Preparation method of reticular macromolecular flame-retardant wood material

By growing metal-organic framework materials and bio-based flame retardants in situ on wood to form a network of macromolecular layers, the flammability of wood and the shortcomings of existing flame retardants are solved, achieving environmentally friendly and efficient flame retardant modification and expanding the application fields.

CN118927362APending Publication Date: 2024-11-12BEIJING FORESTRY UNIVERSITY
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411334934.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Wood is flammable, and existing flame retardants have problems such as releasing toxic fumes, reducing mechanical strength when added in large quantities, and easy loss of flame retardants. Existing technologies are difficult to achieve environmentally friendly and efficient flame retardant modification.

Method used

By combining bio-based flame retardants with metal-organic framework materials, a network of macromolecular flame retardant layers is formed on wood materials through in-situ polymerization, thereby improving flame retardant performance.

Benefits of technology

It improves the flame retardant properties of wood materials, reduces the risk of fire, maintains the environmental friendliness and mechanical strength of the materials, and expands the application fields.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a preparation method of a reticular macromolecular flame-retardant wood material, and relates to the field of flame retardance of wood materials. The method comprises the following steps: by taking a wood material as a matrix, pretreating the wood material, preparing a two-dimensional metal node macromolecular material precursor solution, growing or dipping in situ, rinsing the surface, drying and the like. Two-dimensional metal node macromolecules are used as a component 1, and phytic acid, itaconic acid, cyclodextrin, chitosan, furfural, sodium alginate and other bio-based flame retardants are used as a component 2. The flame retardant can be firmly attached to the surface and the interior of the wood material by means of in-situ growth or dipping, the wood material with excellent flame retardance is prepared, and the preparation method can be widely applied to wood materials such as poplar, cedarwood, basswood, pinus koraiensis, fraxinus mandshurica, shaving boards, fiberboards and blockboards. According to the method, the flame retardant property of the wood material is greatly improved, the application field of the wood material is widened, and the method has the characteristics of being environmentally friendly and high in operability and has wide application prospects in the flame retardant field.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a two-dimensional node network macromolecular flame-retardant wood material, in particular to a halogen-free, environmentally friendly flame-retardant wood material. Technical Background

[0002] Wood materials have been widely used in the fields of construction and furniture due to their advantages such as light weight, high strength, easy processing, biodegradability and renewability. With the continuous improvement of people's living standards, the consumption of wood materials is increasing. However, the oxygen index of wood materials is generally lower than 22%, which belongs to the category of flammable materials and has the disadvantage of being flammable when exposed to fire. Once a fire occurs, it will cause immeasurable harm to the safety of life and property of users. Therefore, wood materials represented by wooden floors, wall panels and furniture should have certain flame retardant properties to ensure the safety of life and property of users.

[0003] In view of the disadvantage of wood materials being flammable, flame retardant treatment is used to modify wood materials and improve their fire resistance. Flame retardants include halogen flame retardants, phosphorus flame retardants, metal hydroxide flame retardants, etc. Among them, halogen flame retardants have the problem of releasing toxic fumes during the flame retardant process. For example, CN102152354B uses decabromodiphenylethane to vacuum impregnate poplar wood, but it may release toxic fumes that cause irreversible damage to the human body. Metal hydroxides such as aluminum hydroxide are added to wood materials as flame retardants to achieve the purpose of improving the flame retardant effect, but usually a larger amount of addition is required to achieve a better flame retardant effect. At the same time, there are problems such as easy loss of flame retardants and decreased mechanical strength after addition. Therefore, flame retardant wood materials need to be developed in the direction of environmental protection and better performance.

[0004] Porous multi-node molecules represented by metal-organic framework materials are porous materials that combine metal ions and organic ligands, and are widely used in the fields of adsorption, catalysis, and drug transport. Phytic acid, sodium alginate, chitosan, etc. are natural flame retardants extracted from nature, which have the advantages of being non-toxic and green and environmentally friendly. Using the above two as monomers, metal node network macromolecules are prepared by in-situ polymerization to form a network macromolecular flame retardant layer on the wood material, thereby improving the flame retardant properties of the wood material and achieving the purpose of flame retardancy and catalytic flue gas. The present invention uses bio-based flame retardants and metal-organic framework materials as main components, and the two work together to promote the improvement of the flame retardant properties of wood materials and reduce the risk of fire. Summary of the invention

