Medical silica gel line surface coating process
Through the silicone wire surface coating process of cooling, atomization and curing steps, the surface modified base film is formed using a modified silicone resin suspension and bake it at high temperature or UV light curing, which solves the pollution problem caused by the surface adhesion performance of the silicone wire. , achieving smooth and dirty-free feel and environmentally friendly production.
Patent Information
- Application Number
- CN202410987250.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
AI Technical Summary
Silicone medical wires lead to impurities adhesion and contamination due to surface adhesion properties. Traditional spraying oil-feeling processes have problems such as high odor, environmental pollution and high costs.
The silicone wire surface coating process using cooling, atomization and curing steps is adopted, and the surface-modified base film is formed using a modified silicone suspension, and cured by high-temperature baking or UV light to ensure that the surface of the wire is smooth and pollution-free.
It realizes a smooth and stain-free feel on the surface of the silicone wire, reduces odor problems and environmental pollution, reduces processing costs, and improves appearance performance and production efficiency.
Smart Images

Figure CN118926057A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of medical cable coating technology, and in particular to a surface coating process for medical silicone wires. Background Art
[0002] Silicone is a high-performance polymer material. Silicone products and modified silicone products can be found in many fields. In the field of medical wire preparation, silicone has a wider range of applications. It is relatively low in cost, highly practical, and not prone to rejection, making it the preferred material for making various medical elastic products.
[0003] In actual production, silicone wires often have good surface adhesion properties, which causes impurities in the air to adhere to the wire surface, affecting the appearance of the wire. The stickiness of the wire surface also makes the wire feel bad when used, and in actual applications, it is easy to stick to the skin surface and cause pollution.
[0004] Therefore, silicone medical wire products usually need to be surface treated during preparation. The traditional surface treatment method is to spray hand oil, but when spraying hand oil for silicone wire surface treatment, on the one hand, the product has a strong odor, causing serious environmental pollution, and on the other hand, the hand oil requires a long curing time, and the processing cost is high, which is not conducive to meeting the requirements of environmental protection performance. Summary of the invention
[0005] In order to solve the above technical problems, the present application provides a medical silicone wire surface coating process, comprising the following steps:
[0006] S1, a cooling step, continuously passing the silicone wire to be coated through a cooling area so that the surface temperature of the silicone wire to be coated is cooled;
[0007] S2, an atomization step, preparing a surface modification solution, continuously spraying a fine oil mist prepared from the surface modification solution on an atomization area, passing a silicone wire to be coated through the atomization area, so that a layer of surface modification base film is coated on the surface of the silicone wire;
[0008] S3, a curing step, passing the silicone wire with the surface modified base film through the curing area, so that the surface modified base film of the silicone wire is cured, and the coating is completed.
[0009] Preferably, in step S1, the silicone wire to be coated is in the cooling area for more than 10 seconds to ensure that the surface of the silicone wire is sufficiently cooled.
[0010] Preferably, the cooling area is connected to the atomizing area, and the silicone wire to be coated enters the atomizing area immediately after leaving the cooling area.
[0011] Preferably, in step S3, the curing method of the curing area includes high temperature baking curing and UV light curing.
[0012] Preferably, when high temperature curing is adopted, the curing temperature is in the range of 120°C-200°C, and the silicone wire stays in the curing area for not less than 10 seconds; when UV light curing is adopted, the energy intensity of UV light should be not less than 5000mJ / cm 2 .
[0013] Preferably, the surface modification solution is one or more of a modified silicone resin suspension, a silicone solution, and a modified silicone oil.
[0014] Preferably, the preparation steps of the modified silicone resin suspension are:
[0015] C1. Add methylphenyl silicone resin and dispersing aid into an organic solvent and mix evenly to obtain a dispersion;
[0016] C2. Add phenolic epoxy resin, coupling agent and catalyst to the dispersion, stir and heat to 100-140° C. for 1 hour, and cool to room temperature to obtain a suspension;
[0017] C3. Add potassium acetate powder, coupling agent and adhesion promoter to the suspension, stir at 200-300 r / min for 10-20 min at room temperature to obtain a modified silicone resin suspension.
[0018] Preferably, in step C1, the mass ratio of methylphenyl silicone resin, organic solvent and dispersing aid is (2-3): (6-8): (0.3-0.5).
[0019] Preferably, in step C2, the mass ratio of dispersion A, phenolic epoxy resin, coupling agent and catalyst is (35-45): (30-40): (0.5-2): (0.5-2).
