General method for preparing multi-element platinum-ruthenium-based nanotube catalyst with self-supporting structure
The self-supporting structure multivariate platinum-ruthenium-based nanotube catalyst was prepared by the template method, which solved the problem of the activity attenuation of existing platinum-ruthenium alloy catalysts under acidity and high potential, and achieved efficient, environmentally friendly and low-cost catalyst preparation, significantly improving the catalysis Activity and durability.
Patent Information
- Application Number
- CN202410965428.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing platinum-ruthenium alloy catalysts have rapid activity attenuation under acidic, oxygen-rich and high potentials. The traditional preparation methods are costly and unfriendly, and the carbon support is prone to oxidation and corrosion, resulting in the failure of the catalyst.
The self-supporting structure multivariate platinum-ruthenium-based nanotube catalyst was prepared by the template method combined with high-temperature calcination technology. The Te nanowires were used as templates and the reduction agent was used to gradually reduce Ru, Pt and transition metals to form a hollow tubular structure, which improved the stability of the catalyst. and activity.
The catalyst is efficient, stable, environmentally friendly and low-cost preparation, which improves the catalytic activity and durability, and significantly improves the catalytic performance of methanol oxidation reaction.
Smart Images

Figure CN118925756A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of catalyst preparation, and in particular to a universal method for preparing a self-supporting multi-element platinum-ruthenium-based nanotube catalyst. Background Art
[0002] The binary platinum-ruthenium alloy catalyst is currently recognized as the most efficient methanol oxidation catalyst. However, due to the significant difference in the crystal structure of platinum and ruthenium, the degree of alloying is low. Therefore, in acidic, oxygen-rich and high-potential conditions, ruthenium atoms are easily oxidized and dissolved, which eventually causes the catalytic activity of the platinum-ruthenium alloy to decay rapidly.
[0003] At present, the preparation methods of synthetic platinum-ruthenium alloy mainly adopt solvothermal method, sol-gel method, impregnation reduction method, electrochemical deposition method, microemulsion method, etc. These methods all require the use of strong reducing agents for reduction and more organic chemical reagents in the process of synthesizing catalysts, so they are costly and environmentally unfriendly.
[0004] In addition, the synthesized platinum-ruthenium alloy catalyst usually needs to be loaded on a carrier with a high specific surface area to improve the dispersibility of the platinum-ruthenium catalyst. The carrier material is usually carbon or modified carbon. Under acidic, oxygen-rich and high-potential operating conditions, these carbon carriers are prone to oxidative corrosion, causing the catalyst to fall off and render the catalyst ineffective. Summary of the invention
[0005] Based on the above-mentioned defects of the prior art, the present invention provides a universal method for preparing self-supporting structured multi-component platinum-ruthenium-based nanotube catalysts, which adopts a mature template method combined with high-temperature calcination technology to synthesize self-supporting multi-component platinum-ruthenium-based alloy nanotube catalysts with unique morphology. The method has the characteristics of simple preparation process, environmental friendliness, low cost, high catalytic activity, good stability and scalability.
[0006] The purpose of the present invention can be achieved through the following technical solutions:
[0007] A general method for preparing a self-supporting structured multi-element platinum-ruthenium-based nanotube catalyst comprises the following steps:
[0008] (1) Weigh 52.5 mg Na2TeO3 (sodium tellurite), 1 g AA (ascorbic acid), 90 mg CTAB (hexadecyltrimethylammonium bromide), and 185 mg PVP (polyvinyl pyrrolidone) into a 45 mL glass bottle, add 40 mL of ultrapure water, and sonicate until the solid powder is completely dissolved. Then heat to 90 °C, keep for 1 h, and cool to room temperature. At this time, the color inside the glass bottle is dark green. After pouring out the sample, add an appropriate amount of ethanol to precipitate Te, and then repeatedly wash it by centrifugation with ethanol to obtain Te nanowires, which are then dispersed in 20 mL of ethylene glycol (EG) solution for later use.
