Short-process manufacturing method of large-diameter thin-wall thick aluminum alloy seamless pipe for pressure vessel
The production of aluminum alloy pipes through one-time extrusion molding method solves the problems of low production efficiency and poor surface quality of large-scale thin-wall aluminum alloy pipes, and achieves the effects of shortening production cycles, improving efficiency and reducing costs.
Patent Information
- Application Number
- CN202411307258.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-19
- Publication Date
- 2024-11-12
AI Technical Summary
The existing large-size thin-wall aluminum alloy pipes have low production efficiency and poor surface quality, long production cycle, high energy consumption and low yield, making it difficult to meet user needs.
Aluminum alloy pipes are produced by one-time extrusion molding. By selecting suitable aluminum alloy ingots and extrusion molds, the mold and needle tip sizes are determined according to the extrusion temperature and shrinkage ratio of the alloy, heating and slowly extruding are carried out to ensure microstructure No overburn and surface quality.
Shorten the production cycle, improve production efficiency, significantly improve yield and surface quality, and reduce production costs.
Abstract
Description
Technical Field
[0001] The invention relates to a short-process manufacturing method for a large-diameter, thin-walled, thick aluminum alloy seamless pipe for a pressure vessel. Background Art
[0002] Aluminum alloy seamless pipes are widely used in the fields of electricity, transportation, chemical industry, machinery, aerospace, national defense and military industry. In recent years, the user departments have put forward higher requirements for the quality of aluminum alloy products, which requires the production department to further improve the surface quality of products while ensuring various technical indicators, meet the urgent needs of users, improve production efficiency, respond to the requirements of green development, increase the enterprise's finished product rate, and reduce production costs.
[0003] At present, thin-walled pipes are all produced by drawing or rolling. Large-size thin-walled pipes generally adopt the drawing process, which requires multiple drawing and matching multiple annealing. The problems of long production cycle, high energy consumption, low yield rate, and difficulty in surface quality control are prominent, which seriously restrict the production cycle and cost reduction and efficiency improvement. Therefore, in order to improve production efficiency, shorten production cycle, optimize production process, shorten production cycle, improve production efficiency, and save production cost, it is necessary to provide a short-process manufacturing method for large-diameter thin-walled thick aluminum alloy seamless pipes for pressure vessels. Summary of the invention
[0004] The purpose of the present invention is to solve the problems of low production efficiency and poor surface quality of existing large-size thin-walled aluminum alloy pipes, and to provide a short-process manufacturing method for large-diameter, thin-walled and thick aluminum alloy seamless pipes for pressure vessels.
[0005] The short-process manufacturing method of a large-diameter, thin-walled, thick aluminum alloy seamless pipe for a pressure vessel of the present invention is specifically carried out according to the following steps:
[0006] 1. Select cylindrical aluminum alloy ingot as raw material; select extrusion die and extrusion needle according to the size of aluminum alloy ingot;
[0007] 2. placing the aluminum alloy ingot into an ingot heating furnace and heating the ingot to the upper limit of the extrusion temperature of the selected alloy;
[0008] 3. After reaching the upper limit of extrusion temperature, transfer to the extrusion barrel for extrusion to complete the short-process manufacturing of large-diameter, thin-walled, thick aluminum alloy seamless pipes for pressure vessels.
[0009] Beneficial effects of the present invention:
[0010] The present invention produces large-size thin-walled aluminum alloy pipes by one-time extrusion molding. The present invention determines the size of the mold and needle tip according to the shrinkage ratio characteristics of the alloy, and reasonably matches the size of the extrusion mold and the needle tip to ensure that the product standard requirements are met. The extrusion temperature of the ingot adopts the upper limit of the extrusion temperature of the selected alloy to ensure that the microstructure is not overburned. After the ingot reaches the temperature, it is placed in the extrusion cylinder and slowly pressed and extruded at a slow speed to ensure the surface quality and controllability; one-time extrusion molding shortens the production cycle, improves production efficiency, and has significant effects on improving quality, increasing efficiency and reducing costs. DETAILED DESCRIPTION
[0011] Specific implementation method 1: In this implementation method, a short-process manufacturing method of a large-diameter, thin-walled, thick aluminum alloy seamless pipe for a pressure vessel is specifically carried out in the following steps:
[0012] 1. Select cylindrical aluminum alloy ingot as raw material; select extrusion die and extrusion needle according to the size of aluminum alloy ingot;
[0013] 2. placing the aluminum alloy ingot into an ingot heating furnace and heating the ingot to the upper limit of the extrusion temperature of the selected alloy;
[0014] 3. After reaching the upper limit of extrusion temperature, transfer to the extrusion barrel for extrusion to complete the short-process manufacturing of large-diameter, thin-walled, thick aluminum alloy seamless pipes for pressure vessels.
