Flotation method for spodumene ore

By combining a fine mud surface modifier and anionic collector with a cascade recovery process, the negative impact of fine mud minerals on spodumene flotation was resolved, improving the recovery rate and concentrate quality of spodumene minerals, reducing reagent costs, and enhancing separation efficiency.

CN118925943APending Publication Date: 2024-11-12CHINA ENFI ENG CORP +1

Patent Information

Application Number
CN202411191931.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing spodumene mineral flotation technology cannot effectively regulate the negative effects of fine-grained minerals or mud minerals in the process, resulting in poor lithium concentrate quality, large flotation agent consumption, and low separation process efficiency.

Method used

By employing a fine mud surface modifier and a highly selective anionic collector, combined with a cascade recovery process, and through the compounding of modifiers, metal ion activators, and collectors, the surface modification and electrical regulation of fine mud minerals are achieved, and the mineral particles are separated by utilizing the difference in their flotation rates.

Benefits of technology

It improves the recovery rate and concentrate quality of spodumene minerals, reduces the cost of flotation reagents, enhances separation efficiency and process adaptability, and reduces the negative impact of fine slime on spodumene flotation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118925943A_ABST
    Figure CN118925943A_ABST
Patent Text Reader

Abstract

The invention discloses a spodumene ore flotation method which sequentially comprises the steps that spodumene ore is crushed and ground to obtain ore pulp, a regulator, a metal ion activating agent and a collecting agent are sequentially added into the ore pulp, air inflation is conducted after stirring, separation is conducted, and spodumene concentrate and tailing products are obtained. A process of adding a fine silt surface modification masking agent is further included between the steps of adding the adjusting agent and the metal ion activating agent, and the fine silt surface modification masking agent comprises an OH-surface modifier component with the performance of enhancing the electronegativity expression of the fine silt surface and a fine silt mineral surface electrostatic masking agent component with the electrostatic masking performance; the collecting agent is formed by compounding multiple types of anion active collecting components and oil-water emulsifying components. The step recovery and the process fine silt regulation and control are carried out according to the difference of the floating speed of mineral particles in the separation. The method overcomes the defect that the existing spodumene mineral flotation technology cannot effectively regulate the negative influence of micro-fine particle minerals or fine silt minerals in the process, and can improve the mineral dissociation efficiency and the lithium concentrate quality.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of ore flotation, and in particular to a spodumene ore flotation method. Background Art

[0002] Limited by the genesis of lithium ore, the natural endowment of spodumene ore resources is relatively poor, the content of spodumene minerals is generally low, the mineral composition and the relationship between minerals in the ore are complex, etc., and mineral beneficiation methods are often required to enrich and recover lithium minerals before lithium metal extraction and metallurgy. After years of technological replacement and development, the beneficiation technology of lithium-containing minerals, flotation enrichment and recovery of lithium minerals from low-grade spodumene ores, is still the dominant method for the development of lithium ore resources.

[0003] The flotation enrichment process of spodumene minerals often requires the selective separation of lithium-containing minerals from a variety of silicate minerals / aluminosilicate minerals (feldspar (sodium / potassium feldspar), quartz, mica (black / white / phlogopite), chlorite, tourmaline, calcite, etc.). Due to the differences in the degree of mineral crystallization (particle size, morphology, etc.), the occurrence relationship between minerals, the hardness of minerals and their crushing characteristics in the original ore, it is inevitable that fine or micro-fine mineral mud will be produced during the mineral crushing and dissociation. This type of fine mud often has a very adverse effect on the flotation enrichment of spodumene minerals, such as easily entering the flotation concentrate to reduce the quality of lithium concentrate, competing for the adsorption of flotation agents and greatly increasing the consumption of reagents, and being difficult to discharge tailings and circulated and accumulated in the middlings to reduce the processing efficiency of the sorting process, etc., especially in low-grade spodumene ore, the negative impact of mineral mud is more prominent.

[0004] In order to reduce or avoid the adverse effects of fine mud, the commonly used desludging methods are physical desludging and chemical desludging. Among them, physical desludging includes sedimentation desludging, centrifugal desludging (such as cyclone desludging, centrifuge desludging), etc., and chemical desludging is to use flotation agents to float out fine mud materials in advance before sorting lithium-containing minerals. However, these physical or chemical methods to reduce the impact of fine mud have many technical defects, among which the common deficiencies are: 1) The desludging amount is difficult to be stably controlled, and a large amount of fine mud minerals are often removed, resulting in improper loss of lithium-containing minerals; 2) The selectivity for mineral particle size is not high, and coarse-grained minerals are lost during the desludging process.

[0005] In addition, the shortcomings of flotation desludging are that the desludging flotation agent used is relatively non-selective and has low efficiency in capturing fine mud, which makes the desludging effect unsatisfactory; the sedimentation desludging takes a relatively long time and requires a large area; when desludging with a hydrocyclone, the quality of desludging depends on the operating efficiency of the cyclone or cyclone group, and problems such as equipment wear and pipeline blockage often affect the desludging effect. Therefore, how to effectively deal with the negative impact of spodumene mineral flotation fine mud is one of the major difficult problems that need to be broken through in spodumene ore flotation.

[0006] On the whole, the existing spodumene mineral flotation technology still does not have a highly selective and easy-to-dispose process for how to effectively regulate the negative impact of fine-grained minerals or fine mud minerals in the process; at the same time, in order to avoid excessive loss of fine mud lithium minerals in demudified minerals, the advantageous full-size flotation is still the most effective solution. Therefore, the development of new spodumene ore flotation separation technology, especially full-size flotation technology, with a suitable reagent system and flotation process matching, reduces the improper impact of mud minerals, and improves the selectivity of mud mineral orientation control, which is of great significance to reducing the cost of flotation reagents and improving the quality of lithium concentrate. However, the existing technology does not have a selective orientation control technology for fine mud minerals, which often results in large amounts of flotation agents, high fine mud lithium loss rate, poor quality of lithium concentrate, and low efficiency of the sorting process. Summary of the invention

[0007] Therefore, the technical problem to be solved by the present invention is to overcome the defect that the existing spodumene mineral flotation technology cannot effectively regulate the negative impact of fine-grained minerals or fine mud minerals in the process, thereby providing a spodumene ore flotation method that solves the above problem.

[0008] A spodumene ore flotation method comprises the following steps: grinding the spodumene ore to obtain ore pulp, adding a regulator, a metal ion activator, and a collector to the ore pulp in sequence, stirring the ore pulp, aerating the ore pulp, and performing separation to obtain spodumene concentrate and tailings products;

[0009] The process of adding a fine mud surface modification masking agent between the steps of adding the adjusting agent and the metal ion activator includes an OH-surface modification agent component having the performance of enhancing the negative charge expression of the fine mud surface and a fine mud mineral surface electrostatic masking agent component having electrostatic masking performance;

[0010] The collector is compounded by multiple types of anionic active collecting components and oil-water emulsifying components;

[0011] The separation is carried out by step recovery and regulation of process fine mud according to the difference in the floating speed of mineral particles.

[0012] The OH-surface modifier component includes one or more of sodium hydroxide, potassium hydroxide, ammonia, methylamine, and dimethylamine;

[0013] And / or, the electrostatic masking agent component on the surface of the fine mud mineral is a cationic electrostatic masking agent and / or an amphoteric electrostatic masking agent;

[0014] And / or, the ratio of the OH-surface modification adjusting agent component to the fine mud mineral surface electrostatic masking agent component is 1:(0.1-0.25).

[0015] The electrostatic masking agent component on the surface of fine mud minerals includes one or more of N-butylpyridinium nitrate, N-hexadecylpyridinium-nitrate, aminoalkyl polyethylene glycol ether, 4-methyl-2-(methylimino)-1-imidazolineamine, 2-methoxyimidazoline, 1-(benzyl)imidazoline-2-one, 1-methyl-2-benzimidazolinone, N,N-dimethyl-β-hydroxyethyl octadecanoylamide-γ-propyl quaternary ammonium nitrate, poly-2-methacryloyloxyethyl trimethylammonium chloride, and polyvinyl benzyl trimethyl quaternary ammonium salt;

[0016] And / or, based on the treated spodumene ore dry ore, the addition amount of the OH-surface modifier component is 100-2000 g / t;

[0017] And / or, based on the treated dry spodumene ore, the added amount of the electrostatic masking agent component on the surface of the fine mud mineral is 10-500 g / t.

[0018] In the step of crushing and grinding the spodumene ore to obtain ore pulp, the fineness of the ore pulp is -0.074 mm, accounting for 60% to 95%.

