Bismuth subcarbonate in-situ composite bismuth oxyhalide photocatalyst as well as preparation method and application thereof

The in-situ synthesis of bismuth oxycarbonate composite bismuth oxide photocatalysts via acid etching solves the problems of poor catalytic performance and environmental pollution of existing bismuth oxide photocatalysts, achieving efficient and stable visible light catalytic performance and easy recyclability of the photocatalyst.

CN118925766APending Publication Date: 2024-11-12JIANGSU UNIV OF TECH

Patent Information

Application Number
CN202410979744.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing bismuth halide photocatalysts suffer from poor catalytic performance, high electron-hole recombination rates, difficulty in recycling and reuse, and environmental pollution risks.

Method used

A bicarbonate oxybismuth in situ composite bismuth oxide photocatalyst was synthesized by acid etching. By reacting Bi(NO3)3·5H2O and K2CO3 in dilute nitric acid solution to form Bi2O2CO3, and then mixing it with hydrogen halic acid solution, a Bi2O2CO3/BiOX (X=Cl, Br) composite material with a regular lamellar supported structure was prepared.

Benefits of technology

The prepared Bi2O2CO3/BiOX composite material was synthesized at room temperature and pressure, which is low in cost and short in time. It has high visible light response capability and stable photocatalytic performance, and still maintains strong activity after multiple cycles, making it suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118925766A_ABST
    Figure CN118925766A_ABST
Patent Text Reader

Abstract

The embodiment of the invention relates to a bismuth oxycarbonate in-situ composite bismuth oxyhalide photocatalyst as well as a preparation method and application thereof, and belongs to the technical field of photocatalytic materials. The preparation method of the bismuth oxycarbonate in-situ composite bismuth oxyhalide photocatalyst in the embodiment of the invention comprises the following steps: step 1, dissolving bismuth salt in a dilute nitric acid solution, and uniformly mixing and stirring at room temperature to obtain a solution A; dissolving carbonate in water, and uniformly stirring at room temperature to obtain a solution B; step 2, slowly dropwise adding the solution B into the solution A, stirring at normal temperature after dropwise adding, carrying out a co-precipitation reaction, centrifuging, washing and drying to obtain a precursor; and 3, adding the precursor into a halogen acid solution, carrying out ultrasonic treatment, uniformly mixing and stirring at room temperature, centrifuging, washing and drying to obtain the bismuth oxycarbonate in-situ composite bismuth oxyhalide photocatalyst. The bismuth oxycarbonate in-situ composite bismuth oxyhalide photocatalyst provided by the embodiment of the invention has efficient catalytic degradation performance on organic dyes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The embodiments of the present application relate to the technical field of photocatalytic materials, and in particular to a bismuth oxycarbonate in-situ composite bismuth oxyhalide photocatalyst and a preparation method and application thereof. Background Art

[0002] Photocatalysis is a widely used means to solve environmental pollution problems. Photocatalytic technology is more energy-efficient, efficient and safer than electrocatalysis and thermal catalysis. In recent years, photocatalytic technology has been used more and more widely, and significant progress has been made in the development of high-efficiency photocatalysts. In recent years, the bismuth oxyhalide (BiOX, where X is Cl, Br, etc.) series of photocatalysts have attracted much attention due to their unique layered structure and excellent photocatalytic performance. However, the inherent defects of a single catalyst, such as poor catalytic performance and difficulty in recycling and reuse, limit its application in actual production. BiOCl has become a common photocatalytic material due to its unique layered crystal structure and excellent electrical, magnetic and other properties. However, the high electron-hole recombination rate of BiOCl material reduces its photocatalytic performance. Compared with traditional catalysts and oxidants, BiOBr has a higher valence band position and stronger oxidation ability, but its high internal electron-hole recombination rate is a disadvantage that cannot be ignored.

[0003] The existing Chinese patent with the authorization announcement number CN110064425B discloses a bismuth oxycarbonate-bismuth oxychloride heterojunction and the dichloromethane used in its synthesis method is a Class 2A carcinogen and is listed in the list of harmful air pollutants and harmful water pollutants. The existing Chinese patent with the publication number CN101879455A discloses the preparation and application of a photocatalyst bismuth oxychloride. Although certain results have been achieved in degrading organic pollutants, there is a limitation that it can only absorb ultraviolet light with a low content in sunlight to play its role. The existing Chinese patent with the publication number CN114733534A discloses a bismuth oxybromide-lignin composite photocatalyst and its preparation method and application. The bismuth oxybromide lignin composite photocatalyst includes bismuth oxybromide and lignin, and the lignin in its preparation method is only used as a catalyst carrier. Only a small part of the catalytic activity is improved, but it itself does not participate in charge transfer, and does not generate more photogenerated electron-hole pairs. Summary of the invention

[0004] In view of this, the embodiments of the present application provide a bismuth oxycarbonate in-situ composite bismuth oxyhalide photocatalyst and its preparation method and application, which has high efficient catalytic degradation performance for organic dyes; in addition, the synthesis method is simple, easy to control, has no heating reaction, has a high safety factor and does not pose any environmental pollution risk, and can effectively overcome the defects of the above-mentioned prior art.

