Phosphoric acid group modified rich-pore titanium dioxide-silver composite material as well as preparation method and application thereof
The pore-rich titanium dioxide-silver composite material modified by phosphate groups solved the problem of low photocatalytic reduction efficiency of pure titanium dioxide in CO2. The PO43-TiO2-Ag composite material was prepared by solvent thermal method, achieving efficient photocatalytic CO2 reduction , improving photocatalytic activity and stability.
Patent Information
- Application Number
- CN202410983980.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-22
AI Technical Summary
Pure titanium dioxide has low efficiency in CO2 photocatalytic reduction, and its wide band gap is limited in utilization of visible light. The prior art does not use metal co-catalysts and phosphate groups to modify semiconductor photocatalytic reduction of photocatalytic CO2.
The pore-rich titanium dioxide-silver composite material modified with phosphate groups was prepared by solvothermal method, and phosphate was introduced to composite with titanium dioxide and silver to enhance photocatalytic activity.
It significantly improves photocatalytic activity, enhances the transmission of electron-hole pairs and the adsorption of CO2 molecules, and can significantly improve photocatalytic performance compared to monomer materials. It has simple process, low cost, and high stability and application potential.
Smart Images

Figure CN118925757A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of functional materials and photocatalytic material preparation, and in particular to a porous titanium dioxide-silver composite material modified with a phosphate group, and a preparation method and application thereof. Background Art
[0002] With the rapid development of human society, the exploitation and utilization of traditional fossil fuels have expanded dramatically, and the emission of greenhouse gases such as CO2 has also increased dramatically, leading to accelerated climate change. Effective development and utilization of solar energy is one of the important ways to meet these challenges. Solar-driven photocatalytic CO2 reduction technology can convert solar energy into chemical energy that is convenient for storage and transportation, which is expected to reduce dependence on fossil fuels and help reduce net CO2 emissions to meet society's requirements for sustainable development. However, due to the high bond energy of the C=O bond of CO2 (>700kJ / mol), relatively high energy is required to convert CO2 to hydrocarbon fuels, which also causes photocatalytic CO2 reduction to often show low efficiency. Semiconductors with suitable band gaps and high photocatalytic activity are more suitable for photocatalytic CO2 reduction. TiO2 has become one of the most popular catalysts for CO2 photocatalytic reduction due to its stability, non-toxicity, strong redox ability and low price. However, the conversion efficiency of pure TiO2 to CO2 is very low because of its wide band gap, limited utilization of visible light, and fast rate of recombination of photogenerated charges. Its application in the photocatalytic reduction of carbon dioxide is greatly limited.
[0003] In recent years, many strategies have been proposed to improve the photocatalytic performance of TiO2, such as element doping, heterojunction construction, surface site construction, and co-catalyst modification. These methods can effectively improve the photocatalytic activity of single TiO2. Among them, metal co-catalyst modification is considered to be an effective method to improve charge separation. Since the Fermi level of n-type semiconductors is higher than that of metals, when n-type semiconductors and metals are in close contact, the energy band bends, and the photogenerated electrons will transfer from the semiconductor to the metal until the Fermi level of the two is balanced, and the Schottky barrier can inhibit the backflow of electrons, which can further enhance the charge separation efficiency. Among various metal co-catalysts, silver is a relatively excellent co-catalyst. It can not only improve the charge separation ability, but also greatly improve the light absorption of semiconductor materials. And due to the local surface plasmon resonance effect of silver, more electrons can be generated for photocatalytic CO2 reduction reaction.
[0004] In addition to the charge separation efficiency, the adsorption and activation of CO2 molecules and active intermediates are closely related to the performance of photocatalytic CO2 reduction. In practical research, some Lewis bases are often used as surface adsorption sites to promote the adsorption and activation of CO2 molecules, such as WO42-, -NH2, PO43-, etc. Related studies have shown that in addition to being able to act as a Lewis base to promote the adsorption of CO2 molecules, phosphate group species also have some special functions, such as enhancing the charge transfer rate and surface redox rate. However, so far, there is no related technology for using metal co-catalysts and PO43- to modify semiconductor photocatalysts for photocatalytic CO2 reduction. Summary of the invention
[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a porous titanium dioxide-silver composite material modified with phosphate groups and a preparation method and application thereof, so as to solve the problems raised in the above background technology.