[0015] Specific embodiment 2: This embodiment is different from specific embodiment 1 in that the outer diameter of the aluminum alloy ingot in step 1 is 402-408 mm, the inner diameter is 207-213 mm, and the length is 590-610 mm. Others are the same as specific embodiment 1.
[0016] Specific implementation method 3: This implementation method is different from specific implementation method 2 in that the outer diameter of the aluminum alloy ingot in step 1 is 405 mm, the inner diameter is 210 mm, and the length is 600 mm. The rest is the same as specific implementation method 2.
[0017] Specific embodiment 4: This embodiment differs from specific embodiment 1 in that the aluminum alloy ingot in step 1 is 5xxx aluminum alloy. Other aspects are the same as those of specific embodiment 1.
[0018] Specific implementation method 5: This implementation method is different from the specific implementation method 1 in that the inner diameter of the extrusion die in step 1 is 158-160 mm. The rest is the same as the specific implementation method 1.
[0019] Specific implementation example 6: This implementation example is different from the specific implementation example 1 in that the outer diameter of the extrusion needle in step 1 is 158-159 mm. The rest is the same as the specific implementation example 1.
[0020] Specific embodiment 7: This embodiment is different from specific embodiment 4 in that the upper limit of the extrusion temperature in step 2 is 495-505° C. The rest is the same as specific embodiment 4.
[0021] Specific embodiment eight: This embodiment differs from specific embodiment seven in that the upper limit of the extrusion temperature in step two is 510° C. The rest is the same as specific embodiment seven.
[0022] Specific embodiment 9: This embodiment is different from specific embodiment 1 in that the extrusion speed in step 3 is 0.2-0.5 mm / s. The rest is the same as specific embodiment 1.
[0023] The following examples are used to verify the beneficial effects of the present invention:
[0024] Embodiment 1:
[0025] The method for short-process manufacturing of large-diameter, thin-walled, thick aluminum alloy seamless pipes for pressure vessels in this embodiment is carried out according to the following steps: The extrusion speed during extrusion in step three is 0.2 mm / s.
[0026] 1. Determination of mold and needle tip size:
[0027] Select 5xxx aluminum alloy ingot, the aluminum alloy ingot is cylindrical; select an extrusion die and an extrusion needle according to the size of the aluminum alloy ingot; the inner diameter of the die is 160mm; the outer diameter of the extrusion needle is 159mm; the outer diameter of the aluminum alloy ingot is 405mm, the inner diameter is 210mm, and the length is 600mm;
[0028] 2. placing the aluminum alloy ingot into an ingot heating furnace, and heating the ingot to the upper limit of the extrusion temperature of the selected alloy; the upper limit of the extrusion temperature is 510° C.;
[0029] 3. After reaching the upper limit of the extrusion temperature, the tube is transferred to the extrusion barrel for extrusion to complete the short-process manufacturing of large-diameter, thin-walled, thick aluminum alloy seamless tubes for pressure vessels; the extrusion speed during the extrusion is 0.2 mm / s.
[0030] This embodiment produces large-sized thin-walled aluminum alloy pipes by one-time extrusion molding. The present invention determines the size of the die and needle tip according to the shrinkage ratio characteristics of the alloy, and achieves reasonable matching of the extrusion die and needle tip size to ensure that the product standard requirements are met. The extrusion temperature of the ingot adopts the upper limit of the extrusion temperature of the selected alloy to ensure that the microstructure is not overburned. After the ingot reaches the temperature, it is placed in the extrusion cylinder and slowly pressed up and extruded at a slow speed to ensure the surface quality and controllability; one-time extrusion molding shortens the production cycle, improves production efficiency, and has significant effects on improving quality, increasing efficiency and reducing costs.
[0031] Embodiment 2:
[0032] The method for short-process manufacturing of large-diameter, thin-walled, thick aluminum alloy seamless pipes for pressure vessels in this embodiment is carried out according to the following steps: The extrusion speed during extrusion in step three is 0.2 mm / s.
