Compression molding process of thermoplastic carbon fiber composite material / metal hybrid laminated board

By optimizing the molding process parameters, including metal layer surface treatment and transition layer filling, the problem of insufficient bonding strength between thermoplastic carbon fiber composite materials and metal layer is solved, and the mechanical properties and stability of hybrid laminates are significantly improved. It is suitable for aviation High demand areas such as aerospace and automobile industry.

CN118927678APending Publication Date: 2024-11-12BEIJING NAT INNOVATION INST OF LIGHTWEIGHT LTD +1

Patent Information

Application Number
CN202411113637.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the existing molding process, the interface bonding strength between the thermoplastic carbon fiber composite material and the metal layer is insufficient, resulting in material deformation and poor mechanical properties, affecting product quality and performance.

Method used

By optimizing the molding process parameters, including surface treatment of metal layers, filling transition layers, and precise control of temperature and pressure, ensuring accurate alignment and positioning of each layer of materials, using appropriate metals and composite materials, optimizing the stacking design and molding process .

Benefits of technology

It significantly improves the interface combination strength and mechanical properties of thermoplastic carbon fiber composite/metal hybrid laminate, reduces thermal stress and material deformation between the laminates, improves the overall structural strength and durability of the product, and is suitable for high-performance applications.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the field of composite material molding, and provides a compression molding process for a thermoplastic carbon fiber composite material / metal hybrid laminated board, which realizes optimal combination of a composite material and a metal layer and improves the mechanical property and durability of the laminated board by optimizing temperature parameters. The method comprises the following steps: selecting aluminum alloy or stainless steel as a metal layer and carbon fiber prepreg as a composite material layer; according to design requirements, compression molding is carried out after layering and lamination, and temperature setting and control are one of key steps. And placing the laminated structure in a mold, heating to 220-240 DEG C at the rate of 4-8 DEG C / min, keeping the temperature for 30-2 hours, and maintaining the pressure of 3-7 MPa for 10-30 minutes. After curing is completed, nondestructive testing and mechanical property testing are conducted on the laminated board, and the product quality and performance are ensured. The hybrid laminated board produced by the process has the advantages of high strength and light weight, and is suitable for the fields of aerospace, automobile industry and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of composite material molding, and in particular relates to a compression molding process of a thermoplastic carbon fiber composite material / metal hybrid laminate. Background Art

[0002] The combination of composite materials and metal laminates has been widely used in the fields of aerospace and automotive industries. At present, compression molding has gradually become an important molding method for composite / metal hybrid laminates due to its advantages such as high efficiency, low cost and easy automation. During the compression molding process, the resin in the composite material needs to fully flow and infiltrate the fibers at an appropriate temperature, while forming a strong bond with the metal layer. This requires strict control of parameters such as heating temperature, heating rate, holding time, pressure, and pressurization time during the molding process to ensure the best combination and performance of thermoplastic carbon fiber composites and metal layers. If the temperature is not properly controlled, it may lead to incomplete resin curing, resin exudation, carbon fiber filament deviation, interlayer delamination or excessive internal stress of the material, thus affecting the quality and performance of the final product. Therefore, the accuracy and stability of the temperature setting during the compression molding process are crucial to the quality of the final product.

[0003] Therefore, by optimizing the molding process parameters, the bonding effect between the thermoplastic carbon fiber composite material and the metal layer during the molding process is improved, and the mechanical properties and durability of the thermoplastic carbon fiber composite material / metal hybrid laminate are enhanced to meet the needs of high-performance application fields. Summary of the invention

[0004] In view of the problem of insufficient interface bonding strength, the purpose of the present invention is to provide an optimized preparation process for compression molding, which mainly solves the problems of low interface bonding strength, material deformation, poor mechanical properties, etc. of thermoplastic carbon fiber composite materials / metal hybrid laminates caused by improper process during the molding process.

[0005] To achieve the above object, according to one aspect of the present invention, a temperature setting method for improving the quality and mechanical properties of a thermoplastic carbon fiber composite material / metal hybrid laminate is provided, and the process mainly comprises the following steps:

[0006] Step 1: Select appropriate metal and composite materials. The metal layer and the composite layer are laid symmetrically according to performance requirements.

[0007] Step 2: Surface treatment. Clean the surface of the metal layer to ensure that the surface is clean. Grind the surface of the metal layer to increase the roughness, thereby improving the bonding force between the metal layer and the composite material layer.

[0008] Step 3: Lay the transition layer. Use the thermoplastic transition film as a transition layer and lay it evenly on the metal layer combined with the composite layer to further improve the bonding strength between the composite layer and the metal layer. Ensure that the transition layer and the contact surface are completely fitted and free of bubbles.