[0006] To achieve the above object, the present invention provides the following technical solutions:
[0007] A method for preparing a porous titanium dioxide-silver composite material modified with a phosphate group comprises the following steps:
[0008] S1. Ultrasonic dispersion of modified nano-titanium dioxide into deionized water, adding 1 mol / L silver nitrate solution, stirring evenly to obtain a mixed solution;
[0009] S2, adding 1 mol / L sodium hydroxide solution and ammonium hypophosphite to the mixed solution obtained in step S1, stirring for 0.4-0.8 h, putting it into a reactor and heating it at 40-140° C. for 6-24 h to obtain a reaction solution;
[0010] S3, cooling the reaction solution obtained in step S2 to room temperature, washing with distilled water until the supernatant is neutral, washing with anhydrous ethanol for the last time, and vacuum drying the product at 50-80° C. for 10-16 h to obtain a titanium dioxide-silver composite material modified with phosphate groups.
[0011] Furthermore, the modified nano titanium dioxide in step S1 is prepared by the following method:
[0012] S101, ultrasonically dispersing nano-titanium dioxide into a mixed solution of deionized water, ethanol and ethyl propionate, and then adding sodium hydroxide to adjust the pH of the solution to 8-11;
[0013] S102, adding carboxymethyl chitosan, tetraethylene glycol monooctyl ether and sodium styrene sulfonate to the mixed solution of deionized water, ethanol and ethyl propionate in step S101, and then putting the mixture into a reactor to react at 80-160° C. for 4-10 hours;
[0014] S103, filtering the reaction liquid in the reaction kettle after the reaction in step S102, washing with ethanol, and vacuum drying at 150-250° C. to obtain modified nano titanium dioxide.
[0015] Furthermore, in step S101, the mass ratio of ethyl propionate, ethanol and deionized water is 1:3:10, and the mass ratio of nano-titanium dioxide to the mixed solution of deionized water, ethanol and ethyl propionate is 1:(10-30).
[0016] Furthermore, in step S102, the mass ratio of the mixed solution of tetraethylene glycol monooctyl ether, sodium styrene sulfonate and carboxymethyl chitosan to deionized water, ethanol and ethyl propionate is 1:(1-3):(5-10):(80-120).
[0017] Furthermore, in step S1, the mass ratio of the modified nano-titanium dioxide to deionized water is 1:(10-14), and the mass ratio of the silver nitrate solution to deionized water is 1:(26-32).
[0018] Furthermore, the mass ratio of the sodium hydroxide solution in step S2 to the deionized water in step S1 is 1:(15-20), and the mass ratio of the ammonium hypophosphite in step S2 to the deionized water in step S1 is 1:(14-18).
[0019] A phosphoric acid group-modified titanium dioxide-silver composite material is prepared by adopting the preparation method of the phosphoric acid group-modified porous titanium dioxide-silver composite material.
[0020] The invention discloses an application of a titanium dioxide-silver composite material modified with a phosphate group in the field of photocatalytic carbon dioxide reduction to prepare hydrocarbon fuels.
[0021] Furthermore, the application of the titanium dioxide-silver composite material modified with phosphate groups in the field of preparing hydrocarbon fuels by photocatalytic carbon dioxide reduction adopts the following method:
[0022] The titanium dioxide-silver composite material modified with phosphate groups is uniformly mixed with deionized water, and catalytically converts carbon dioxide under light.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] 1. The present invention successfully synthesized a titanium dioxide-silver composite material modified with a phosphate group by a solvothermal method. The chemical formula of the composite material is PO4 3- -TiO 2 -Ag, silver ions are reduced by ammonium hypophosphite to generate silver, phosphate is successfully introduced, and phosphate and silver are compounded with titanium dioxide;
[0025] 2. In the composite material obtained by the present invention, due to TiO 2 The large contact area between Ag and Ag and the abundant surface alkaline sites are conducive to the effective transmission and utilization of electron-hole pairs and the adsorption of CO2 molecules, which can significantly enhance the photocatalytic activity compared with monomer materials.