[0005] The first aspect of the embodiment of the present application provides a method for preparing a bismuth oxycarbonate in-situ composite bismuth oxyhalide photocatalyst, comprising the following steps:

[0006] Step 1: dissolving a bismuth salt in a dilute nitric acid solution, mixing and stirring at room temperature to obtain a solution A; dissolving a carbonate in water, stirring and stirring at room temperature to obtain a solution B;

[0007] Step 2, slowly adding the solution B to the solution A, stirring at room temperature for coprecipitation reaction after the addition is complete, and obtaining a precursor after centrifugation, washing and drying;

[0008] Step 3: adding the precursor to a hydrohalic acid solution, mixing and stirring evenly at room temperature after ultrasonic treatment, and obtaining a bismuth oxycarbonate in-situ composite bismuth oxyhalide photocatalyst after centrifugation, washing and drying.

[0009] In some embodiments that may include the above embodiments, in step 1, the bismuth salt is Bi(NO3)3·5H2O; or

[0010] The concentration of the dilute nitric acid solution is 0.05-0.15 mol / L; or

[0011] The carbonate is K2CO3.

[0012] In some embodiments that may include the above embodiments, in step 1, the molar amount of Bi(NO3)3·5H2O:K2CO3 is 4:(10-13).

[0013] In some embodiments that may include the above embodiments, in step 2, the solution B is slowly added dropwise to the solution A using a syringe pump, and the injection speed of the syringe pump is 10-13 ml / h.

[0014] In some embodiments that may include the above embodiments, in step 2, the co-precipitation reaction time is 1.5-2h.

[0015] In some embodiments that may include the above embodiments, in step 2 or step 3, the drying is performed in a vacuum drying oven, the drying temperature is 60-80° C., and the drying time is 2-3 hours.

[0016] In some embodiments that may include the above embodiments, in step 3, the concentration of the hydrohalic acid solution is 0.05-0.15 mol / L, preferably 0.1 mol / L; or

[0017] The hydrohalic acid solution is HCl solution and / or HBr solution.

[0018] Specifically, the method for preparing the bismuth oxycarbonate in-situ composite bismuth oxyhalide photocatalyst comprises the following steps:

[0019] Step 1: Dissolve Bi(NO3)3·5H2O in HNO3 solution, mix and stir evenly at room temperature, marked as solution A; dissolve K2CO3 in H2O, stir evenly at room temperature, marked as solution B;

[0020] Step 2: transfer the solution B into a syringe pump and slowly add it dropwise to the solution A. After the addition is complete, stir at room temperature. After the stirring is complete, centrifuge and wash;

[0021] Step 3: Place the product obtained after washing in step 2 in a drying oven at a corresponding temperature and dry it until it cools to room temperature to obtain a pure sample of Bi2O2CO3;

[0022] Step 4: Weigh an appropriate amount of the pure Bi2O2CO3 sample obtained in step 3 and put it into a certain amount of hydrohalic acid solution. Use a magnetic stirrer to stir to ensure that the bismuth oxycarbonate is evenly dispersed in the hydrohalic acid solution. After stirring for 20 minutes, the precipitate is washed, filtered and collected. The obtained precipitate is dried in a drying oven at 80°C to obtain Bi2O2CO3 / BiOX (X=Cl, Br) composite materials with different composite ratios.

[0023] The second aspect of the embodiment of the present application also provides a bismuth oxycarbonate in-situ composite bismuth oxyhalide photocatalyst prepared by the above-mentioned preparation method.

[0024] The third aspect of the embodiments of the present application also provides an application of the above-mentioned bismuth oxycarbonate in-situ composite bismuth oxyhalide photocatalyst in the degradation of organic dyes.

[0025] In some embodiments that may include the above embodiments, the following steps are included: mixing the bismuth oxycarbonate in-situ composite bismuth oxyhalide photocatalyst with an aqueous solution of organic pollutants, stirring, and after reaching adsorption-desorption equilibrium under dark conditions, performing a photocatalytic reaction under illumination conditions in the visible light wavelength range to complete the removal of organic pollutants; or

[0026] The amount of the bismuth oxycarbonate in-situ composite bismuth oxyhalide photocatalyst added is 16 mg of catalyst per milliliter of aqueous solution of organic pollutants; or

[0027] The aqueous solution of organic pollutants contains 10 mg / L or 20 mg / L of organic pollutants; or

[0028] The organic pollutant is rhodamine B or crystal violet;

[0029] The wavelength range of the visible light is ≥420nm, and the light source is an LED lamp with a power of 100W; or

[0030] The photocatalytic reaction is carried out at room temperature, and the photocatalytic reaction time is 30-90 minutes.

