Machining method for improving performance of fractured clamp
By adopting multi-axis linked CNC machine tools, laser processing and heat treatment technology in the processing of expansion and breakage fixtures, combined with electroplating and nitriding treatment, the problem of high fixture wear and scrap rate in the processing of expansion and breakage links is solved, and higher processing is achieved Extended quality and service life, reducing production costs.
Patent Information
- Application Number
- CN202411042646.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-12
AI Technical Summary
During the cracking process of the expansion link, there are problems such as large slag drop at the cracking position, inclined cracks, excessive flatness of the expansion section, wear and even breakage of the fixture, resulting in a reduced service life of the equipment and a high product waste rate, affecting the normality of the manufacturing department Production and increase costs.
The multi-axis linked CNC machine tool is used for semi-finishing, combined with laser processing, vacuum heat treatment, quenching, tempering and electroplating hard chromium treatment, and nitriding and carburizing of the moving sleeve and fixed sleeve to improve the fixture Hardness, wear resistance and stability ensures precise assembly and high-quality processing of parts.
By improving the hardness and wear resistance of the fixture, extending its service life, reducing waste rate, ensuring the accuracy of cracking position and the flatness of the swelling section, reducing production costs, improving production efficiency and enterprise competitiveness.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of expansion-fracture clamp processing, and in particular to a processing method for improving the performance of the expansion-fracture clamp. Background Art
[0002] Accurately machining the mating surfaces of split parts and combining them accurately has always been a difficult problem in the field of mechanical machining. The expansion and breaking process makes accurate matching possible. It is a revolutionary new processing technology in the field of split parts processing. It has the characteristics of fewer processing steps, high manufacturing precision, energy saving and consumption reduction, and reduced production costs. It has been rapidly applied to the production of engine connecting rods, etc. In recent years, with the development of the world's automobile industry and market competition, the application of this technology in the processing of engine cylinder crankshaft holes has become the focus of research in the foreign automobile industry. The expansion and breaking processing technology of split parts utilizes the fracture characteristics of the material, symmetrically processes two expansion and breaking grooves on the inner side of the cylindrical hole of the part to form an initial fracture source, and then applies a normal stress perpendicular to the predetermined fracture surface to cause the split parts to brittlely fracture at the fracture source into a body and a cover.
[0003] During the cracking process of the expansion-breaking connecting rod, there is a large amount of slag at the cracking position, the crack is tilted, the flatness of the expansion section is out of tolerance, the fixture is worn or even broken, the service life of the equipment is reduced, the processing quality is seriously affected, and the product scrap rate remains high, which seriously affects the normal production of the manufacturing department and increases costs. Therefore, this application proposes a processing method to improve the performance of the expansion-breaking fixture. Summary of the invention
[0004] The purpose of the present invention is to propose a processing method for improving the performance of a breaking fixture in order to solve the problem that the product scrap rate remains high during the breaking connecting rod cracking processing in the background technology.
[0005] The technical solution of the present invention is a processing method for improving the performance of a breaking fixture, comprising the following steps:
[0006] S1, semi-finishing:
[0007] Use multi-axis linkage CNC machine tools to process the expansion and breaking fixtures, select tool diameters between 0.5-1mm, cutting speeds between 50-100m / min, increase the flow and pressure of the coolant, and reduce heat accumulation;
[0008] S2. Expansion groove processing: laser processing of expansion groove, the depth is between 0.5-1mm;
[0009] S3. Heat treatment:
[0010] S301. The fixture is placed in a vacuum heat treatment furnace, and vacuum heat treatment is performed to heat the fixture to 1000-1100°C to transform its internal structure into austenite;
[0011] S302. Quenching: The workpiece is rapidly cooled by water, and the quenching temperature is between 850-950℃;
[0012] S303. Tempering: Tempering is performed by heating the workpiece, and the tempering temperature is between 200-400°C;
[0013] S304. Cooling: Cool the workpiece naturally to room temperature;
[0014] S4, pull rod processing: use a grinder to grind the pull rod surface, and then use a polishing machine to polish the pull rod surface;
[0015] The tie rod is placed in an electroplating tank for hard chrome electroplating, and then heat treated. The tie rod is placed in a tempering furnace for tempering at 200-300°C for 1-2 hours;
[0016] S5, the movable sleeve and the fixed sleeve are carburized, including:
[0017] S501. The movable sleeve and the fixed sleeve are placed in a heating furnace for preheating at a temperature of 300-400°C;
[0018] S502. The preheated movable sleeve and fixed sleeve are placed in a nitriding furnace for nitriding treatment at a temperature of 500-600°C for 2-4 hours;
[0019] S503. The nitrided movable sleeve and fixed sleeve are placed in a tempering furnace for stress relief annealing;
[0020] S504. The movable sleeve and the fixed sleeve are carburized at a temperature of 900-950°C for 2-4 hours;
[0021] S6. Assemble, assemble the processed pull rod, movable sleeve and fixed sleeve onto the fixture to obtain the expansion and breaking fixture.
