Composite binding phase super-coarse hard alloy and preparation method thereof

Through high-energy ball milling and hydrogen sintering processes, NiO is refined and WC grain growth is promoted, and the problems of poor agglomeration and wettability after Ni are added are solved. A composite bonded phase ultra-coarse cemented carbide with good mechanical properties is prepared, realizing the WC grain distribution is uniform and has high intensity.

CN118926521APending Publication Date: 2024-11-12CHONGYI ZHANGYUAN TUNGSTEN +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410994859.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the prior art, when preparing ultra-coarse carbides, Ni is easily agglomerated and poor wettability after adding Ni, which leads to difficulty in sintering and densification of alloys, affects performance, and is short of cobalt resources and has high cost.

Method used

High-energy ball mill is used to fine-grain and make it evenly distributed. The secondary ball mill selects a light ball mill to maintain coarse WC grains. Then, during the sintering process, NiO is converted into fine-grained and uniformly distributed Ni, which is ultra-fine generated by WO3 reaction. WC is rapidly dissolved and precipitated on the crude WC grains to promote the growth and development of WC grains, and the composite bonded phase ultra-coarse cemented carbide is prepared through hydrogen sintering process.

Benefits of technology

The WC grain distribution is uniform, the bending strength is ≥2350MPa, and the Vickers hardness is ≥1050kgf/mm2, which improves the mechanical properties and densification effect of the alloy, avoids the formation of Ni pools, and reduces the use of cobalt.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118926521A_ABST
    Figure CN118926521A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of powder metallurgy, and particularly relates to a composite binding phase ultra-coarse hard alloy and a preparation method thereof.NiO is refined through high-energy ball milling and evenly distributed in composite powder, mild ball milling is selected for secondary ball milling, the advantages of coarse WC crystal grains are kept, and superfine NiO-WO3-C composite powder is evenly attached to the coarse WC crystal grains. And then in the sintering process, NiO is converted into fine-grained and uniformly-distributed Ni in situ, so that the possibility that a Ni pool is formed due to Ni agglomeration in the sintering stage is reduced. The superfine WC which is generated by WO3 reaction and has high activity is quickly dissolved in a composite binding phase of which the solubility is greater than that of Co, and then is separated out on superior coarse WC crystal grains, so that the growth and development of the WC crystal grains are promoted. According to the composite binding phase ultra-coarse hard alloy prepared through the technology, WC grains are evenly distributed and completely developed, the alloy has good mechanical performance, the average grain size of WC ranges from 5.5 micrometers to 7.5 micrometers, the bending strength is larger than or equal to 2350 MPa, and the Vickers hardness is larger than or equal to 1050 kgf / mm < 2 >.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of powder metallurgy, and in particular relates to a composite bonding phase ultra-coarse cemented carbide and a preparation method thereof. Background Art

[0002] Cemented carbide is a high-hardness, high-wear-resistant composite material made by powder metallurgy method with refractory metal WC as hard phase and metal cobalt as bonding phase. It is widely used in mining, cutting, grinding, military, aerospace and other industrial fields. The mechanical properties of cemented carbide are closely related to the microstructure of WC grain size and bonding phase. Compared with ordinary cemented carbide, super-coarse cemented carbide has good red hardness due to its coarse grains, complete crystal development, fewer internal defects of WC grains and stable structure. In addition, the WC grains of super-coarse cemented carbide are coarser and the specific surface area is smaller, which makes the Co layer thicker, thus having excellent impact toughness and good thermal conductivity. Therefore, super-coarse cemented carbide is widely used in mining tool materials such as oil drill teeth, stamping dies, coal machine teeth, shield cutters, etc. At the same time, the rapid development of modern manufacturing industry has put forward higher requirements on the performance of super-coarse cemented carbide.