[0031] Specifically, an appropriate amount of Bi2O2CO3 / BiOX (X = Cl, Br) composite material was weighed and dissolved in wastewater, and rhodamine B and crystal violet were selected as simulated organic pollutants for photocatalytic degradation experiments. The dark reaction stage was carried out under lightless conditions, and after the dark reaction adsorption and desorption were balanced, the light source was turned on at room temperature for photocatalytic degradation.

[0032] Compared with the prior art, the embodiments of the present application have the following beneficial effects:

[0033] (1) The present application uses an acid corrosion method to synthesize a binary composite material with a regular lamellar loading structure. The synthesis process of the Bi2O2CO3 / BiOX (X=Cl, Br) composite material is short in time, low in cost, and low in energy consumption. At the same time, it is synthesized under normal temperature and pressure conditions, which is suitable for industrial and mass production. The obtained composite photocatalyst has broad application prospects;

[0034] (2) The Bi2O2CO3 / BiOX (X = Cl, Br) composite photocatalyst prepared in this application has significantly enhanced photocatalytic performance for organic pollutants and has a high degree of reduction in organic pollutants;

[0035] (3) The Bi2O2CO3 / BiOX (X = Cl, Br) composite photocatalyst prepared in the present application has good visible light response ability, strong photocatalytic performance and stable state, and can still maintain strong photocatalytic activity after multiple cycles. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0037] Figure 1 X-ray diffraction (XRD) diagrams of Examples 1 and 2 and Comparative Examples 1 and 2 of the present application;

[0038] Figure 2 X-ray diffraction (XRD) diagrams of Examples 3 and 4 and Comparative Examples 1 and 3 of the present application;

[0039] Figure 3 It is a scanning electron microscope (SEM) image of Example 2 and Example 4 of the present application, wherein Figure 3 (a) is the SEM image of Bi2O2CO3 / BiOCl. Figure 3 (b) is the SEM image of Bi2O2CO3 / BiOBr;

[0040] Figure 4 This is a scanning electron microscope (SEM) image of Comparative Example 1 of the present application;

[0041] Figure 5 This is a scanning electron microscope (SEM) image of Comparative Example 2 of the present application;

[0042] Figure 6 This is a scanning electron microscope (SEM) image of Comparative Example 3 of the present application;

[0043] Figure 7 This is a graph showing the degradation performance of Rhodamine B in Examples 1 and 2 of the present application and Comparative Examples 1 and 2 in a visible light catalytic system;

[0044] Figure 8 This is a graph showing the degradation performance of Rhodamine B in Examples 3 and 4 of the present application and Comparative Examples 1 and 3 in a visible light catalytic system;

[0045] Fig. 9 This is a graph showing the degradation performance of crystal violet in Examples 1 and 2 of the present application and Comparative Examples 1 and 2 in a visible light catalytic system;

[0046] Fig.10 This is a graph showing the degradation performance of crystal violet in Examples 3 and 4 of the present application and Comparative Examples 1 and 3 in a visible light catalytic system. DETAILED DESCRIPTION

[0047] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0048] Unless otherwise specified, the experimental methods used in the examples of this application are all conventional methods.

[0049] In the following examples and comparative examples, unless otherwise specified, all raw materials can be obtained by commercial purchase or conventional methods.

[0050] Example 1

[0051] A method for preparing a Bi2O2CO3 / BiOCl photocatalyst comprises the following steps:

[0052] (1) Weigh 4 mmol of Bi(NO3)3·5H2O and dissolve it in 10 ml of HNO3 solution (concentration: 0.1 mol / L). Stir on a magnetic stirrer for 30 min at room temperature to fully dissolve it.

[0053] (2) Weigh 10 mmol of K2CO3 and dissolve it in 50 ml of aqueous solution. Stir it on a magnetic stirrer for 30 min at room temperature to fully dissolve it.

[0054] (3) The completely dissolved K2CO3 solution was transferred into a 10 ml syringe, and the syringe was placed in a syringe pump and slowly added dropwise to the solution in step (1) at a rate of 10 ml / h. During this period, the magnetic stirrer was kept stirring at a constant speed, and the coprecipitation reaction was carried out for 2 hours;

[0055] (4) After the reaction is completed, the obtained sample is washed with ethanol 5 times and water 5 times alternately, centrifuged, and placed in a vacuum drying oven at 60° C. for 2 h to obtain a pure sample of bismuth oxycarbonate;

[0056] (5) Weigh 1 mmol of pure Bi2O2CO3 sample and put it into 6 ml of HCl solution (0.1 mol / L). Use a magnetic stirrer to stir to ensure that bismuth carbonate is evenly dispersed in the HCl solution. After stirring for 20 min, wash the resulting precipitate with water 6 times and centrifuge it through a centrifuge. Dry the resulting precipitate in a drying oven at 80°C for 2 h to obtain a photocatalyst named BCl-6.