[0022] Optionally, in step S1, the coolant flow rate is between 10-20 L / min, and the pressure is between 1-2 MPa.
[0023] Optionally, in step S2, the power of the laser processing is between 100-500 W, and the scanning speed is between 500-1000 mm / s.
[0024] Optionally, in step S301, the vacuum degree of the vacuum heat treatment is 10 -3 -10 -5 Between Pa.
[0025] Optionally, in step S4, the polishing surface roughness is between Ra0.2-0.4 μm.
[0026] Optionally, in step S4, the thickness of the electroplating layer is between 0.05-0.1 mm.
[0027] Optionally, in step S502, the preheated movable sleeve and fixed sleeve are placed in a nitriding furnace for nitriding treatment at a temperature of 550° C. for 3 hours.
[0028] Optionally, in step S502, the thickness of the nitride layer is 0.2-0.3 mm.
[0029] Optionally, in step S503, the annealing temperature is 500-600° C. and the time is 2-4 hours.
[0030] Optionally, in step S505, the carburizing treatment is performed at a temperature of 925° C. for 3 hours.
[0031] Compared with the prior art, the present invention has the following beneficial technical effects:
[0032] 1. Improve the service life of the fixture: By increasing the hardness and wear resistance, the wear and damage of the fixture can be reduced and its service life can be extended. Reduce the scrap rate: Precise processing and quality control can improve the reliability and stability of the fixture, thereby reducing the generation of scrap during the expansion and breaking process.
[0033] 2. Improve processing quality: Good fixture performance can ensure that the cracking position of the parts is accurate, the cracks are neat, and the flatness of the expanded section meets the requirements, thereby improving the processing quality of the product. By nitriding the movable and fixed sleeves of the expansion fixture, and electroplating the working surface of the pull rod of the expansion fixture with hard chrome, the hardness is increased, and then the surface is ground to meet the process requirements, so as to reduce friction during work and increase its wear resistance. Reducing the damage and maintenance frequency of the fixture can reduce downtime and improve the production efficiency of the workshop. Extending the service life of the fixture and reducing the scrap rate can reduce production costs and improve the competitiveness of the enterprise.
[0034] The present invention greatly reduces the wear and damage of the clamp, prolongs its service life, and simultaneously reduces the generation of waste products in the expansion and breaking process, thereby improving production efficiency and reducing production costs. DETAILED DESCRIPTION
[0035] The following describes the embodiments of the present invention by specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be noted that the following embodiments and features in the embodiments can be combined with each other without conflict.
[0036] Example 1
[0037] The processing method for improving the performance of the expansion and breaking fixture includes the following steps:
[0038] S1, semi-finishing:
[0039] A multi-axis linkage CNC machine tool is used to process the expansion and breaking fixture. The tool diameter is 0.5mm, the cutting speed is 50m / min, the flow rate and pressure of the coolant are increased, and the heat accumulation is reduced. The coolant flow rate is 10L / min and the pressure is 1MPa.