[0005] In order to overcome the shortcomings of the above-mentioned technologies, the present invention proposes a method for preparing a reticular macromolecular flame-retardant wood material. With bio-based and metal organic framework materials as the main components, the metal organic framework materials and bio-based flame retardants are loaded on the wood material by in-situ growth or high-pressure impregnation, comprising the following steps:

[0006] (1) Preparation of metal organic framework prepolymer: A certain amount of growth regulator and metal salt are dispersed in an organic solvent in sequence, and the resulting solution is stirred and sonicated, which is recorded as solution A. Subsequently, a certain amount of organic ligand is dissolved in an organic solvent, and the resulting solution is stirred and sonicated, which is recorded as solution B. Solution B is poured into solution A to form a metal organic framework material precursor solution, and the above solution is transferred to a polytetrafluoroethylene-lined container, stirred, and then sonicated.

[0007] (2) In-situ polymerization of the organic metal framework material inside the wood material: the organic metal framework prepolymer is transferred to a reactor, and then a wood material with a certain moisture content is added, and a hydrothermal reaction is carried out at a certain temperature for a certain period of time.

[0008] (3) Synthesis of two-dimensional node network macromolecules inside wood: The reactor was cooled to room temperature, the wood material in the reactor was taken out, a certain amount of bio-based flame retardant was added to the solution after the reaction, and the wood material taken out before was added after stirring. The reaction was carried out under certain temperature conditions for a certain time, the reactor was cooled to room temperature, the wood material in the reactor was taken out, and after rinsing with a solvent, the weight was kept at 103°C until there was no significant change.

[0009] Preferably, the metal organic framework material precursor solution in step (1) includes metal salts such as zirconium, zinc, cobalt, nickel, iron, chromium, etc., the organic ligand includes 2-methylimidazole, terephthalic acid, 2-aminoterephthalic acid, etc., the growth regulator includes formic acid, acetic acid, benzoic acid, boric acid, hydrochloric acid, hydrofluoric acid, etc., and the organic solvent includes a mixed solution of N,N-dimethylformamide or N,N-dimethylacetamide. The addition ratio of inorganic metal salt, organic ligand, growth regulator, and organic solvent is (0.1-0.5) g: (0.1-0.5) g: (1-2.5) mL: (30-50) mL.

[0010] Preferably, in step (1), the wood material may be poplar, fir, ash, basswood, paulownia, particle board, fiberboard, plywood, blockboard, etc., and the moisture content of the wood material is 5-50%, preferably 5-12%.

[0011] Preferably, in step (1), the ultrasonic power is 100-1000 W, the ultrasonic time is greater than 30 min, the ultrasonic temperature is 20-40° C., and the ultrasonic frequency is 50-60 Hz; the stirring time is greater than 75 min, the stirring temperature is lower than 40° C., and the stirring speed is 400-900 r / min.

[0012] Preferably, in step (1), the synthesis temperature is 100-120° C., and the synthesis time is 12-24 hours.

[0013] Preferably, in step (2), the bio-based flame retardant is phytic acid, sodium alginate, chitosan, cyclodextrin, tannic acid, etc. For liquid bio-based flame retardants such as phytic acid, the concentration is 30-70%. The added mass ratio of the sum of the mass of the bio-based flame retardant, the metal salt and the organic ligand is 1:10-12.

[0014] Preferably, in step (2), the bio-based flame retardant can be directly added to the metal organic framework material precursor solution in step (1) and synthesized in a one-step method.

[0015] Preferably, the reaction temperature in step (2) is 60-70° C. and the reaction time is 10-12 h.

[0016] Preferably, the solvent for rinsing in step (3) is one or a mixture of N,N-dimethylformamide, methanol, ethanol, deionized water, glycerol, etc., and the number of rinsing is 3 to 10 times. The drying temperature is 80 to 103° C. and the drying time is 8 to 12 hours. DETAILED DESCRIPTION

[0017] In order to better illustrate the technical means and preparation process of the present invention, the present invention is explained below in conjunction with specific implementation cases.