[0057] Example 2

[0058] A method for preparing a Bi2O2CO3 / BiOCl photocatalyst comprises the following steps:

[0059] (1) Weigh 4 mmol of Bi(NO3)3·5H2O and dissolve it in 10 ml of HNO3 solution (concentration: 0.1 mol / L). Stir on a magnetic stirrer for 30 min at room temperature to fully dissolve it.

[0060] (2) Weigh 10 mmol of K2CO3 and dissolve it in 50 ml of aqueous solution. Stir it on a magnetic stirrer for 30 min at room temperature to fully dissolve it.

[0061] (3) The completely dissolved K2CO3 solution was transferred into a 10 ml syringe, and the syringe was placed in a syringe pump and slowly added dropwise to the solution in step (1) at a rate of 10 ml / h. During this period, the magnetic stirrer was kept stirring at a constant speed, and the coprecipitation reaction was carried out for 2 hours;

[0062] (4) After the reaction is completed, the obtained sample is washed with ethanol 5 times and water 5 times alternately, centrifuged, and placed in a vacuum drying oven at 80° C. for 2 h to obtain a pure sample of bismuth carbonate;

[0063] (5) Weigh 1 mmol of pure Bi2O2CO3 sample and put it into 12 ml of HCl solution (0.1 mol / L). Use a magnetic stirrer to stir to ensure that bismuth carbonate is evenly dispersed in the HCl solution. After stirring for 20 min, wash the resulting precipitate with water 6 times and centrifuge it through a centrifuge. Dry the resulting precipitate in a drying oven at 80°C for 2 h to obtain a photocatalyst named BCl-12.

[0064] The BCl-12 photocatalyst prepared in this example was subjected to X-ray diffraction, and the obtained XRD spectrum was as follows: Figure 1 As shown in the figure, the diffraction peaks of BCl-12 photocatalyst all come from Bi2O2CO3 (PDF#97-009-4740) and BiOCl (PDF#97-002-9143), and no other peaks appear, which indicates that BiOCl is generated during the HCl corrosion process and no other impurities are introduced. This preliminarily proves that the BCl-12 photocatalyst was successfully synthesized.

[0065] The BCl-12 photocatalyst prepared in this example was observed by scanning electron microscope. The SEM image is as follows: Figure 3 As shown in (a), it can be seen that BCl-12 presents a structure in which small nanosheets are attached to large nanosheets and are evenly distributed. Combined with the XRD spectrum, it can be judged that a BCl-12 photocatalyst with good crystallinity has been synthesized.

[0066] Example 3

[0067] A method for preparing a Bi2O2CO3 / BiOBr photocatalyst comprises the following steps:

[0068] (1) Weigh 4 mmol of Bi(NO3)3·5H2O and dissolve it in 10 ml of HNO3 solution (concentration: 0.1 mol / L). Stir on a magnetic stirrer for 30 min at room temperature to fully dissolve it.

[0069] (2) Weigh 10 mmol of K2CO3 and dissolve it in 50 ml of aqueous solution. Stir it on a magnetic stirrer for 30 min at room temperature to fully dissolve it.

[0070] (3) The completely dissolved K2CO3 solution was transferred into a 10 ml syringe, and the syringe was placed in a syringe pump and slowly added dropwise to the solution in step (1) at a rate of 10 ml / h. During this period, the magnetic stirrer was kept stirring at a constant speed, and the coprecipitation reaction was carried out for 2 hours;

[0071] (4) After the reaction is completed, the obtained sample is washed with ethanol 5 times and water 5 times alternately, centrifuged, and placed in a vacuum drying oven at 60° C. for 2 h to obtain a pure sample of bismuth oxycarbonate;

[0072] (5) Weigh 1 mmol of pure Bi2O2CO3 sample and put it into 6 ml of HBr solution (0.1 mol / L). Use a magnetic stirrer to stir to ensure that bismuth oxycarbonate is evenly dispersed in the HBr solution. After stirring for 20 min, wash the resulting precipitate with water 6 times and centrifuge it through a centrifuge. Dry the resulting precipitate in a drying oven at 80°C for 2 h to obtain a photocatalyst named BBr-6.

[0073] Example 4

[0074] A method for preparing a Bi2O2CO3 / BiOBr photocatalyst comprises the following steps:

[0075] (1) Weigh 4 mmol of Bi(NO3)3·5H2O and dissolve it in 10 ml of HNO3 solution (concentration: 0.1 mol / L). Stir on a magnetic stirrer for 30 min at room temperature to fully dissolve it.