[0009] (2) taking a certain concentration of ruthenium metal precursor solution and placing it in a reducing agent solution for ultrasonic dispersion, transferring it to a three-necked flask, adding the prepared and dispersed Te nanowire-ethylene glycol solution, stirring and heating to a certain temperature and condensing and refluxing, after a sufficient reaction time, then adding a certain concentration of platinum metal precursor and transition metal precursor solution to continue the reaction, and cooling to room temperature; repeatedly washing with ethanol and centrifuging and collecting, placing it in a drying oven for one night to obtain the catalyst; during the reaction, under the action of the reducing agent, the Ru in the solution is reduced to 1.5 wt. % by mass. 3+ , Pt 4+ The transition metal ions continuously obtain electrons from the surface of Te nanowires for reduction, while the Te atoms on the surface are continuously oxidized and dissolved. The precious metals Ru, Pt and transition metal atoms gradually replace the Te atoms on the surface. As time goes by, when the rate of Te atoms migrating outward is greater than the rate of precious metal reduction, the internal Te atoms will continue to move outward, eventually forming a multi-component transition metal-doped TePtRu nanotube structure with a hollow tubular structure.
[0010] Furthermore, the platinum metal precursor includes one of chloroplatinic acid, potassium chloroplatinate, potassium chloroplatinite, tetraammineplatinum chloride, sodium tetrachloroplatinate and ammonium platinum chloride.
[0011] Furthermore, the ruthenium metal precursor includes one of ruthenium acetylacetonate, hexaammineruthenium chloride, ruthenium chloride, and ruthenium acetate.
[0012] Further, the transition metal is one of Ir (iridium), Pd (palladium), Rh (rhodium), Au (gold), and Ag (silver); specifically, the transition metal precursor includes one of hexachloroiridium hydrate, iridium acetate, iridium tetrachloride hydrate, ammonium hexachloroiridate, sodium tetrachloropalladate, trimethylpalladium acetate, sodium chloropalladate, palladium nitrate, rhodium chloride, ammonium chlororhodiumate, rhodium acetate, rhodium nitrate, potassium chloroaurate, sodium tetrachloroaurate, tetrachloroauric acid, ammonium tetrachloroaurate, silver acetate, silver acetylacetonate, and silver nitrate.
[0013] Furthermore, the concentration of the ruthenium metal precursor is 0.05-0.15 mol / L; the concentration of the platinum metal precursor is 0.09-0.25 mol / L; and the concentration of the transition metal precursor is 0.1-0.2 mol / L.
[0014] Furthermore, in step (2), the reaction temperature is 170-190° C., and the reaction time is 1-5 h.
[0015] Furthermore, the reducing agent solution is one of ethylene glycol, a mixed solution of ethylene glycol and ascorbic acid, and a mixed solution of ethylene glycol and sodium citrate.
[0016] Furthermore, in step (2), the drying temperature is 60-90°C.
[0017] Beneficial effects of the present invention:
[0018] The preparation method of the invention has the characteristics of simple synthesis, mild conditions, large-scale production and environmental friendliness.
[0019] The multi-component platinum-ruthenium-based catalyst synthesized by the present invention has the following advantages: 1) a unique hollow tubular structure, which makes the utilization rate of precious metals higher; 2) the components have a spatial concentration gradient distribution, which makes the synergistic catalytic effect between the components more significant; 3) a self-supporting structure is formed, which has better stability and durability; 4) it has a high catalytic reaction activity for the catalytic oxidation of methanol. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] The present invention will be further described below in conjunction with the accompanying drawings.
[0021] Figure 1 SEM and TEM images of Te nanowires prepared in Example 1: (a, b) SEM scanning electron microscope images at different magnifications, (c, d) TEM transmission electron microscope images at different magnifications.
[0022] Figure 2 Characterization images of the catalyst prepared in Example 2: (a) low-magnification TEM image, (b) low-magnification TEM dark field phase, (c) high-magnification HR-TEM image, (d) STEM-EDS energy spectrum and element mapping, (e, f) STEM-EDS line scan energy spectrum and element intensity distribution diagram (the red arrow indicates the scanning direction).
[0023] Figure 3 XPS photoelectron spectra of the catalyst prepared in Example 2: (a) full spectrum, (b-e) high-resolution photoelectron spectra of Te3d, Ru3p, Pt4f and Ir4f respectively.