[0018] Embodiment 1:

[0019] (1) Use a sliding table saw to cut out defect-free poplar wood of size 50×10×10 mm, and use a blast drying oven to dry the poplar wood to a moisture content of less than 12% for standby use. Take 0.358g of zirconium tetrachloride and disperse it in 15.2mL N,N-dimethylformamide and 2mL of glacial acetic acid, stir the resulting solution for 20min (200r / min, temperature) and then ultrasonicate for 20min (temperature 25℃, power 240W) to obtain solution A. Subsequently, 0.388g of 2-aminoterephthalic acid was added to 28mL of N,N-dimethylformamide to obtain solution B. The above solution B was added to solution A to obtain a metal organic framework material precursor solution, which was transferred to a polytetrafluoroethylene-lined container, stirred for 15min and then ultrasonicated for 20min (temperature 25℃, power 240W) to obtain solution C. The previously dried poplar wood was added to solution C and transferred to the reactor. At the same time, the hydrothermal reaction was carried out at 120° C. for 24 h.

[0020] (2) The reactor was cooled to room temperature, the reactor was taken out, the poplar wood block in the reactor was taken out, 8 g of phytic acid with a mass fraction of 50% was added to the solution after the reaction, and the mixture was stirred at 25°C and 200 r / min for 120 min and heated at 80°C for 12 h.

[0021] (3) The reactor was cooled to room temperature, the poplar wood in the reactor was taken out, and it was repeatedly rinsed with deionized water for 5 times, and dried at 103° C. for 12 h until the weight no longer changed significantly.

[0022] The LOI value of the network macromolecular flame retardant wood material prepared by the above preparation steps increased from 21% of the control sample to 30.0%, and the residual carbon content increased from 18% to 41.6%, reaching the standard of flame retardant material.

[0023] Embodiment 2:

[0024] (1) 0.358 g zirconium tetrachloride was dispersed in 15.2 mL N,N-dimethylformamide and 2 mL acetic acid, and the resulting solution was stirred for 20 min (200 r / min) and then ultrasonicated for 20 min (temperature 25°C, power 240 W) to obtain solution A. Subsequently, 0.356 g terephthalic acid was added to 28 mL N,N-dimethylformamide to obtain solution B, and the above solution B was added to solution A, and the mixture was transferred to a polytetrafluoroethylene-lined container, stirred for 15 min (200 r / min) and then ultrasonicated for 20 min (temperature 25°C, power 240 W). The above ultrasonicated solution was transferred to a reactor, and defect-free poplar wood with a size of 50×10×10 mm and a moisture content of 5% was added at the same time, and hydrothermally reacted at 120°C for 24 h.

[0025] (2) The reactor was cooled to room temperature, the poplar wood in the reactor was taken out, 8 g of phytic acid with a mass fraction of 50% was added to the solution after the reaction, and the solution was heated at 80° C. for 12 h.

[0026] (3) The reactor was cooled to room temperature, the poplar wood in the reactor was taken out, and the surface of the wood block was rinsed 5 times with N,N-dimethylformamide solution at 80°C until the weight no longer changed significantly.

[0027] The LOI value of the network macromolecular flame retardant wood material prepared by the above preparation steps increased from 21% of the control sample to 28.0%, and the maximum heat release peak and total heat release decreased by 55.9% and 68.6% respectively.

[0028] Example 3

[0029] 0.358 g of zirconium tetrachloride, 0.388 g of 2-aminoterephthalic acid and 8 g of phytic acid were dispersed in 43 mL of N,N-dimethylformamide and 2 mL of glacial acetic acid. The resulting solution was stirred for 20 min (200 r / min), and then ultrasonicated for 20 min (temperature 25°C, power 240 W). Defective poplar wood with a size of 50×10×10 mm and a moisture content of 5% was placed in the solution, and then transferred to a reactor together with the solution and reacted at 120°C for 24 h.

[0030] After the reaction was completed, the mixture was cooled to room temperature, the prepared poplar wood block was taken out, and the surface of the wood block was repeatedly rinsed with methanol solution for 7 times, and then placed in an oven at 80°C to dry to constant weight.

[0031] The LOI value of the network macromolecular flame retardant wood material prepared by the above preparation steps increased from 21% of the control sample to 30.0%, and the residual carbon content increased from 18% to 39%.