[0003] At present, the methods for preparing ultra-coarse cemented carbide mainly include: flexible ball milling, chemical coating, and ultra-fine WC dissolution. The flexible ball milling method is a method for preparing ultra-coarse cemented carbide by reducing the ball milling efficiency. However, during the ball milling process, the coarse WC grains are easily crushed into fine WC by ball milling, so that the cemented carbide after sintering cannot meet the requirements of coarse cemented carbide. The chemical coating method is a method of using chemical coprecipitation coating reaction to deposit cobalt oxalate on the surface of WC powder, followed by one-step reduction to prepare WC-Co composite powder, and then pressing and sintering to prepare ultra-coarse cemented carbide. The chemical coating method avoids the ball milling process, but due to the disadvantages of high cost and complex process, its promotion and application are limited. The ultra-fine WC dissolution method is to prepare ultra-coarse cemented carbide by adding highly active ultra-fine WC, and promoting the growth of WC grains through the dissolution-precipitation effect in the sintering stage. However, ultra-fine WC is prone to agglomeration, resulting in many fine WC grains in the alloy, making it difficult to prepare ultra-coarse cemented carbide with uniform distribution of WC grains. Cobalt is a global strategic material with relatively small reserves. In recent years, as the demand for cobalt in the battery industry continues to increase, the price of cobalt has become increasingly expensive. Partial substitution of Ni for Co as a binder phase can effectively reduce the amount of Co used, which is conducive to the sustainable and healthy development of the cemented carbide industry. In addition, Ni can form a solid solution with Co, which can significantly improve the strength of the binder phase, thereby improving the overall strength of the material. However, since Ni belongs to the HCP crystal system and has good plasticity, this plasticity makes nickel prone to plastic deformation during wet grinding, forming flaky nickel powder agglomerates. In addition, WC-Ni cemented carbide has poor Ni / WC wettability, and Ni tends to agglomerate during liquid phase sintering, making it difficult to sinter and densify the alloy, forming abnormal Ni pool structure, thereby affecting the alloy performance. Summary of the invention

[0004] In order to solve the problems existing in the prior art, the main purpose of the present invention is to provide a composite binder phase ultra-coarse cemented carbide and a preparation method thereof.

[0005] To solve the above technical problems, according to one aspect of the present invention, the present invention provides the following technical solutions:

[0006] A method for preparing a composite binder phase ultra-coarse cemented carbide comprises the following steps:

[0007] S1, taking carbon powder, NiO powder and WO3 powder, and subjecting them to high-energy ball milling to obtain ultrafine NiO-WO3-C composite powder with an average particle size of less than 0.3 μm;

[0008] S2, taking ultrafine NiO-WO3-C composite powder and WC, Co powder and ball milling to obtain WC-Co-NiO-WO3-C composite powder;

[0009] The S3 and WC-Co-NiO-WO3-C composite powders are pressed into compacts and then sintered using a hydrogen sintering process to obtain a composite bonding phase ultra-coarse cemented carbide.

[0010] As a preferred embodiment of the method for preparing a composite binder phase ultra-coarse cemented carbide according to the present invention, in step S1, the mass ratio of carbon powder, NiO powder and WO3 powder is (12-18): (30-50): (32-58).

[0011] As a preferred embodiment of the method for preparing a composite binder phase ultra-coarse cemented carbide according to the present invention, wherein: in the step S1, the ball milling speed is 350-500 r / min, the ball milling time is 12-48 h, the ball-to-material ratio is (8-10):1, and the ball milling medium is alcohol.

[0012] As a preferred embodiment of the method for preparing a composite binder phase ultra-coarse cemented carbide described in the present invention, wherein: in the step S1, after the ball milling is completed, the NiO-WO3-C composite powder is dried at a drying temperature of 80 to 120°C and a drying time of 1 to 5 hours.

[0013] As a preferred embodiment of the method for preparing a composite binder phase ultra-coarse cemented carbide according to the present invention, in step S2, the mass ratio of NiO-WO3-C composite powder to WC and Co powder is (5-10):(90-95).

[0014] As a preferred embodiment of the method for preparing a composite binder phase ultra-coarse cemented carbide according to the present invention, wherein: in the step S2, the Fisher grain size of WC is 12 to 30 μm.

[0015] As a preferred embodiment of the method for preparing a composite binder phase ultra-coarse cemented carbide described in the present invention, wherein: in the step S2, the ball milling speed is 100-350 r / min, the ball milling time is 4-10 h, the ball-to-material ratio is (3-5):1, the ball milling medium is alcohol, and paraffin accounting for 2wt% of the total mass of the powder is added during ball milling.