[0024] Figure 4Electrochemical performance diagrams of four catalysts: commercial Pt / C, PtTe NTs, TePtRu NTS and Ir-doped TePtRu NTs. (a) CV curve of Ir-doped TePtRu NTs activation, the electrolyte is 0.5M H2SO4 solution, and the scan rate is 250mV / s; (b) CV curve; (c) ECSA change diagram; (d) CV curve of the four catalysts after normalization to Pt loading, the electrolyte is 0.5M H2SO4+1.0MCH3OH solution, and the scan rate is 50mV / s; (e) Mass activity and specific activity bar graph obtained by normalizing Pt loading and ECSA with positive peak current; (f) CV curve of CO dissolution test of commercial Pt / C, TePtRu NTS and Ir-doped TePtRu NTs catalysts, the electrolyte is 0.5M H2SO4, and the scan rate is 50mV / s.
[0025] Figure 5 Changes in the components of (a) TePtRu NTs and (b) Ir-doped TePtRu NTs catalysts before and after electrochemical activation and after durability.
[0026] Figure 6 Durability tests of three catalysts: commercial Pt / C, TePtRu NTs and Ir-doped TePtRu NTs: (a-c) CV curves of the three catalysts before and after 1000 cycles of cyclic scanning, the electrolyte is 0.5M H2SO4 saturated with N2, and the scanning rate is 50mV / s; (d-f) CV curves of the catalytic activity of the three catalysts before and after 1000 cycles of cyclic scanning in 0.5M H2SO4+1.0M CH3OH electrolyte saturated with N2, and the scanning rate is 50mV / s; (g) MA and ECSA changes of the three catalysts before and after 1000 cycles of CV scanning; (h) SA changes of the three catalysts before and after 1000 cycles of CV scanning; (i) Constant potential chronoamperometry curves of the three catalysts at 0.6V vsSCE potential.
[0027] Figure 7 TEM images of the catalysts after durability testing: (a) commercial Pt / C; (b) TePtRu NTs; (c) Ir-dopedTePtRu NTs. DETAILED DESCRIPTION
[0028] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] Example 1
[0030] Weigh 52.5 mg Na2TeO3 (sodium tellurite), 1 g AA (ascorbic acid), 90 mg CTAB (hexadecyltrimethylammonium bromide), and 185 mg PVP (polyvinylpyrrolidone) and place them in a 45 mL glass bottle. Add 40 mL of ultrapure water and sonicate until the solid powder is completely dissolved. Then heat to 90°C, keep for 1 hour, and cool to room temperature. At this time, the color inside the glass bottle is dark green. After pouring out the sample, add an appropriate amount of ethanol to precipitate Te, and then repeatedly centrifuge and wash with ethanol to obtain Te nanowires.
[0031] The method for preparing Te nanowires in Example 1 is an improvement on the method previously reported by Qian Yita. After the improvement, not only can the preparation time be greatly shortened to 1 hour, but also the uniformity and stability of the synthesized Te nanowires can be ensured. Figure 1 The surface morphology of the improved Te nanowire template was tested by SEM ( Figure 1 (a) and (b)) show that the surface structure of the Te nanowires synthesized by this method is complete and uniform, and there are no surface oxidized TeO2 particles. At the same time, the length of the Te nanowires reaches several microns, indicating that the synthesized Te nanowires have good uniformity and stability. Further TEM characterization ( Figure 1 (c) and (d)) show that the synthesized Te nanowires are uniform in size, with a diameter of approximately 7 to 10 nm and a length of approximately several microns, indicating that the synthesized Te nanowires have a very high aspect ratio. This feature will be helpful for the exposure of surface active sites after loading precious metals such as Pt, Ru, and Ir and the mass transfer process of methanol molecules.
[0032] Example 2
[0033] The Te nanowires prepared in Example 1 were dispersed in 20 mL of ethylene glycol;
[0034] Take ruthenium acetylacetonate and place it in ethylene glycol (EG) solution for ultrasonic dispersion (concentration of 0.1 mol / L), transfer it to a 100 mL three-necked flask, add Te nanowire-ethylene glycol solution, stir and heat to 180 ° C and condense and reflux, react for 3 hours, then add 0.18 mol / L chloroplatinic acid and hexachloroiridium hydrate solution to continue the reaction and cool to room temperature. After repeated washing with ethanol and centrifugation, the catalyst sample was placed in an 80 ° C drying oven for one night for use, and an Ir-doped PtRu-based catalyst was obtained, which was recorded as Ir-doped TePtRu NTs catalyst.