[0032] In summary, the present invention improves the flame retardant properties of wood materials by in-situ growth of metal organic framework materials on wood materials, loading metal organic framework materials on the surface and northern pores of wood materials, and bio-based flame retardants. It not only solves the disadvantage of wood materials being flammable, but also overcomes the disadvantage of poor availability of metal organic framework materials due to their amorphous state. The present invention has the advantages of low cost, strong operability, environmental friendliness, and large-scale preparation, which expands the application field of wood materials and provides a new perspective for the functional utilization of wood materials.

[0033] The above describes the specific embodiments of the present invention. However, professionals in the field should understand that the above embodiments are intended to illustrate the principles of the invention, and the present invention is not limited to the specific embodiments. Any technical changes to the present invention are within the scope of protection of the present invention without departing from the technology of the present invention.

Claims

1. A method for preparing a reticular macromolecular flame retardant wood material, comprising the following steps: (1) Preparation of metal organic framework prepolymer: a certain amount of growth regulator and metal salt are dispersed in an organic solvent in turn, and the resulting solution is stirred and sonicated, which is recorded as solution A. Subsequently, a certain amount of organic ligand is dissolved in an organic solvent, and the resulting solution is stirred and sonicated, which is recorded as solution B. Solution B is poured into solution A to form a metal organic framework material precursor solution, and the above solution is transferred to a polytetrafluoroethylene-lined container, stirred and sonicated; (2) In-situ polymerization of the organic metal framework material inside the wood material: the organic metal framework prepolymer is transferred to a reactor, and then a wood material with a certain moisture content is added, and a hydrothermal reaction is carried out at a certain temperature for a certain time; (3) Synthesis of two-dimensional node network macromolecules inside wood: The reactor was cooled to room temperature, the wood material in the reactor was taken out, a certain amount of bio-based flame retardant was added to the solution after the reaction, and the wood material taken out before was added after stirring. The reaction was carried out under certain temperature conditions for a certain time, the reactor was cooled to room temperature, the wood material in the reactor was taken out, and after rinsing with a solvent, the weight was kept at 103°C until there was no significant change; The metal organic framework material precursor solution in step 1 includes one or more mixtures of metal salts such as zirconium, zinc, cobalt, nickel, iron, chromium, etc., one or more mixtures of 2-methylimidazole, terephthalic acid, 2-aminoterephthalic acid organic ligands, and one or more mixtures of formic acid, acetic acid, benzoic acid, boric acid, hydrochloric acid, and hydrofluoric acid growth regulators, and the organic solvent is one or more mixtures of N,N-dimethylformamide or N,N-dimethylacetamide; The addition ratio of the inorganic metal salt, organic ligand, growth regulator and organic solvent in the metal organic framework material precursor solution of step (1) is (0.1-0.5) g: (0.1-0.5) g: (1-2.5) mL: (30-50) mL; The wood material of step (1) is poplar, fir, ash, basswood, paulownia, particle board, fiberboard, plywood, blockboard, and has a moisture content of 5-50%; The ultrasonic power of step (1) is 100-1000W, the ultrasonic time is 1-120min, the ultrasonic temperature is 20-40°C, and the ultrasonic frequency is 50-60Hz; the stirring time is 10-240min, the stirring temperature is 20-30°C, and the stirring speed is 100-900r / min; The reaction temperature of step (1) is 25 to 180° C., and the hydrothermal time is 3 to 96 hours; The bio-based flame retardant in step (2) is one or a mixture of phytic acid, sodium alginate, itaconic acid, cyclodextrin, chitosan, ricinoleic acid, and tannic acid; for liquid bio-based flame retardants, the concentration is 30-70%; the added mass ratio of the sum of the mass of the bio-based flame retardant, the metal salt, and the organic ligand is 1:1-15; The step (2) is heating at 60 to 80° C. for 1 to 24 hours; The solvent used for rinsing in step (3) is one or a mixture of N,N-dimethylformamide, methanol, ethanol, ethylene glycol, propylene glycol, and deionized water, and the number of rinsing times is 3 to 10 times; the drying temperature is 60 to 103° C., and the drying time is 6 to 24 hours.

Citation Information

Cited By

  • Bamboo modification method based on in-situ packaging

    CN119635778A

  • High-temperature-resistant flame-retardant wood composite board and preparation method thereof

    CN122560187A