[0020] Preferably, in step C3, the mass ratio of the suspension, potassium acetate powder and adhesion promoter is (60-80):(0.5-1):(2-3).
[0021] From the above, it can be seen that the application provided by this application can obtain the following beneficial effects: through the above-mentioned silicone wire surface coating process, the surface of the medical silicone wire is smooth and clean, the touch feel is comparable to the effect of applying tactile oil, and no displacement occurs, the product odor problem is solved, it has good appearance performance, and there is no environmental pollution in the processing process, which solves the problem of strong product odor and environmental pollution caused by spraying tactile oil, and has broad application prospects in the field of medical wire preparation. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the technical solutions in the embodiments of the present application or the prior art, the drawings required for use in the description of the embodiments of the present application or the prior art are briefly introduced below. Obviously, the drawings described below are only part of the embodiments of the present application, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative labor.
[0023] Figure 1 This is a process flow chart of the surface coating of the medical silicone wire according to an embodiment of the present application.
[0024] Figure 2 This is a schematic diagram of the surface coating process of the medical silicone wire in the embodiment of the present application. DETAILED DESCRIPTION
[0025] The technical solutions in the embodiments of the present application will be described clearly and completely below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0026] Example
[0027] In order to solve the above technical problems, this embodiment provides a medical silicone wire surface coating process, such as Figure 1 As shown, the following steps are included:
[0028] S1, a cooling step, continuously passing the silicone wire to be coated through a cooling area so that the surface temperature of the silicone wire to be coated is cooled;
[0029] The silicone wire to be coated moves continuously under the action of the traction wheel, and then the silicone wire to be coated passes through the cooling area. Figure 2 As shown, the cooling area can be a cooling box equipped with a refrigeration device. When the silicone wire to be coated passes through the cooling box, the surface of the silicone wire is cooled by the cooling box. The silicone wire to be coated stays in the cooling area for more than 10 seconds. The temperature in the cooling box is preferably set at 5-10°C to ensure that the surface of the silicone wire can be fully cooled.
[0030] S2, an atomization step, preparing a surface modification solution, continuously spraying a fine oil mist prepared from the surface modification solution on an atomization area, passing a silicone wire to be coated through the atomization area, so that a layer of surface modification base film is coated on the surface of the silicone wire;
[0031] In this step, the cooling area and the atomization area are seamlessly connected, and the silicone wire to be coated enters the atomization area immediately after leaving the cooling area. The surface modification solution is pressurized into mist or vibrated into mist to form a fine oil mist. The oil mist is then filled in the entire atomization area through a spraying device, and the silicone wire enters the atomization area immediately after leaving the cooling area. The oil mist in the atomization area is fully and evenly in contact with the surface of the silicone wire. Since the surface of the silicone wire has been cooled, the oil mist is liquefied when it contacts the surface of the silicone wire, and a layer of base film is coated on the surface of the silicone wire. The atomization area can be a closed space formed inside the atomization box, and the silicone wire passes through the atomization box and is filled with oil mist. Ensure that all angles of the wire can be fully and evenly attached with oil mist.
[0032] S3, a curing step, passing the silicone wire with the surface modified base film through the curing area, so that the surface modified base film of the silicone wire is cured, and the coating is completed.
[0033] In this step, the curing method of the curing area includes high temperature baking curing and UV light curing. In the embodiment, a curing oven is used for high temperature baking curing, the baking temperature is in the range of 120℃-200℃, and the silicone wire stays in the curing area for not less than 10s; it is also possible that UV light curing can be used in other embodiments. When UV light curing is used, the energy intensity of the UV light is not less than 5000mJ / cm 2 The base film is fixedly attached to the surface of the wire by thermal curing.
[0034] In the above scheme, the surface modification solution is one or more of a modified silicone resin suspension, a silicone solution, and a modified silicone oil.
[0035] Preferably, the surface modification solution of this embodiment adopts a modified silicone resin suspension, wherein silicone resin has outstanding weather resistance, and is resistant to yellowing even under strong ultraviolet irradiation, and is a thermosetting plastic with excellent thermal oxidation stability. The preparation steps of the modified silicone resin suspension are:
[0036] C1. Add methylphenyl silicone resin and dispersing aid into organic solvent and mix them evenly to obtain dispersion; the organic solvent in this step includes one or more of xylene, n-butanol, cyclohexanone and methyl ethyl ketone. Methylphenyl silicone resin has excellent electrical insulation properties and can maintain its good insulation properties in a wide temperature and frequency range. At the same time, methylphenyl silicone resin has excellent flexibility and thermoplasticity, and is suitable for coating base materials used on cables.