[0026] 3. The composite material is synthesized in one step, has a simple preparation process, low cost, and convenient operation. The modified nano titanium dioxide is evenly dispersed, and the introduced ammonium radicals generate gas during the hot solvent method, which jointly promotes the uniform attachment of silver ions on the surface of titanium dioxide. The composite material has high stability, meets actual production needs, and has great application potential. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 The process flow chart of preparing the titanium dioxide-silver composite material modified with phosphoric acid groups of the present invention;
[0028] Figure 2 The process flow chart of preparing modified nano titanium dioxide in the present invention;
[0029] Figure 3 is an X-ray diffraction analysis (XRD) pattern of the titanium dioxide-silver composite material modified with phosphate groups in Example 1 of the present invention;
[0030] Figure 4 The X-ray photoelectron spectroscopy (XPS) diagram of the titanium dioxide-silver composite material and nano-titanium dioxide modified with phosphate groups in Example 1 of the present invention;
[0031] Figure 5 The high-resolution fine spectrum of Ti 2p in the X-ray photoelectron spectroscopy (XPS) analysis of the titanium dioxide-silver composite material modified with phosphoric acid groups and nano-titanium dioxide in Example 1 of the present invention;
[0032] Figure 6 The high-resolution fine spectrum of Ag 3d in the X-ray photoelectron spectroscopy (XPS) analysis of the titanium dioxide-silver composite material modified with phosphate groups in Example 1 of the present invention;
[0033] Figure 7 is a high-resolution fine spectrum of P 2p in the X-ray photoelectron spectroscopy (XPS) analysis of the titanium dioxide-silver composite material modified with phosphate groups in Example 1 of the present invention;
[0034] Figure 8 This is a scanning electron microscope image (SEM) of nano-titanium dioxide;
[0035] Fig. 9 This is a scanning electron microscope image (SEM) of the titanium dioxide-silver composite material modified with phosphate groups in Example 1 of the present invention;
[0036] Fig.10 This is a transmission electron microscopy (TEM) image of the titanium dioxide-silver composite material modified with phosphate groups in Example 1 of the present invention;
[0037] Fig.11 This is a photocatalytic CO2 reduction activity diagram of the titanium dioxide-silver composite material, nano titanium dioxide and titanium dioxide-silver composite material modified with phosphate groups in Example 1 of the present invention. DETAILED DESCRIPTION
[0038] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0039] See also Figure 1-11 , the present invention provides a technical solution:
[0040] Example 1
[0041] A method for preparing a porous titanium dioxide-silver composite material modified with a phosphate group comprises the following steps:
[0042] S1. Disperse 0.3 g of modified nano-titanium dioxide into 70 ml of deionized water by ultrasonic wave at a frequency of 20 kHz, add 0.12 ml of 1 mol / L silver nitrate solution, stir evenly, and obtain a mixed solution;
[0043] S2, adding 4 ml of 1 mol / L sodium hydroxide solution and 0.22 g of ammonium hypophosphite to the mixed solution obtained in step S1, stirring for 0.5 h, and then placing the mixture in a reactor and heating at 80° C. for 15 h to obtain a reaction solution;
[0044] S3, cooling the reaction solution obtained in step S2 to room temperature and washing with distilled water until the supernatant is neutral, washing with anhydrous ethanol for the last time, and vacuum drying the product at 60° C. for 12 h to obtain a titanium dioxide-silver composite material modified with phosphate groups.
[0045] The modified nano titanium dioxide is prepared by the following method:
[0046] S101, ultrasonically dispersing 1.0 g of nano-titanium dioxide into 20 g of a mixed solution containing deionized water, ethanol and ethyl propionate, wherein the masses of deionized water, ethanol and ethyl propionate are 14.3 g, 4.3 g and 1.4 g, respectively, and the frequency of the ultrasonic wave is 18 kHz, and then sodium hydroxide is added to adjust the pH of the solution to 9;
[0047] S102, adding 1.63 g of carboxymethyl chitosan, 0.2 g of tetraethylene glycol monooctyl ether and 0.37 g of sodium styrene sulfonate to the mixed solution of deionized water, ethanol and ethyl propionate in step S101, mixing and placing in a reactor to react at 120° C. for 6 h;
[0048] S103, filtering the reaction liquid in the reaction kettle after the reaction in step S102, washing with ethanol, and vacuum drying at 210° C. to obtain modified nano titanium dioxide.
[0049] Example 2
[0050] A method for preparing a porous titanium dioxide-silver composite material modified with a phosphate group comprises the following steps:
[0051] S1. Disperse 0.6 g of modified nano-titanium dioxide into 60 ml of deionized water by ultrasonic wave at a frequency of 18 kHz, add 0.23 ml of 1 mol / L silver nitrate solution, stir evenly, and obtain a mixed solution;
[0052] S2, adding 4 ml of 1 mol / L sodium hydroxide solution and 0.43 g of ammonium hypophosphite to the mixed solution obtained in step S1, stirring for 0.4 h, and then placing the mixture in a reactor and heating at 40° C. for 24 h to obtain a reaction solution;
[0053] S3, cooling the reaction solution obtained in step S2 to room temperature and washing with distilled water until the supernatant is neutral, washing with anhydrous ethanol for the last time, and vacuum drying the product at 50° C. for 16 h to obtain a titanium dioxide-silver composite material modified with phosphate groups.