[0016] As a preferred embodiment of the method for preparing a composite binder phase ultra-coarse cemented carbide described in the present invention, wherein: in the step S2, the WC-Co-NiO-WO3-C composite powder is dried after the ball milling, the drying temperature is 80-120°C, and the drying time is 1-3h.

[0017] As a preferred embodiment of the method for preparing a composite binder phase ultra-coarse cemented carbide described in the present invention, wherein: in the step S3, the sintering process is: first, the temperature is raised to 500°C, and the temperature is kept for 60 minutes to complete dewaxing, and the H2 flow rate is 80-120L / min; then the temperature is raised to 650°C, and the temperature is kept for 60-90 minutes, and then the temperature is raised to 950°C, and the temperature is kept for 60 minutes to end the pre-sintering stage; finally, the temperature is raised to the liquid phase sintering temperature of 1450-1480°C, and the temperature is kept for 60-120 minutes, and the furnace is filled with argon and pressurized to 5-10MPa, and the composite binder phase coarse cemented carbide is obtained after cooling with the furnace.

[0018] To solve the above technical problem, according to another aspect of the present invention, the present invention provides the following technical solution:

[0019] A composite bonding phase ultra-coarse cemented carbide is prepared by adopting the above-mentioned composite bonding phase ultra-coarse cemented carbide preparation method.

[0020] As a preferred embodiment of the composite binder phase ultra-coarse cemented carbide of the present invention, wherein: the WC grains of the composite binder phase ultra-coarse cemented carbide are evenly distributed, the average grain size is 5.5-7.5 μm, the bending strength is ≥2350 MPa, and the Vickers hardness is ≥1050 kgf / mm 2 .

[0021] The beneficial effects of the present invention are as follows:

[0022] The present invention proposes a composite binder phase ultra-coarse cemented carbide and a preparation method thereof. NiO is refined by high-energy ball milling and evenly distributed in the composite powder. Light ball milling is selected for secondary ball milling to maintain the dominance of coarse WC grains, so that the ultra-fine NiO-WO3-C composite powder is evenly attached to the coarse WC grains. Subsequently, during the sintering process, NiO is in-situ converted into fine-grained and evenly distributed Ni, reducing the possibility of Ni pool formation due to Ni agglomeration during the sintering stage. The highly active ultra-fine WC generated by the WO3 reaction quickly dissolves in the composite binder phase with a solubility greater than Co, and then precipitates on the dominant coarse WC grains, promoting the growth and development of WC grains. The WC grains of the composite binder phase ultra-coarse cemented carbide prepared by this process are evenly distributed and fully developed, and the alloy has good mechanical properties, the average WC grain size is 5.5-7.5μm, the bending strength is ≥2350MPa, and the Vickers hardness is ≥1050kgf / mm 2 . BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.

[0024] Figure 1 This is a picture of the cemented carbide prepared in Example 1 of the present invention.

[0025] Figure 2 This is a picture of the cemented carbide prepared in Example 2 of the present invention.

[0026] Figure 3 This is a picture of the cemented carbide prepared in Example 3 of the present invention.

[0027] Figure 4 This is a picture of the cemented carbide prepared in Comparative Example 1 of the present invention.

[0028] Figure 5 This is a picture of the cemented carbide prepared in Comparative Example 2 of the present invention.

[0029] Figure 6 This is a picture of the cemented carbide prepared in Comparative Example 3 of the present invention.

[0030] Figure 7 This is a picture of the cemented carbide prepared in Comparative Example 4 of the present invention.

[0031] Figure 8 This is a picture of the cemented carbide prepared in Comparative Example 5 of the present invention.

[0032] Fig. 9 This is a picture of the cemented carbide prepared in Comparative Example 6 of the present invention.

[0033] Fig.10 This is a picture of the cemented carbide prepared in Comparative Example 7 of the present invention.

[0034] Fig.11 This is a picture of the cemented carbide prepared in Comparative Example 8 of the present invention.