[0019] The adjusting agent is used to provide inorganic CO 3 2- The carbonation adjusting agent is preferably one or more of sodium carbonate, ammonium carbonate, potassium carbonate, sodium bicarbonate, and potassium bicarbonate;

[0020] And / or, based on the treated dry spodumene ore, the added amount of the adjusting agent is 400-8000 g / t.

[0021] The metal ion activator is a metal ion activator having a metal ion radius close to that of the Al / Li ion, preferably a metal ion activator of calcium or magnesium, more preferably one or more of calcium sulfate, calcium nitrate, calcium chloride, magnesium sulfate, magnesium nitrate, and magnesium chloride;

[0022] And / or, based on the treated dry spodumene ore, the added amount of the metal ion activator is 50-1000 g / t.

[0023] The collector is compounded by multiple types of anionic active collecting components and oil-water emulsifying components;

[0024] The multiple categories of anion active collecting components include a combination of at least two categories of fatty acids and salts, sulfonates, sulfates, phosphonates, and hydroxamic acid collectors;

[0025] The oil-water emulsified component includes one or more of neutral oils, polyether esters, polyether silicones, and polyether amines;

[0026] And / or, based on the treated dry spodumene ore, the added amount of the collector is 100 to 4000 g / t.

[0027] The fatty acids and their salts include one or more of oleic acid / sodium oleate, stearic acid / sodium stearate, palmitic acid / sodium palmitate, lauric acid / sodium laurate, hexadecanoic acid / sodium hexadecanoate, and a fatty acid mixture; preferably, the fatty acid mixture includes one or more of oxidized paraffin soap, tall oil, cyclopentane acid soap, and complex fatty acid sodium;

[0028] And / or, the sulfonate is sodium dodecylbenzene sulfonate, sodium dodecyl sulfonate, sodium petroleum sulfonate, complex Sodium fatty acid sulfonate One or more of;

[0029] And / or, the sulfate is one or more of sodium dodecyl sulfate, sodium tetradecyl sulfate, sodium hexadecyl sulfate;

[0030] And / or, the hydroxamic acid is one or more of benzyl hydroxamic acid and alkyl hydroxamic acid;

[0031] and / or, the oil-water emulsified component includes one of kerosene, diesel, silicone oil, polyoxyethylene ether, polyether alcohol, polyether amine, and trihydroxypropane polypropylene glycol ether;

[0032] And / or, the compounding ratio of the multiple types of anionic active collecting components to the oil-water emulsification components is 1:(0.02-0.1).

[0033] The sorting method includes:

[0034] Rapid flotation is used to first separate the easily floatable minerals with some target minerals, and then a fine mud surface modification masking agent is added after the easily floatable minerals are floated out, so that the relatively slow-floating fine mud minerals are controlled in the second half of the flotation process, and the relatively slow-floating minerals / mineral fine mud are modified and adjusted to achieve secondary direction control of fine mud minerals;

[0035] Or, use rapid flotation to first sort out the easily floatable minerals with some target minerals, and then dissociate the relatively slow-floating foam products by grinding and scrubbing, and then adjust the direction of fine mud by scrubbing the surface of the minerals;

[0036] Alternatively, rapid flotation is used to first separate out the easily floating minerals containing part of the target minerals, and the easily floating minerals are selected for the first time. The bottom product obtained by selection, the foam product of the bottom product of the rapid flotation and the scavenging foam product with a high fine mud content of the bottom product of the fine mud slow flotation are mixed, and then the scrubbing slurry is obtained by grinding and scrubbing and then dissociating. The medium ore with a high fine mud content that is selected and thrown out by the scrubbing slurry is introduced into the roughing bottom product of the fine mud slow flotation.

[0037] The flotation process is any one of the following (1)-(3);

[0038] (1) Within 1 to 2 minutes, the foam floats out for rapid flotation to obtain the foam product roughing I of the easily floatable mineral and the bottom product tailings pulp E, then add the fine mud surface modification masking agent to the tailings pulp E, the amount of the fine mud surface modification masking agent added is 1 / 5 to 1 / 20 of the amount of the fine mud surface modification masking agent added in the previous time, and after 0.5 to 2 minutes of re-modification, re-competition and re-dispersion, obtain the slurry F to be scavenged, then add the metal ion activator + collector or collector for 2 to 5 minutes of pulping and perform fine mud slow floating for 2 to 6 minutes to obtain the roughing II and the bottom product F, the amount of the metal ion activator added is 1 / 5 to 1 / 2 of the amount of the first metal ion activator added, and the amount of the collector added is the amount of the first collector added. The amount of the added amount is 1 / 5 to 1 / 20, and a metal ion activator and a collector are added to the bottom product F for scavenging. The scavenging number is at least one, and the scavenging time is 2 to 6 minutes. Scavenging I and subsequent foam products are obtained in sequence according to the scavenging number. The tailings pulp after the last scavenging is the flotation tailings; the roughing II is cleaned once to obtain the concentrating I and the bottom product G; the concentrating I and the roughing I are mixed, and then separated by 2 to 3 times of 2 to 6 minutes to finally obtain lithium concentrate and the bottom product H; the bottom product G and the foam products of scavenging I and subsequent foam products are returned to the tailings pulp E in the form of middlings for circulation, and the bottom product H is returned to the pulp as the middlings for circulation; wherein, a concentrating adjuster is added during the concentrating, preferably a carbonation adjuster;

[0039] (2) Within 1 to 2 minutes, the foam floats out for rapid flotation to obtain the foam product roughing I of the easily floatable minerals and the tailings pulp E of the bottom product. The tailings pulp E is then subjected to 1 to 2 minutes of slow fine mud flotation to obtain roughing II and the slurry F to be scavenged. Subsequently, a metal ion activator and a collector are added to the slurry F to be scavenged for 2 to 5 minutes of slurry adjustment and scavenging. The slurry adjustment and scavenging times are at least twice, and the scavenging time is 2 to 6 minutes. Scavenging I and the foam products after scavenging I are obtained in sequence according to the slurry adjustment and scavenging times. The tailings pulp after the last scavenging is the floating pulp. The tailings are selected; the roughing II and the scavenging I are combined and then ground and scrubbed for 1 to 2 minutes to obtain the re-grinding pulp G, the re-grinding pulp G is beneficiated to obtain the beneficiation I and the bottom product H, the beneficiation I and the roughing I are mixed and then beneficiated 1 to 2 times to obtain lithium concentrate and the bottom product K, and the beneficiation operation time is 2 to 6 minutes; wherein the bottom product H is returned to the pulp as the middling ore for circulation, the bottom product K is returned to the re-grinding pulp G, and the foam product after the scavenging I is returned to the pulp to be scavenged F; wherein, a beneficiation adjusting agent is added during the beneficiation, preferably a carbonate adjusting agent;

[0040] (3) Within 1 to 2 minutes, the foam floats out for rapid flotation to obtain the foam product roughing I of the easily floatable minerals and the tailings pulp E of the bottom product. The tailings pulp E is then subjected to 1 to 2 minutes of slow fine mud flotation to obtain roughing II and the slurry F to be scavenged. Subsequently, a metal ion activator and a collector are added to the slurry F to be scavenged for 2 to 5 minutes of slurry adjustment and scavenging. The slurry adjustment and scavenging times are at least twice, and the scavenging time is 2 to 6 minutes. Scavenging I and the foam products after scavenging I are obtained in sequence according to the slurry adjustment and scavenging times. The tailings pulp after the last scavenging is the flotation tailings. The roughing I is refined to obtain refined I and bottom product G; then the bottom product G, scavenging I and roughing II are mixed and ground and scrubbed for 1 to 2 minutes to obtain scrubbed slurry H; the scrubbed slurry H is refined to obtain refined II and bottom product K; refined II and refined I are mixed and refined 1 to 2 times to obtain lithium concentrate and bottom product M; the bottom product M is returned to the scrubbing slurry H, the bottom product K is returned to the tailing slurry E, and the foam product after scavenging I is returned to the slurry F to be scavenged; wherein, a refinement adjusting agent is added during the refinement, preferably a carbonation adjusting agent.

[0041] Based on the treated spodumene dry ore, the amount of the beneficiation adjusting agent is 100-1000g / t.

[0042] The technology of the present invention is applicable to the low-temperature, normal-temperature and heated flotation processes of spodumene minerals, and the applicable temperature is 5-60°C.