[0037] Furthermore, in step C1, the mass ratio of methylphenyl silicone resin, organic solvent and dispersing aid is (2-3): (6-8): (0.3-0.5), preferably, the mass ratio of methylphenyl silicone resin, organic solvent and dispersing aid is 3:8:0.5, and they are evenly mixed to obtain a dispersion.
[0038] C2. Add phenolic epoxy resin, coupling agent and catalyst to the dispersion, stir and heat to 100-140° C. for 1 hour, and cool to room temperature to obtain a suspension;
[0039] In step C2, the mass ratio of dispersion A, phenolic epoxy resin, coupling agent, and catalyst is (35-45): (30-40): (0.5-2): (0.5-2). The catalyst may be an organic tin catalyst or other commonly used catalyst. Preferably, the mass ratio of dispersion A, phenolic epoxy resin, coupling agent, and catalyst is 40:30:1:1. Existing pure silicone resin has the problem of insufficient mechanical strength and excessive thermoplasticity when used in coating. For this reason, in this step, the dispersion is copolymerized with the phenolic epoxy resin to obtain high temperature resistance, thermoplasticity, and excellent mechanical strength properties, which meet the requirements of wire surface coating and are environmentally friendly.
[0040] C3. Add potassium acetate powder, coupling agent and adhesion promoter to the suspension, stir at 200-300 r / min for 10-20 min at room temperature to obtain a modified silicone resin suspension.
[0041] In step C3, the mass ratio of the suspension, potassium acetate powder, and adhesion promoter is (60-80): (0.5-1): (2-3). Preferably, the mass ratio of the suspension, potassium acetate powder, and adhesion promoter is 70: 1: 2. Adding potassium acetate powder as a buffer can reduce the curing temperature of the suspension, improve the curing efficiency of the modified silicone resin base film when the wire passes through the curing area, effectively reduce the time required for curing, improve production efficiency, and use the adhesion promoter to improve the adhesion to the surface of the wire. After mixing the suspension, potassium acetate powder and adhesion promoter, stir at a speed of 200-300r / min for 10-20min at room temperature to finally obtain a modified silicone resin suspension. The modified silicone resin suspension is used in the above-mentioned silicone wire surface coating process to make the surface of the medical silicone wire smooth and clean, and the touch feel is comparable to the effect of hand-feeling oil coating, and there is no displacement, which solves the product odor problem, has good appearance performance, and has no environmental pollution during the processing process, solving the problem of strong product odor and environmental pollution caused by spraying hand-feeling oil. And when used in the field of medical wire preparation, the above-mentioned raw materials are non-toxic and harmless and are not easy to cause rejection reactions.
[0042] Example 2
[0043] This embodiment provides a surface coating process for medical silicone wires. The difference from Embodiment 1 is that in the preparation step C2 of the modified silicone resin suspension in this embodiment, no phenolic epoxy resin is added, and the other steps are the same as those in Embodiment 1.
[0044] Example 3
[0045] This embodiment provides a surface coating process for medical silicone wires. The difference from Embodiment 1 is that in the preparation step C3 of the modified silicone resin suspension in this embodiment, potassium acetate powder is not added, and the other steps are the same as those in Embodiment 1.
[0046] Comparison Example
[0047] A control example is also provided for comparison with the above-mentioned embodiment. In this control example, the existing hand-feeling oil is sprayed on the surface of the medical silicone wire, and a finished silicone wire is obtained through drying.
[0048]
[0049] Table 1 is a test data table of the silicone wires obtained in each embodiment
[0050] As shown in Table 1, it is a test data table of the silicone wires prepared in the above embodiments. Embodiment 1 is modified by silicone resin and phenolic epoxy resin, while Embodiment 2 only uses silicone resin without adding phenolic epoxy resin. According to the comparison of the data of Embodiment 1 and Embodiment 2 in Table 1, it can be seen that the cyclic bending performance, mechanical strength performance and high temperature anti-aging performance of the cable prepared in Embodiment 1 are better than those in Embodiment 2. It can be seen that after the modified silicone resin suspension prepared by the formula and method of Embodiment 1 is coated on the surface of the wire, it has high temperature resistance, thermoplasticity and excellent mechanical strength performance, which meets the requirements of wire surface coating.