[0035] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0036] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] The present invention provides a composite binder phase ultra-coarse cemented carbide and a preparation method thereof, which has the following advantages:

[0038] (1) Plastic nickel is changed into brittle NiO, and two ball milling processes are used. The first high-energy ball milling refines NiO and makes it evenly distributed in the composite powder. The second ball milling selects light ball milling to maintain the dominance of coarse WC grains, so that the ultrafine NiO-WO3-C composite powder is evenly attached to the coarse WC grains. Subsequently, during the sintering process, NiO is in situ converted into fine-grained and evenly distributed Ni, reducing the possibility of Ni pool formation due to Ni agglomeration during the sintering stage. The highly active ultrafine WC generated by the WO3 reaction quickly dissolves in the composite binder phase with a solubility greater than Co, and then precipitates on the dominant coarse WC grains, promoting the growth and development of WC grains. The problem of agglomeration caused by insufficient ball milling after Ni addition and the agglomeration of Ni during liquid phase sintering due to poor wettability of Ni / WC are solved, as well as the problem of agglomeration of ultrafine WC grains in the preparation of ultra-coarse cemented carbide by ultrafine WC dissolution method, which affects the uneven distribution of WC grains;

[0039] (2) By optimizing the sintering process, WO3 and NiO are transformed into dispersed high-activity WC and Ni in situ before sintering densification, which promotes the preparation of high-performance ultra-coarse cemented carbide.

[0040] (3) Since the solubility of WC in Ni is greater than that in Co, the ultrafine WC generated by the reaction immediately dissolves in the Ni generated in situ, and then precipitates on the coarse WC grains, promoting the growth of WC grains and making the coarse WC grains grow fully.

[0041] According to one aspect of the present invention, the present invention provides the following technical solution:

[0042] A method for preparing a composite binder phase ultra-coarse cemented carbide comprises the following steps:

[0043] S1, taking carbon powder, NiO powder and WO3 powder, and subjecting them to high-energy ball milling to obtain ultrafine NiO-WO3-C composite powder with an average particle size of less than 0.3 μm;

[0044] S2, taking ultrafine NiO-WO3-C composite powder and WC, Co powder and ball milling to obtain WC-Co-NiO-WO3-C composite powder;

[0045] The S3 and WC-Co-NiO-WO3-C composite powders are pressed into compacts and then sintered using a hydrogen sintering process to obtain a composite bonding phase ultra-coarse cemented carbide.

[0046] Preferably, in step S1, the mass ratio of carbon powder, NiO powder and WO3 powder is (12-18):(30-50):(32-58).

[0047] Preferably, in step S1, the ball milling speed is 350-500 r / min, the ball milling time is 12-48 h, the ball-to-material ratio is (8-10):1, and the ball milling medium is alcohol.

[0048] Preferably, in step S1, after the ball milling is completed, the NiO-WO3-C composite powder is dried at a temperature of 80 to 120°C and a drying time of 1 to 5 hours.

[0049] Preferably, in step S2, the mass ratio of NiO-WO3-C composite powder to WC and Co powder is (5-10):(90-95).

[0050] Preferably, in step S2, the Fisher grain size of WC is 12-30 μm.

[0051] Preferably, in step S2, the ball milling speed is 100-350 r / min, the ball milling time is 4-10 h, the ball-to-material ratio is (3-5):1, the ball milling medium is alcohol, and paraffin accounting for 2 wt% of the total mass of the powder is added during ball milling.

[0052] Preferably, in step S2, after the ball milling, the WC-Co-NiO-WO3-C composite powder is dried at a temperature of 80 to 120°C and a drying time of 1 to 3 hours.

[0053] Preferably, in step S3, the sintering process is: first, the temperature is raised to 500°C, and the temperature is kept for 60 minutes to complete dewaxing, and the H2 flow rate is 80-120L / min; then the temperature is raised to 650°C, and the temperature is kept for 60-90 minutes, and then the temperature is raised to 950°C, and the temperature is kept for 60 minutes to end the pre-sintering stage; finally, the temperature is raised to the liquid phase sintering temperature of 1450-1480°C, and the temperature is kept for 60-120 minutes. The furnace is filled with argon and pressurized to 5-10MPa, and a composite bonding phase coarse cemented carbide is obtained after cooling with the furnace.