[0043] The technical solution of the present invention has the following advantages:

[0044] 1. A spodumene ore flotation method provided by the present invention adjusts the surface activity expression of mineral fine mud and weakens the performance of improper adsorption of collector by mineral fine mud by adding a fine mud surface modification masking agent having fine mud electrostatic masking performance and enhancing the expression of negative charge on the surface of fine mud. At the same time, a sorting process is matched to carry out step-by-step recovery and process fine mud regulation according to the difference in the floating rate of mineral particles, so as to achieve the regulation and control of the fine mud mineral trend, avoid the negative influence of mineral fine mud on spodumene flotation, and then improve the process mineral sorting efficiency.

[0045] Specifically, the fine mud minerals express stronger electrical reactivity than the target minerals, and a fine mud surface modification masking agent coupled with enhanced hydroxylation and electrostatic masking is used to selectively change the expression of the charge properties of the fine mud minerals, and supplemented with a highly selective anionic lithium mineral combination collector to achieve highly selective separation of spodumene minerals and gangue minerals. Based on the characteristics of slow floating of fine mud minerals and fast floating of target minerals, a step-rate recovery process is adopted based on the difference in mineral flotation rates, combined with the selectivity of the reagent system, to effectively control the direction of fine mud minerals and improve the efficiency of mineral sorting. Low-cost reagents are used with low consumption, and the sorting process has strong adaptability; lithium is highly selectively floated from all-grade materials, with a high lithium recovery rate, which improves the mineral dissociation efficiency and improves the quality of lithium concentrate.

[0046] Among them, the fine mud surface modification masking agent added in the present invention is mainly used to increase the difference in floatability between mineral fine mud and target mineral, and includes at least three functions: first: it can preferentially and selectively adsorb on the surface of mineral fine mud by electrostatic attraction, neutralize or modify the surface electrical properties of fine mud mineral, and increase the surface charge difference between fine mud mineral and target mineral; second: it uses electrostatic masking to express the charge of fine mud, thereby reducing the improper adsorption of subsequent collectors by fine mud minerals in the system to form floating with foam, and reducing the amount of collector used; third: it can effectively enhance the relative aggregation ability of fine mud minerals, enhance their apparent gravity of sedimentation, and enhance the discharge of mineral fine mud with tailings. That is, the role of the fine mud surface modification masking agent of the present invention in the ore pulp is: to supplement or increase the free OH- concentration, and the free OH- quickly adsorbs and occupies the surface of the dissociated fine mud mineral, so that the negative charge expression of the hydration / hydroxylation of the fine mud mineral surface is stronger; simultaneously, a fine mud mineral surface electrostatic masking agent component with electrostatic masking function and relatively slow diffusion is used. This component adsorbs and covers the hydroxylated mineral fine mud surface based on the action of electrostatic force, thereby weakening the charge expression of the fine mud mineral; at the same time, the remaining OH- that is not competitively adsorbed by the fine mud mineral acts on relatively coarse-grained mineral particles. Due to the difference in the active components of the dissociated surface of different minerals, the Si on the surface of the target mineral is preferentially alkali-dissolved, forming active sites with strong expression of the surface Al site, thereby increasing the difference in floatability between the mineral fine mud and the target mineral.

[0047] On the basis of the application of the fine mud surface modification masking agent, according to the potential trend behavior of the flotation fine mud, a system of collectors that can quickly float out the target mineral is selectively used. The collector does not react or reacts very weakly with the electrostatic masking agent covering the surface of the fine mud mineral, but can quickly capture the surface of the spodumene mineral, so that the surface of the target lithium mineral forms a surface for the collector to selectively adsorb and mineralize. At the same time, the combined collector can quickly form foam after being aerated, so as to achieve the purpose of quickly floating some easily floating lithium-containing minerals. Synchronously based on the differential expression of the floating rate of the target mineral and the fine mud mineral, a process flow with better sorting efficiency is matched, and the role of the coupling agent and the sorting process is coordinated to further strengthen the control of the fine mud trend and improve the mineral sorting efficiency.

[0048] 2. A spodumene ore flotation method of the present invention further provides a separation method, including:

[0049] Rapid flotation is used to first separate out the easy-floating minerals with some target minerals, and then a fine mud surface modification masking agent is added after the easy-floating minerals are floated out. The relatively slow-floating fine mud minerals are controlled in the second half of the flotation process, and the relatively slow-floating minerals / mineral fine mud are modified and adjusted to achieve secondary direction control of the fine mud minerals. In this method, in addition to using a fine mud surface modification masking agent to modify the surface of fine mud minerals before the front-end rapid flotation, a fine mud surface modification masking agent is added after the easy-floating minerals are floated out by rapid flotation, and a fine mud slow flotation method is used to control the relatively slow-floating fine mud minerals in the second half of the flotation process, which can effectively reduce the accumulation of fine mud minerals in the roughing operation and is conducive to the migration of fine mud minerals with scavenging tailings; specifically, the foam product containing more fine mud and relatively slow floating is treated by a selection method, and the foam product after scavenging of the medium ore containing more fine mud after selection and the relatively slow-floating medium ore after slow flotation treatment is returned to the fine mud slow flotation operation process, so as to reduce the adverse effects of fine mud minerals on the rapid flotation roughing operation, and effectively reduce the adverse effects caused by the accumulation and circulation of fine mud in the rapid flotation process;

[0050] Alternatively, a portion of the target minerals can be first floated out quickly, and the relatively slow-floating foam products can be scrubbed / re-dissociated through grinding, so that the direction of fine mud can be regulated by scrubbing the mineral surface reagents. The process effectively reduces the accumulation of slow-floating fine mud minerals in the roughing operation. In this method, in addition to the advantages of using fine mud surface modification masking agents at the front end, its advantages include: first, the relatively slow-floating fine mud minerals can be effectively controlled in the second half of the flotation process, thereby strengthening the control of the direction of fine mud; second, for relatively slow-floating fine mud minerals, the surface of the fine mud minerals can be scrubbed by re-grinding, thereby reducing the reagents adsorbed by the fine mud minerals and facilitating their sedimentation into the tailings; third, the coarse-grained undissociated / difficult-to-dissociate mineral complexes can be re-dissociated to strengthen the flotation recovery of the target minerals; specifically, rapid flotation is used to preferentially and rapidly float out the easy-floating minerals with part of the target minerals, while the relatively slow-floating minerals with more fine mud are removed. After the slow-floating foam product (fine mud slow flotation-roughing) is combined with the scavenging foam product (fine mud slow flotation-first scavenging), the minerals in the foam product are scrubbed by grinding to reduce the adsorption of reagents on the surface of the fine mud. The foam product and the bottom product of the re-grinding pulp obtained after the first concentration are combined with the foam product obtained by rapid flotation for further concentration. The bottom products thrown out of the re-grinding pulp after the first concentration are mostly slow-floating and difficult-to-control fine mud minerals. They are returned to the rapid flotation stage, or returned to the fine mud slow flotation roughing operation, to enhance the migration trend of fine mud minerals to the tailings;

[0051] Alternatively, under the condition of using a fine mud surface modification masking agent, a rapid flotation is used to first separate out the easy-floating minerals with part of the target minerals, and then the easy-floating minerals are subjected to the first concentration, and the bottom product obtained by the concentration is mixed with a relatively slow-floating mineral fine mud foam product and a scavenging foam product with a high fine mud content, and then the grinding, scrubbing and re-dissociation method is adopted to scrub the reagents on the surface of the fine mud minerals and realize the dissociation of the mineral conjoined bodies to obtain the re-grinded scrubbing slurry, and the scrubbing slurry is subjected to the second concentration, and the medium ore with a high fine mud content thrown out by the second concentration is introduced into the fine mud slow floating slurry. In the roughing operation, the fine mud can be efficiently controlled to circulate in the second half of the process, thereby realizing effective control of the fine mud. In this method, in addition to the advantageous effect of the surface modification masking agent of the front-end fine mud, it has the advantage of preferentially floating out easy-to-float lithium-containing minerals. The process can also effectively and simultaneously solve the problem of re-dissociation of fine mud and mineral intergrowths, realize the effective dissociation of mineral-poor / rich intergrowth minerals in one step, coordinate the direction of the medium ore with high fine mud mineral content produced by the selection and scanning, and control the direction of the secondary fine mud produced by the regrinding at the same time, so as to realize the control of the migration direction of the difficult-to-treat mineral fine mud in the system. BRIEF DESCRIPTION OF THE DRAWINGS

[0052] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0053] Figure 1 is a process flow chart of Example 1 of the present invention;

[0054] Figure 2 is a process flow chart of Example 2 of the present invention;

[0055] Figure 3 It is a process flow chart of Example 3 of the present invention. DETAILED DESCRIPTION

[0056] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.

[0057] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.

