In addition, the precious metals used are expensive. In the case of large industrial demand, the cost cannot be controlled and it can only be used in gases with relatively single exhaust gas components. Therefore, when the exhaust gas composition is complex and the exhaust gas emission quality requirements are high, its advantages cannot be brought into play.
[0006] In summary, there is an urgent need for an efficient catalyst that can catalyze a variety of halogen-containing volatile organic compounds, has a long service life, has excellent catalytic effect, and whose preparation cost can be controlled within an industrially acceptable range and can be mass-produced. Summary of the invention
[0007] In order to solve the problem that the catalysts existing in the prior art of treating halogen-containing volatile organic compounds are difficult to take into account anti-poisoning, mild catalytic conditions, and universal applicability to waste gases with complex components while maintaining high efficiency, the present application provides a catalyst for catalytic combustion of chlorine-containing organic waste gas, and a preparation method and application thereof, which utilizes vanadium and tungsten as transition state metal elements with many variable valence states. They are used in the preparation process of precious metal catalysts to change the interaction between active components and achieve better adaptation to various catalytic reactions.
[0008] This application adopts the following technical solutions:
[0009] A method for preparing a catalyst for catalytic combustion of chlorine-containing organic waste gas comprises the following steps:
[0010] S1, washing and drying the inorganic oxide raw material and then calcining it to obtain an inorganic oxide support;
[0011] S2, placing the inorganic oxide support in a cerium salt solution, impregnating I, drying II, and then calcining II to obtain an inorganic oxide support loaded with cerium;
[0012] S3, mixing a solution containing vanadium salt and tungsten salt with a ruthenium trichloride solution to form a precursor liquid, placing the inorganic oxide carrier loaded with cerium into the precursor liquid, impregnating II, drying III and then calcining III to obtain the catalyst for catalytic combustion of chlorine-containing organic waste gas.
[0013] Optionally, in step S2, the concentration of the cerium salt solution is 0.01 to 0.02 mol / mL in terms of molar concentration of cerium element.
[0014] Optionally, in step S3, the volume of the solution containing the vanadium salt and the tungsten salt is the same as the saturated adsorption volume of the liquid at the saturated water absorption rate of the inorganic oxide support.
[0015] After calculating the water absorption rate of the inorganic oxide support, the vanadium salt and the tungsten salt are dissolved in water to prepare a solution with the same volume as the water absorption rate of the inorganic oxide support. Then a small amount of ruthenium trichloride solution is added and stirred evenly until the granular salt in the water completely disappears to form a precursor aqueous solution.
[0016] Optionally, in step S3, the molar ratio of vanadium element to tungsten element in the vanadium salt and the tungsten salt is 1 to 10:1;
[0017] Optionally, in step S3, the concentration of the vanadium salt is 0.0025 to 0.003 mol / mL in terms of molar concentration of vanadium element.
[0018] Optionally, in step S3, the concentration of the ruthenium trichloride solution is 0.000048 to 0.00006 mol / mL in terms of molar concentration of ruthenium element.
[0019] Optionally, in step S3, the volume ratio of the solution containing vanadium salt and tungsten salt to the ruthenium trichloride solution is 12 to 48:1.
[0020] Optionally, the conditions of impregnation I and impregnation II independently include: an impregnation time of 3 to 5 hours.
[0021] Optionally, the conditions of impregnation I and impregnation II also include complete impregnation.
[0022] The main method of judging whether the impregnation is complete is to shake the beaker repeatedly intermittently for half an hour, repeat 4 to 5 times, and observe that there are no water drops on the beaker wall, and the surface color of the carrier changes after absorbing water. This is used to judge whether the impregnation is uniform. There is no residue of cerium solution in step S2, and the precursor solution in step S3 is also completely absorbed.
[0023] Optionally, the conditions of calcination I, calcination II, and calcination III independently include: calcination temperature 400-500° C., calcination time 4-8 h;
[0024] Optionally, the conditions of drying I, drying II, and drying III independently include: drying temperature of 80 to 110° C., and drying time of 6 to 12 hours.
[0025] Optionally, the inorganic oxide is selected from at least one of cerium oxide powder, zeolite, sepiolite, porous carbon material, spherical silica, monolithic honeycomb ceramics, and spherical alumina.