[0035] Comparative Example 1
[0036] Compared with Example 2, no iridium metal precursor solution was added, and the rest of the preparation process was the same. The obtained catalyst was recorded as TePtRu NTs catalyst.
[0037] Comparative Example 2
[0038] Commercial Pt / C catalyst.
[0039] The catalysts of Example 2 and Comparative Examples 1-2 were subjected to structural characterization and surface chemical configuration analysis:
[0040] Structural characterization: Figure 2 The morphology and component analysis of the catalyst prepared in Example 2 are shown in the low magnification TEM image ( Figure 2 (a) It can be clearly seen that the synthesized catalyst has a clear hollow tubular structure. In addition, the HR-TEM image shows that the catalyst lattice spacing is 0.22nm ( Figure 2 (c)), corresponding to the (111) crystal plane of Pt or Ir in the alloy; Figure 2 (d) shows the STEM-EDS spectrum of the catalyst. It can be seen that Ru, Pt, Ir, and Te elements are distributed throughout the nanotubes, and the signal intensity of the surface Ru, Pt, and Ir elements is greater than that of the Te template, indicating that Ru, Pt, Ir and other components are mainly distributed on the surface of the nanotubes.
[0041] Surface chemical configuration analysis: XPS photoelectron spectroscopy is used for analysis. The test results are as follows: Figure 3 As shown, Figure 3 (a) shows the XPS full spectrum data of Ir-doped TePtRu NTs. It can be seen from the figure that in the binding energy (E b ) are at 61.04eV, 71.52eV, 284.5eV, 284.4eV, 461.5eV, 530eV and 575.75eV, which correspond to the characteristic peaks of Ir 4f, Pt 4f, C1s, Ru3d, Ru3p, O1s and Te3d elements, respectively, indicating that the corresponding element distributions all appear in the synthesized catalysts. Figure 3 (b-e) correspond to the high-resolution spectra of Te 3d, Ru 3p, Pt 4f and Ir 4f, respectively. Figure 3 (b) From the peak fitting curve, it can be seen that Te atoms exist mainly in an oxidized state on the surface. The two weak peaks at 573.3 eV and 583.73 eV correspond to the Te(0) valence band peaks, while the two strong peaks at 575.82 eV and 586.21 eV correspond to the oxidation peaks of Te(4+). Figure 3(c) shows the Ru 3p XPS high-resolution spectrum, in which Ru is mainly in the metallic state. The two strong peaks at 461.60 eV and 483.69 eV correspond to the peaks of the Ru metallic state, while the two weak peaks at 463.49 eV and 485.27 eV correspond to the peaks of the Ru oxidation state. Figure 3 (d) shows the high-resolution XPS spectrum of Pt 4f, from which we can see that the Pt element is mainly in the metallic state, with two strong peaks located at E b The positions of 72.13 eV and 71.44 eV correspond to Pt 4f 5 / 2 and Pt4f 7 / 2 , while the two weak peaks at 74.80 eV and 75.73 eV correspond to the oxidation state of Pt. Figure 3 (e) is the high-resolution XPS spectrum of Ir 4f. The two strong peaks at 60.91eV and 61.55eV correspond to zero-valent Ir atoms, while the two weak peaks at 63.94eV and 64.63eV correspond to the peaks of Ir oxidation state. From the high-resolution XPS images of these four elements, it can be seen that the noble metal elements mainly exist in the metallic state on the surface of the catalyst. Studies have shown that the metallic structure is conducive to the adsorption and catalytic oxidation process of methanol molecules.