[0009] Step 4: Layer design and stacking. Design the laying order and structure of composite material layers and metal layers according to usage requirements and mechanical performance requirements; during the stacking process, use fixtures or positioning tools to ensure that each layer of material remains accurately aligned and positioned.

[0010] Step 5: Clean the mold. Clean the mold to ensure that the mold surface is clean and free of debris, and evenly apply release agent on all contact surfaces.

[0011] Step 6: Lay out the layers. Place the appropriately sized laminate structure in the preheated mold, ensuring that each layer of material is positioned accurately in the mold.

[0012] Step 7: Molding and post-processing. Set the molding temperature to 220-240℃ and keep it warm for 30min-2h. Then, pressurize at 3-7MPa for 10-30min and cool naturally to room temperature. Open the mold and take out the molded laminate, making sure not to damage the surface of the laminate; finally, perform necessary post-processing operations, and you can also apply painting or coating as needed to further enhance the durability and aesthetics of the laminate.

[0013] Step 8: Quality inspection. Perform nondestructive testing and mechanical property testing on the cured laminate to check for bubbles, cracks and other defects inside; ensure that the mechanical properties of the laminate meet the design requirements.

[0014] Preferably, the raw material of the composite material layer is PA6 thermoplastic carbon fiber prepreg.

[0015] Preferably, the metal layer is aluminum alloy or stainless steel, and its thickness is between 0.3 and 2.0 mm.

[0016] Preferably, as further preferred, the transition layer is selected as a thermoplastic film, which is determined according to the characteristics of the composite material and the performance requirements of the composite layer.

[0017] Preferably, as further preferred, the heating temperature is set between 220°C and 240°C.

[0018] Preferably, the heating rate of the mold is controlled between 4° C. and 8° C. per minute.

[0019] Preferably, the curing temperature is maintained for 30 minutes to 2 hours, which is determined according to the characteristics of the resin system and the composite material.

[0020] Preferably, the pressure is applied during the period of maintaining the final curing temperature and is maintained between 3 and 7 MPa.

[0021] Preferably, the cooling mode is natural cooling.

[0022] Preferably, alcohol cleaning is used to remove surface dirt and oil to ensure cleanliness.

[0023] Preferably, the quality inspection content is whether there are bubbles, cracks and other defects inside, and the mechanical property inspection is tensile, compression, bending and impact testing.

[0024] By optimizing the molding temperature setting, the quality and performance of the thermoplastic carbon fiber composite material / metal hybrid laminate are improved. Compared with the prior art, the present invention has the following beneficial effects:

[0025] 1. The present invention improves the interface bonding strength: by surface treating the metal layer and selecting an appropriate transition layer, the interface bonding strength between the metal layer and the thermoplastic carbon fiber layer is improved. The optimized molding temperature and pressure settings ensure the full flow and curing of the adhesive, further enhancing the interlayer bonding effect, thereby significantly improving the overall structural strength of the composite material.

[0026] 2. The present invention reduces thermal stress and material deformation between layers: By precisely controlling the molding temperature range and the heat preservation time, the present invention effectively reduces the thermal stress and material deformation problems caused by temperature changes during the molding process. The temperature control during the molding process ensures uniform heating inside the material, and the appropriate cooling rate avoids the internal stress and deformation caused by rapid cooling, ensuring the final dimensional stability and shape accuracy of the product.

[0027] 3. Improved mechanical properties of the present invention: The present invention adopts a hybrid structure model of composite materials / metals. Through reasonable stacking design and molding process, the composite materials have excellent mechanical properties, such as high tensile strength>1200MPa and bending modulus>100GPa. The optimized molding temperature and pressure settings enable the carbon fiber layer and the metal layer to give full play to their respective advantages. The final product shows significant improvements in strength, stiffness and toughness, and is suitable for high-demand application fields such as aerospace and automotive industries. DETAILED DESCRIPTION

[0028] The following examples are used to illustrate the present invention, but they are not intended to limit the scope of the present invention.

[0029] Embodiment 1:

[0030] The present invention provides a technical process of compression molding, and the specific steps are as follows:

[0031] Step 1: Select the appropriate metal and composite material. The metal layer is made of stainless steel, and the thermoplastic carbon fiber prepreg resin is PA6, with a density of 1.13g / cm 3 The laying method is 4 layers of 0° / 90° cross laying. Cut each layer of material into 30×30cm size according to the mold requirements 2 of sheets.