[0054] The modified nano titanium dioxide is prepared by the following method:
[0055] S101, ultrasonically dispersing 1.0 g of nano-titanium dioxide into 10 g of a mixed solution containing deionized water, ethanol and ethyl propionate, wherein the masses of deionized water, ethanol and ethyl propionate are 7.12 g, 2.13 g and 0.71 g, respectively, and the frequency of the ultrasonic wave is 15 kHz, and then sodium hydroxide is added to adjust the pH of the solution to 8;
[0056] S102, adding 0.62 g of carboxymethyl chitosan, 0.13 g of tetraethylene glycol monooctyl ether and 0.13 g of sodium styrene sulfonate to the mixed solution of deionized water, ethanol and ethyl propionate in step S101, mixing and placing in a reactor to react at 80° C. for 10 h;
[0057] S103, filtering the reaction liquid in the reaction kettle after the reaction in step S102, washing with ethanol, and vacuum drying at 150° C. to obtain modified nano titanium dioxide.
[0058] Example 3
[0059] A method for preparing a porous titanium dioxide-silver composite material modified with a phosphate group comprises the following steps:
[0060] S1. Disperse 0.5 g of modified nano-titanium dioxide into 84 ml of deionized water by ultrasonic wave at a frequency of 24 kHz, add 0.22 ml of 1 mol / L silver nitrate solution, stir evenly, and obtain a mixed solution;
[0061] S2, adding 3 ml of 1 mol / L sodium hydroxide solution and 0.84 g of ammonium hypophosphite to the mixed solution obtained in step S1, stirring for 0.8 h, and then placing the mixture in a reactor and heating at 140° C. for 6 h to obtain a reaction solution;
[0062] S3, cooling the reaction solution obtained in step S2 to room temperature and washing with distilled water until the supernatant is neutral, washing with anhydrous ethanol for the last time, and vacuum drying the product at 80° C. for 10 h to obtain a titanium dioxide-silver composite material modified with phosphate groups.
[0063] The modified nano titanium dioxide is prepared by the following method:
[0064] S101, ultrasonically dispersing 1 g of nano-titanium dioxide into 30 ml of a mixed solution containing deionized water, ethanol and ethyl propionate, wherein the masses of deionized water, ethanol and ethyl propionate are 21.3 g, 6.37 g and 2.12 g, respectively, and the frequency of the ultrasonic wave is 21 kHz, and then sodium hydroxide is added to adjust the pH of the solution to 11;
[0065] S102, adding 0.62 g of carboxymethyl chitosan, 0.12 g of tetraethylene glycol monooctyl ether and 0.12 g of sodium styrene sulfonate to the mixed solution of deionized water, ethanol and ethyl propionate in step S101, mixing and placing in a reactor to react at 160° C. for 4 h;
[0066] S103, filtering the reaction liquid in the reaction kettle after the reaction in step S102, washing with ethanol, and vacuum drying at 250° C. to obtain modified nano titanium dioxide.
[0067] Example 4
[0068] A method for preparing a porous titanium dioxide-silver composite material modified with a phosphate group comprises the following steps:
[0069] S1. Disperse 0.3 g of modified nano-titanium dioxide into 76 ml of deionized water by ultrasonic wave at a frequency of 21 kHz, add 0.16 ml of 1 mol / L silver nitrate solution, stir evenly, and obtain a mixed solution;
[0070] S2, adding 3 ml of 1 mol / L sodium hydroxide solution and 0.52 g of ammonium hypophosphite to the mixed solution obtained in step S1, stirring for 0.5 h, and then placing the mixture in a reactor and heating at 100° C. for 8 h to obtain a reaction solution;
[0071] S3, cooling the reaction solution obtained in step S2 to room temperature and washing with distilled water until the supernatant is neutral, washing with anhydrous ethanol for the last time, and vacuum drying the product at 60° C. for 12 h to obtain a titanium dioxide-silver composite material modified with phosphate groups.