[0042] Electrochemical performance characterization: The electrochemical test was conducted using a classic three-electrode system on an American Pine instrument electrochemical workstation. Before the formal test, all catalysts were fully activated in a N2-saturated 0.5M H2SO4 electrolyte. Taking Ir-doped TePtRu NTs catalyst as an example, Figure 4 As shown in (a), the CV curves after 50, 100 and 200 cycles of cyclic scanning in the potential range of -0.2 to 1.0 V at a scanning rate of 250 mV / s in N2-saturated 0.5 M H2SO4 electrolyte. We noticed that there are two characteristic peaks at 0.1 V and 0.8 V, corresponding to the oxidation and dissolution peaks of Te atoms, respectively. As the cyclic scanning proceeds, the peak intensities of these two locations gradually decrease, while the H underpotential adsorption and desorption peak located between -0.2 and 0.1 V gradually increases, indicating that the Te atoms on the surface are continuously dissolved and reduced, causing the Pt atoms near the surface to be continuously exposed. Figure 5The component changes of Ir-dopedTePtRu NTs and TePtRu NTs catalysts before and after electrochemical activation and durability testing were characterized. It can be clearly seen from the figure that the Te component is significantly reduced after activation, which is consistent with the results observed by CV. In addition, the Ru component of the undoped Ir TePtRu NTs catalyst also showed a significant decrease after activation, indicating that the pure TePtRu NTs catalyst cannot stably maintain high activity in the working environment, while the Ir-doped TePtRu NTs catalyst after Ir doping has been significantly improved, which is consistent with the results obtained by previous DFT calculations. The CV curve after activation and stabilization is shown in Figure 2. Figure 4 (b) By upd The electrochemical active area of the corresponding catalyst can be obtained by integrating the adsorption charge in the region. The calculation shows that Ir-doped TePtRu NTs has the largest electrochemical active area (78.4 m 2 / g Pt ), compared with TePtRu NTs (47.6m 2 / g Pt )、PtTe NTs(68.7m 2 / g Pt ) and Pt / C(43.4m 2 / g Pt ) are both bigger( Figure 4 (c)). This is mainly attributed to the unique hollow structure of Ir-dopedTePtRu NTs, which allows more surface active sites to be exposed on the inner and outer surfaces, and the Ir doping improves the stability of the catalyst structure and components. In order to facilitate the quantitative analysis of the electrochemical performance of each catalyst, we normalized the methanol oxidation current of four catalysts, commercial Pt / C, PtTe NTs, TePtRu NTs and Ir-doped TePtRu NTs, to the Pt loading, and obtained the mass activity CV curves of each catalyst ( Figure 4 (d)), it can be clearly seen from the figure that the Ir-doped TePtRu NTs catalyst has the highest mass activity peak, and the methanol oxidation peak potential is the same as that of TePtRu NTs, indicating that the doping of Ir atoms improves the intrinsic catalytic activity of PtRu. After further normalizing the Pt loading and ECSA with the pre-oxidation peak current, the mass activity and specific activity bar graphs of the four catalysts were obtained respectively ( Figure 4 (e) shows that the mass activity of Ir-doped TePtRu NTs catalyst is 1.90 A / mg PtThey are 1.55 times, 2.1 times and 3.53 times of TePtRu NTs, PtTe NTs and Pt / C respectively, and its specific activity is also 1.93 times greater than that of Pt / C, indicating that the Ir-doped TePtRu NTs catalyst has better electrocatalytic oxidation performance of CH3OH than the undoped TePtRu NTs catalyst and commercial Pt / C.
[0043] In addition, for the MOR reaction, the ability of the catalyst to resist CO poisoning is also an important parameter to measure its electrochemical performance. In the MOR performance test, it is usually measured by comparing the positive scan oxidation front peak (I f ) and the reverse scan peak (I b ) Ratio I f / I b The size of the catalyst material is used to measure its ability to resist CO poisoning. f / I b The calculation of the ratio found that the I of Ir-doped TePtRu NTs f / I b The ratio is 1.14, which is higher than that of undoped TePtRu NTs (1.03), PtTe NTs (0.90), and commercial Pt / C (0.78), indicating that Ir-doped TePtRu NTs have the best resistance to CO poisoning.