[0076] (2) Weigh 10 mmol of K2CO3 and dissolve it in 50 ml of aqueous solution. Stir it on a magnetic stirrer for 30 min at room temperature to fully dissolve it.

[0077] (3) The completely dissolved K2CO3 solution was transferred into a 10 ml syringe, and the syringe was placed in a syringe pump and slowly added dropwise to the solution in step (1) at a rate of 10 ml / h. During this period, the magnetic stirrer was kept stirring at a constant speed, and the coprecipitation reaction was carried out for 2 hours;

[0078] (4) After the reaction is completed, the obtained sample is washed with ethanol 5 times and water 5 times alternately, centrifuged, and placed in a vacuum drying oven at 80° C. for 2 h to obtain a pure sample of bismuth carbonate;

[0079] (5) Weigh 1 mmol of pure Bi2O2CO3 sample and put it into 12 ml of HBr solution (0.1 mol / L). Use a magnetic stirrer to stir to ensure that bismuth oxycarbonate is evenly dispersed in the HBr solution. After stirring for 20 min, wash the resulting precipitate with water 6 times and centrifuge it through a centrifuge. Dry the resulting precipitate in a drying oven at 80°C for 2 h to obtain a photocatalyst named BBr-12.

[0080] The BBr-12 photocatalyst prepared in this example was subjected to X-ray diffraction, and the obtained XRD spectrum was as follows: Figure 2 As shown. The diffraction peaks of BBr-12 photocatalyst all come from Bi2O2CO3 (PDF#97-009-4740) and BiOBr (PDF#97-006-1225), and no other peaks appear, which indicates that BiOBr is generated during the HBr corrosion process and no other impurities are introduced. This preliminarily proves that the BBr-12 photocatalyst was successfully synthesized.

[0081] The BBr-12 photocatalyst prepared in this example was observed by scanning electron microscope. The SEM image is as follows: Figure 3 As shown in (b), it can be seen that BBr-12 presents a structure in which small nanosheets are attached to large nanosheets and are evenly distributed. Combined with the XRD spectrum, it can be judged that a BBr-12 photocatalyst with good crystallinity has been synthesized.

[0082] Comparative Example 1

[0083] The preparation method of bismuth oxycarbonate comprises the following steps:

[0084] (1) Weigh 4 mmol of Bi(NO3)3·5H2O and dissolve it in 10 ml of HNO3 solution (concentration: 0.1 mol / L). Stir on a magnetic stirrer for 30 min at room temperature to fully dissolve it.

[0085] (2) Weigh 10 mmol of K2CO3 and dissolve it in 50 ml of aqueous solution. Stir it on a magnetic stirrer for 30 min at room temperature to fully dissolve it.

[0086] (3) The completely dissolved K2CO3 solution was transferred into a 10 ml syringe, and the syringe was placed in a syringe pump and slowly added dropwise to the solution in step (1) at a rate of 10 ml / h. During this period, the magnetic stirrer was kept stirring at a constant speed, and the coprecipitation reaction was carried out for 2 hours;

[0087] (4) After the reaction is completed, the obtained sample is washed with ethanol 5 times and water 5 times alternately, centrifuged through a centrifuge, and placed in a vacuum drying oven at 60°C for 2 h to obtain a pure Bi2O2CO3 sample.

[0088] The Bi2O2CO3 photocatalyst prepared in this comparative example was observed by scanning electron microscope. The SEM image is as follows: Figure 4 As shown, it can be seen that Bi2O2CO3 presents a nanosheet shape. Further magnification shows that there are obvious lattice fringes and they are evenly distributed. Combined with the XRD spectrum, it can be judged that a Bi2O2CO3 photocatalyst with good crystallinity has been synthesized.

[0089] Comparative Example 2

[0090] The preparation method of bismuth oxychloride comprises the following steps:

[0091] (1) Weigh 4 mmol of Bi(NO3)3·5H2O and dissolve it in 10 ml of HNO3 solution (concentration: 0.1 mol / L). Stir on a magnetic stirrer for 30 min at room temperature to fully dissolve it.

[0092] (2) Weigh 10 mmol of K2CO3 and dissolve it in 50 ml of aqueous solution. Stir it on a magnetic stirrer for 30 min at room temperature to fully dissolve it.