[0054] According to another aspect of the present invention, the present invention provides the following technical solution:

[0055] A composite bonding phase ultra-coarse cemented carbide is prepared by adopting the above-mentioned composite bonding phase ultra-coarse cemented carbide preparation method.

[0056] Preferably, the WC grains of the composite binder phase ultra-coarse cemented carbide are evenly distributed, the average grain size is 5.5-7.5 μm, the bending strength is ≥2350 MPa, and the Vickers hardness is ≥1050 kgf / mm 2 .

[0057] The technical solution of the present invention is further described below in conjunction with specific embodiments.

[0058] Example 1

[0059] A method for preparing a composite binder phase ultra-coarse cemented carbide comprises the following steps:

[0060] S1. Take carbon powder, NiO powder and WO3 powder and perform high-energy ball milling to obtain ultrafine NiO-WO3-C composite powder; the mass ratio of carbon powder, NiO powder and WO3 powder is 13:30:57; the ball milling speed is 350r / min, the ball milling time is 12h, the ball-to-material ratio is 8:1, and the ball milling medium is alcohol; after the ball milling, the NiO-WO3-C composite powder is dried at a drying temperature of 100℃ and a drying time of 3h.

[0061] S2. Take ultrafine NiO-WO3-C composite powder and WC-Co powder for ball milling to obtain WC-Co-NiO-WO3-C composite powder; the mass ratio of NiO-WO3-C composite powder to WC-Co powder is 5:95; according to the composition of the composite binder phase cemented carbide, which is WC-8 (Co, Ni), a specific WC-Co powder is selected, the Fisher particle size of WC is 12μm, the ball milling speed is 200r / min, the ball milling time is 6h, the ball-to-material ratio is 3:1, the ball milling medium is alcohol, and 2wt% of paraffin wax accounting for the total mass of the powder is added during ball milling. After the ball milling, the WC-Co-NiO-WO3-C composite powder is dried at a drying temperature of 100°C and a drying time of 1h.

[0062] The S3 and WC-Co-NiO-WO3-C composite powders were pressed and sintered using a hydrogen sintering process. The sintering process was as follows: first, the temperature was raised to 500°C and kept for 60 minutes to complete dewaxing, with a H2 flow rate of 100L / min; then the temperature was raised to 650°C and kept for 60 minutes, and then the temperature was raised to 950°C and kept for 60 minutes to end the pre-sintering stage; finally, the temperature was raised to the liquid phase sintering temperature of 1470°C and kept for 60 minutes. The furnace was filled with argon and pressurized to 5MPa, and a composite bonding phase coarse cemented carbide was obtained after cooling with the furnace.

[0063] The picture of the composite binder phase rough cemented carbide obtained in this embodiment is as follows Figure 1 As shown, its WC grains are coarse, the average grain size reaches 5.5μm, the WC grains are evenly distributed, the bending strength reaches 2617.43MPa, and the Vickers hardness reaches 1089kgf / mm 2 .

[0064] Example 2

[0065] A method for preparing a composite binder phase ultra-coarse cemented carbide comprises the following steps:

[0066] S1. Take carbon powder, NiO powder and WO3 powder and perform high-energy ball milling to obtain ultrafine NiO-WO3-C composite powder; the mass ratio of carbon powder, NiO powder and WO3 powder is 15:50:35; the ball milling speed is 400r / min, the ball milling time is 24h, the ball-to-material ratio is 10:1, and the ball milling medium is alcohol; after the ball milling, the NiO-WO3-C composite powder is dried at a drying temperature of 100℃ and a drying time of 3h.

[0067] S2. Take ultrafine NiO-WO3-C composite powder and WC-Co powder for ball milling to obtain WC-Co-NiO-WO3-C composite powder; the mass ratio of NiO-WO3-C composite powder to WC-Co powder is 5:95; according to the composition of the composite binder phase cemented carbide, which is WC-8 (Co, Ni), a specific WC-Co powder is selected, the Fisher particle size of WC is 12μm, the ball milling speed is 200r / min, the ball milling time is 4h, the ball-to-material ratio is 3:1, the ball milling medium is alcohol, and 2wt% of paraffin wax accounting for the total mass of the powder is added during ball milling. After the ball milling, the WC-Co-NiO-WO3-C composite powder is dried at a drying temperature of 100°C and a drying time of 1h.