[0040] S2. Expansion groove processing: laser processing is used to process the expansion groove, the depth is 0.5mm, the power of laser processing is 100W, and the scanning speed is 500mm / s;
[0041] S3. Heat treatment:
[0042] S301. Place the fixture in a vacuum heat treatment furnace and perform vacuum heat treatment at a vacuum degree of 10 -3 Pa, heating the fixture to 1000°C to transform its internal structure into austenite;
[0043] S302. Quenching: The workpiece is rapidly cooled by water, and the quenching temperature is 850°C;
[0044] S303. Tempering: Tempering the workpiece by heating it at a tempering temperature of 200°C;
[0045] S304. Cooling: Cool the workpiece naturally to room temperature;
[0046] S4, pull rod processing: use a grinder to grind the pull rod surface, and then use a polishing machine to polish the pull rod surface, and the polished surface roughness is Ra0.2μm;
[0047] The pull rod is placed in an electroplating tank for hard chrome electroplating, the thickness of the electroplating layer is 0.05 mm, and heat treatment is performed after electroplating. The pull rod is placed in a tempering furnace and tempered at 200°C for 1 hour;
[0048] S5, Movable sleeve and fixed sleeve processing:
[0049] S501. The movable sleeve and the fixed sleeve are placed in a heating furnace for preheating at a temperature of 300°C;
[0050] S502. The preheated movable sleeve and fixed sleeve are placed in a nitriding furnace for nitriding treatment. The thickness of the nitriding layer is 0.2 mm, the nitriding temperature is 500 ° C, and the time is 2 hours;
[0051] S503. The nitrided movable sleeve and fixed sleeve are placed in a tempering furnace for stress relief annealing at a temperature of 500°C for 2 hours;
[0052] S504. The movable sleeve and the fixed sleeve are carburized or carbonitrided at a temperature of 900°C for 2 hours;
[0053] S6. Assemble, assemble the processed pull rod, movable sleeve and fixed sleeve onto the fixture to obtain the expansion and breaking fixture.
[0054] Example 2
[0055] The processing method for improving the performance of the expansion and breaking fixture includes the following steps:
[0056] S1, semi-finishing:
[0057] A multi-axis CNC machine tool was used to process the expansion and breaking fixture. The tool diameter was 0.6 mm, the cutting speed was 60 m / min, the flow rate and pressure of the coolant were increased, and the heat accumulation was reduced. The coolant flow rate was 13 L / min and the pressure was 1.3 MPa.
[0058] S2. Expansion groove processing: laser processing is used to process the expansion groove, the depth is 0.6mm, the power of laser processing is 200W, and the scanning speed is 600mm / s;
[0059] S3. Heat treatment:
[0060] S301. Place the fixture in a vacuum heat treatment furnace and perform vacuum heat treatment at a vacuum degree of 10 -4 Pa, heating the fixture to 1020°C to transform its internal structure into austenite;
[0061] S302. Quenching: The workpiece is quickly cooled by water, and the quenching temperature is 870°C;
[0062] S303. Tempering: Tempering is performed by heating the workpiece at a tempering temperature of 250°C;
[0063] S304. Cooling: Cool the workpiece naturally to room temperature;
[0064] S4, pull rod processing: use a grinder to grind the pull rod surface, and then use a polishing machine to polish the pull rod surface, and the polished surface roughness is Ra0.3μm;
[0065] The pull rod is placed in an electroplating tank for hard chrome electroplating, the thickness of the electroplating layer is 0.06 mm, and heat treatment is performed after electroplating. The pull rod is placed in a tempering furnace and tempered at 230°C for 1.5 hours;
[0066] S5, Movable sleeve and fixed sleeve processing:
[0067] S501. The movable sleeve and the fixed sleeve are placed in a heating furnace for preheating at a temperature of 330°C;
[0068] S502. The preheated movable sleeve and fixed sleeve are placed in a nitriding furnace for nitriding treatment. The thickness of the nitriding layer is 0.23 mm, the nitriding temperature is 530 ° C, and the time is 3 hours;
[0069] S503. The nitrided movable sleeve and fixed sleeve are placed in a tempering furnace for stress relief annealing at a temperature of 530°C for 3 hours;
[0070] S504. The movable sleeve and the fixed sleeve are carburized or carbonitrided at a temperature of 910°C for 3 hours;
[0071] S6. Assemble, assemble the processed pull rod, movable sleeve and fixed sleeve onto the fixture to obtain the expansion and breaking fixture.