[0093] (3) The completely dissolved K2CO3 solution was transferred into a 10 ml syringe, and the syringe was placed in a syringe pump and slowly added dropwise to the solution in step (1) at a rate of 10 ml / h. During this period, the magnetic stirrer was kept stirring at a constant speed, and the coprecipitation reaction was carried out for 2 hours;

[0094] (4) After the reaction is completed, the obtained sample is washed with ethanol 5 times and water 5 times alternately, centrifuged, and placed in a vacuum drying oven at 80° C. for 2 h to obtain a pure sample of bismuth carbonate;

[0095] (5) Weigh 1 mmol of pure Bi2O2CO3 sample and put it into 100 ml of HCl solution (0.1 mol / L). Use a magnetic stirrer to stir to ensure that bismuth oxycarbonate is evenly dispersed in the HCl solution. After stirring for 20 min, wash the resulting precipitate with water 6 times and centrifuge it through a centrifuge. Dry the resulting precipitate in a drying oven at 80°C for 2 h to obtain a pure BiOCl sample.

[0096] The BiOCl photocatalyst prepared in this comparative example was observed by scanning electron microscope. Figure 5 As shown, BiOCl is in the shape of a nanosheet. Further magnification shows that BiOCl is composed of many irregular nanosheets stacked together with a smooth surface. Combined with the XRD spectrum, it can be further determined that a BiOCl photocatalyst with good crystallinity has been synthesized.

[0097] Comparative Example 3

[0098] The preparation method of bismuth oxybromide comprises the following steps:

[0099] (1) Weigh 4 mmol of Bi(NO3)3·5H2O and dissolve it in 10 ml of HNO3 solution (concentration: 0.1 mol / L). Stir on a magnetic stirrer for 30 min at room temperature to fully dissolve it.

[0100] (2) Weigh 10 mmol of K2CO3 and dissolve it in 50 ml of aqueous solution. Stir it on a magnetic stirrer for 30 min at room temperature to fully dissolve it.

[0101] (3) The completely dissolved K2CO3 solution was transferred into a 10 ml syringe, and the syringe was placed in a syringe pump and slowly added dropwise to the solution in step (1) at a rate of 10 ml / h. During this period, the magnetic stirrer was kept stirring at a constant speed, and the coprecipitation reaction was carried out for 2 hours;

[0102] (4) After the reaction is completed, the obtained sample is washed with ethanol 5 times and water 5 times alternately, centrifuged, and placed in a vacuum drying oven at 80° C. for 2 h to obtain a pure sample of bismuth carbonate;

[0103] (5) Weigh 1 mmol of pure Bi2O2CO3 sample and put it into 100 ml of HBr solution (0.1 mol / L). Use a magnetic stirrer to stir to ensure that bismuth oxycarbonate is evenly dispersed in the HBr solution. After stirring for 20 min, wash the resulting precipitate with water 6 times and centrifuge it through a centrifuge. Dry the resulting precipitate in a drying oven at 80°C for 2 h to obtain a pure BiOBr sample.

[0104] The BiOBr photocatalyst prepared in this comparative example was observed by scanning electron microscope. Figure 6 As shown, it can be seen that BiOBr presents a nanosheet shape. Further magnification shows that BiOBr is composed of many irregular nanosheets stacked in a smooth surface. Combined with the XRD spectrum, it can be further determined that a BiOBr photocatalyst with good crystallinity has been synthesized.

[0105] Degradation performance

[0106] 1. Degradation of Rhodamine B

[0107] The BiOCl / Bi2O2CO3 composite materials of the above-mentioned embodiments 1 and 2, the pure Bi2O2CO3 samples of the comparative example 1, and the pure BiOCl samples of the comparative example 2 were subjected to a photocatalytic degradation experiment under a visible light catalytic system. The simulated organic pollutant was Rhodamine B and the amount of sewage was 40 ml. With an LED lamp as the light source (power of 100 W, visible light wavelength range ≥ 420 nm), the dark reaction was 30 min to reach adsorption-desorption equilibrium, the light reaction was 30 min and 4 ml of sample was drawn every 5 min, centrifuged at 4000 rpm for 3 min, and measured and recorded at its maximum absorption wavelength using an ultraviolet-visible spectrophotometer. The degradation efficiency was expressed as C / C0, where C represented the sample concentration at different time periods, and C0 represented the sample concentration at the initial state. Figure 7 This is a graph showing the photocatalytic performance of the BiOCl / Bi2O2CO3 composite materials of Examples 1 and 2, the pure Bi2O2CO3 sample of Comparative Example 1, and the pure BiOCl sample of Comparative Example 2 for Rhodamine B in a visible light catalytic system.

[0108] Depend on Figure 7 It can be seen that the photocatalytic performance of Bi2O2CO3 / BiOCl composite samples is better than that of pure BiOCl and Bi2O2CO3, and the photocatalytic performance of BCl-12 is the best. Figure 7 The blank control (Blank) refers to the degradation reaction without adding any photocatalyst.

[0109] In summary, the Bi2O2CO3 / BiOCl composite photocatalyst has enhanced visible light response and photocatalytic activity, and can efficiently photocatalytically remove organic pollutants.