[0026] Optionally, the vanadium salt is selected from at least one of ammonium metavanadate, sodium metavanadate, potassium metavanadate, sodium orthovanadate, vanadyl sulfate, vanadyl oxalate, vanadium tetrachloride, and vanadium trichloride.
[0027] Optionally, the tungsten salt is selected from at least one of sodium tungstate, calcium tungstate, cobalt tungstate, cadmium tungstate, ferrous tungstate, and ammonium tungstate.
[0028] Optionally, the cerium salt is selected from at least one of cerium nitrate, cerium oxalate and cerium sulfate;
[0029] Optionally, the specific surface area of the inorganic oxide is 5 to 500 m 2 / g.
[0030] Optionally, the particle size of the inorganic oxide carrier is 2 to 200 μm.
[0031] According to another aspect of the present application, a catalyst for catalytic combustion of chlorine-containing organic waste gas prepared by the above preparation method is provided, wherein the molar ratio of the vanadium element to the tungsten element in the catalyst is 1:1-10;
[0032] The content of vanadium element is 0.01-0.5wt%;
[0033] The content of ruthenium element is 0.01 to 5 wt%;
[0034] The active component elements include cerium, vanadium, tungsten and ruthenium.
[0035] According to another aspect of the present application, there is also provided a catalyst for catalytic combustion of chlorine-containing organic waste gas prepared by the above preparation method, and the use of the above catalyst for catalytic combustion of chlorine-containing organic waste gas in catalytic combustion of halogen-containing volatile organic matter.
[0036] Optionally, the application includes: preheating the organic waste gas containing mixed halogen volatile organic compounds at 200-450° C. and contacting it with a catalyst for catalytic combustion of chlorine-containing organic waste gas fixed in a catalytic combustion device.
[0037] Optionally, the application specifically includes: assembling a monolithic or granular catalyst for catalytic combustion of chlorine-containing organic waste gas onto a reaction bed of a catalytic combustion device, blowing the organic waste gas containing mixed halogen volatile organic matter through the above device by a fan, so that the organic waste gas is preheated to 200-450°C under the action of a heat exchanger and an electric heating tube, and then contacts with the catalyst on the surface of the catalytic combustion assembly on the reaction bed and undergoes a catalytic combustion reaction to generate tail gas containing carbon dioxide, water, hydrogen chloride and chlorine. The tail gas is absorbed by a spray tower containing an alkaline solution to remove hydrogen chloride and chlorine, and finally carbon dioxide and water are discharged, thereby achieving the purification of halogen volatile organic matter.
[0038] The beneficial effects of this application include:
[0039] The catalyst for catalytic combustion of chlorine-containing organic waste gas provided by the present application adopts three active components, and ruthenium is loaded in the mesopores on the surface of the inorganic oxide carrier by thermal decomposition. The addition of precious metal ruthenium can effectively prevent the influence of halogen elements such as chlorine, and avoid catalyst poisoning during the operation of the catalyst. The addition of vanadium and tungsten can effectively change the loading capacity of ruthenium in the carrier, which can make it firmly fixed in the carrier, thereby extending its service life. The catalyst also has efficient catalytic oxidation ability, good corrosion resistance and poisoning resistance, and solves the shortcomings of active component shedding, short service life and non-corrosion resistance during the use of existing catalysts. The preparation method of the catalyst for catalytic combustion of chlorine-containing organic waste gas provided by the present application is simple, can be well connected with industry, and the preparation cost is relatively low, and can be applied on a large scale. The catalyst of the present application is used in catalytic combustion treatment applications containing halogenated volatile organic compounds. The catalytic temperature is relatively low, and in the process of large-scale industrial use, energy consumption can be greatly reduced, which not only responds to the country's low-carbon requirements, but also improves industrial acceptability. The exhaust gas components after catalytic combustion treatment are relatively simple and green, and do not require secondary treatment, with good ecological and environmental benefits. DETAILED DESCRIPTION
[0040] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.
[0041] Unless otherwise specified, the raw materials in the examples of this application were purchased through commercial channels.
[0042] Unless otherwise specified, conventional methods were used for testing and instrument settings were those recommended by the manufacturer.
[0043] The element content in the catalyst is the theoretical loading amount, that is, when the impregnation is complete, the element components in the impregnation solution are completely absorbed and regarded as the content when all the raw metal elements are loaded. The element content = (element weight / total catalyst weight)*100%.