[0058] Example 1

[0059] A spodumene ore flotation method, such as Figure 1 As shown, including:

[0060] (1) Preparation of crushing and dissociation of ore minerals: crush and grind the material to be processed to -0.074 mm, accounting for 70%, and add 1000g / t of sodium carbonate during the grinding process to obtain grinding slurry A.

[0061] Among them, the ore minerals are the raw ore of complex embedded low-grade spodumene ore collected from Xinjiang. 2 O content is 0.95%, 92% of lithium-containing minerals are spodumene, and the gangue minerals are mainly mixed minerals of quartz, sodium / potassium feldspar, mica, chlorite, calcite, kaolin, etc. Among them, the content of easily crushed and muddy minerals such as mica, chlorite, calcite, kaolin, etc. is relatively high, accounting for 20% of such minerals; when the ore is ground to -0.074mm, accounting for 70%, the monomer dissociation degree of spodumene mineral is 92%, but more fine mud minerals are produced at the same time. In addition, spodumene minerals and gangue minerals have a close symbiotic relationship.

[0062] (2) Electrostatic masking and stirring modification of fine mud minerals: The grinding slurry A is subjected to mechanical stirring slurry modification, and a fine mud surface modification masking agent is added during stirring to electrostatically mask the fine mud minerals and selectively dissolve the surface OH- of the target mineral. The slurry modification time is 15 minutes to obtain a modified slurry B; wherein the fine mud surface modification masking agent is composed of sodium hydroxide and N-hexadecylpyridine-nitrate in a mass ratio of 1:0.2, and the amount of the fine mud surface modification masking agent is 300 g / t.

[0063] (3) Metal ion activation modification adjustment: 100 g / t of magnesium sulfate was added to the modified slurry B to complete the metal ion activation modification and obtain ion-activated slurry C.

[0064] (4) Lithium mineral capture and mineralization slurry adjustment: 1200 g / t of a combined collector is added to the ion-activated pulp C to carry out a mineralization capture reaction of spodumene minerals. The stirring capture and mineralization reaction time is 5 min, and a mineralized pulp D is obtained after stirring; the collector is a combined collector, which is a combination of a fatty acid, a hydroxamic acid and an emulsifier thereof, and the amount of each component is (tall oil + oleic acid + alkyl hydroxamic acid): silicone oil = (400 + 400 + 300) + 100 g / t.

[0065] (5) Lithium mineral fast flotation recovery - fine mud mineral slow flotation controlled separation, the sorting and separation methods are as follows:

[0066] The foam floats out for rapid flotation to obtain the foam product roughing I of the easy-floating mineral within 2 minutes and the tailings pulp E of the bottom product, and then add the fine mud surface modification masking agent to the tailings pulp E, the dosage of the fine mud surface modification masking agent is 50g / t, and after 1min of re-modification, re-competition and re-dispersion, the pulp F to be scavenged is obtained, and then the above-mentioned collector 100g / t is added to carry out slurry adjustment for 3min, after slurry adjustment, the fine mud slowly floats for 2min, and the roughing II and the bottom product F are obtained, and the metal ion activator 50g / t and the collector 100g / t are added to the bottom product F for 3min of slurry adjustment, and then scavenging for 4min, the scavenging times are one time, and the scavenging I and tailings pulp are obtained, and the tailings pulp is the tailings for flotation; in the roughing II, add 500 g / t of sodium carbonate is added for mixing for 2 minutes, and then beneficiation is performed to obtain beneficiation I and bottom product G; beneficiation I is mixed with roughing I, and then 500 g / t of sodium carbonate is added for mixing for 2 minutes, and beneficiation II and bottom product H1 are obtained after 3 minutes of beneficiation. 300 g / t of sodium carbonate is added to be mixed for 2 minutes, and beneficiation III and bottom product H2 are obtained after 3 minutes of beneficiation. Beneficiation III is the final lithium concentrate; bottom product G and scavenging I are returned to tailings slurry E in the form of middlings for circulation, bottom product H1 is returned to the slurry as middlings for circulation, and bottom product H2 is returned to the beneficiation step as middlings. In this embodiment, bottom product H2 is mixed with beneficiation I and roughing I for subsequent beneficiation.

[0067] In the lithium concentrate obtained by the above method in this embodiment, Li 2 O content is 5.45%, Li 2 The O recovery rate was 83.2%.

[0068] Example 2

[0069] A spodumene ore flotation method, such as Figure 2 As shown, including:

[0070] (1) Preparation of crushing and dissociation of ore minerals: crush and grind the material to be processed to -0.074 mm, accounting for 70%, and add 1000g / t of sodium carbonate during the grinding process to obtain grinding slurry A.

[0071] Among them, the ore minerals are complex embedded low-grade spodumene mines collected from Xinjiang. 2O content is 0.95%, 92% of lithium-containing minerals are spodumene, and the gangue minerals are mainly mixed minerals of quartz, sodium / potassium feldspar, mica, chlorite, calcite, kaolin, etc. Among them, the content of easily crushed and muddy minerals such as mica, chlorite, calcite, kaolin, etc. is relatively high, accounting for 20% of such minerals; when the ore is ground to -0.074mm, accounting for 70%, the monomer dissociation degree of spodumene mineral is 92%, but more fine mud minerals are produced at the same time. In addition, spodumene minerals and gangue minerals have a close symbiotic relationship.

[0072] (2) Electrostatic masking and stirring modification of fine mud minerals: The grinding slurry A is subjected to mechanical stirring slurry modification, and a fine mud surface modification masking agent is added during stirring to electrostatically mask the fine mud minerals and selectively dissolve the surface OH- of the target mineral. The slurry modification time is 15 minutes to obtain a modified slurry B; wherein the fine mud surface modification masking agent is composed of sodium hydroxide and N-hexadecylpyridine-nitrate in a mass ratio of 1:0.2, and the amount of the fine mud surface modification masking agent is 300 g / t.

[0073] (3) Metal ion activation modification adjustment: 100 g / t of magnesium sulfate was added to the modified slurry B to complete the metal ion activation modification and obtain ion-activated slurry C.

[0074] (4) Lithium mineral capture and mineralization slurry adjustment: 1200 g / t of a combined collector is added to the ion-activated pulp C to carry out a mineralization capture reaction of spodumene minerals. The stirring capture and mineralization reaction time is 5 min, and a mineralized pulp D is obtained after stirring; the collector is a combined collector, which is a combination of a fatty acid, a hydroxamic acid and an emulsifier thereof, and the amount of each component is (tall oil + oleic acid + alkyl hydroxamic acid): silicone oil = (400 + 400 + 300) + 100 g / t.

[0075] (5) Lithium mineral fast flotation recovery - fine mud mineral slow flotation controlled separation, the sorting and separation methods are as follows:

[0076] The foam floats out for rapid flotation to obtain the foam product roughing I of the easy-floating mineral within 1.5 minutes and the tailings pulp E of the bottom product. The tailings pulp E is used to continue the fine mud slow flotation for 2 minutes to obtain roughing II and the pulp F to be scavenged. Subsequently, 30g / t of metal ion activator is added to the pulp F to be scavenged for 3 minutes of slurry adjustment, and then 100g / t of collector is added for 3 minutes of slurry adjustment. After slurry adjustment, scavenging is performed twice, and the scavenging time is 3 minutes. Scavenging I and scavenging II are obtained in sequence according to the number of slurry adjustment and scavenging. The tailings pulp after the second scavenging is the flotation tailings; the roughing II and scavenging I are combined and ground and scrubbed for 1 minute to obtain the regrinding pulp G. The regrinding -0.074mm accounts for 90.1% of the pulp G. 500g / t of sodium carbonate is added to the reground pulp G for 2 minutes of mixing, and the selected I and the bottom product H are obtained after 3 minutes of concentration; the selected I and the rougher selected I are mixed, and then 500g / t of sodium carbonate is added to mix for 2 minutes, and the selected II and the bottom product K1 are obtained after 3 minutes of concentration. The selected II is added with 300g / t of sodium carbonate for 2 minutes of mixing, and the selected III and the bottom product K2 are obtained after 3 minutes of concentration; among which, the bottom product H is returned to the pulp as the middling ore for circulation, the bottom product K1 is returned to the reground pulp G, the bottom product K2 is returned to be mixed with the selected I and the rougher selected I, and the scavenged II is returned to the pulp F to be scavenged.

[0077] In the lithium concentrate obtained by the above method in this embodiment, Li 2 O content is 5.76%, Li 2 The O recovery rate was 84.3%.

[0078] Example 3

[0079] A spodumene ore flotation method, such as Figure 3 As shown, including:

[0080] (1) Preparation of crushing and dissociation of ore minerals: crush and grind the material to be processed to -0.074 mm, accounting for 70%, and add 1000g / t of sodium carbonate during the grinding process to obtain grinding slurry A.