[0044] In addition to considering the activity of the catalyst and its ability to resist CO poisoning, the durability of the catalyst is also an important aspect of catalyst research. In order to comprehensively evaluate the durability of the synthesized catalyst, we used two electrochemical test methods to characterize it, namely, cyclic CV scanning and constant potential chronoamperometry (CA). First, we performed 1000 cycles of CV scanning on the synthesized TePtRu NTs, Ir-doped TePtRu NTs, and commercial Pt / C catalysts. Figure 6 As shown in Figures (a-c), the CV curves of the three catalysts before and after 1000 cycles of cyclic scanning in 0.5M H2SO4 electrolyte solution saturated with N2, the scanning rate is 50mV / s, the potential scanning range is -0.2~1.0V, by calculating the integrated charge of the H region, we found that after 1000 cycles of CV cycle scanning in 0.5M H2SO4+1.0M CH3OH electrolyte solution, the electrochemical active areas (ECSA) of commercial Pt / C, TePtRu NTs and Ir-dopedTePtRu NTs catalysts decreased by 55%, 18.7% and increased by 11%, respectively ( Figure 6(g) shows that in a strong acidic medium, the doping of Ir atoms can effectively improve the stability of the catalyst, while commercial Pt / C and undoped TePtRu NTs are constantly etched and dissolved, resulting in a reduction in the number of active sites of the catalyst, causing a rapid decrease in ECSA. Figure 6 (d-f) Comparison of the mass activity (MA) of each catalyst after normalizing the peak current before MOR oxidation to the Pt loading. It is found that the MA of commercial Pt / C, TePtRu NTs and Ir-doped TePtRu NTs catalysts are reduced by 44.1%, 26.8% and 3.64%, respectively. Figure 5 (g) shows that Ir doping can significantly enhance the durability of PtRu alloy. At the same time, we also compared the specific activities of various catalysts, such as Figure 6 As shown in (h), although the SA of the two NTs catalysts decreased, which is mainly due to the fact that SA is determined by MA and ECSA, the SA after the durability test is higher than that of commercial Pt / C, indicating that the NTs catalyst with a one-dimensional structure has higher catalytic activity. To further verify this result, we also tested it by CA. Figure 6 (i) shows the chronoamperometric curves obtained at a constant potential of 0.6 V vs. SCE in a 0.5 M H2SO4 + 1.0 M CH3OH electrolyte saturated with N2. From the figure, we can see that the current of the three catalysts drops rapidly in the initial period and then tends to a stable value. This is mainly due to the initial poisoning of the catalyst surface by the carbonaceous intermediates of methanol oxidation. After 4000 s of catalytic reaction, the Ir-doped TePtRu NTs catalyst still has a current of 0.485 A / mg Pt The mass activity is much higher than 0.081A / mg of TePtRu NTs. Pt and 0.007A / mg of commercial Pt / C Pt , which shows that the Ir-doped TePtRu NTs catalyst has excellent catalytic activity and durability, and this result is consistent with the above-mentioned CV test. This excellent electrochemical performance can be attributed to the following aspects. First, the synergistic catalytic effect between multiple components. The doping of Ir can not only enhance the interaction between Pt-Ir, Pt-Ru and Ru-Ir, but also promote the adsorption of methanol molecules and the activation of water molecules; second, the 1D nanotube catalyst itself can expose more active sites and provide fast electron transmission channels and mass transfer processes. Finally, we also performed TEM characterization on the catalyst samples after the durability test, such as Figure 7As shown in the figure, the TePtRu NTs and Ir-doped TePtRu NTs catalysts still maintain a complete morphology with a small number of holes in the middle, while for the commercial Pt / C catalyst, obvious agglomeration occurs, which may be due to the corrosion of the C support and the migration and agglomeration of Pt atoms, which will lead to the deactivation of the catalyst.
[0045] The above specific implementation method part specifically introduces the analytical method involved in the present invention. It should be noted that the above introduction is only to help those skilled in the art better understand the method and ideas of the present invention, rather than limiting the relevant content. Without departing from the principle of the present invention, those skilled in the art may also make appropriate adjustments or modifications to the present invention, and the above adjustments and modifications shall also fall within the scope of protection of the present invention.
Claims
1. A general method for preparing a self-supporting multi-element platinum-ruthenium-based nanotube catalyst, characterized in that: The following steps are involved: (1) preparing Te nanowires and dispersing them in an ethylene glycol solution for later use; (2) A certain concentration of ruthenium metal precursor solution is measured and placed in a reducing agent solution for uniform ultrasonic dispersion, and then transferred to a three-necked flask, and then the prepared and uniformly dispersed Te nanowire-ethylene glycol solution is added, stirred and heated to a certain temperature and condensed and refluxed. After the reaction time is sufficient, a certain concentration of platinum metal precursor and transition metal precursor solution are added to continue the reaction and cool to room temperature; after repeated washing with ethanol and centrifugation, the solution is placed in a drying oven and dried overnight to obtain the catalyst.