[0068] The S3 and WC-Co-NiO-WO3-C composite powders were pressed and sintered using a hydrogen sintering process. The sintering process was as follows: first, the temperature was raised to 500°C and kept for 60 minutes to complete dewaxing, with a H2 flow rate of 100L / min; then the temperature was raised to 650°C and kept for 90 minutes, then the temperature was raised to 950°C and kept for 60 minutes to end the pre-sintering stage; finally, the temperature was raised to the liquid phase sintering temperature of 1470°C and kept for 60 minutes, and the furnace was filled with argon and pressurized to 5MPa, and a composite bonding phase coarse cemented carbide was obtained after cooling with the furnace.

[0069] The picture of the composite binder phase rough cemented carbide obtained in this embodiment is as follows Figure 2 As shown, its WC grains are coarse, the average grain size reaches 6.0μm, the WC grains are evenly distributed, the bending strength reaches 2463.65MPa, and the Vickers hardness reaches 1063kgf / mm 2 .

[0070] Example 3

[0071] A method for preparing a composite binder phase ultra-coarse cemented carbide comprises the following steps:

[0072] S1. Take carbon powder, NiO powder and WO3 powder and perform high-energy ball milling to obtain ultrafine NiO-WO3-C composite powder; the mass ratio of carbon powder, NiO powder and WO3 powder is 15:50:35; the ball milling speed is 400r / min, the ball milling time is 24h, the ball-to-material ratio is 10:1, and the ball milling medium is alcohol; after the ball milling, the NiO-WO3-C composite powder is dried at a drying temperature of 100℃ and a drying time of 3h.

[0073] S2. Take ultrafine NiO-WO3-C composite powder and WC-Co powder for ball milling to obtain WC-Co-NiO-WO3-C composite powder; the mass ratio of NiO-WO3-C composite powder to WC-Co powder is 10:90; according to the composition of the composite binder phase cemented carbide, which is WC-8 (Co, Ni), a specific WC-Co powder is selected, the Fisher particle size of WC is 30μm, the ball milling speed is 250r / min, the ball milling time is 8h, the ball-to-material ratio is 3:1, the ball milling medium is alcohol, and 2wt% of paraffin wax accounting for the total mass of the powder is added during ball milling. After the ball milling, the WC-Co-NiO-WO3-C composite powder is dried at a drying temperature of 100°C and a drying time of 1h.

[0074] The S3 and WC-Co-NiO-WO3-C composite powders were pressed and sintered using a hydrogen sintering process. The sintering process was as follows: first, the temperature was raised to 500°C and kept for 60 minutes to complete dewaxing, with a H2 flow rate of 100L / min; then the temperature was raised to 650°C and kept for 90 minutes, then the temperature was raised to 950°C and kept for 60 minutes to end the pre-sintering stage; finally, the temperature was raised to the liquid phase sintering temperature of 1470°C and kept for 90 minutes. The furnace was filled with argon and pressurized to 9MPa, and a composite bonding phase coarse cemented carbide was obtained after cooling with the furnace.

[0075] The picture of the composite binder phase rough cemented carbide obtained in this embodiment is as follows Figure 3 As shown, its WC grains are coarse, the average grain size reaches 7.5μm, the WC grains are evenly distributed, the bending strength reaches 2357.84MPa, and the Vickers hardness reaches 1056kgf / mm 2 .

[0076] Comparative Example 1

[0077] The difference from Example 1 is that in step S1, the mass ratio of carbon powder, NiO powder and WO3 powder is 18.5:30:51.5.

[0078] The picture of the cemented carbide obtained in this comparative example is as follows Figure 4As shown, carburization occurs, and there are many abnormally grown grains. The uniformity of WC distribution is poor, the average grain size is 7.5μm, the bending strength is 1837.52MPa, and the Vickers hardness is 1013kgf / mm 2 .

[0079] Comparative Example 2

[0080] The difference from Example 1 is that step S1 is not performed, and ultrafine WC is used in step S2 instead of ultrafine NiO-WO3-C composite powder.