[0081] Among them, the ore minerals are complex embedded low-grade spodumene mines collected from Xinjiang. 2 O content is 0.95%, 92% of lithium-containing minerals are spodumene, and the gangue minerals are mainly mixed minerals of quartz, sodium / potassium feldspar, mica, chlorite, calcite, kaolin, etc. Among them, the content of easily crushed and muddy minerals such as mica, chlorite, calcite, kaolin, etc. is relatively high, accounting for 20% of such minerals; when the ore is ground to -0.074mm, accounting for 70%, the monomer dissociation degree of spodumene mineral is 92%, but more fine mud minerals are produced at the same time. In addition, spodumene minerals and gangue minerals have a close symbiotic relationship.

[0082] (2) Electrostatic masking and stirring modification of fine mud minerals: The grinding slurry A is subjected to mechanical stirring slurry modification, and a fine mud surface modification masking agent is added during stirring to electrostatically mask the fine mud minerals and selectively dissolve the surface OH- of the target mineral. The slurry modification time is 15 minutes to obtain a modified slurry B; wherein the fine mud surface modification masking agent is composed of sodium hydroxide and N-hexadecylpyridine-nitrate in a mass ratio of 1:0.2, and the amount of the fine mud surface modification masking agent is 300 g / t.

[0083] (3) Metal ion activation modification adjustment: 100 g / t of magnesium sulfate was added to the modified slurry B to complete the metal ion activation modification and obtain ion-activated slurry C.

[0084] (4) Lithium mineral capture and mineralization slurry adjustment: 1200 g / t of a combined collector is added to the ion-activated pulp C to carry out a mineralization capture reaction of spodumene minerals. The stirring capture and mineralization reaction time is 5 min, and a mineralized pulp D is obtained after stirring; the collector is a combined collector, which is a combination of a fatty acid, a hydroxamic acid and an emulsifier thereof, and the amount of each component is (tall oil + oleic acid + alkyl hydroxamic acid): silicone oil = (400 + 400 + 300) + 100 g / t.

[0085] (5) Lithium mineral fast flotation recovery - fine mud mineral slow flotation controlled separation, the sorting and separation methods are as follows:

[0086] The foam floats out for rapid flotation to obtain the foam product roughing I of the easy-to-float mineral within 2 minutes and the tailings pulp E of the bottom product. The tailings pulp E is then subjected to 2 minutes of slow fine mud flotation to obtain roughing II and the pulp F to be scavenged. Subsequently, 30 g / t of metal ion activator is added to the pulp F to be scavenged for 2 minutes of slurry adjustment, and then 100 g / t of collector is added for 2 minutes of slurry adjustment. After slurry adjustment, scavenging is performed. The slurry adjustment and scavenging times are twice, the first scavenging time is 4 minutes, and the second scavenging time is 3 minutes. Scavenging I and scavenging II are obtained in sequence according to the slurry adjustment and scavenging times. The tailings pulp after the second scavenging is the flotation tailings; 500 g / t of sodium carbonate is added to the selection I for 2 minutes. The mixture is mixed and concentrated for 3 minutes to obtain concentrated I and bottom product G; then the bottom product G, scavenging I and roughing II are mixed and ground and scrubbed for 1.5 minutes to obtain scrubbed slurry H, in which -0.074 mm accounts for 90%, 500 g / t of sodium carbonate is added to the scrubbing slurry H for 2 minutes, and concentrated for 3 minutes to obtain concentrated II and bottom product K. After mixing concentrated II and concentrated I, 300 g / t of sodium carbonate is added and mixed for 2 minutes, and concentrated for 3 minutes to obtain concentrated III and bottom product M, and concentrated III is lithium concentrate; bottom product M is returned to the scrubbing slurry H, bottom product K is returned to the tailing slurry E, and scavenging II is returned to the slurry F to be scavenged.

[0087] In the lithium concentrate obtained by the above method in this embodiment, Li 2 O content is 5.71%, Li 2 The O recovery rate was 84.8%.

[0088] Example 4

[0089] A spodumene ore flotation method is different from Example 1 in that the parameter conditions in steps (1)-(4) are different, and the other parameters are exactly the same as Example 1. Steps (1)-(4) specifically include:

[0090] (1) Preparation of crushing and dissociation of ore minerals: crush and grind the material to be processed to -0.074 mm, accounting for 95%, and add 1500g / t of sodium carbonate during the grinding process to obtain grinding slurry A.

[0091] (2) Electrostatic masking and stirring modification of fine mud minerals: The grinding slurry A is subjected to mechanical stirring slurry modification, and a fine mud surface modification masking agent is added during stirring to electrostatically mask the fine mud minerals and selectively dissolve the surface OH- of the target minerals. The slurry modification time is 15 min to obtain a modified slurry B; wherein the fine mud surface modification masking agent is composed of sodium hydroxide and N-hexadecylpyridine-nitrate in a mass ratio of 1:0.1, and the amount of the fine mud surface modification masking agent is 110 g / t.

[0092] (3) Metal ion activation modification adjustment: 1000 g / t of magnesium sulfate was added to the modified slurry B to complete the metal ion activation modification and obtain ion-activated slurry C.

[0093] (4) Lithium mineral capture and mineralization slurry adjustment: 2000 g / t of combined collector is added to the ion-activated pulp C to carry out the mineralization capture reaction of spodumene mineral. The stirring capture mineralization reaction time is 2 min, and the mineralized pulp D is obtained after stirring; the collector is a combined collector, which is a combination of fatty acid, hydroxamic acid and its emulsifier, and the amount of each component is (tall oil + oleic acid + alkyl hydroxamic acid): silicone oil = (400 + 400 + 300) + 20 g / t.

[0094] In the lithium concentrate obtained by the above method in this embodiment, Li 2 O content is 5.12%, Li 2 The O recovery rate was 86.3%.

[0095] Example 5

[0096] A spodumene ore flotation method is different from Example 1 in that the parameter conditions in steps (1)-(4) are different, and the other parameters are exactly the same as Example 1. Steps (1)-(4) specifically include:

[0097] (1) Preparation of crushing and dissociation of ore minerals: crush and grind the material to be processed to -0.074 mm, accounting for 60%, and add 3000g / t of sodium carbonate during the grinding process to obtain grinding slurry A.

[0098] (2) Electrostatic masking and stirring modification of fine mud minerals: The grinding slurry A is subjected to mechanical stirring slurry modification, and a fine mud surface modification masking agent is added during stirring to electrostatically mask the fine mud minerals and selectively dissolve the surface OH- of the target mineral. The slurry modification time is 40 minutes to obtain a modified slurry B; wherein the fine mud surface modification masking agent is composed of sodium hydroxide and N-hexadecylpyridine-nitrate in a mass ratio of 1:0.25, and the amount of the fine mud surface modification masking agent is 2500g / t.

[0099] (3) Metal ion activation modification adjustment: 100 g / t of magnesium sulfate was added to the modified slurry B to complete the metal ion activation modification and obtain ion-activated slurry C.

[0100] (4) Lithium mineral capture and mineralization slurry adjustment: 100 g / t of a combined collector is added to the ion-activated pulp C to carry out a mineralization capture reaction of spodumene minerals. The stirring capture and mineralization reaction time is 10 min, and a mineralized pulp D is obtained after stirring; the collector is a combined collector, which is a combination of a fatty acid, a hydroxamic acid and an emulsifier thereof, and the amount of each component is (tall oil + oleic acid + alkyl hydroxamic acid): silicone oil = (400 + 400 + 300) + 80 g / t.

[0101] In the lithium concentrate obtained by the above method in this embodiment, Li 2 O content is 5.67%, Li 2 The O recovery rate was 82.3%.

[0102] Example 6

[0103] A spodumene ore flotation method is different from Example 1 in that the parameter conditions in steps (1)-(4) are different, and the other parameters are exactly the same as Example 1. Steps (1)-(4) specifically include:

[0104] (1) Preparation of crushing and dissociation of ore minerals: crush and grind the material to be processed to -0.074 mm, accounting for 70%, and add 1000g / t potassium carbonate during the grinding process to obtain grinding slurry A.

[0105] (2) Electrostatic masking and stirring modification of fine mud minerals: The grinding slurry A is subjected to mechanical stirring slurry modification, and a fine mud surface modification masking agent is added during stirring to electrostatically mask the fine mud minerals and selectively dissolve the OH- on the surface of the target mineral. The slurry modification time is 15 minutes to obtain a modified slurry B; wherein the fine mud surface modification masking agent is composed of potassium hydroxide and aminoalkyl polyethylene glycol ether in a mass ratio of 1:0.2, and the amount of the fine mud surface modification masking agent is 300 g / t.

