External field strengthening forming method for aluminum bronze valve body

By adopting an external field strengthening method combining infrared induction heating and mechanical stirring in aluminum bronze alloy valve body casting, combined with multi-material composite core and inert gas protection, the problems of sand clamping and air holes in aluminum bronze alloy valve body casting are solved. , realizes high-quality and low-cost casting production, and improves the reliability and service life of castings.

CN118926485APending Publication Date: 2024-11-12SHENYANG RES INST OF FOUNDRY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410913472.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

During the casting process, the aluminum bronze alloy valve body is prone to defects such as sand, slag, and pores, which are difficult to meet the requirements of internal quality, surface quality and dimensional accuracy. The high oxidation tendency and low vapor pressure of the material lead to reliability and service life. limit.

Method used

Using an external field strengthening method combining infrared induction heating and mechanical stirring, combining medium frequency induction furnaces and multi-material composite cores, including external metallic forms, internal 3D printed sand forms and refractory risers, casting forming is achieved through sintering removal, and using inertia Gas protection and open casting systems reduce oxidation and inclusion.

Benefits of technology

It improves the internal and external quality of the aluminum bronze valve body, reduces shrinkage and loose defects, shortens the manufacturing cycle, and achieves high-quality and low-cost casting production, and complies with the performance indicators of GB/T 12225-2018 standards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118926485A_ABST
    Figure CN118926485A_ABST
Patent Text Reader

Abstract

The invention aims to provide an external field strengthening forming method for an aluminum bronze valve body, and particularly relates to the field of copper alloy valve body manufacturing. The aluminum bronze valve body is manufactured through a gravity casting method, an external field strengthening method combining infrared induction heating strengthening and mechanical stirring strengthening is adopted, smelting is conducted through a medium-frequency induction furnace, and components are precisely controlled; and forming and manufacturing of the aluminum bronze valve body are completed through the multi-material composite core and sintering removal. The method has the advantages that the chemical components of the aluminum bronze valve body casting are precisely controlled, the mechanical property is improved, the whole precise forming is realized, the internal and external quality of the aluminum bronze valve body casting is improved, the machining allowance is reduced, and the manufacturing period is shortened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of copper alloy valve body manufacturing, and in particular provides an aluminum bronze valve body outfield strengthening forming method. Background Art

[0002] The valve body is a major part of the valve, which forms an effective sealing space with the valve core, valve seat, sealing ring, etc., and is mainly used to bear the medium and the pressure it brings. The valve body has a complex structure, large wall thickness differences, and many thermal nodes, which is very unfavorable for solidification and shrinkage compensation. It is difficult to control sand inclusion, slag inclusion and surface pore defects in ordinary sand gravity casting, and it is difficult to meet the requirements of internal quality, surface quality, and dimensional accuracy.

[0003] The crystallization temperature range of aluminum bronze alloy is small (about 30°C), which belongs to lamellar solidification, and the volume shrinkage rate (4.1%) and linear shrinkage rate (2.49%) are relatively high. It is very easy to produce casting defects such as shrinkage holes and looseness during solidification; due to the high aluminum content in the material, it has a strong tendency to oxidize, and it is easy to form secondary oxidation slag during the pouring process; the vapor pressure of aluminum bronze liquid is low, the air absorption tendency is large, and pores are easily generated; this limits the reliability and service life of the aluminum bronze high-pressure valve body. Summary of the invention

[0004] The invention provides an external field strengthening forming method for an aluminum bronze valve body, which has the advantages of improving the internal and external quality of an aluminum bronze valve body casting, reducing machining allowances, shortening manufacturing cycles, and the like.

[0005] To achieve the above object, the present invention provides the following technical solutions:

[0006] A method for strengthening the forming of an aluminum bronze valve body by an external field, wherein the aluminum bronze valve body is manufactured by a gravity casting method, an external field strengthening method combining infrared induction heating strengthening and mechanical stirring strengthening is adopted, melting and pouring is performed by a medium frequency induction furnace and the composition is precisely controlled, and a multi-material composite core and sintering removal are used to complete the forming and manufacturing of the valve body.

[0007] Furthermore, the infrared induction heating is enhanced by placing an induction coil at the riser, and controlling the liquid and semi-solid state of the metal in the riser is achieved by induction heating; a stirring blade is arranged above the inside of the induction coil, a rotating shaft is arranged inside the stirring blade, and a motor is arranged above the rotating shaft.