[0044] The molar ratio of vanadium to tungsten in the catalyst is a theoretical ratio, that is, the molar ratio of vanadium to tungsten when the impregnation is complete and the element components in the impregnation solution are completely absorbed and the raw material metal elements are considered to be fully loaded.
[0045] In this embodiment, the conversion rate is calculated as follows:
[0046] (import peak area - outlet peak area) / import peak area × 100%.
[0047] The inlet peak area and the outlet peak area are obtained by sampling with a gas chromatograph.
[0048] According to one embodiment of the present application, the catalyst for catalytic combustion of chlorine-containing organic waste gas is composed of an inorganic oxide carrier and an active component coating supported on the carrier, wherein the inorganic oxide carrier is spherical alumina with a specific surface area of 5 to 500 m 2 / g, the molar ratio of transition metal vanadium to tungsten is 1 to 10, and the weight percentage of precious metal ruthenium is 0.01 to 5%. The application of the prepared catalyst in the catalytic combustion of halogen-containing volatile organic matter includes: taking an appropriate amount of catalyst, placing it in a tubular fixed bed reactor for testing, and the experimental conditions are as follows: 20% oxygen, 80% nitrogen, the mixed gas is placed in a micro pump and then heated by a heating belt and blown into the reaction system, wherein the mixed gas is a mixed gas containing chloroform, dichloromethane, ethyl acetate, chlorobenzene, and DMF, and the concentration of the mixed gas is controlled to be 500 to 1000 ppm, the relative humidity is 50%, and the reaction space velocity is 15000 to 20000 h -1 .
[0049] Example 1
[0050] Preparation of catalyst:
[0051] S1, washing the spherical alumina raw material, drying it at 110°C for 8 hours, and then calcining it at 500°C for 8 hours to obtain an inorganic oxide carrier for standby use;
[0052] The adsorption isotherm of the sample was tested using a physical adsorption instrument (Machine ASAP3020, USA). Then, based on the characteristics of the sample, the BET theoretical model was selected to calculate the specific surface area of the sample. The specific surface area of spherical alumina is about 300 m 2 / g; the crystal structure of the sample was tested by XRD (Bruker D8 Advance, Germany), and the particle size of the oxide was calculated to be about 150 μm according to the Scherrer formula.
[0053] S2, placing the inorganic oxide support in a cerium salt solution (the concentration of the cerium salt solution is 0.01 mol / mL based on the molar concentration of the cerium element), immersing for 3 hours to completely immerse, filtering, drying at 110° C. for 8 hours, and then calcining at 450° C. for 8 hours to obtain an inorganic oxide support loaded with cerium for use;
[0054] S3. Add ammonium metavanadate (vanadium salt) and ammonium paratungstate (tungsten salt) into water to prepare a mixed solution (the molar concentration of vanadium element in the mixed solution is 0.0025 mol / mL, and the molar concentration of tungsten element is 0.00000192 mol / mL), and add ruthenium trichloride into water to prepare a ruthenium trichloride solution (the molar concentration of ruthenium element in the ruthenium trichloride solution is 0.000048 mol / mL); then mix the mixed solution with the ruthenium trichloride aqueous solution in a volume ratio of 24:1 to form a precursor liquid; then place the cerium-loaded inorganic oxide support into the precursor liquid (the volume of the solution containing vanadium salt and tungsten salt is the same as the saturated adsorption volume of the liquid at the saturated water absorption rate of the inorganic oxide support, and the saturated water absorption rate of the inorganic oxide support is marked as 0.5 mL / g by the manufacturer when purchased), immerse for 4 hours to completely immerse, dry at 80°C for 4 hours, and then calcine at 400°C for 8 hours to obtain the catalyst for catalytic combustion of chlorine-containing organic waste gas, marked as catalyst #1.
[0055] In the catalyst #1, the content of vanadium element is 8 wt %, and the molar ratio of vanadium element to tungsten element is 1:1.
[0056] Application in catalytic combustion of halogenated volatile organic compounds:
[0057] 52g of catalyst #1 was placed in a tubular fixed bed reactor for testing. The experimental conditions were as follows: a mixture of 20% oxygen, 80% nitrogen and chlorine-containing organic waste gas (the waste gas component was DMF (22.8mg / m 3 )、Toluene (205mg / m 3 ), chlorobenzene (114.9 mg / m 3 ), dichloromethane (2862.6mg / m 3 ), ethyl acetate (653 mg / m 3 ) is placed in a micro pump and then heated to 130°C by a heating belt. After preheating, it is blown into the reaction system, contacts the catalyst fixed in the fixed bed reactor and undergoes a catalytic combustion reaction. During the process, the mixed gas concentration is controlled to be 500ppm, the relative humidity is 50%, and the reaction space velocity is 15000h -1 The conversion rates of the catalytic combustion reaction at different times and temperatures are shown in Table 1.