[0106] (3) Metal ion activation modification adjustment: 100 g / t of calcium nitrate was added to the modified slurry B to complete the metal ion activation modification and obtain ion-activated slurry C.

[0107] (4) Lithium mineral capture and mineralization slurry adjustment: 1200 g / t of a combined collector is added to the ion-activated pulp C to carry out a mineralization capture reaction of the spodumene mineral. The stirring capture and mineralization reaction time is 5 minutes, and a mineralized pulp D is obtained after stirring; the collector is a combined collector, which is a combination of fatty acid, hydroxamic acid and its emulsifier, and the amount of each component is (sodium dodecyl sulfate+cyclohexane acid soap+benzyl hydroxamic acid): kerosene=(400+400+300)+100 g / t.

[0108] In the lithium concentrate obtained by the above method in this embodiment, Li 2 O content is 5.55%, Li 2 The O recovery rate was 83.8%.

[0109] Example 7

[0110] A spodumene ore flotation method, which is different from Example 1 in that the parameter conditions in step (5) are different, and the other conditions are exactly the same as Example 1. Step (5) specifically comprises:

[0111] The foam floats out for rapid flotation to obtain the foam product roughing I of the easy-floating mineral within 1 minute and the tailings pulp E of the bottom product, and then the fine mud surface modification masking agent is added to the tailings pulp E, the dosage of the fine mud surface modification masking agent is 60g / t, and after 0.5min of re-modification, re-competition and re-dispersion, the pulp F to be scavenged is obtained, and then the above-mentioned collector 240g / t is added for 2min of slurry adjustment, and the fine mud is slowly floated for 6min after slurry adjustment to obtain roughing II and the bottom product F, and the metal ion activator 20g / t and the collector 240g / t are added to the bottom product F for 5min of slurry adjustment, and then scavenged for 2min, the scavenging times are one time, and scavenging I and tailings pulp are obtained, and the tailings pulp is the tailings for flotation; in the roughing II 100 g / t of sodium carbonate was added for mixing for 2 minutes, and then the process was concentrated to obtain concentrated I and bottom product G; concentrated I was mixed with roughing I, and then 100 g / t of sodium carbonate was added for mixing for 5 minutes, and concentrated for 2 minutes to obtain concentrated II and bottom product H1, 100 g / t of sodium carbonate was added to concentrated II for mixing for 5 minutes, and concentrated for 2 minutes to obtain concentrated III and bottom product H2, and concentrated III was finally obtained as lithium concentrate; bottom product G and scavenging I were returned to tailings slurry E in the form of middlings for circulation, bottom product H1 was returned to the slurry as middlings for circulation, and bottom product H2 was returned to the concentration step as middlings. In this embodiment, bottom product H2 was mixed with concentrated I and roughing I for subsequent concentration.

[0112] In the lithium concentrate obtained by the above method in this embodiment, Li 2 The O content is 5.66%, Li 2 The O recovery rate was 84.3%.

[0113] Example 8

[0114] A spodumene ore flotation method, which is different from Example 1 in that the parameter conditions in step (5) are different, and the other conditions are exactly the same as Example 1. Step (5) specifically comprises:

[0115] The foam floats out for rapid flotation to obtain the foam product roughing I of the easy-floating mineral within 2 minutes and the tailings pulp E of the bottom product, and then add the fine mud surface modification masking agent to the tailings pulp E, the dosage of the fine mud surface modification masking agent is 15g / t, and after 2 minutes of re-modification, re-competition and re-dispersion, the pulp F to be scavenged is obtained, and then the above-mentioned collector 60g / t is added to carry out slurry adjustment for 5 minutes. After slurry adjustment, the fine mud slowly floats for 4 minutes to obtain roughing II and the bottom product F, and the metal ion activator 30g / t and the collector 60g / t are added to the bottom product F for 2 minutes of slurry adjustment, and then scavenging for 6 minutes, the scavenging times are one time, and scavenging I and tailings pulp are obtained. The tailings pulp is the tailings for flotation; carbonate is added to the roughing II The selected product I and the roughing selected product I are mixed with 1000g / t of sodium carbonate for 6 minutes, and then the selected product I and the bottom product G are obtained by concentration; the selected product I and the roughing selected product I are mixed, and then 1000g / t of sodium carbonate is added for mixing for 2 minutes, and the selected product II and the bottom product H1 are obtained by concentration for 6 minutes. 1000g / t of sodium carbonate is added to the selected product II for mixing for 2 minutes, and the selected product III and the bottom product H2 are obtained by concentration for 6 minutes. The selected product III is the lithium concentrate finally obtained; the bottom product G and the scavenging selected product I are returned to the tailings slurry E in the form of middlings for circulation, the bottom product H1 is returned to the slurry as the middlings for circulation, and the bottom product H2 is returned to the concentration step as the middlings. In this embodiment, the bottom product H2 is mixed with the selected product I and the roughing selected product I for subsequent concentration.

[0116] In the lithium concentrate obtained by the above method in this embodiment, Li 2 O content is 5.42%, Li 2 The O recovery rate was 83.6%.

[0117] Example 9

[0118] A spodumene ore flotation method, which is different from Example 2 in that the parameter conditions in step (5) are different, and the other conditions are exactly the same as Example 2. Step (5) specifically comprises:

[0119] The foam floats out for rapid flotation to obtain the foam product roughing I of the easy-floating mineral within 1 minute and the tailings pulp E of the bottom product. The tailings pulp E is used to continue the fine mud slow flotation for 1.5 minutes to obtain roughing II and the pulp F to be scavenged. Subsequently, 20g / t of metal ion activator is added to the pulp F to be scavenged for 2 minutes of slurry adjustment, and then 240g / t of collector is added for 2 minutes of slurry adjustment. After slurry adjustment, scavenging is performed twice, and the scavenging time is 6 minutes. Scavenging I and scavenging II are obtained in sequence according to the number of slurry adjustment and scavenging. The tailings pulp after the second scavenging is the flotation tailings; the roughing II and scavenging I are combined and ground and scrubbed for 1 minute to obtain the regrinding pulp G. The regrinding -0.074mm accounts for more than 90% of the pulp G. 100g / t of sodium carbonate is added to the reground pulp G for mixing for 3 minutes, and the selected product I and the bottom product H are obtained after 2 minutes of concentration; the selected product I and the roughing selected product I are mixed, and then 100g / t of sodium carbonate is added to the mixed product I for 3 minutes, and the selected product II and the bottom product K1 are obtained after 2 minutes of concentration. The selected product II is added with 100g / t of sodium carbonate for mixing for 3 minutes, and the selected product III and the bottom product K2 are obtained after 2 minutes of concentration; among which, the bottom product H is returned to the pulp as the middling ore for circulation, the bottom product K1 is returned to the reground pulp G, the bottom product K2 is returned to be mixed with the selected product I and the roughing selected product I, and the scavenged selected product II is returned to the pulp F to be scavenged.

[0120] In the lithium concentrate obtained by the above method in this embodiment, Li 2 O content is 5.72%, Li 2 The O recovery rate was 84.3%.

[0121] Example 10

[0122] A spodumene ore flotation method, which is different from Example 2 in that the parameter conditions in step (5) are different, and the other conditions are exactly the same as Example 2. Step (5) specifically comprises:

[0123] The foam floats out for rapid flotation to obtain the foam product roughing I of the easy-to-float mineral within 2 minutes and the tailings pulp E of the bottom product. The tailings pulp E is used to continue the fine mud slow flotation for 1 minute to obtain roughing II and the scavenging pulp F to be scavenged. Subsequently, 50g / t of metal ion activator is added to the slurry F to be scavenged for 5 minutes, and then 60g / t of collector is added for 5 minutes of slurry mixing. After slurry mixing, scavenging is performed twice, and the scavenging time is 2 minutes. Scavenging I and scavenging II are obtained in sequence according to the number of slurry mixing and scavenging. The tailings pulp after the second scavenging is the flotation tailings; the roughing II and scavenging I are combined and ground and scrubbed for 1 minute to obtain the regrinding pulp G. The regrinding pulp G -0.074mm accounts for more than 90%, 1000g / t of sodium carbonate is added to the regrind pulp G for 5 minutes of mixing, and after 6 minutes of concentration, concentrated I and bottom product H are obtained; concentrated I and roughing I are mixed, and then 1000g / t of sodium carbonate is added to mix for 5 minutes, and concentrated for 6 minutes to obtain concentrated II and bottom product K1, and concentrated II is added with 1000g / t of sodium carbonate for 5 minutes, and concentrated for 6 minutes to obtain concentrated III and bottom product K2; among which, bottom product H is returned to the pulp as middling ore for circulation, bottom product K1 is returned to the regrind pulp G, bottom product K2 is returned to be mixed with concentrated I and roughing I, and scavenged II is returned to the pulp F to be scavenged.