[0081] The picture of the cemented carbide obtained in this comparative example is as follows Figure 5 As shown, the average grain size of WC reaches 4.5μm, there is agglomeration of ultrafine WC grains and some abnormally grown grains, and the WC grain distribution is non-uniform. The bending strength is 2237.71MPa and the Vickers hardness is 1073kgf / mm 2 .

[0082] Comparative Example 3

[0083] The difference from Example 1 is that WC powder is used to replace WO3 powder in step S1.

[0084] The picture of the cemented carbide obtained in this comparative example is as follows Figure 6 As shown, the average grain size of WC reaches 4.5 μm, the agglomeration of ultrafine WC grains is reduced, the WC grain distribution is more uniform than that of comparative example 2, the bending strength is 2301.12 MPa, and the Vickers hardness is 1053 kgf / mm 2 .

[0085] Comparative Example 4

[0086] The difference from Example 1 is that Co3O4 powder is used to replace NiO powder in step S1.

[0087] The picture of the cemented carbide obtained in this comparative example is as follows Figure 7 As shown, the average grain size of WC reaches 4.5 μm, a small amount of ultrafine WC grains agglomerate, and the grain distribution uniformity is inferior to that of Example 1. The bending strength is 2236.89 MPa and the Vickers hardness is 1078 kgf / mm 2 .

[0088] Comparative Example 5

[0089] The difference from Example 1 is that Ni powder is used to replace NiO powder in step S1.

[0090] The picture of the cemented carbide obtained in this comparative example is as follows Figure 8As shown, the average grain size of WC reaches 5.0 μm, a small amount of ultrafine WC grains agglomerate, and the grain distribution uniformity is inferior to that of Example 1. The bending strength is 2231.59 MPa and the Vickers hardness is 1064 kgf / mm 2 .

[0091] Comparative Example 6

[0092] The difference from Example 1 is that in step S2, the mass ratio of NiO-WO3-C composite powder to WC-Co powder is 20:80.

[0093] The picture of the cemented carbide obtained in this comparative example is as follows Fig. 9 As shown in the figure, the average grain size of WC reaches 7.5μm, there are many abnormally grown grains, the grain distribution uniformity is poor, the bending strength is 2137.24MPa, and the Vickers hardness is 1011kgf / mm 2 .

[0094] Comparative Example 7

[0095] The difference from Example 1 is that in step S2, the mass ratio of NiO-WO3-C composite powder to WC-Co powder is 2:98.

[0096] The picture of the cemented carbide obtained in this comparative example is as follows Fig.10 As shown, the average grain size of WC reaches 3.5μm, there are many ultrafine WC grains, and the grain distribution is non-uniform. The bending strength is 2410.59MPa and the Vickers hardness is 1118kgf / mm 2 .

[0097] Comparative Example 8

[0098] The difference from Example 1 is that WO3 powder is not added in step S1.

[0099] The picture of the cemented carbide obtained in this comparative example is as follows Fig.11 As shown in the figure, the average grain size of WC reaches 2.9μm, with more fine grains, and the proportion of WC grains in the balanced morphology is small. The bending strength is 2134.52MPa and the Vickers hardness is 1183kgf / mm 2 .

[0100] Comparative Example 9

[0101] The difference from Example 1 is that in step S3, "then heat to 950°C, keep warm for 60 minutes, and end the pre-sintering stage" is used to replace "then heat to 650°C, keep warm for 60 to 90 minutes, then heat to 950°C, keep warm for 60 minutes, and end the pre-sintering stage".

[0102] In this comparative example, since the heating rate in the process of reaching 950° C. is too fast, WO3 cannot be fully reduced and carbonized, and a decarburized phase exists in the obtained cemented carbide.

[0103] It can be seen from the above embodiments and comparative examples that the present invention refines NiO through high-energy ball milling and makes it evenly distributed in the composite powder, and selects light ball milling for the secondary ball milling to maintain the advantage of coarse WC grains, so that the ultrafine NiO-WO3-C composite powder is evenly attached to the coarse WC grains. Subsequently, during the sintering process, NiO is converted into fine-grained and evenly distributed Ni in situ, reducing the possibility of Ni pool formation due to Ni agglomeration during the sintering stage. The highly active ultrafine WC generated by the WO3 reaction quickly dissolves in the composite binder phase with a solubility greater than Co, and then precipitates on the dominant coarse WC grains, promoting the growth and development of WC grains. The composite binder phase ultra-coarse cemented carbide WC grains prepared by this process are evenly distributed and fully developed, and the alloy has good mechanical properties, the average WC grain size is 5.5-7.5μm, the bending strength is ≥2350MPa, and the Vickers hardness is ≥1050kgf / mm 2 .