[0110] The BiOBr / Bi2O2CO3 composite materials of the above-mentioned Examples 3 and 4, the pure Bi2O2CO3 samples of Comparative Example 1, and the pure BiOBr samples of Comparative Example 3 were subjected to a photocatalytic degradation experiment under a visible light catalytic system. The simulated organic pollutant was Rhodamine B and the amount of sewage was 40 ml. An LED lamp was used as a light source (power was 100 W, and the visible light wavelength range was ≥ 420 nm). The dark reaction lasted for 30 min to reach adsorption-desorption equilibrium. The light reaction lasted for 30 min and 4 ml of sample was drawn every 5 min. The sample was centrifuged at 4000 rpm for 3 min, and measured and recorded at its maximum absorption wavelength using an ultraviolet-visible spectrophotometer. The degradation efficiency was expressed as C / C0, where C represented the sample concentration at different time periods, and C0 represented the sample concentration at the initial state. Figure 8 This is a graph showing the photocatalytic performance of the BiOBr / Bi2O2CO3 composite materials of Examples 3 and 4, the pure Bi2O2CO3 sample of Comparative Example 1, and the pure BiOBr sample of Comparative Example 3 for Rhodamine B in a visible light catalytic system.

[0111] Depend on Figure 8 It can be seen that the photocatalytic performance of Bi2O2CO3 / BiOBr composites is better than that of pure BiOBr and Bi2O2CO3, and BBr-12 has the best photocatalytic performance. Figure 8 The blank control (Blank) refers to the degradation reaction without adding any photocatalyst.

[0112] In summary, the Bi2O2CO3 / BiOBr composite photocatalyst has enhanced visible light response and photocatalytic activity, and can efficiently photocatalytically remove organic pollutants.

[0113] 2. Degradation of crystal violet

[0114] The BiOCl / Bi2O2CO3 composite materials of the above-mentioned embodiments 1 and 2, the pure Bi2O2CO3 samples of the comparative example 1, and the pure BiOCl samples of the comparative example 2 were subjected to a photocatalytic degradation experiment under a visible light catalytic system. The simulated organic pollutant was crystal violet and the amount of sewage was 40 ml. With an LED lamp as the light source (power of 100 W, visible light wavelength range ≥ 420 nm), the dark reaction was 30 min to reach adsorption-desorption equilibrium, the light reaction was 30 min and 4 ml of sample was drawn every 5 min, centrifuged at 4000 rpm for 3 min, and measured and recorded at its maximum absorption wavelength using an ultraviolet-visible spectrophotometer. The degradation efficiency was expressed as C / C0, where C represented the sample concentration at different time periods, and C0 represented the sample concentration at the initial state. Fig. 9This is a graph showing the photocatalytic performance of the BiOCl / Bi2O2CO3 composite materials of Examples 1 and 2, the pure Bi2O2CO3 sample of Comparative Example 1, and the pure BiOCl sample of Comparative Example 2 to crystal violet in a visible light catalytic system.

[0115] Depend on Fig. 9 It can be seen that the photocatalytic performance of Bi2O2CO3 / BiOCl composite samples is better than that of pure BiOCl and Bi2O2CO3, and the photocatalytic performance of BCl-12 is the best. Fig. 9 The blank control (Blank) refers to the degradation reaction without adding any photocatalyst.

[0116] In summary, the Bi2O2CO3 / BiOCl composite photocatalyst has enhanced visible light response and photocatalytic activity, and can efficiently photocatalytically remove organic pollutants.

[0117] The BiOBr / Bi2O2CO3 composite materials of the above-mentioned Examples 3 and 4, the pure Bi2O2CO3 samples of Comparative Example 1, and the pure BiOBr samples of Comparative Example 3 were subjected to a photocatalytic degradation experiment under a visible light catalytic system. The simulated organic pollutant was crystal violet and the amount of sewage was 40 ml. An LED lamp was used as a light source (power was 100 W, and the visible light wavelength range was ≥ 420 nm). The dark reaction lasted for 30 min to reach adsorption-desorption equilibrium. The light reaction lasted for 30 min and 4 ml of sample was drawn every 5 min. The sample was centrifuged at 4000 rpm for 3 min, and measured and recorded at its maximum absorption wavelength using an ultraviolet-visible spectrophotometer. The degradation efficiency was expressed as C / C0, where C represented the sample concentration at different time periods, and C0 represented the sample concentration at the initial state. Fig.10 This is a graph showing the photocatalytic performance of the BiOBr / Bi2O2CO3 composite materials of Examples 3 and 4, the pure Bi2O2CO3 sample of Comparative Example 1, and the pure BiOBr sample of Comparative Example 3 for crystal violet in a visible light catalytic system.