[0124] In the lithium concentrate obtained by the above method in this embodiment, Li 2 The O content is 5.84%, Li 2 The O recovery rate was 83.1%.

[0125] Embodiment 11

[0126] A spodumene ore flotation method, which is different from Example 3 in that the parameter conditions in step (5) are different, and the other conditions are exactly the same as Example 3. Step (5) specifically comprises:

[0127] The foam floats out for rapid flotation to obtain the foam product roughing I of the easy-to-float mineral within 1 minute and the tailings pulp E of the bottom product. The tailings pulp E is then subjected to 1.5 minutes of slow fine mud flotation to obtain roughing II and the pulp F to be scavenged. Subsequently, 20 g / t of metal ion activator is added to the pulp F to be scavenged for 2 minutes of slurry adjustment, and then 240 g / t of collector is added for 3 minutes of slurry adjustment. After slurry adjustment, scavenging is performed twice, the first scavenging time is 6 minutes, and the second scavenging time is 6 minutes. Scavenging I and scavenging II are obtained in sequence according to the number of slurry adjustment and scavenging. The tailings pulp after the second scavenging is the flotation tailings; 100 g / t of sodium carbonate is added to the roughing I for 3 minutes. n, and after 6 minutes of concentration, concentrated I and bottom product G are obtained; then the bottom product G, scavenging I and roughing II are mixed and ground and scrubbed for 2 minutes to obtain scrubbed slurry H, in which -0.074 mm accounts for more than 90%, 100 g / t of sodium carbonate is added to the scrubbing slurry H for 6 minutes of mixing, and concentrated II and bottom product K are obtained after 6 minutes of concentration, concentrated II and concentrated I are mixed and then 100 g / t of sodium carbonate is added for 5 minutes of mixing, and concentrated III and bottom product M are obtained after 2 minutes of concentration, and concentrated III is lithium concentrate; bottom product M is returned to the scrubbing slurry H, bottom product K is returned to the tailing slurry E, and scavenging II is returned to the slurry F to be scavenged.

[0128] In the lithium concentrate obtained by the above method in this embodiment, Li 2 O content is 5.68%, Li 2 The O recovery rate was 84.6%.

[0129] Example 12

[0130] A spodumene ore flotation method, which is different from Example 3 in that the parameter conditions in step (5) are different, and the other conditions are exactly the same as Example 3. Step (5) specifically comprises:

[0131] The foam floats out for rapid flotation to obtain the foam product roughing I of the easy-floating mineral within 1.5 minutes and the tailings pulp E of the bottom product. The tailings pulp E is then subjected to 1 minute of fine mud slow floating to obtain roughing II and the pulp F to be scavenged. Subsequently, 50 g / t of metal ion activator is added to the pulp F to be scavenged for 2 minutes of slurry adjustment, and then 60 g / t of collector is added for 5 minutes of slurry adjustment. After slurry adjustment, scavenging is performed twice, the first scavenging time is 2 minutes, and the second scavenging time is 2 minutes. Scavenging I and scavenging II are obtained in sequence according to the number of slurry adjustment and scavenging. The tailings pulp after the second scavenging is the flotation tailings; 1000 g / t of sodium carbonate is added to the roughing I for 5 minutes. The mixture is mixed and concentrated for 2 minutes to obtain concentrated I and bottom product G; then the bottom product G, scavenging I and roughing II are mixed and ground and scrubbed for 2 minutes to obtain scrubbed slurry H, in which -0.074 mm accounts for more than 90%. 1000 g / t of sodium carbonate is added to the scrubbing slurry H for 2 minutes of mixing, and concentrated for 2 minutes to obtain concentrated II and bottom product K. After mixing concentrated II and concentrated I, 1000 g / t of sodium carbonate is added and mixed for 3 minutes, and concentrated for 6 minutes to obtain concentrated III and bottom product M, and concentrated III is lithium concentrate; bottom product M is returned to the scrubbing slurry H, bottom product K is returned to the tailing slurry E, and scavenging II is returned to the slurry F to be scavenged.

[0132] In the lithium concentrate obtained by the above method in this embodiment, Li 2 O content is 5.83%, Li 2 The O recovery rate was 82.3%.

[0133] Comparative Example 1

[0134] A spodumene ore flotation method adopts a conventional desludging-flotation process to flotate the ore mineral in Example 1. Specifically, when desludging with a particle size of 15 μm by a hydrocyclone, 12% to 15% of fine mud products are easily removed. On the one hand, 10% to 12% of Li is lost by removing fine mud. 2 O, flotation index is highly dependent on the amount of desludging, and the stability of the separation process is also highly dependent on the desludging process. 2 The recovery rate of O was 77.3%, and the recovery rate of Li 2 The O content is 5.03%.

[0135] Comparative Example 2

[0136] A spodumene ore flotation method adopts a full-size flotation process to flot the ore mineral in Example 1. Specifically, the same processing method as Example 1 is adopted, except that step (2) is omitted, and the process of step (5) is as follows:

[0137] The foam floats out for rapid flotation to obtain the foam product roughing I of the easy-to-float minerals within 2 minutes and the tailings pulp E of the bottom product. The tailings pulp E is then subjected to 2 minutes of fine mud slow flotation to obtain roughing II and the pulp F to be scavenged. Subsequently, 30 g / t of metal ion activator is added to the pulp F to be scavenged for 2 minutes of slurry adjustment, and then 100 g / t of collector is added for 2 minutes of slurry adjustment. After slurry adjustment, scavenging is performed. The slurry adjustment and scavenging times are twice, the first scavenging time is 4 minutes, and the second scavenging time is 3 minutes. Scavenging I and scavenging II are obtained in sequence according to the slurry adjustment and scavenging times. The tailings pulp after the second scavenging is the flotation tailings. 500 g / t of sodium carbonate is added to I and mixed for 2 minutes, and concentrated for 3 minutes to obtain concentrated I and bottom product G; then the bottom product G, scavenging I and roughing II are mixed to obtain slurry H, and 500 g / t of sodium carbonate is added to mix for 2 minutes, and concentrated for 3 minutes to obtain concentrated II and bottom product K. After mixing concentrated II and concentrated I, 300 g / t of sodium carbonate is added to mix for 2 minutes, and concentrated for 3 minutes to obtain concentrated III and bottom product M, and concentrated III is lithium concentrate; bottom product M is returned to the scrubbing slurry H, bottom product K is returned to the tailing slurry E, and scavenging II is returned to the slurry F to be scavenged.

[0138] Obtaining Li in lithium concentrate under optimal conditions 2 The recovery rate of O was 76.9%, and the recovery rate of Li 2 The O content is 5.12%.

[0139] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.

Claims

1. A spodumene ore flotation method, comprising the steps of crushing the spodumene ore to obtain slurry, adding a regulator, a metal ion activator, and a collector to the slurry, stirring the spodumene ore, aerating the slurry, and performing separation to obtain spodumene concentrate and tailings products; characterized in that: The process of adding a fine mud surface modification masking agent between the steps of adding the adjusting agent and the metal ion activator includes an OH-surface modification agent component having the performance of enhancing the negative charge expression of the fine mud surface and a fine mud mineral surface electrostatic masking agent component having electrostatic masking performance; The collector is compounded by multiple types of anionic active collecting components and oil-water emulsifying components; The separation is carried out by step recovery and regulation of process fine mud according to the difference in the floating speed of mineral particles.

2. The method according to claim 1, characterized in that The OH-surface modifier component includes one or more of sodium hydroxide, potassium hydroxide, ammonia, methylamine, and dimethylamine; And / or, the electrostatic masking agent component on the surface of the fine mud mineral is a cationic electrostatic masking agent and / or an amphoteric electrostatic masking agent; And / or, the ratio of the OH-surface modification adjusting agent component to the fine mud mineral surface electrostatic masking agent component is 1:(0.1-0.25).