[0072] The modified nano titanium dioxide is prepared by the following method:
[0073] S101, ultrasonically dispersing 1 g of nano-titanium dioxide into 17.5 g of a mixed solution containing deionized water, ethanol and ethyl propionate, wherein the masses of deionized water, ethanol and ethyl propionate are 12.5 g, 3.75 g and 1.25 g, respectively, and the frequency of the ultrasonic wave is 19 kHz, and then sodium hydroxide is added to adjust the pH of the solution to 9;
[0074] S102, adding 1.6 g of carboxymethyl chitosan, 0.175 g of tetraethylene glycol monooctyl ether and 0.31 g of sodium styrene sulfonate to the mixed solution of deionized water, ethanol and ethyl propionate in step S101, mixing and placing in a reactor to react at 100° C. for 5 h;
[0075] S103, filtering the reaction liquid in the reaction kettle after the reaction in step S102, washing with ethanol, and vacuum drying at 240° C. to obtain modified nano titanium dioxide.
[0076] The nano titanium dioxide in the above embodiments is prepared by the following method:
[0077] 6 mL of tetrabutyl titanate was added to 150 mL of ethylene glycol, and then heated to 120°C and refluxed for 1 hour after ultrasonic treatment for 10 minutes. After the reaction was completed, 60 mL of water was added to the precursor obtained after centrifugation, and then calcined at 500°C for 2 hours to obtain nano titanium dioxide.
[0078] The final product obtained in Example 1 was subjected to XRD analysis, and the results were as follows: Figure 2As shown in the figure, the synthesized TiO 2 Anatase TiO 2 Its diffraction peaks are consistent with the standard spectrum 21-1272Anatase, and no other peaks appear, indicating that TiO 2 The successful synthesis of PO4 3- -TiO 2 -Ag composite material's diffraction peaks correspond to TiO2 (21-1272) and Ag (1-1164), among which the composite material has Ag diffraction peaks near 44° and 64°, indicating the successful construction of the composite material.
[0079] In order to further prove the composite material composition and element valence of the synthesized material, XPS analysis was performed on the composite material synthesized in Example 1. Figure 3 As shown; from the XPS total spectrum (a), it can be seen that the composite material synthesized in this embodiment is composed of five elements: Ti, Ag, O, P and C, among which C is the carbon element introduced in the test. The results further confirm the elemental composition of the composite material. Through single element valence analysis, the Ti element exists in the form of +4 valence; the difference between the spin-orbit splitting peaks of the Ag element is 6.0 eV, proving that the main existence form of the Ag element is single substance Ag; the XPS results further confirm that PO4 3- -TiO 2 -Synthesis of Ag composites.
[0080] Figure 7 and Figure 8 They are respectively the modified nano-TiO 2 and PO4 3- -TiO 2 -Ag composite material SEM image, it can be seen that TiO 2 The surface has a porous structure, and the morphology does not change after solvent thermal treatment. The particle size of Ag nanoparticles is extremely small. 2 The surface distribution is uniform without aggregation, and the product has good catalytic effect.
[0081] Fig. 9 PO4 obtained in this example 3- -TiO 2 -Ag composite material TEM image, TiO 2 (101) and Ag(111) exist, and the particle size of Ag is about 10-20nm.
[0082] The PO4 obtained in this example 3- -TiO 2 -Ag composite materials, TiO 2 and the control group without silver salt addition3- -TiO 2 Photocatalytic reduction of CO 2 Activity test, the specific steps include: 1mL deionized water is dripped into 50mg catalytic sample (PO4 3- -TiO 2 -Ag composite materials, monomer TiO 2 Or the control group without adding silver salt PO4 3- -TiO 2 ), after ultrasonication for 2 minutes, evenly put it into a culture dish with a diameter of 3.4 cm, add 10 mL of deionized water at the bottom of the photoreactor, and then put the culture dish into the bottom of the reactor, pass high-purity CO2 gas for 30 minutes to remove the air in the reactor, and then seal the photoreactor, use a 300W Xe lamp to irradiate the photoreactor, take 1 mL of the gaseous product every 1 hour, and use gas chromatography to analyze the composition until the illumination ends after 4 hours.
[0083] The results are as follows Fig.10 As shown, the test results show that PO4 3- -TiO 2 The photocatalytic activity is better than that of TiO 2 ,PO4 3- -TiO 2 -Ag composites are significantly more active than TiO 2 and PO4 3- -TiO 2 .