[0058] Table 1
[0059] 5h 7h 720h 200℃ 30.52% 31.17% 30.12% 250℃ 35.30% 36.12% 37.15% 300℃ 47.53% 47.96% 47.35% 350℃ 73.25% 73.52% 73.23% 400℃ 88.95% 87.93% 87.51% 450℃ 98.32% 98.54% 97.96%
[0060] Example 2
[0061] The method for preparing the catalyst is the same as that in Example 1, except that in step S3, ammonium paratungstate (tungsten salt) is added to water to prepare a mixed solution (the molar concentration of the tungsten element is 0.00000192 mol / mL), and the prepared catalyst for catalytic combustion of chlorine-containing organic waste gas is marked as catalyst #2;
[0062] The molar ratio of vanadium element to tungsten element in catalyst #2 is 1:2.
[0063] The method of application in catalytic combustion of halogen-containing volatile organic compounds is the same as that in Example 1. The conversion rates of the catalytic combustion reaction at different times and temperatures are shown in Table 2.
[0064] Table 2
[0065] 5h 7h 720h 200℃ 33.35% 33.25% 33.03 250℃ 39.30% 39.86% 39.65% 300℃ 53.59% 52.66% 54.25% 350℃ 70.35% 71.58% 71.63% 400℃ 90.53% 90.63% 90.61% 450℃ 98.72% 98.94% 98.56%
[0066] Example 3
[0067] The method for preparing the catalyst is the same as that in Example 1, except that, in step S3, ammonium paratungstate (tungsten salt) is added to water to prepare a mixed solution (the molar concentration of the tungsten element is 0.000000384 mol / mL), and the prepared catalyst for catalytic combustion of chlorine-containing organic waste gas is marked as catalyst #3;
[0068] The molar ratio of vanadium element to tungsten element in catalyst #3 is 1:5.
[0069] The method of application in catalytic combustion of halogen-containing volatile organic compounds is the same as that in Example 1. The conversion rates of the catalytic combustion reaction at different times and temperatures are shown in Table 3.
[0070] Table 3
[0071] 5h 7h 720h 200℃ 31.52% 34.12% 34.03 250℃ 37.80% 38.12% 41.68% 300℃ 54.54% 53.87% 52.21% 350℃ 71.07% 70.43% 72.34% 400℃ 90.24% 91.13% 90.13% 450℃ 98.21% 99.01% 98.36%
[0072] Example 4
[0073] The method for preparing the catalyst is the same as that in Example 1, except that in step S3, ammonium paratungstate (tungsten salt) is added to water to prepare a mixed solution (the molar concentration of the tungsten element is 0.000000192 mol / mL), and the prepared catalyst for catalytic combustion of chlorine-containing organic waste gas is marked as catalyst #4;
[0074] The molar ratio of vanadium element to tungsten element in catalyst #4 is 1:10.
[0075] The method of application in catalytic combustion of halogen-containing volatile organic compounds is the same as that in Example 1. The conversion rates of the catalytic combustion reaction at different times and temperatures are shown in Table 4.
[0076] Table 4
[0077] 5h 7h 720h 200℃ 32.67% 31.12% 30.03 250℃ 39.80% 38.52% 39.61% 300℃ 55.64% 54.87% 53.71% 350℃ 72.27% 70.43% 71.64% 400℃ 89.24% 90.13% 93.19% 450℃ 97.21% 99.23% 98.77%
[0078] In summary, from the conversion rate data of the application of catalysts #1 to #4 in Examples 1 to 4 in the catalytic combustion of halogen-containing volatile organic compounds, it can be seen that when the vanadium-tungsten ratio is 1:1, the conversion efficiency is higher than that of catalysts with other ratios, and the results are also the same during the staged heating process. In addition, in Example 1, the activity of the catalyst is still very high after a long reaction of 720 hours, and it is not poisoned or deactivated, which proves that it can effectively resist chlorine. The catalyst is taken out and rubbed, and there is no detachment of the active components on the surface. This phenomenon is also verified by XRD characterization analysis. The results show that its crystal structure is not destroyed, which proves that its active component loading is very firm.