[0072] Example 3
[0073] The processing method for improving the performance of the expansion and breaking fixture includes the following steps:
[0074] S1, semi-finishing:
[0075] A multi-axis linkage CNC machine tool is used to process the expansion and breaking fixture. The tool diameter is 0.8mm, the cutting speed is 75m / min, the flow rate and pressure of the coolant are increased, and the heat accumulation is reduced. The coolant flow rate is 15L / min and the pressure is 1.5MPa.
[0076] S2. Expansion groove processing: laser processing is used to process the expansion groove, the depth is 0.8mm, the power of laser processing is 300W, and the scanning speed is 750mm / s;
[0077] S3. Heat treatment:
[0078] S301. Place the fixture in a vacuum heat treatment furnace and perform vacuum heat treatment at a vacuum degree of 10 -4 Pa, heating the fixture to 1050°C to transform its internal structure into austenite;
[0079] S302. Quenching: The workpiece is rapidly cooled by water, and the quenching temperature is 900°C;
[0080] S303. Tempering: Tempering the workpiece by heating it at a temperature of 300°C;
[0081] S304. Cooling: Cool the workpiece naturally to room temperature;
[0082] S4, pull rod processing: use a grinder to grind the pull rod surface, and then use a polishing machine to polish the pull rod surface, and the polished surface roughness is Ra0.3μm;
[0083] The pull rod is placed in an electroplating tank for hard chrome electroplating, the thickness of the electroplating layer is 0.08 mm, and heat treatment is performed after electroplating. The pull rod is placed in a tempering furnace and tempered at a temperature of 250°C for 1.5 hours;
[0084] S5, Movable sleeve and fixed sleeve processing:
[0085] S501. The movable sleeve and the fixed sleeve are placed in a heating furnace for preheating at a temperature of 350°C;
[0086] S502. The preheated movable sleeve and fixed sleeve are placed in a nitriding furnace for nitriding treatment. The thickness of the nitriding layer is 0.25 mm, the nitriding temperature is 550 ° C, and the time is 3 hours;
[0087] S503. The nitrided movable sleeve and fixed sleeve are placed in a tempering furnace for stress relief annealing at a temperature of 550°C for 3 hours;
[0088] S504. The movable sleeve and the fixed sleeve are carburized or carbonitrided at a temperature of 925°C for 3 hours;
[0089] S6. Assemble, assemble the processed pull rod, movable sleeve and fixed sleeve onto the fixture to obtain the expansion and breaking fixture.
[0090] Example 4
[0091] The processing method for improving the performance of the expansion and breaking fixture includes the following steps:
[0092] S1, semi-finishing:
[0093] A multi-axis CNC machine tool is used to process the expansion and breaking fixture. The tool diameter is 0.9 mm, the cutting speed is 90 m / min, the flow rate and pressure of the coolant are increased, and the heat accumulation is reduced. The coolant flow rate is 18 L / min and the pressure is 1.8 MPa.
[0094] S2. Expansion groove processing: laser processing is used to process the expansion groove, the depth is 0.9mm, the power of laser processing is 400W, and the scanning speed is 900mm / s;
[0095] S3. Heat treatment:
[0096] S301. Place the fixture in a vacuum heat treatment furnace and perform vacuum heat treatment at a vacuum degree of 10 -4 Pa, heating the fixture to 1080°C to transform its internal structure into austenite;
[0097] S302. Quenching: The workpiece is quickly cooled by water, and the quenching temperature is 920°C;
[0098] S303. Tempering: Tempering is performed by heating the workpiece at a tempering temperature of 380°C;
[0099] S304. Cooling: Cool the workpiece naturally to room temperature;
[0100] S4, pull rod processing: use a grinder to grind the pull rod surface, and then use a polishing machine to polish the pull rod surface, and the polished surface roughness is Ra0.3μm;
[0101] The tie rod is placed in an electroplating tank for hard chrome electroplating, the thickness of the electroplating layer is 0.08 μm, and heat treatment is performed after electroplating. The tie rod is placed in a tempering furnace and tempered at 280°C for 1.8 hours;
[0102] S5, Movable sleeve and fixed sleeve processing:
[0103] S501. The movable sleeve and the fixed sleeve are placed in a heating furnace for preheating at a temperature of 380°C;
[0104] S502. The preheated movable sleeve and fixed sleeve are placed in a nitriding furnace for nitriding treatment. The thickness of the nitriding layer is 0.28 mm, the nitriding temperature is 580 ° C, and the time is 3 hours;
[0105] S503. The nitrided movable sleeve and fixed sleeve are placed in a tempering furnace for stress relief annealing at a temperature of 590°C for 3 hours;
[0106] S504. The movable sleeve and the fixed sleeve are carburized or carbonitrided at a temperature of 940°C for 3 hours;
[0107] S6. Assemble, assemble the processed pull rod, movable sleeve and fixed sleeve onto the fixture to obtain the expansion and breaking fixture.