[0051] By comparing Example 1 and Example 3, it can be seen that when potassium acetate powder is not added in the preparation of the modified silicone resin suspension, the coating adhesion effect of Example 3 is poor, and cracks are present after the cyclic bending test. At the same time, the baking and curing time after coating on the wire surface becomes longer, and the baking and curing time of Example 3 is more than twice that of Example 1. It can be seen that the formula of Example 1 has the effect of reducing the curing time, which can achieve the purpose of shortening the process time and process, thereby greatly improving efficiency.
[0052] By comparing Example 1 and the control example, it can be seen that the control example adopts the existing process of coating the surface of the medical silicone wire with hand-feel oil, and the medical silicone wire obtained has an odor problem, and the mechanical strength performance and high-temperature anti-aging performance of the coating layer are worse than those of Example 1. At the same time, in the coating process, the baking and curing time of the hand-feel oil is too long, and the baking and curing time is more than three times that of Example 1, which is not conducive to the improvement of production capacity. The formula and process of Example 1 greatly shorten the time cost compared with the existing technology.
[0053] In summary, the process and formula of Example 1 are the best implementation methods. Through the above-mentioned silicone wire surface coating process, the surface of the medical silicone wire is smooth and clean, the touch feel is comparable to the effect of applying hand-feel oil, and there is no displacement, which solves the product odor problem, has good appearance performance, and has no environmental pollution during the processing process, which solves the problem of strong product odor and environmental pollution caused by spraying hand-feel oil, and has broad application prospects in the field of medical wire preparation.
[0054] The above-described implementation methods do not constitute a limitation on the protection scope of the technical solution. Any modification, equivalent replacement and improvement made within the spirit and principle of the above-described implementation methods shall be included in the protection scope of the technical solution.
Claims
1. A surface coating process for medical silicone wire, characterized by: The following steps are involved: S1, a cooling step, continuously passing the silicone wire to be coated through a cooling area so that the surface temperature of the silicone wire to be coated is cooled; S2, an atomization step, preparing a surface modification solution, continuously spraying a fine oil mist prepared from the surface modification solution on an atomization area, passing a silicone wire to be coated through the atomization area, so that a layer of surface modification base film is coated on the surface of the silicone wire; S3, a curing step, passing the silicone wire with the surface modified base film through the curing area, so that the surface modified base film of the silicone wire is cured, and the coating is completed.
2. The surface coating process of medical silicone wire according to claim 1, characterized in that: In step S1, the silicone wire to be coated is in the cooling area for more than 10 seconds to ensure that the surface of the silicone wire is sufficiently cooled.
3. The surface coating process of medical silicone wire according to claim 1, characterized in that: The cooling area is connected to the atomizing area, and the silicone wire to be coated enters the atomizing area immediately after leaving the cooling area.
4. The surface coating process of medical silicone wire according to claim 1, characterized in that: In step S3, the curing method of the curing area includes high temperature baking curing and UV light curing.
5. The surface coating process of medical silicone wire according to claim 4, characterized in that: When high temperature baking is used for curing, the baking temperature is within the range of 120℃-200℃, and the silicone wire stays in the curing area for no less than 10s; When UV light curing is used, the energy intensity of UV light should not be less than 5000mJ / cm 2 .
6. The surface coating process of medical silicone wire according to claim 1, characterized in that: The surface modification solution is one or more of modified silicone resin suspension, silicone solution, and modified silicone oil.
7. The surface coating process of medical silicone wire according to claim 6, characterized in that: The preparation steps of the modified silicone resin suspension include: C1. Add methylphenyl silicone resin and dispersing aid into an organic solvent and mix evenly to obtain a dispersion; C2. Add phenolic epoxy resin, coupling agent and catalyst to the dispersion, stir and heat to 100-140° C. for 1 hour, and cool to room temperature to obtain a suspension; C3. Add potassium acetate powder, coupling agent and adhesion promoter to the suspension, stir at 200-300 r / min for 10-20 min at room temperature to obtain a modified silicone resin suspension.
8. The surface coating process of medical silicone wire according to claim 7, characterized in that: In step C1, the mass ratio of methylphenyl silicone resin, organic solvent and dispersing aid is (2-3): (6-8): (0.3-0.5).
9. The surface coating process of medical silicone wire according to claim 7, characterized in that: In step C2, the mass ratio of dispersion A, phenolic epoxy resin, coupling agent and catalyst is (35-45): (30-40): (0.5-2): (0.5-2).
10. The surface coating process of medical silicone wire according to claim 7, characterized in that: In step C3, the mass ratio of the suspension, potassium acetate powder and adhesion promoter is (60-80):(0.5-1):(2-3).