2. A universal method for preparing a self-supporting multi-element platinum-ruthenium-based nanotube catalyst according to claim 1, characterized in that: The platinum metal precursor includes one of chloroplatinic acid, potassium chloroplatinate, potassium chloroplatinite, tetraammineplatinum chloride, sodium tetrachloroplatinate and ammonium platinum chloride.
3. The method for preparing a self-supporting multi-element platinum-ruthenium-based nanotube catalyst according to claim 1, characterized in that: The ruthenium metal precursor includes one of ruthenium acetylacetonate, hexaammineruthenium chloride, ruthenium chloride, and ruthenium acetate.
4. The method for preparing a self-supporting multi-element platinum-ruthenium-based nanotube catalyst according to claim 1, characterized in that: The transition metal is one of Ir, Pd, Rh, Au, and Ag; the transition metal precursor includes one of hexachloroiridium hydrate, iridium acetate, iridium tetrachlorohydrate, ammonium hexachloroiridate, sodium tetrachloropalladate, trimethylpalladium acetate, sodium chloropalladate, palladium nitrate, rhodium chloride, ammonium chlororhodiumate, rhodium acetate, rhodium nitrate, potassium chloroaurate, sodium tetrachloroaurate, tetrachloroauric acid, ammonium tetrachloroaurate, silver acetate, silver acetylacetonate, and silver nitrate.
5. The method for preparing a self-supporting multi-element platinum-ruthenium-based nanotube catalyst according to claim 1, characterized in that: The concentration of the ruthenium metal precursor is 0.05-0.15 mol / L; the concentration of the platinum metal precursor is 0.09-0.25 mol / L; and the concentration of the transition metal precursor is 0.1-0.2 mol / L.
6. A universal method for preparing a self-supporting multi-element platinum-ruthenium-based nanotube catalyst according to claim 1, characterized in that: In step (2), the reaction temperature is 170-190° C. and the reaction time is 1-5 h.
7. A universal method for preparing a self-supporting multi-element platinum-ruthenium-based nanotube catalyst according to claim 1, characterized in that: The reducing agent solution is one of ethylene glycol, a mixed solution of ethylene glycol and ascorbic acid, and a mixed solution of ethylene glycol and sodium citrate.
8. The method for preparing a self-supporting multi-element platinum-ruthenium-based nanotube catalyst according to claim 1, characterized in that: The drying temperature in step (2) is 60-90°C.
9. The method for preparing a self-supporting multi-element platinum-ruthenium-based nanotube catalyst according to claim 1, characterized in that: The specific operation of step (1) is as follows: weigh 52.5 mg of Na2TeO3, 1 g of AA, 90 mg of CTAB and 185 mg of PVP and place them in a 45 mL glass bottle, add 40 mL of ultrapure water, and sonicate until the solid powder is completely dissolved, then heat to 90°C, keep for 1 hour, and cool to room temperature. At this time, the color inside the glass bottle is dark green; pour out the sample and add an appropriate amount of ethanol to precipitate Te, then repeatedly centrifuge and wash with ethanol to obtain Te nanowires, which are dispersed in 20 mL of ethylene glycol solution for use.
Citation Information
Patent Citations
PtRu / graphene nano electro-catalyst and preparation method thereof
CN101740786A
Preparation method of ternary alloy platinum-ruthenium-copper catalyst and application of ternary alloy platinum-ruthenium-copper catalyst in methanol catalysis
CN114899438A
METHOD FOR MANUFACTURING PtRu ALLOY CATALYST FOR FUEL CELL, PtRu ALLOY CATALYST FOR FUEL CELL AND METHANOL FUEL CELL USING THE CATALYST
JP2005324156A
ULTRATHIN, TERNARY ALLOY PtRuFe NANOWIRES, AND METHODS OF MAKING SAME
US20160293969A1