[0008] Furthermore, the mechanical stirring is strengthened into mechanical stirring in the riser, and the metal flow shrinkage compensation is achieved by fixing the mechanical stirring device, wherein the mechanical stirring device is composed of a supporting mechanism, an electrode, a rotating shaft and special material blades.

[0009] Furthermore, a medium frequency induction furnace is used for smelting, and inert gas protection is used for pouring through a pouring channel. The inert gas is high-purity argon with a purity of 99%. The inert gas is introduced in three ways: top cover, bottom vertical, and oblique surround. The pouring temperature is 1180±5°C.

[0010] Furthermore, the multi-material composite core consists of an external metal mold, an internal 3D printed sand mold and a refractory riser. The multi-material composite core realizes valve body forming through the rapid cooling effect of the external metal mold, the high-precision forming of the internal 3D printed sand mold and the good shrinkage compensation effect of the refractory riser.

[0011] Furthermore, the aluminum bronze valve body composition comprises, by mass fraction, 8.5% to 11.0% aluminum, 2.0% to 4.0% iron, and the remainder copper and other impurities.

[0012] Furthermore, the sintering removal is the removal of the internal 3D printed sand mold. After forming, the valve body is heated to 450°C and kept warm for 1 hour. The 3D printed sand mold loses its strength due to the burning of the binder at high temperature and becomes loose sand particles, thereby realizing the removal of the internal core.

[0013] Furthermore, the valve body is provided with an internal core after molding.

[0014] The beneficial effects of the present invention are:

[0015] (1) A composite core of "metal mold + 3D printed sand core + refractory riser" is used, and an open pouring system is designed to allow the copper liquid to fill the mold smoothly. A filter is added to the runner to remove inclusions, and inert gas is introduced into the cavity during the pouring process to avoid secondary oxidation, thereby improving the internal and external quality of this type of copper alloy valve body and achieving high-quality manufacturing;

[0016] (2) An external field strengthening method combining infrared induction heating and mechanical stirring is used to control the liquid and semi-solid states of the metal in the riser, thereby reducing casting defects such as shrinkage cavities and looseness caused by laminar solidification and high volume shrinkage and linear shrinkage.

[0017] (3) The sintering removal method is used to remove the 3D printed sand mold inside the valve body casting. It has low cost and short cycle, strong practicality and promotion value, and is easy to realize engineering application. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 Aluminum bronze valve body Schematic diagram of valve body structure.

[0019] Figure 2 Schematic diagram of the external field strengthening casting process of aluminum bronze valve body.

[0020] Figure 3 Image of the additive sand core for the 3D printed aluminum bronze valve body.

[0021] Figure 4 Schematic diagram of the inner structure of the aluminum bronze valve body metal mold.

[0022] Figure 5 Schematic diagram of the outer structure of the aluminum bronze valve body metal mold.

[0023] Figure numerals: 1-valve body casting; 2-pouring channel; 3-riser; 4-induction coil; 5-stirring blade; 6-rotating shaft; 7-motor DETAILED DESCRIPTION

[0024] The present invention will be further described below in conjunction with the embodiments and the accompanying drawings, but is not limited thereto.

[0025] Example 1

[0026] The aluminum bronze alloy valve body is precision cast by external field strengthening forming method. The aluminum bronze alloy valve body structure is as follows Figure 1 As shown, the casting profile is 250×215×225mm.

[0027] 1) Process design: The maximum wall thickness of the valve body parts is 39mm, the minimum wall thickness is 6mm, the reduction is set to 1.8%, the outer surface machining allowance is +6mm, the inner cavity machining allowance is +5mm, and the internal core is provided with a full-body chiller (φ20mm) to form a sequential solidification direction.

[0028] 2) Composite core preparation: Figure 3 The aluminum-bronze alloy valve body casting is divided into modules and layers. The internal core is manufactured by sand mold 3D printing. The sand mold uses 3D printed resin sand as molding sand, modified furan resin as binder, and toluenesulfonic acid as curing agent. The sand mold is printed layer by layer by inkjet. The external casting uses a gray cast iron metal mold. The overall structure is designed according to the exhaust system, locking mechanism and parting mechanism, and is manufactured by mechanical processing.

[0029] 3) Melting and pouring: Melting is carried out in a medium frequency induction furnace, and pouring is carried out through the pouring channel 2 under inert gas protection. The inert gas is high-purity argon (purity 99%), and the inert gas is introduced in three ways: top cover, bottom vertical and oblique surround. The pouring temperature is 1180±5℃.