[0032] Step 2: Surface treatment of the contact surface of the metal layer. Improve the surface roughness by grinding, thereby enhancing the bonding force between the metal layer and the composite material layer. Clean the surface of the metal layer with alcohol to ensure that the surface is clean, tidy and free of oil stains.

[0033] Step 3: Lay the transition layer. Choose a thermoplastic film as the transition layer, lay it flat and cover the metal layer that is combined with the composite material layer, and further improve the bonding strength between the composite material layer and the metal layer. Make sure that the transition layer and the contact surface are completely fitted and free of bubbles.

[0034] Step 4: Layer design and stacking. According to the use requirements and mechanical performance requirements, select the laying order and structure of metal-composite-metal structure; ensure that each layer of material is in close contact to avoid gaps and defects; use fixtures or positioning tools to ensure that each layer of material is accurately aligned and positioned during the stacking process.

[0035] Step 5: Mold cleaning and coating. Clean the mold thoroughly to ensure that the surface is clean, free of oil and debris. Then, apply a layer of release agent on the mold surface to ensure that every contact surface is covered to facilitate demolding after molding and increase the success rate of the sample.

[0036] Step 6: Lay out the layers. Place the layered structure of appropriate size in the mold to ensure that each layer of material is accurately positioned in the mold to effectively avoid misalignment between layers.

[0037] Step 7: Molding and post-processing. Raise the temperature to 230°C at a heating rate of 6°C / min, keep it warm for 1h, and then keep it at a pressure of 5MPa for 15min. After cooling naturally to room temperature, open the mold and take out the molded laminate, making sure not to damage the surface of the hybrid laminate; finally, grind the laminate to remove burrs.

[0038] Embodiment 2:

[0039] The present invention provides a technical process of compression molding, and the specific steps are as follows:

[0040] Step 1: Select appropriate metal and composite materials. The metal layer is made of aluminum alloy, and the thermoplastic carbon fiber prepreg resin is PA6, with a density of 1.13g / cm 3The laying method is to lay 5 layers in one direction. Cut each layer of material into 30×30cm according to the mold requirements. 2 of sheets.

[0041] Step 2: Surface treatment of the contact surface of the metal layer. Improve the surface roughness by grinding, thereby enhancing the bonding force between the metal layer and the composite material layer. Clean the surface of the metal layer with alcohol to ensure that the surface is clean, tidy and free of oil stains.

[0042] Step 3: Lay the transition layer. Choose a thermoplastic film as the transition layer, lay it flat and cover the metal layer that is combined with the composite material layer, and further improve the bonding strength between the composite material layer and the metal layer. Make sure that the transition layer and the contact surface are completely fitted and free of bubbles.

[0043] Step 4: Layer design and stacking. According to the use requirements and mechanical performance requirements, select the laying order and structure of metal-composite-metal structure; ensure that each layer of material is in close contact to avoid gaps and defects; use fixtures or positioning tools to ensure that each layer of material is accurately aligned and positioned during the stacking process.

[0044] Step 5: Mold cleaning and coating. Clean the mold thoroughly to ensure that the surface is clean, free of oil and debris. Then, apply a layer of release agent on the mold surface to ensure that every contact surface is covered to facilitate demolding after molding and increase the success rate of the sample.

[0045] Step 6: Lay out the layers. Place the layered structure of appropriate size in the mold to ensure that each layer of material is accurately positioned in the mold to effectively avoid misalignment between layers.

[0046] Step 7: Molding and post-processing. The temperature was raised to 225°C at a heating rate of 6°C / min, kept at that temperature for 1 hour, and then kept at a pressure of 4MPa for 20 minutes. After cooling naturally to room temperature, the mold was opened and the molded laminate was taken out, ensuring that the surface of the hybrid laminate was not damaged; finally, the laminate was polished to remove burrs.

[0047] As an optional embodiment, the preparation method of metal-composite material-metal multilayer hybrid laminate is taken as an example: thermoplastic carbon fiber prepreg is selected as the middle layer, the metal layer is used as the upper layer and the lower layer, and each layer of material is cut according to the mold size. The metal material is polished and cleaned to improve the adhesion of the metal and carbon fiber prepreg, and then the transition layer is covered on the surface, and then the prepared carbon fiber prepreg is laid on the metal material. In the same way, the prepared metal layer is superimposed on the thermoplastic carbon fiber prepreg. The thermoplastic carbon fiber composite material has the advantages of good thermal stability, light bulk density, and high temperature resistance. After special processing, it can be made into a thermoplastic carbon fiber composite board, and the metal of the upper and lower layers has good impact resistance, heat dissipation, corrosion resistance, etc., so that the composite material of the hybrid laminate formed in the end has high strength (tensile strength of 1200MPa to 1500MPa), high stiffness, light weight, excellent corrosion resistance and good thermal stability.