[0079] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.
Claims
1. A method for preparing a catalyst for catalytic combustion of chlorine-containing organic waste gas, characterized in that: The steps include: S1, washing and drying the inorganic oxide raw material and then calcining it to obtain an inorganic oxide support; S2, placing the inorganic oxide support in a cerium salt solution, impregnating I, drying II, and then calcining II to obtain an inorganic oxide support loaded with cerium; S3, mixing a solution containing vanadium salt and tungsten salt with a ruthenium trichloride solution to form a precursor liquid, placing the inorganic oxide carrier loaded with cerium into the precursor liquid, impregnating II, drying III and then calcining III to obtain the catalyst for catalytic combustion of chlorine-containing organic waste gas.
2. The preparation method according to claim 1, characterized in that: In step S2, the concentration of the cerium salt solution is 0.01-0.02 mol / mL in terms of molar concentration of cerium element.
3. The preparation method according to claim 1, characterized in that: In step S3, the volume of the solution containing vanadium salt and tungsten salt is the same as the saturated adsorption volume of the liquid at the saturated water absorption rate of the inorganic oxide support.
4. The preparation method according to claim 1, characterized in that: In step S3, the molar ratio of vanadium element to tungsten element in the vanadium salt and tungsten salt is 1 to 10:1; Preferably, in step S3, the concentration of the vanadium salt is 0.0025 to 0.003 mol / mL in terms of molar concentration of vanadium element.
5. The preparation method according to claim 1, characterized in that: In step S3, the concentration of the ruthenium trichloride solution is 0.000048 to 0.00006 mol / mL in terms of molar concentration of ruthenium element; Preferably, in step S3, the volume ratio of the solution containing vanadium salt and tungsten salt to the ruthenium trichloride solution is 12-48:
1.
6. The preparation method according to claim 1, characterized in that: The conditions of calcination I, calcination II and calcination III independently include: calcination temperature 400-500° C., calcination time 4-8 h; Preferably, the conditions of impregnation I and impregnation II independently include: an impregnation time of 3 to 5 hours; Preferably, the conditions of drying I, drying II and drying III independently include: drying temperature of 80 to 110° C. and drying time of 6 to 12 h.
7. The preparation method according to claim 1, characterized in that: The inorganic oxide is selected from at least one of cerium oxide powder, zeolite, sepiolite, porous carbon material, spherical silicon dioxide, monolithic honeycomb ceramics, and spherical aluminum oxide; Preferably, the vanadium salt is selected from at least one of ammonium metavanadate, sodium metavanadate, potassium metavanadate, sodium orthovanadate, vanadyl sulfate, vanadyl oxalate, vanadium tetrachloride, and vanadyl trichloride; Preferably, the tungsten salt is selected from at least one of sodium tungstate, calcium tungstate, cobalt tungstate, cadmium tungstate, ferrous tungstate, and ammonium tungstate; Preferably, the cerium salt is selected from at least one of cerium nitrate, cerium oxalate and cerium sulfate; Preferably, the specific surface area of the inorganic oxide is 5 to 500 m 2 / g; Preferably, the particle size of the inorganic oxide carrier is 2 to 200 μm.
8. The catalyst for catalytic combustion of chlorine-containing organic waste gas prepared by the preparation method according to any one of claims 1 to 7, characterized in that: In the catalyst, the molar ratio of the vanadium element to the tungsten element is 1:1 to 10; The content of vanadium element is 0.01-0.5wt%; The content of ruthenium element is 0.01 to 5 wt%; The active component elements include cerium, vanadium, tungsten and ruthenium.
9. Use of the catalyst for catalytic combustion of chlorine-containing organic waste gas prepared by the preparation method according to any one of claims 1 to 7, and the catalyst for catalytic combustion of chlorine-containing organic waste gas according to claim 8 in catalytic combustion of halogen-containing volatile organic matter.
10. The use according to claim 9, characterized in that: The application comprises: preheating the organic waste gas containing mixed halogen volatile organic matter at 200-450° C. and then contacting the organic waste gas with a catalyst fixed in a catalytic combustion device for catalytic combustion of chlorine-containing organic waste gas.