[0104] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.

Claims

1. A method for preparing a composite binder phase ultra-coarse cemented carbide, characterized in that: The steps include: S1, taking carbon powder, NiO powder and WO3 powder, and subjecting them to high-energy ball milling to obtain ultrafine NiO-WO3-C composite powder with an average particle size of less than 0.3 μm; S2, taking ultrafine NiO-WO3-C composite powder and WC, Co powder and ball milling to obtain WC-Co-NiO-WO3-C composite powder; The S3 and WC-Co-NiO-WO3-C composite powders are pressed into a green compact and then sintered using a hydrogen sintering process to obtain a composite bonding phase ultra-coarse cemented carbide.

2. The method for preparing a composite binder phase ultra-coarse cemented carbide according to claim 1, characterized in that: In the step S1, the mass ratio of carbon powder, NiO powder and WO3 powder is (12-18):(30-50):(32-58).

3. The method for preparing a composite binder phase ultra-coarse cemented carbide according to claim 1, characterized in that: In the step S1, the ball milling speed is 350-500 r / min, the ball milling time is 12-48 h, the ball-to-material ratio is (8-10):1, and the ball milling medium is alcohol.

4. The method for preparing a composite binder phase ultra-coarse cemented carbide according to claim 1, characterized in that: In the step S1, after the ball milling is completed, the NiO-WO3-C composite powder is dried at a temperature of 80 to 120°C for a drying time of 1 to 5 hours.

5. The method for preparing a composite binder phase ultra-coarse cemented carbide according to claim 1, characterized in that: In the step S2, the mass ratio of the NiO-WO3-C composite powder to the WC and Co powders is (5-10):(90-95).

6. The method for preparing a composite binder phase ultra-coarse cemented carbide according to claim 1, characterized in that: In the step S2, the Fisher grain size of WC is 12-30 μm.

7. The method for preparing a composite binder phase ultra-coarse cemented carbide according to claim 1, characterized in that: In step S2, the ball milling speed is 100-350 r / min, the ball milling time is 4-10 h, the ball-to-material ratio is (3-5):1, the ball milling medium is alcohol, and paraffin accounting for 2 wt% of the total mass of the powder is added during ball milling.

8. The method for preparing a composite binder phase ultra-coarse cemented carbide according to claim 1, characterized in that: In the step S2, after the ball milling is completed, the WC-Co-NiO-WO3-C composite powder is dried at a temperature of 80 to 120°C and a drying time of 1 to 3 hours.

9. The method for preparing a composite binder phase ultra-coarse cemented carbide according to claim 1, characterized in that: In the step S3, the sintering process is: first, the temperature is raised to 500°C, and the temperature is kept for 60 minutes to complete dewaxing, and the H2 flow rate is 80-120L / min; then the temperature is raised to 650°C, and the temperature is kept for 60-90 minutes, and then the temperature is raised to 950°C, and the temperature is kept for 60 minutes to end the pre-sintering stage; finally, the temperature is raised to the liquid phase sintering temperature of 1450-1480°C, and the temperature is kept for 60-120 minutes. The furnace is filled with argon and pressurized to 5-10MPa, and a composite bonding phase coarse cemented carbide is obtained after cooling with the furnace.

10. A composite binder phase ultra-coarse cemented carbide, prepared by the preparation method of the composite binder phase ultra-coarse cemented carbide according to any one of claims 1 to 9, wherein the WC grains of the composite binder phase ultra-coarse cemented carbide are uniformly distributed, the average grain size is 5.5 to 7.5 μm, the bending strength is ≥2350 MPa, and the Vickers hardness is ≥1050 kgf / mm 2 .

Citation Information

Cited By

  • Ball milling process for ultra-coarse hard alloy

    CN120170090A