[0033] 1. Determination of mold and needle tip size:
[0034] Select 5xxx aluminum alloy ingot, the aluminum alloy ingot is cylindrical; select an extrusion die and an extrusion needle according to the size of the aluminum alloy ingot; the inner diameter of the die is 160mm; the outer diameter of the extrusion needle is 158mm; the outer diameter of the aluminum alloy ingot is 403mm, the inner diameter is 209mm, and the length is 600mm;
[0035] 2. placing the aluminum alloy ingot into an ingot heating furnace, and heating the ingot to the upper limit of the extrusion temperature of the selected alloy; the upper limit of the extrusion temperature is 510° C.;
[0036] 3. After reaching the upper limit of the extrusion temperature, the tube is transferred to the extrusion barrel for extrusion to complete the short-process manufacturing of large-diameter, thin-walled, thick aluminum alloy seamless tubes for pressure vessels; the extrusion speed during the extrusion is 0.2 mm / s.
[0037] This embodiment produces large-sized thin-walled aluminum alloy pipes by one-time extrusion molding. The present invention determines the size of the die and needle tip according to the shrinkage ratio characteristics of the alloy, and achieves reasonable matching of the extrusion die and needle tip size to ensure that the product standard requirements are met. The extrusion temperature of the ingot adopts the upper limit of the extrusion temperature of the selected alloy to ensure that the microstructure is not overburned. After the ingot reaches the temperature, it is placed in the extrusion cylinder and slowly pressed up and extruded at a slow speed to ensure the surface quality and controllability; one-time extrusion molding shortens the production cycle, improves production efficiency, and has significant effects on improving quality, increasing efficiency and reducing costs.
Claims
1. A short-process manufacturing method for large-diameter, thin-walled, thick aluminum alloy seamless pipes for pressure vessels, characterized in that The short-process manufacturing method of large-diameter, thin-walled, thick aluminum alloy seamless pipes for pressure vessels is specifically carried out in the following steps:
1. Select cylindrical aluminum alloy ingot as raw material; select extrusion die and extrusion needle according to the size of aluminum alloy ingot; 2. placing the aluminum alloy ingot into an ingot heating furnace and heating the ingot to the upper limit of the extrusion temperature of the selected alloy; 3. After reaching the upper limit of extrusion temperature, transfer to the extrusion barrel for extrusion to complete the short-process manufacturing of large-diameter, thin-walled, thick aluminum alloy seamless pipes for pressure vessels.
2. The short-process manufacturing method of a large-diameter, thin-walled, thick aluminum alloy seamless pipe for a pressure vessel according to claim 1, characterized in that The aluminum alloy ingot in step 1 has an outer diameter of 402-408 mm, an inner diameter of 207-213 mm, and a length of 590-610 mm.
3. The short-process manufacturing method of a large-diameter, thin-walled, thick aluminum alloy seamless pipe for a pressure vessel according to claim 2, characterized in that The aluminum alloy ingot in step 1 has an outer diameter of 405 mm, an inner diameter of 210 mm, and a length of 600 mm.
4. The short-process manufacturing method of a large-diameter, thin-walled, thick aluminum alloy seamless pipe for a pressure vessel according to claim 1, characterized in that The aluminum alloy ingot described in step 1 is 5xxx aluminum alloy.
5. The short-process manufacturing method of a large-diameter, thin-walled, thick aluminum alloy seamless pipe for a pressure vessel according to claim 1, characterized in that The inner diameter of the extrusion die in step 1 is 158-160 mm.
6. The short-process manufacturing method of a large-diameter, thin-walled, thick aluminum alloy seamless pipe for a pressure vessel according to claim 1, characterized in that The outer diameter of the extrusion needle in step 1 is 158-159 mm.
7. The short-process manufacturing method of a large-diameter, thin-walled, thick aluminum alloy seamless pipe for a pressure vessel according to claim 4, characterized in that The upper limit of the extrusion temperature in step 2 is 495-505°C.
8. The short-process manufacturing method of a large-diameter, thin-walled, thick aluminum alloy seamless pipe for a pressure vessel according to claim 7, characterized in that The upper limit of the extrusion temperature in step 2 is 510°C.
9. The short-process manufacturing method of a large-diameter, thin-walled, thick aluminum alloy seamless pipe for a pressure vessel according to claim 1, characterized in that The extrusion speed during the extrusion in step 3 is 0.2 to 0.5 mm / s.
Citation Information
Patent Citations
Perforating and extruding production method of seamless aluminum-alloy tubular product
CN103357688A
Aluminum alloy thin-wall pipe extrusion process
CN112517653A
High-strength aluminum alloy seamless tube extrusion process method and device
CN114210752A
Method for preparing aluminum alloy large-specification thin-wall pipe through one-time extrusion forming
CN116274456A
Method for manufacturing hot-deformed thin-walled pipe products made of titanium and titanium alloys
RU2754542C1