3. The method according to claim 2, characterized in that The electrostatic masking agent component on the surface of fine mud minerals includes one or more of N-butylpyridinium nitrate, N-hexadecylpyridinium-nitrate, aminoalkyl polyethylene glycol ether, 4-methyl-2-(methylimino)-1-imidazolineamine, 2-methoxyimidazoline, 1-(benzyl)imidazoline-2-one, 1-methyl-2-benzimidazolinone, N,N-dimethyl-β-hydroxyethyl octadecanoylamide-γ-propyl quaternary ammonium nitrate, poly-2-methacryloyloxyethyl trimethylammonium chloride, and polyvinyl benzyl trimethyl quaternary ammonium salt; And / or, based on the treated spodumene ore dry ore, the addition amount of the OH-surface modifier component is 100-2000 g / t; And / or, based on the treated dry spodumene ore, the added amount of the electrostatic masking agent component on the surface of the fine mud mineral is 10-500 g / t.

4. The method according to any one of claims 1 to 3, characterized in that: In the step of crushing and grinding the spodumene ore to obtain ore pulp, the fineness of the ore pulp is -0.074 mm, accounting for 60% to 95%.

5. The method according to any one of claims 1 to 3, characterized in that: The adjusting agent is used to provide inorganic CO3 2- The carbonation adjusting agent is preferably one or more of sodium carbonate, ammonium carbonate, potassium carbonate, sodium bicarbonate, and potassium bicarbonate; And / or, based on the treated dry spodumene ore, the added amount of the adjusting agent is 400-8000 g / t.

6. The method according to any one of claims 1 to 3, characterized in that: The metal ion activator is a metal ion activator having a metal ion radius close to that of the Al / Li ion, preferably a metal ion activator of calcium or magnesium, more preferably one or more of calcium sulfate, calcium nitrate, calcium chloride, magnesium sulfate, magnesium nitrate, and magnesium chloride; And / or, based on the treated dry spodumene ore, the added amount of the metal ion activator is 50-1000 g / t.

7. The method according to any one of claims 1 to 3, characterized in that: The multiple categories of anion active collecting components include a combination of at least two categories of fatty acids and salts, sulfonates, sulfates, phosphonates, and hydroxamic acid collectors; The oil-water emulsified component includes one or more of neutral oils, polyether esters, polyether silicones, and polyether amines; And / or, based on the treated dry spodumene ore, the added amount of the collector is 100 to 4000 g / t.

8. The method according to claim 7, characterized in that The fatty acids and their salts include one or more of oleic acid / sodium oleate, stearic acid / sodium stearate, palmitic acid / sodium palmitate, lauric acid / sodium laurate, hexadecanoic acid / sodium hexadecanoate, and a fatty acid mixture; preferably, the fatty acid mixture includes one or more of oxidized paraffin soap, tall oil, cyclopentane acid soap, and complex fatty acid sodium; And / or, the sulfonate is one or more of sodium dodecylbenzene sulfonate, sodium dodecyl sulfonate, sodium petroleum sulfonate, and sodium complex fatty acid sulfonate; And / or, the sulfate is one or more of sodium dodecyl sulfate, sodium tetradecyl sulfate, sodium hexadecyl sulfate; And / or, the hydroxamic acid is one or more of benzyl hydroxamic acid and alkyl hydroxamic acid; and / or, the oil-water emulsified component includes one of kerosene, diesel, silicone oil, polyoxyethylene ether, polyether alcohol, polyether amine, and trihydroxypropane polypropylene glycol ether; And / or, the compounding ratio of the multiple types of anionic active collecting components to the oil-water emulsification components is 1:(0.02-0.1).

9. The method according to claim 1, characterized in that: The sorting method includes: Rapid flotation is used to first separate the easily floatable minerals with some target minerals, and then a fine mud surface modification masking agent is added after the easily floatable minerals are floated out, so that the relatively slow-floating fine mud minerals are controlled in the second half of the flotation process, and the relatively slow-floating minerals / mineral fine mud are modified and adjusted to achieve secondary direction control of fine mud minerals; Or, use rapid flotation to first sort out the easily floatable minerals with some target minerals, and then dissociate the relatively slow-floating foam products by grinding and scrubbing, and then adjust the direction of fine mud by scrubbing the surface of the minerals; Alternatively, rapid flotation is used to first separate out the easily floating minerals containing part of the target minerals, and the easily floating minerals are selected for the first time. The bottom product obtained by selection, the foam product of the bottom product of the rapid flotation and the scavenging foam product with a high fine mud content of the bottom product of the fine mud slow flotation are mixed, and then the scrubbing slurry is obtained by grinding and scrubbing and then dissociating. The medium ore with a high fine mud content that is selected and thrown out by the scrubbing slurry is introduced into the roughing bottom product of the fine mud slow flotation.

10. The method according to claim 9, characterized in that The sorting process is any one of the following (1)-(3); (1) The foam is floated out for rapid flotation to obtain a foam product roughing I of the easily floatable mineral and a bottom product tailing pulp E, and then a fine mud surface modification masking agent is added to the tailing pulp E, and the pulp F to be scavenged is obtained after re-modification, competition and re-dispersion, and then a metal ion activator + collector or collector is added to adjust the pulp and perform fine mud slow flotation to obtain a roughing II and a bottom product F, and a metal ion activator and a collector are added to the bottom product F for scavenging, and the scavenging number is at least one, and the number of scavenging times is repeated according to the number of scavenging times. The froth products of scavenging I and subsequent froth products are obtained in sequence, and the tailings pulp after the last scavenging is the tailings of flotation; after the roughing II is cleaned once, the concentrating I and the bottom product G are obtained; the concentrating I and the roughing I are mixed, and then separated by concentrating to finally obtain lithium concentrate and the bottom product H; the bottom product G and the froth products of scavenging I and subsequent froth products are returned to the tailings pulp E in the form of middlings for circulation, and the bottom product H is returned to the pulp as the middlings for circulation; wherein, a concentrating adjusting agent is added during the concentrating, preferably a carbonation adjusting agent; (2) The foam is floated out for rapid flotation to obtain a foam product roughing I of easily floatable minerals and a tailing pulp E of a bottom product. The tailing pulp E is then subjected to slow flotation of fine mud to obtain a roughing II and a scavenged pulp F. Subsequently, a metal ion activator and a collector are added to the scavenged pulp F for slurry adjustment and scavenging. The slurry adjustment and scavenging times are at least two. Scavenging I and foam products after scavenging I are obtained in sequence according to the slurry adjustment and scavenging times. The tailing pulp after the last scavenging is the tailings for flotation. The roughing II and scavenging I are combined and then ground and scrubbed to obtain a regrinding pulp G. The regrinding pulp G is subjected to concentration to obtain a concentration I and a bottom product H. The concentration I and the roughing I are mixed and then concentrated to obtain a lithium concentrate and a bottom product K. The bottom product H is returned to the pulp as a middling ore for circulation, the bottom product K is returned to the regrinding pulp G, and the foam product after scavenging I is returned to the slurry F for scavenging. A concentration adjusting agent is added during the concentration, preferably a carbonate adjusting agent. (3) The foam is floated out for rapid flotation to obtain a foam product roughing I of easily floatable minerals and a bottom product tailings pulp E. The tailings pulp E is then subjected to slow fine mud flotation to obtain a roughing II and a scavenged pulp F. Subsequently, a metal ion activator and a collector are added to the scavenged pulp F for slurry adjustment and scavenging. The slurry adjustment and scavenging times are at least two times. Scavenging I and foam products after scavenging I are obtained in sequence according to the slurry adjustment and scavenging times. The tailings pulp after the last scavenging is the flotation tailings. The roughing I is finely concentrated to obtain finely concentrated I and a bottom product G. Subsequently, the bottom product G, scavenging I and roughing II are mixed and then ground and scrubbed to obtain a scrubbed pulp H. The scrubbed pulp H is finely concentrated to obtain finely concentrated II and a bottom product K. Finely concentrated II and finely concentrated I are mixed and finely concentrated to obtain lithium concentrate and a bottom product M. The bottom product M is returned to the scrubbing pulp H, the bottom product K is returned to the tailings pulp E, and the scavenging I is finely concentrated to obtain lithium concentrate and a bottom product M. The foam product is then returned to the slurry F to be scavenged; during the concentration, a concentration regulator is added. A carbonation regulator is preferred.

Citation Information

Patent Citations

  • Collecting agent for copper converter slag flotation and use method thereof

    CN102962142A

  • Method for flotation of lepidolite without desliming

    CN111298978A

  • Flotation method of peaty slate lead zinc ore with high oxidation rate

    CN113457852A

  • Lepidolite flotation collecting agent and application thereof

    CN114160313A

  • Method for grinding and floating separation of lithium ore and lithium concentrate product

    CN117019407A

Cited By

  • Glass plate processing, transporting and detecting line and glass production process

    CN120887228A

  • Method for sorting aluminosilicate minerals

    CN122230899A

  • Method for sorting aluminosilicate minerals

    CN122230899B