[0108] Example 5
[0109] The processing method for improving the performance of the expansion and breaking fixture includes the following steps:
[0110] S1, semi-finishing:
[0111] A multi-axis CNC machine tool is used to process the expansion and breaking fixture. The tool diameter is 1mm, the cutting speed is 100m / min, the flow rate and pressure of the coolant are increased, and the heat accumulation is reduced. The coolant flow rate is 20L / min and the pressure is 2MPa.
[0112] S2. Expansion groove processing: laser processing is used to process the expansion groove, the depth is 1mm, the laser processing power is 500W, and the scanning speed is 1000mm / s;
[0113] S3. Heat treatment:
[0114] S301. Place the fixture in a vacuum heat treatment furnace and perform vacuum heat treatment at a vacuum degree of 10 -5 Pa, heating the fixture to 1100°C to transform its internal structure into austenite;
[0115] S302. Quenching: The workpiece is rapidly cooled by water, and the quenching temperature is 950°C;
[0116] S303. Tempering: Tempering is performed by heating the workpiece at a tempering temperature of 400°C;
[0117] S304. Cooling: Cool the workpiece naturally to room temperature;
[0118] S4, pull rod processing: use a grinder to grind the pull rod surface, and then use a polishing machine to polish the pull rod surface, and the polished surface roughness is Ra0.4μm;
[0119] The pull rod is placed in an electroplating tank for hard chrome electroplating, the thickness of the electroplating layer is 0.1 mm, and heat treatment is performed after electroplating. The pull rod is placed in a tempering furnace and tempered at 300°C for 2 hours;
[0120] S5, Movable sleeve and fixed sleeve processing:
[0121] S501. The movable sleeve and the fixed sleeve are placed in a heating furnace for preheating at a temperature of 400°C;
[0122] S502. The preheated movable sleeve and fixed sleeve are placed in a nitriding furnace for nitriding treatment. The thickness of the nitriding layer is 0.3 mm, the nitriding temperature is 600 ° C, and the time is 4 hours;
[0123] S503. The nitrided movable sleeve and fixed sleeve are placed in a tempering furnace for stress relief annealing at a temperature of 600°C for 4 hours;
[0124] S504. The movable sleeve and the fixed sleeve are carburized or carbonitrided at a temperature of 950°C for 4 hours;
[0125] S6. Assemble, assemble the processed pull rod, movable sleeve and fixed sleeve onto the fixture to obtain the expansion and breaking fixture.
[0126] The present invention adopts a multi-axis linkage CNC machine tool for semi-finishing, which can improve the dimensional accuracy and surface quality of the fixture. By laser processing the expansion and breaking groove, the depth and shape of the groove can be accurately controlled to ensure the expansion and breaking performance of the fixture. During the heat treatment process, the fixture is heated to a high temperature and quickly cooled to transform its internal structure into austenite, and then tempered, which can effectively improve the hardness, strength and toughness of the fixture. Grinding and polishing the pull rod can improve its surface finish and dimensional accuracy; electroplating hard chrome treatment can increase the surface hardness and wear resistance; heat treatment can further improve the toughness and fatigue resistance of the pull rod. Preheating treatment can reduce the deformation of the movable sleeve and fixed sleeve in the subsequent processing process; nitriding treatment can improve the surface hardness and wear resistance; stress relief annealing treatment can eliminate residual stress and improve dimensional stability; carburizing or carbonitriding treatment can further improve wear resistance and fatigue life. Accurately assembling the processed pull rod, movable sleeve and fixed sleeve on the fixture can ensure the overall performance and use effect of the fixture.