[0118] Depend on Fig.10 It can be seen that the photocatalytic performance of Bi2O2CO3 / BiOBr composites is better than that of pure BiOBr and Bi2O2CO3, and BBr-12 has the best photocatalytic performance. Fig.10 The blank control (Blank) refers to the degradation reaction without adding any photocatalyst.

[0119] In summary, the Bi2O2CO3 / BiOBr composite photocatalyst has enhanced visible light response and photocatalytic activity, and can efficiently photocatalytically remove organic pollutants.

[0120] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.

Claims

1. A method for preparing a bismuth oxycarbonate in-situ composite bismuth oxyhalide photocatalyst, It is characterized in that The following steps are involved: Step 1: dissolving a bismuth salt in a dilute nitric acid solution, mixing and stirring at room temperature to obtain a solution A; dissolving a carbonate in water, stirring and stirring at room temperature to obtain a solution B; Step 2, slowly adding the solution B to the solution A, stirring at room temperature for coprecipitation reaction after the addition is complete, and obtaining a precursor after centrifugation, washing and drying; Step 3: adding the precursor to a hydrohalic acid solution, mixing and stirring evenly at room temperature after ultrasonic treatment, and obtaining a bismuth oxycarbonate in-situ composite bismuth oxyhalide photocatalyst after centrifugation, washing and drying.

2. The method for preparing the bismuth oxycarbonate in-situ composite bismuth oxyhalide photocatalyst according to claim 1, It is characterized in that In step 1, the bismuth salt is Bi(NO 3 ) 3 ·5H 2 O; or The concentration of the dilute nitric acid solution is 0.05-0.15 mol / L; or The carbonate is K 2 CO 3 .

3. The method for preparing the bismuth oxycarbonate in-situ composite bismuth oxyhalide photocatalyst according to claim 2, It is characterized in that In step 1, the Bi(NO 3 ) 3 ·5H 2 O:K 2 CO 3 The molar dosage is 4:(10-13).

4. The method for preparing the bismuth oxycarbonate in-situ composite bismuth oxyhalide photocatalyst according to claim 1, It is characterized in that In step 2, the solution B is slowly added dropwise to the solution A using a syringe pump, and the injection speed of the syringe pump is 10-13 ml / h.

5. The method for preparing the bismuth oxycarbonate in-situ composite bismuth oxyhalide photocatalyst according to claim 1, It is characterized in that In step 2, the coprecipitation reaction time is 1.5-2h.

6. The method for preparing the bismuth oxycarbonate in-situ composite bismuth oxyhalide photocatalyst according to claim 1, It is characterized in that In step 2 or step 3, the drying is performed in a vacuum drying oven, the drying temperature is 60-80° C., and the drying time is 2-3 hours.

7. The method for preparing the bismuth oxycarbonate in-situ composite bismuth oxyhalide photocatalyst according to claim 1, It is characterized in that In step 3, the concentration of the hydrohalic acid solution is 0.05-0.15 mol / L; or The hydrohalic acid solution is HCl solution and / or HBr solution.

8. An in-situ bismuth oxycarbonate composite bismuth oxyhalide photocatalyst prepared by the preparation method according to any one of claims 1 to 7.

9. Use of the bismuth oxycarbonate in-situ composite bismuth oxyhalide photocatalyst as claimed in claim 8 in the degradation of organic dyes.

10. The use according to claim 9, It is characterized in that The method comprises the following steps: mixing the bismuth oxycarbonate in-situ composite bismuth oxyhalide photocatalyst with an aqueous solution of organic pollutants, stirring, and after reaching adsorption-desorption equilibrium under dark conditions, performing a photocatalytic reaction under illumination conditions in the visible light wavelength range to complete the removal of the organic pollutants; or The amount of the bismuth oxycarbonate in-situ composite bismuth oxyhalide photocatalyst added is 16 mg of catalyst per milliliter of aqueous solution of organic pollutants; or The aqueous solution of organic pollutants contains 10 mg / L or 20 mg / L of organic pollutants; or The organic pollutant is rhodamine B or crystal violet; The wavelength range of the visible light is ≥420nm, and the light source is an LED lamp with a power of 100W; or The photocatalytic reaction is carried out at room temperature, and the photocatalytic reaction time is 30-90 minutes.

Citation Information

Patent Citations

  • Bismuth subcarbonate photocatalyst and preparation method thereof

    CN102527420A

  • Preparation method of bismuth oxyhalide / bismuth oxide visible-light photocatalyst

    CN104525225A

  • Iodine intercalated bismuthyl carbonate as well as preparation method and application thereof

    CN113828338A

  • Preparation method for preparing bismuthyl carbonate photocatalyst by utilizing inactivated bismuth oxyiodide

    CN116282148A

Cited By

  • Bi / Bi2O2CO3 nanoflower sheet reconstructed and derived from Bi / BiOBr as well as preparation method and application of Bi / Bi2O2CO3 nanoflower sheet