[0048] The composite material of the hybrid laminate of the present invention can achieve the dual effects of high strength and light weight, and has multiple advantages such as excellent corrosion resistance and good thermal stability. It has a wide range of applications and can be used in multiple fields such as aerospace, automobiles, etc.

[0049] The embodiments of the present invention are provided for the purpose of illustration and description. Although the embodiments of the present invention have been shown and described above, it can be understood that the above embodiments are exemplary and cannot be understood as limitations of the present invention. Ordinary technicians in this field can change, modify, replace and deform the above embodiments within the scope of the present invention.

[0050] Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A compression molding method for a thermoplastic carbon fiber composite material / metal hybrid laminate, the preparation method comprising the following steps: Step 1: Select appropriate metal and composite materials. The metal layer and the composite layer are laid symmetrically according to performance requirements. Step 2: Surface treatment of the metal layer. Clean the surface of the metal layer to ensure that the surface is clean. Grind the surface of the metal layer to increase the roughness, thereby improving the bonding force between the metal layer and the composite material layer. Step 3: Lay the transition layer. Use the thermoplastic transition film as a transition layer and lay it evenly on the metal layer combined with the composite layer to further improve the bonding strength between the composite layer and the metal layer. Ensure that the transition layer and the contact surface are completely fitted and free of bubbles. Step 4: Layer design and stacking. Design the laying order of composite material layers and metal layers according to usage requirements and mechanical performance requirements; during the stacking process, use fixtures or positioning tools to ensure that each layer of material remains accurately aligned and positioned. Step 5: Clean the mold. Clean the mold to ensure that the mold surface is clean and free of debris, and evenly apply mold release on all contact surfaces. Step 6: Lay out the layers. Place the appropriately sized laminate structure in the preheated mold, ensuring that each layer of material is positioned accurately in the mold. Step 7: Molding and post-processing. Set the molding temperature to 220-240℃ and keep it warm for 30min-2h. Then, pressurize at 3-7MPa for 10-30min and cool naturally to room temperature. Open the mold and take out the molded laminate, making sure that the surface of the laminate is not damaged; finally, perform post-processing operations such as cutting and grinding, and you can also paint or coat the surface as needed to further enhance the durability and aesthetics of the laminate. Step 8: Quality inspection. Perform nondestructive testing and mechanical property testing on the cured laminate to check for bubbles, cracks and other defects inside; ensure that the mechanical properties of the laminate meet the design requirements. By using the temperature setting method in the above steps, a high-performance thermoplastic carbon fiber composite material / metal hybrid laminate can be prepared, which is suitable for application fields requiring high strength and light weight.

2. The laminate material according to claim 1, characterized in that: The raw material of the composite material layer is PA6 thermoplastic carbon fiber prepreg.

3. The laminate material according to claim 1, characterized in that: The metal layer is made of aluminum alloy or stainless steel, and its thickness is between 0.3 and 2.0 mm.

4. The transition layer between composite material plies as claimed in claim 1, characterized in that: The transition layer is selected as a thermoplastic film.

5. The method for setting temperature during molding according to claim 1, characterized in that The heating temperature is set at 220-240°C.

6. The temperature rise rate setting in the molding process according to any one of claims 1 to 5, characterized in that: The rate of heating of the mold is controlled between 4° C. and 8° C. per minute.

7. The molding heat preservation time according to any one of claims 1 to 5, characterized in that: The molding temperature holding time is 30 minutes to 2 hours, which is determined according to the characteristics of the resin system and the composite material.

8. The working pressure according to any one of claims 1 to 5, characterized in that: The pressure is applied after the end of the holding period and maintained between 3 and 7 MPa.

9. The mold cooling rate according to any one of claims 1 to 5, characterized in that: The cooling mode is natural cooling.

10. The cleaning method for molds and metal materials according to claim 1, characterized in that: Use alcohol cleaning to remove surface dirt and oil to ensure cleanliness.

11. The quality inspection content according to any one of claims 1 to 10, characterized in that: Whether there are bubbles, cracks and other defects inside, the mechanical properties are tested by tensile, compression, bending and impact tests.

Citation Information

Patent Citations

  • Fiber-metal composite laminate, forming die therefor and forming method

    CN109986860A

  • Metal-carbon fiber reinforced plastic composite and method for manufacturing metal-carbon fiber reinforced plastic composite

    US20210024705A1

Cited By

  • Bicycle carbon fiber frame butt joint point reinforced connection process

    CN120422486A