[0127] The clamp prepared by the invention reduces the wear and damage of the clamp, prolongs its service life, and reduces the generation of waste products in the expansion and breaking process, thereby improving production efficiency and reducing production costs.
[0128] The above specific embodiments are only several optional embodiments of the present invention. Based on the technical solutions of the present invention and the relevant inspirations of the above embodiments, those skilled in the art can make various alternative improvements and combinations to the above specific embodiments.
Claims
1. A processing method for improving the performance of a breaking fixture, characterized in that: The following steps are involved: S1, semi-finishing: Use a multi-axis linkage CNC machine tool to process the expansion and breaking fixture, select a tool diameter between 0.5-1mm, and a cutting speed between 50-100m / min; S2. Expansion groove processing: laser processing of expansion groove, the depth is between 0.5-1mm; S3. Heat treatment: S301. The fixture is placed in a vacuum heat treatment furnace, and vacuum heat treatment is performed to heat the fixture to 1000-1100°C to transform its internal structure into austenite; S302. Quenching: The workpiece is rapidly cooled by water, and the quenching temperature is between 850-950℃; S303. Tempering: Tempering is performed by heating the workpiece, and the tempering temperature is between 200-400°C; S304. Cooling: Cool the workpiece naturally to room temperature; S4, pull rod processing: use a grinder to grind the pull rod surface, and then use a polishing machine to polish the pull rod surface; The tie rod is placed in an electroplating tank for hard chrome electroplating, and then heat treated. The tie rod is placed in a tempering furnace for tempering at 200-300°C for 1-2 hours; S5, the movable sleeve and the fixed sleeve are carburized, including: S501. The movable sleeve and the fixed sleeve are placed in a heating furnace for preheating at a temperature of 300-400°C; S502. The preheated movable sleeve and fixed sleeve are placed in a nitriding furnace for nitriding treatment at a temperature of 500-600°C for 2-4 hours; S503. The nitrided movable sleeve and fixed sleeve are placed in a tempering furnace for stress relief annealing; S504. The movable sleeve and the fixed sleeve are carburized at a temperature of 900-950°C for 2-4 hours; S6. Assemble, assemble the processed pull rod, movable sleeve and fixed sleeve onto the fixture to obtain the expansion and breaking fixture.
2. A processing method for improving the performance of a breaking fixture according to claim 1, characterized in that: In step S1, the coolant flow rate is between 10-20 L / min, and the pressure is between 1-2 MPa.
3. A processing method for improving the performance of a breaking fixture according to claim 1, characterized in that: In step S2, the power of the laser processing is between 100-500 W, and the scanning speed is between 500-1000 mm / s.
4. A processing method for improving the performance of a breaking fixture according to claim 1, characterized in that: In step S301, the vacuum degree of the vacuum heat treatment is 10 -3 -10 -5 Between Pa.
5. A processing method for improving the performance of a breaking fixture according to claim 1, characterized in that: In the step S4, the polishing surface roughness is between Ra0.2-0.4 μm.
6. A processing method for improving the performance of a breaking fixture according to claim 5, characterized in that: In step S4, the thickness of the electroplating layer is between 0.05-0.1 mm.
7. A processing method for improving the performance of a breaking fixture according to claim 1, characterized in that: The step S502: placing the preheated movable sleeve and fixed sleeve into a nitriding furnace for nitriding treatment at a temperature of 550° C. for 3 hours.
8. A processing method for improving the performance of a breaking fixture according to claim 1, characterized in that: In the step S502, the thickness of the nitride layer is 0.2-0.3 mm.
9. A processing method for improving the performance of a breaking fixture according to claim 1, characterized in that: In the step S503, the annealing temperature is 500-600° C. and the time is 2-4 hours.
10. A processing method for improving the performance of a breaking fixture according to claim 1, characterized in that: In the step S505, the carburizing treatment is performed at a temperature of 925° C. for 3 hours.
Citation Information
Patent Citations
Fracture splitting fixture for natural fracture surface joint surfaces of parts and fracture splitting method of fracture splitting fixture
CN103264291A
Expanding-breaking clamp for machining connecting rod
CN103273299A
A method of manufacturing an article by diffusion bonding and superplastic forming