[0030] 4) Riser induction heating: After pouring, when the aluminum bronze alloy is in a semi-solid state, such as Figure 2 , start the induction coil 4 prefabricated on the periphery of the riser 3, induction heat the alloy in the riser 3, change the alloy from paste to liquid, and increase the fluidity of the supplementary liquid. A stirring blade 5 is arranged above the induction coil 4, a rotating shaft 6 is arranged inside the stirring blade, and a motor 7 is arranged above the rotating shaft 6.

[0031] 5) Mechanical stirring: After the riser 3 is induction heated, the mechanical stirring device prefabricated at the top of the riser 3 is started to mechanically stir the alloy liquid in the riser 3. The relative movement of the liquid alloy improves the shrinkage compensation capacity of the riser 3 and eliminates or reduces shrinkage defects.

[0032] 6) Unpacking the external mold: Split the external metal mold according to the pre-set parting plane. Figure 4 , Figure 5 .

[0033] 7) Sintering removal: The valve body casting 1 after the outer mold is removed is heated at a temperature of 280°C ± 5°C and a holding time of 1.5 hours. The 3D printed sand mold loses strength due to the burning of the binder at high temperature and becomes loose sand particles, thereby achieving lossless removal of the internal core.

[0034] Compared with conventional casting methods, the overall composition and performance indicators of the aluminum bronze alloy valve body casting 1 cast by the casting method of the present invention meet or exceed the requirements of GB / T 12225-2018 standard. See Table 1 and Table 2 for details.

[0035] Table 1 Chemical composition and impurity content of samples of the present invention (mass fraction / %)

[0036]

[0037] Table 2 Mechanical properties of samples of the present invention

[0038]

[0039] The above examples are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the invention should be included in the protection scope of the present invention.

Claims

1. A method for strengthening the external field forming of aluminum bronze valve body, Features: An aluminum bronze valve body casting (1) is manufactured by gravity casting, an external field strengthening method combining infrared induction heating strengthening and mechanical stirring strengthening is adopted, melting and pouring is performed in a medium frequency induction furnace and the composition is precisely controlled, and the valve body is formed and manufactured by using a multi-material composite core and sintering removal.

2. The external field strengthening forming method of aluminum bronze valve body according to claim 1, Features: Infrared induction heating is enhanced by placing an induction coil (4) at the riser (3) to control the state of the metal in the riser (3) in liquid or semi-solid state by induction heating; a stirring blade (5) is arranged above the inside of the induction coil (4), a rotating shaft (6) is arranged inside the stirring blade, and a motor (7) is arranged above the rotating shaft (6).

3. The external field strengthening forming method of aluminum bronze valve body according to claim 1, Features: The smelting is carried out in a medium frequency induction furnace, and the inert gas is protected by a pouring channel (2) for pouring. The inert gas is high-purity argon with a purity of 99%. The inert gas is introduced in three ways: top cover, bottom vertical and oblique surrounding. The pouring temperature is 1180±5°C.

4. The method for strengthening the outer field forming of aluminum bronze valve body according to claim 1, Features: The mechanical stirring is strengthened by mechanical stirring in the riser (3), and the metal flow compensation is realized by fixing the mechanical stirring device, wherein the mechanical stirring device is composed of a supporting mechanism, an electrode, a rotating shaft and a special material blade.

5. The method for strengthening the outer field forming of aluminum bronze valve body according to claim 1, Features: The multi-material composite core consists of an external metal mold, an internal 3D printed sand mold and a refractory riser. The multi-material composite core realizes valve body forming through the rapid cooling effect of the external metal mold, the high-precision forming of the internal 3D printed sand mold and the good shrinkage compensation effect of the refractory riser.

6. The external field strengthening forming method of aluminum bronze valve body according to claim 1, Features: The aluminum bronze valve body composition comprises the following components by mass fraction: 8.5% to 11.0% aluminum, 2.0% to 4.0% iron, and the remainder copper and other impurities.

7. The method for strengthening the forming of aluminum bronze valve body in an external field according to claim 1, Features: The sintering removal is the removal of the internal 3D printed sand mold. After forming, the valve body is heated to 450°C and kept warm for 1 hour. The 3D printed sand mold loses its strength due to the burning of the binder at high temperature and becomes loose sand particles, thereby realizing the removal of the internal core.

8. The method for strengthening the outer field forming of aluminum bronze valve body according to claim 7, Features: The valve body is molded with an internal core.