[0084] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a porous titanium dioxide-silver composite material modified with a phosphate group, It is characterized in that The steps include: S1. Ultrasonic dispersion of modified nano-titanium dioxide into deionized water, adding 1 mol / L silver nitrate solution, stirring evenly to obtain a mixed solution; S2, adding 1 mol / L sodium hydroxide solution and ammonium hypophosphite to the mixed solution obtained in step S1, stirring for 0.4-0.8 h, putting it into a reactor and heating it at 40-140° C. for 6-24 h to obtain a reaction solution; S3, cooling the reaction solution obtained in step S2 to room temperature and washing with distilled water until the supernatant is neutral, washing with anhydrous ethanol for the last time, and vacuum drying the product at 50-80° C. for 10-16 h to obtain a titanium dioxide-silver composite material modified with a phosphate group.
2. The method for preparing the porous titanium dioxide-silver composite material modified with phosphate groups according to claim 1, It is characterized in that The modified nano titanium dioxide in step S1 is prepared by the following method: S101, ultrasonically dispersing nano-titanium dioxide into a mixed solution of deionized water, ethanol and ethyl propionate, and then adding sodium hydroxide to adjust the pH of the solution to 8-11; S102, adding carboxymethyl chitosan, tetraethylene glycol monooctyl ether and sodium styrene sulfonate to the mixed solution of deionized water, ethanol and ethyl propionate in step S101, and then putting the mixture into a reactor to react at 80-160° C. for 4-10 hours; S103, filtering the reaction liquid in the reaction kettle after the reaction in step S102, washing with ethanol, and vacuum drying at 150-250° C. to obtain modified nano titanium dioxide.
3. The method for preparing the porous titanium dioxide-silver composite material modified with phosphate groups according to claim 2, It is characterized in that In the step S101, the mass ratio of ethyl propionate, ethanol and deionized water is 1:3:10, and the mass ratio of nano-titanium dioxide to the mixed solution of deionized water, ethanol and ethyl propionate is 1:(10-30).
4. The method for preparing the porous titanium dioxide-silver composite material modified with phosphate groups according to claim 2, It is characterized in that In the step S102, the mass ratio of the mixed solution of tetraethylene glycol monooctyl ether, sodium styrene sulfonate and carboxymethyl chitosan to deionized water, ethanol and ethyl propionate is 1:(1-3):(5-10):(80-120).
5. The method for preparing the porous titanium dioxide-silver composite material modified with phosphate groups according to claim 1, It is characterized in that In the step S1, the mass ratio of the modified nano titanium dioxide to the deionized water is 1:(100-250), and the volume ratio of the silver nitrate solution to the deionized water is 1:(260-580).
6. The method for preparing the porous titanium dioxide-silver composite material modified with phosphate groups according to claim 1, It is characterized in that The volume ratio of the sodium hydroxide solution in step S2 to the deionized water in step S1 is 1:(15-28), and the mass ratio of the ammonium hypophosphite in step S2 to the modified nano titanium dioxide in step S1 is 1:(0.73-1.73).
7. A titanium dioxide-silver composite material modified with a phosphate group, It is characterized in that The composite material is prepared by the method for preparing a porous titanium dioxide-silver composite material modified with phosphate groups as described in any one of claims 1 to 6.
8. Use of the titanium dioxide-silver composite material modified with phosphate groups prepared by the preparation method according to any one of claims 1 to 6 or the titanium dioxide-silver composite material modified with phosphate groups according to claim 7 in the field of photocatalytic carbon dioxide reduction to prepare hydrocarbon fuels.
9. Use of the titanium dioxide-silver composite material modified with phosphate groups according to claim 8 in the field of photocatalytic carbon dioxide reduction to prepare hydrocarbon fuels, It is characterized in that Use the following method: The titanium dioxide-silver composite material modified with phosphate groups is uniformly mixed with deionized water, and catalytically converts carbon dioxide under light.
Citation Information
Patent Citations
Antimicrobial hydrophilic finishing technology for plasma-chitosan-based silver-loaded-nanometer titanium oxide for polyester fabric
CN108978179A
Preparation method of noble metal and nonmetal loaded nano titanium dioxide, photocatalyst water-based paint and preparation method thereof
CN110975866A
Titanium dioxide-based catalyst preparation method (options)
RU2243033C1
Supported Precious Metal Catalysts Via Hydrothermal Deposition
US20110251055A1